A high-melting-point polyethylene wax and its preparation method

High-melting-point polyethylene wax was prepared by using ligands and a 1,5-cyclooctadiene nickel(II) catalyst, which solved the problems of low melting point and poor thermal stability of traditional polyethylene wax. It achieved high-temperature stability and narrow molecular weight distribution, making it suitable for high-temperature processing and high-precision applications.

CN123106958APending Publication Date: 2026-11-17SHANGHAI INST OF ORGANIC CHEM CHINESE ACAD OF SCI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510635752.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional polyethylene waxes suffer from problems such as low melting point, poor thermal stability, wide molecular weight distribution, and high oil content, making it difficult to meet the needs of high-temperature processing and high-precision applications.

Method used

A catalyst was prepared by reacting a ligand with nickel(II) 1,5-cyclooctadiene to catalyze the polymerization of ethylene under specific conditions. Combined with inert gas protection and filtration to remove impurities, a polyethylene wax with a high melting point, narrow molecular weight distribution, and low oil content was prepared.

Benefits of technology

This study achieves high-temperature stability and a narrow molecular weight distribution in high-melting-point polyethylene wax, making it suitable for high-temperature processing and high-precision applications, reducing costs and improving product purity and performance stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005406603730000021
    Figure BDA0005406603730000021
  • Figure BDA0005406603730000031
    Figure BDA0005406603730000031
  • Figure BDA0005406603730000061
    Figure BDA0005406603730000061
Patent Text Reader

Abstract

This invention discloses a high-melting-point polyethylene wax and its preparation method. Specifically, this invention discloses a high-melting-point, high-thermal-stability polyethylene wax with the following characteristics: (a) white powder, free from visible mechanical impurities; inorganic content <100ppm; metal content <10ppm; (b) melting point of 115-130℃; enthalpy of fusion ≥200J / g; (c) number-average molecular weight of 1000-10000g / mol, molecular weight distribution PDI <3; (d) temperature Td5 ≥300℃ for 5% thermal weight loss; (e) solubility in alkanes: at >90℃, solubility ≥6g / 100mL; and / or (f) oil content <0.1%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polyethylene wax, specifically, this invention relates to a high melting point polyethylene wax and its preparation method. Background Technology

[0002] Polyethylene wax is an important polymer material widely used in plastics processing, coatings, inks, hot melt adhesives, cosmetics, and other fields. Traditional polyethylene waxes typically have melting points below 110℃, making them unsuitable for high-temperature processing environments; their wide molecular weight distribution leads to unstable performance, hindering high-precision machining requirements. Under high-temperature conditions, traditional polyethylene waxes are prone to thermal decomposition, affecting their performance and application range; their high oil content also impacts their purity and application performance.

[0003] Therefore, there is an urgent need in this field to develop polyethylene waxes with higher melting points and more stable performance to meet the requirements of high-precision high-temperature processing. Summary of the Invention

[0004] One object of the present invention is to provide a polyethylene wax with a high melting point, high temperature stability, and narrow molecular weight distribution.

[0005] Another object of the present invention is to provide a method for preparing high melting point polyethylene wax.

[0006] Another object of the present invention is to provide a use for a high melting point polyethylene wax.

[0007] In a first aspect of the present invention, a high-melting-point polyethylene wax is provided, said high-melting-point polyethylene wax having the following characteristics:

[0008] (a) White powder, free from visible mechanical impurities; inorganic content <100ppm; metal content <10ppm;

[0009] (b) Melting point is 115-130℃; enthalpy of fusion is ≥200J / g;

[0010] (c) Number-average molecular weight is 1000-10000 g / mol, and molecular weight distribution PDI < 3;

[0011] (d) Temperature at which 5% of thermal weight loss occurs, Td5 ≥ 300℃;

[0012] (e) Solubility in alkanes: at >90°C, solubility ≥6 g / 100 mL; and / or

[0013] (f) Oil content < 0.1%.

[0014] In another preferred embodiment, the alkane is a high-boiling-range alkane solvent, preferably a high-boiling-range petroleum ether, heptane, or octane.

[0015] In another preferred embodiment, the high-melting-point polyethylene wax has a melting point of 120-130°C and a melting enthalpy of ≥200 J / g.

[0016] In another preferred embodiment, the number-average molecular weight of the high-melting-point polyethylene wax is 1000-5000 g / mol.

[0017] In another preferred embodiment, the number-average molecular weight of the high-melting-point polyethylene wax is 1000-3000 g / mol.

[0018] In another preferred embodiment, the molecular weight distribution of the high-melting-point polyethylene wax is <2.

[0019] In another preferred embodiment, the temperature T at which the high-melting-point polyethylene wax loses 5% of its thermal weight is... d5 ≥330℃.

[0020] In another preferred embodiment, the temperature T at which the high-melting-point polyethylene wax loses 5% of its thermal weight is... d5 ≥340℃; preferably, the temperature T at which the high-melting-point polyethylene wax loses 5% of its thermal weight is... d5 ≥350℃.

[0021] In another preferred embodiment, the high-melting-point polyethylene wax has a particle size distribution of d. 50 ≤100um.

[0022] In another preferred embodiment, the high-melting-point polyethylene wax does not contain non-hydrocarbon compounds, polycyclic aromatic hydrocarbons, sulfur, or phosphorus.

[0023] In another preferred embodiment, the content of non-hydrocarbon compounds, polycyclic aromatic hydrocarbons, sulfur, and phosphorus in the high-melting-point polyethylene wax is <0.001%; ​​more preferably <0.0001%; ​​and even more preferably <0.00001%.

[0024] In another preferred embodiment, the high-melting-point polyethylene wax contains less than 0.08% oil.

[0025] In a second aspect of the present invention, a method for preparing the polyethylene wax described in the first aspect of the present invention is provided, comprising the following steps:

[0026] Polyethylene wax is obtained by catalytic polymerization of ethylene at 40-120°C and 0.5-5.0 MPa ethylene pressure in the presence of a catalyst and a co-catalyst, or in the presence of a catalyst alone; wherein the catalyst is obtained by reacting a ligand with 1,5-cyclooctadiene nickel(II).

[0027] The ligand has the following structure:

[0028]

[0029] Wherein, R is selected from the following groups: hydrogen, -OR1; R1 is selected from C4-C10 straight-chain alkyl, -(CH2CH2O). n -C1-C4 alkyl; n is an integer from 1 to 3.

[0030] In another preferred embodiment, the catalyst is prepared and used immediately.

[0031] In another preferred embodiment, the catalytic polymerization reaction is carried out at 40-120°C.

[0032] In another preferred embodiment, the ethylene pressure in the catalytic polymerization reaction is 0.5-5.0 MPa.

[0033] In another preferred embodiment, the ethylene pressure is 0.5-2.5 MPa.

[0034] In another preferred embodiment, the reaction temperature is 50-110°C.

[0035] In another preferred embodiment, the reaction time is 1-12 hours.

[0036] In another preferred embodiment, the catalytic polymerization reaction is carried out in a solvent selected from the group consisting of toluene, hexane, heptane, octane, or combinations thereof.

[0037] In another preferred embodiment, the catalyst is prepared by the following method:

[0038] Under inert gas protection, the ligand and 1,5-cyclooctadiene nickel(II) are placed in a solvent and stirred for 10-60 minutes to obtain a catalyst solution, which is then directly used for the catalytic polymerization of ethylene.

[0039] Alternatively, the ligand and 1,5-cyclooctadiene nickel(II) can be added to the reactor separately to prepare a catalyst for ethylene polymerization directly in situ within the reactor;

[0040] The ligand has the following structure:

[0041]

[0042] Wherein, R is selected from the following groups: hydrogen, -OR1; R1 is selected from C4-C10 straight-chain alkyl, -(CH2CH2O). n -C1-C4 alkyl; n is an integer from 1 to 3.

[0043] In another preferred embodiment, the molar ratio of the 1,5-cyclooctadiene nickel(II) to the ligand is (2-40):1; more preferably (8-15):1.

[0044] In another preferred embodiment, the co-catalyst is 1,5-cyclooctadiene nickel(II), and the molar ratio of the co-catalyst to the catalyst is 5-200:1.

[0045] In a third aspect of the invention, a use of the polyethylene wax described in the first aspect of the invention is provided, as a lubricant, dispersant, release agent, additive, plasticizer, tackifier, and regulator.

[0046] It should be understood that, within the scope of this invention, the above-described technical features of this invention and the technical features specifically described below (such as in the embodiments) can be combined with each other to form new or preferred technical solutions. Due to space limitations, they will not be described in detail here. Detailed Implementation

[0047] Through extensive and in-depth research, the inventors have, for the first time, provided a high-melting-point, high-stability polyethylene wax and its preparation method. The polyethylene wax of this invention has a melting peak temperature (Tpm) greater than 115°C and a temperature at which 5% thermal weight loss occurs (T...). d5 With a temperature range of ≥300℃, it is suitable for high-temperature processing environments. Furthermore, the polyethylene wax of this invention has a narrow molecular weight distribution and low oil content, making it suitable for fields requiring high precision and high purity. Based on these characteristics, the inventors completed this invention.

[0048] High melting point polyethylene wax

[0049] Polyethylene wax is a synthetic polyolefin wax, appearing as a white or pale yellow solid in lumps, flakes, or powder. Its relative molecular mass ranges from 1000 to 10000. It possesses advantages such as low toxicity, non-corrosiveness, high softening point, low melt viscosity, wear resistance, heat resistance, chemical resistance, and good lubricity, dispersibility, and flowability. Polyethylene wax exhibits good compatibility with polyolefin resins and can be used to disperse pigments and fillers in masterbatches. In plastics processing, it acts as a lubricant and mold release agent, and it can be used as an ink abrasion resistant agent, making it an indispensable and important chemical raw material in the plastics, rubber, ink, paint, and metal casting industries.

[0050] In particular, the present invention provides a polyethylene wax with a high melting point, narrow molecular weight distribution, and high thermal stability. It is a white powder, free of visible mechanical impurities, with an inorganic content of <100 ppm and a metal content of <10 ppm. Furthermore, it possesses the following characteristics:

[0051] (1) High melting point: the peak melting temperature (Tpm) is 115-130℃, preferably 120-130℃; the enthalpy of melting is ≥200J / g; suitable for high-temperature processing environments;

[0052] (2) High thermal stability: Temperature at which 5% thermal weight loss occurs (T) d5 ≥300℃, preferably ≥320℃, more preferably ≥330℃; more preferably ≥340℃; optimally ≥350℃; ensuring its stability under high temperature conditions;

[0053] (3) Narrow molecular weight distribution: molecular weight distribution <3; preferably, molecular weight distribution <2; preferably, <1.9; preferably, <1.8; stable performance, suitable for high-precision processing;

[0054] (4) Good solubility: Solubility in alkanes: at >90℃, solubility ≥6g / 100mL; wherein the alkanes are high-boiling-range alkane solvents, such as high-boiling-range petroleum ether, heptane or octane.

[0055] (5) Low oil content: oil content <0.1%, preferably <0.08%; high purity, suitable for applications with high purity requirements.

[0056] Furthermore, the polyethylene wax of the present invention has a number average molecular weight of 1000-10000 g / mol, preferably 1000-5000 g / mol, and more preferably 1000-3000 g / mol; the particle size distribution is d 50 ≤100um.

[0057] The testing methods for various characteristics of the high-melting-point polyethylene wax described in this invention utilize detection methods well-known to those skilled in the art, as detailed below:

[0058] (1) The metal content of the polymer can be obtained through elemental analysis;

[0059] (2) The content of inorganic matter can be obtained by ash content determination or thermogravimetric analysis;

[0060] (3) The peak melting temperature T of the polymer was obtained by DSC testing. pm and enthalpy of fusion;

[0061] (4) The temperature at which the polymer loses 5% of its thermal weight is obtained by TGA test; the temperature is controlled to rise from room temperature to 600.0℃ while maintaining a heating rate of 10.0℃ / min; nitrogen flow rate: 50.0mL / min and nitrogen is maintained for 1-2 hours before the test begins.

[0062] (5) The number-average molecular weight and molecular weight distribution of the polymer were obtained by GPC testing;

[0063] (6) Solubility test method: Weigh a certain amount of polymer sample and add it to petroleum ether with a boiling range of (90~120)℃. Heat under reflux with stirring until the sample is completely dissolved in petroleum ether and the system is visually clear. Record the amount of sample dissolved and the volume of solvent at this time, in g / 100mL.

[0064] (7) The oil content of the polymer was obtained by nuclear magnetic resonance hydrogen spectrum test.

[0065] Preparation method of high melting point polyethylene wax

[0066] Currently, there are three methods for producing polyethylene wax. The first method is the polyethylene pyrolysis method, which uses thermal pyrolysis to break down high-molecular-weight polyethylene resin into low-molecular-weight polyethylene wax. This method requires high energy consumption, and the resulting product has a wide molecular weight distribution, making it difficult to completely eliminate the odor from the low molecular weight components, and the formation of black spots is unavoidable. The second method involves refining oligomers—byproducts generated during polyethylene production—to obtain the final polyethylene wax product. This method typically yields a mixture of products with different degrees of polymerization, making quality stability difficult to control. Furthermore, due to the low molecular weight and complex composition of the product, batch stability is poor, and the possibility of precipitation in end-use applications is high. The third method is the ethylene synthesis method, which uses ethylene as a raw material to polymerize polyethylene wax with a specific molecular weight under specific conditions.

[0067] The synthesis of polyethylene wax from ethylene is currently mainly divided into three categories: free radical polymerization, Ziegler-Natta polymerization, and metallocene-catalyzed polymerization. Free radical polymerization is carried out under high temperature and high pressure (generally temperatures exceeding 100℃ and pressures greater than 20 MPa) by initiating ethylene polymerization with free radicals. The resulting polyethylene wax typically has a molecular weight between 3000 and 5000, usually containing long branches and double bonds, and a relatively wide molecular weight distribution. Ziegler-Natta (ZN) catalytic polymerization is the direct polymerization of ethylene under low pressure using a traditional Ziegler-Natta catalyst. The resulting polyethylene wax product has very few branches, resulting in high crystallinity and high density, making it a high-density linear polyethylene wax. However, the process requires sophisticated equipment and technology. Metallocene-catalyzed polymerization uses a metallocene catalyst to catalyze the polymerization of ethylene. This method is characterized by high catalyst activity, low catalyst dosage, and no need for a removal process. Its disadvantages include the catalyst's high sensitivity to water and oxygen, the need for molecular weight control through hydrogenation, and the requirement for expensive methylaluminoxane (MAO) or modified methylaluminoxane (MMAO) as a co-catalyst, leading to excessively high costs.

[0068] In view of this, the present invention provides a novel method for preparing polyethylene wax, which creatively uses a nickel-based catalyst, optimizes the molecular structure and preparation process, and solves the problems of low melting point, poor thermal stability, wide molecular weight distribution and high oil content of traditional polyethylene wax, thus preparing polyethylene wax with high melting point, high thermal stability, narrow molecular weight distribution and low oil content.

[0069] Specifically, the preparation method of the high-melting-point polyethylene wax of the present invention includes the following steps:

[0070] With or without a co-catalyst, ethylene undergoes catalytic polymerization under the action of a catalyst to obtain the high-melting-point polyethylene wax described above.

[0071] The catalyst is obtained by reacting the ligand with 1,5-cyclooctadiene nickel(II);

[0072] The ligand has the following structure:

[0073]

[0074] Wherein, R is selected from the following groups: hydrogen, -OR1; R1 is selected from C4-C10 straight-chain alkyl, -(CH2CH2O). n -C1-C4 alkyl; n is an integer from 1 to 3.

[0075] The straight-chain alkyl group refers to a monovalent saturated aliphatic hydrocarbon group having 1 to 10 carbon atoms, including straight-chain and branched hydrocarbon groups, such as methyl (i.e., CH3-), ethyl (i.e., CH3CH2-), n-propyl (i.e., CH3CH2CH2-), isopropyl (i.e., (CH3)2CH-), n-butyl (i.e., CH3CH2CH2CH2-), isobutyl (i.e., (CH3)2CHCH2-), sec-butyl (i.e., (CH3)(CH3CH2)CH-), tert-butyl (i.e., (CH3)3C-), n-pentyl (i.e., CH3CH2CH2CH2CH2-), and neopentyl (i.e., (CH3)3CCH2-).

[0076] The preparation method of polyethylene wax of the present invention further includes adding silica gel or diatomaceous earth, heating and refluxing for 1-2 hours, filtering while hot to remove inorganic matter or metal, and drying to obtain the polyethylene wax.

[0077] In a preferred embodiment, the method for preparing the high-melting-point polyethylene wax includes the following steps: catalytic polymerization of ethylene at 40-120°C and 0.5-5.0 MPa ethylene pressure in the presence of a catalyst and a co-catalyst, or in the presence of a catalyst alone, to obtain polyethylene wax, wherein the catalyst is obtained by reacting a ligand with 1,5-cyclooctadiene nickel(II).

[0078] The ligand has the following structure:

[0079]

[0080] Wherein, R is selected from the following group: -OR1, where R1 is selected from C5-C8 straight-chain alkyl groups; or -(CH2CH2O). n -C1-C4 alkyl; n is an integer from 1 to 3.

[0081] In one specific embodiment, the reaction of the present invention is carried out in the presence of an inert gas. The inert gas described in this invention is a commonly used inert gas in the art, such as N2, Ar, etc.

[0082] In the preparation method of this invention, the nickel-based catalyst can be obtained by referring to the preparation method of the nickel-based olefin catalyst disclosed in Chinese patent application CN102174129B; furthermore, the nickel-based catalyst of this invention is composed of ligands. It is obtained by reacting with the nickel metal precursor 1,5-cyclooctadiene nickel(II), wherein R is hydrogen, -OR1; R1 is selected from C4-C10 straight-chain alkyl, -(CH2CH2O). n -C1-C4 alkyl; n is an integer from 1 to 3.

[0083] The catalyst can be prepared on-site or in situ during use, or it can be prepared into a solution in advance for later use; wherein the molar ratio of nickel metal precursor to ligand is (2-40):1; preferably (8-15):1.

[0084] The method for preparing polyethylene wax by nickel metal-catalyzed ethylene polymerization of the present invention can be carried out in the presence of a co-catalyst, or it can be prepared by nickel metal catalyst alone; when freshly prepared and used, no additional co-catalyst is required. When a co-catalyst is present, the molar ratio of co-catalyst to catalyst is 5-200:1. The co-catalyst is 1,5-cyclooctadiene nickel(II).

[0085] The ethylene polymerization reaction of the present invention is carried out in an inert solvent, without particular limitation, such as hydrocarbon solvents, cyclic hydrocarbon solvents or aromatic solvents, such as toluene, hexane, heptane, octane, etc.

[0086] The reaction time of the ethylene polymerization reaction of the present invention is not particularly limited, and the reaction time can be 1h-48h (e.g. 1h-24h, 1h-12h, 1h-6h).

[0087] use

[0088] Because the polyethylene wax of this invention has a high melting point, high thermal stability, narrow molecular weight distribution, and low oil content, it is particularly suitable for high-temperature processing and use (e.g., plastic processing) scenarios, maintaining structural stability. The narrow molecular weight distribution of the polyethylene wax allows for stable dispersion in resins, reducing the risk of precipitation during processing and ensuring a smooth, defect-free product surface. Furthermore, the narrow molecular weight distribution of the polyethylene wax allows for uniform pigment dispersion, preventing sedimentation and improving the clarity and color saturation of inks used in printing (e.g., metallic inks, UV-curable inks).

[0089] High melting point provides high-temperature stability, while narrow molecular weight ensures controllable performance; the combination of these two characteristics meets the needs of precision machining, high-performance materials, and harsh environmental applications. Its high melting point allows it to maintain structural stability during high-temperature printing (such as hot stamping), preventing ink sagging or discoloration. As a lubricant, high-melting-point polyethylene wax can improve the processing performance of high-temperature cables (high-temperature resistant silicone cables) while maintaining the stability of the insulation material. When used in automotive coatings and industrial protective coatings, high-melting-point polyethylene wax can enhance surface hardness and scratch resistance, while also withstanding high-temperature baking environments (such as electrophoretic paints and powder coatings). In fast-curing hot melt adhesives, the narrow molecular weight distribution of polyethylene wax enables rapid and uniform melting, enhancing bond strength; in powder coatings, it can optimize coating leveling and reduce orange peel effect.

[0090] Therefore, the polyethylene functional wax of the present invention is suitable for the fields of plastics processing, coatings, inks, hot melt adhesives and cosmetics, and can be used as a lubricant, dispersant, release agent, additive, plasticizer, tackifier and regulator, etc.

[0091] Compared with the prior art, the main advantages of the present invention include:

[0092] (1) The high melting point polyethylene wax of the present invention is obtained by nickel-based catalyst, which avoids the use of expensive metallocene catalysts and co-catalysts such as methylaluminoxane (MAO) and modified methylaluminoxane (MMAO), thus reducing costs.

[0093] (2) The high melting point polyethylene wax of the present invention has a high melting point and high thermal stability, and is suitable for high temperature processing environment.

[0094] (3) The polyethylene wax of the present invention has a narrow molecular weight distribution, which is suitable for high-precision processing.

[0095] (4) The polyethylene wax of the present invention has low oil content and high purity.

[0096] (5) The polyethylene wax of the present invention is applicable to plastic processing, coatings, inks, hot melt adhesives, cosmetics and other fields.

[0097] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods in the following embodiments, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. Percentages and parts are by weight unless otherwise stated.

[0098] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as are familiar to those skilled in the art. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to the methods of this invention. The preferred embodiments and materials described herein are for illustrative purposes only.

[0099] Example 1: Synthesis of ligand L1

[0100]

[0101] ω-bromoacetophenone (0.58 g, 2.9 mmol) and tris(2-methoxyethyloxy)phenylphosphine (1.39 g, 2.9 mmol) were dissolved in DCM (10 mL) and stirred at room temperature for 24 h. After removing most of the solvent under reduced pressure, anhydrous diethyl ether was added to precipitate the phosphate salt. The precipitate was filtered and dried. The phosphate salt was dissolved in a mixed solvent of water and methanol (30 mL, v / v = 1 / 1). A 2N NaOH aqueous solution was added dropwise to the solution until the pH reached 8. The resulting solid was filtered, washed, and dried to give 1.3 g of a white solid, with a yield of 75%.

[0102] 1 H NMR (400MHz, CDCl3) δ7.91-7.89(m,2H),7.72-7.67(m,3H),7.48-7.44(m,3H),7.34-7.28(m,3 H),7.09-7.03(m,3H),6.93-6.90(m,3H),4.46(d,1H),3.89(t,6H),3.28(t,6H),3.15(s,9H).

[0103] Example 2: Synthesis of ligand L2

[0104]

[0105] ω-bromoacetophenone (3.2 g, 16 mmol) and tris(2-n-pentoxy)phenylphosphine (8.3 g, 16 mmol) were dissolved in DCM (20 mL) and stirred at room temperature for 24 h. After removing most of the solvent under reduced pressure, anhydrous diethyl ether was added to precipitate the phosphate salt. The precipitate was filtered and dried. The phosphate salt was dissolved in a mixed solvent of water and methanol (50 mL, v / v = 1 / 1). A 2N NaOH aqueous solution was added dropwise to the solution until the pH reached 8. The resulting solid was filtered, washed, and dried to give 7.4 g of a white solid, with a yield of 72%.

[0106] 1 H NMR (300MHz, CDCl3) δ7.89-7.87(m,2H),7.70-7.62(m,3H),7.46-7.40(m,3H),7.30-7.24(m,3H),7.00-6.9 6(m,3H),6.88-6.83(m,3H),4.46(d,1H),3.75(t,6H),1.36-1.28(m,6H),1.18-1.04(m,12H),0.72(t,9H).

[0107] Example 3

[0108] Weigh ligand L1 and 10 equivalents of 1,5-cyclooctadiene nickel(II) into a stopcock bottle in a glove box, add toluene and stir for 10-30 min to prepare a catalyst solution of 1 μmol / mL for later use.

[0109] After drying a 1L stainless steel reactor, purge it with nitrogen and preheat the reactor to about 70℃. Add 450mL of toluene and control the stirring speed at 300rpm. After stirring for 5 minutes, add catalyst solution (5µlol). Introduce ethylene to bring the pressure inside the reactor to 1.0MPa and control the temperature inside the reactor at 70℃. After the polymerization reaction is completed for 1 hour, cut off the ethylene supply, cool the reaction, release the pressure inside the reactor, quench the reaction, add silica gel or diatomaceous earth to the polymer, heat under reflux for 1-2 hours, and then filter while hot to remove inorganic substances or metal impurities. After drying, a white powdery polymer is obtained. The specific results are shown in Table 1.

[0110] Example 4

[0111] After drying a 1L stainless steel reactor, purged it with nitrogen and preheated the reactor to about 70℃. Add 450mL of toluene and control the stirring speed at 300rpm. After stirring for 5 minutes, add the ligand (L1, 5µl) and 1,5-cyclooctadiene nickel(II) (50µl). Introduce ethylene to bring the pressure inside the reactor to 1.0MPa and control the temperature inside the reactor at 70℃. After the polymerization reaction is completed for 1 hour, cut off the ethylene, cool the reaction, release the pressure inside the reactor, quench the reaction, add silica gel or diatomaceous earth to the polymer, heat under reflux for 1-2 hours, and then filter while hot to remove inorganic or metallic impurities. After drying, a white powdery polymer is obtained. The specific results are shown in Table 1.

[0112] Example 5

[0113] Example 4 was repeated, except that the solvent was hexane. The specific results are shown in Table 1.

[0114] Example 6

[0115] Example 4 was repeated, except that the solvent was heptane. The specific results are shown in Table 1.

[0116] Example 7

[0117] Example 4 was repeated, except that the solvent was heptane and the reaction temperature was 110°C. The specific results are shown in Table 1.

[0118] Example 8

[0119] Example 4 was repeated, except that the solvent was hexane and the reaction temperature was 80°C. The specific results are shown in Table 1.

[0120] Example 9

[0121] Example 4 was repeated, except that the solvent was hexane and the ethylene pressure was 0.5 MPa. The specific results are shown in Table 1.

[0122] Example 10

[0123] Example 4 was repeated, except that the solvent was hexane and the ethylene pressure was 1.5 MPa. The specific results are shown in Table 1.

[0124] Example 11

[0125] Example 4 was repeated, except that the ligand was L2. The specific results are shown in Table 1.

[0126] Example 12

[0127] Example 4 was repeated, except that the ligand was L2 and the ethylene pressure was 1.5 MPa. The specific results are shown in Table 1.

[0128] Table 1

[0129]

[0130]

[0131] As can be seen from the table above, the polyethylene wax prepared by the nickel-based catalyst of the present invention has a high melting point, high thermal stability, a 5% thermal weight loss temperature that is generally >330℃, a narrow molecular weight distribution (PDI <2), and a low oil content (<0.05%), and can be widely used in various high-temperature and fine processing scenarios.

[0132] Test Example 1: Solubility Test

[0133] The polyethylene waxes prepared in Examples 3-12 of this invention were subjected to solubility tests in high-boiling-range petroleum ether (the test methods are as described above), and the results are shown in Table 1. It can be seen that the high-melting-point polyethylene wax of this invention has a solubility ≥6 g / 100 mL in alkane solvents, indicating that the high-melting-point polyethylene wax of this invention has high solubility and can form a uniform dispersion system in alkane solvents, making it suitable for applications in plastics processing, coatings, inks, hot melt adhesives, cosmetics, and other fields.

[0134] All documents mentioned in this invention are incorporated herein by reference as if each document were individually incorporated by reference. Furthermore, it should be understood that after reading the foregoing teachings of this invention, those skilled in the art can make various alterations or modifications to this invention, and these equivalent forms also fall within the scope defined by the appended claims.

Claims

1. A high-melting-point polyethylene wax, characterized in that, The high-melting-point polyethylene wax has the following characteristics: (a) White powder, free from visible mechanical impurities; inorganic content <100ppm; metal content <10ppm; (b) Melting point is 115-130℃; enthalpy of fusion is ≥200J / g; (c) Number-average molecular weight is 1000-10000 g / mol, and molecular weight distribution PDI < 3; (d) Temperature at which 5% of thermal weight loss occurs, Td5 ≥ 300℃; (e) Solubility in alkanes: at >90°C, solubility ≥6 g / 100 mL; and / or (f) Oil content < 0.1%.

2. The polyethylene wax as described in claim 1, characterized in that, The alkane is a high-boiling-range alkane solvent, preferably a high-boiling-range petroleum ether, heptane, or octane.

3. The polyethylene wax as described in claim 1, characterized in that, The number average molecular weight of the high-melting-point polyethylene wax is 1000-5000 g / mol.

4. The polyethylene wax as described in claim 1, characterized in that, The temperature at which the high-melting-point polyethylene wax loses 5% of its thermal weight is T. d5 ≥330℃.

5. The polyethylene wax as described in claim 1, characterized in that, The particle size distribution of the high-melting-point polyethylene wax is in the range of d. 50 ≤100um.

6. The polyethylene wax according to claim 1, characterized in that, The high-melting-point polyethylene wax does not contain non-hydrocarbon compounds, polycyclic aromatic hydrocarbons, sulfur, or phosphorus.

7. A method for preparing the polyethylene wax according to claim 1, characterized in that, Includes the following steps: Polyethylene wax is obtained by catalytic polymerization of ethylene at 40-120°C and 0.5-5.0 MPa ethylene pressure in the presence of a catalyst and a co-catalyst, or in the presence of a catalyst alone; wherein the catalyst is obtained by reacting a ligand with 1,5-cyclooctadiene nickel(II). The ligand has the following structure: Wherein, R is selected from the following groups: hydrogen, -OR1; R1 is selected from C4-C10 straight-chain alkyl, -(CH2CH2O). n -C1-C4 alkyl; n is an integer from 1 to 3.

8. The preparation method according to claim 7, characterized in that, The catalyst is prepared by the following method: Under inert gas protection, the ligand and 1,5-cyclooctadiene nickel(II) are placed in a solvent and stirred for 10-60 minutes to obtain a catalyst solution, which is then directly used for the catalytic polymerization of ethylene. Alternatively, the ligand and 1,5-cyclooctadiene nickel(II) can be added to the reactor separately to prepare a catalyst for ethylene polymerization directly in situ within the reactor; The ligand has the following structure: Wherein, R is selected from the following groups: hydrogen, -OR1; R1 is selected from C4-C10 straight-chain alkyl, -(CH2CH2O). n -C1-C4 alkyl; n is an integer from 1 to 3.

9. The preparation method according to claim 7, characterized in that, The molar ratio of the 1,5-cyclooctadiene nickel(II) to the ligand is (2-40):1; preferably (8-15):

1.

10. The use of the polyethylene wax according to claim 1, characterized in that, It is used as a lubricant, dispersant, release agent, additive, plasticizer, thickener and regulator.

Citation Information

Patent Citations

  • Nickel system olefinic polymerization catalyst and preparation method and application thereof

    CN102174129B