A stress-dissipating polymer binder, its preparation method and application
By employing a polymer binder with a bicyclic structure of force-sensitive groups in sulfide solid-state batteries, the problem of insufficient tensile strength of traditional binders is solved, achieving efficient stress dissipation, improving the mechanical robustness and electrochemical stability of the battery, and extending battery life.
Patent Information
- Application Number
- CN202611437397.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing binders have insufficient tensile strength in sulfide solid-state batteries, which cannot effectively dissipate stress, leading to easy cracking of the electrolyte membrane, interface contact failure, and affecting battery performance and lifespan.
Stress-dissipating polymer binders are prepared by copolymerizing monomers containing bicyclic force-sensitive groups with other functional monomers. Through ring-opening reaction and in-situ chain growth under mechanical stress, interfacial stress is dissipated, maintaining the integrity of the electrode structure.
It significantly improves the elongation at break and toughness of the binder, enhances the mechanical robustness and electrochemical stability of the electrode and electrolyte membrane, and improves the cycle life and rate performance of the battery.
Smart Images

Figure CN123106966A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery technology, specifically relating to a stress-dissipating polymer binder, its preparation method, and its application. Background Technology
[0002] Constructing solid-state electrolyte membranes with high ionic conductivity and high mechanical stability, along with dense electrode membranes, is fundamental to achieving high energy density and long cycle life in sulfide solid-state batteries. Regardless of whether wet or dry film deposition processes are used, binders not only play a role in bonding and fixing but also directly affect the mechanical integrity of the sulfide solid-state electrolyte membrane, the microstructural stability of the composite cathode, and the sustained and tight contact at the electrode / electrolyte solid-solid interface, thus influencing the electrochemical performance of the sulfide solid-state battery.
[0003] Currently, polymer binders used in sulfide solid-state battery applications include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and styrene-butadiene rubber (SBR). These binders suffer from insufficient tensile strength and lack efficient stress dissipation capabilities, leading to a general problem of insufficient tensile strength in sulfide electrolyte membranes prepared based on these binders. These sulfide electrolyte membranes are highly susceptible to microcracks and even fracture during battery assembly and cycling, resulting in interruption of ion transport channels and the risk of localized short circuits. Simultaneously, in composite cathodes, the lattice volume changes occurring in the active materials (such as high-nickel ternary and lithium-rich manganese-based materials) during lithium insertion / extraction generate significant localized stress. Traditional binders can only provide limited buffering and cannot effectively dissipate and redistribute these stresses, leading to microcracks within the cathode, contact failure between active particles and the sulfide electrolyte / conductive agent, and disruption of the ion and electron transport network, resulting in rapid increase in battery impedance and drastic capacity decay. In summary, the insufficient tensile strength and lack of efficient stress dissipation capabilities of traditional binders have become a key bottleneck restricting the electrochemical performance and cycle life of sulfide solid-state batteries.
[0004] Currently, to address the aforementioned issues, researchers have developed many types of sulfide solid-state battery binders. For example, patent CN202311759795.X discloses a sulfide solid electrolyte membrane and its preparation method, which achieves high flexibility and ionic conductivity of the sulfide electrolyte membrane by using a hydrogenated nitrile rubber / styrene-butadiene rubber blend binder. Patent CN202211604948.9 discloses a self-healing binder polymerized from methyl methacrylate and ester monomers for preparing sulfide solid electrolyte films. However, these binders are prone to irreversible plastic deformation or fatigue failure under repeated stress during cycling, failing to continuously offset the interfacial stress caused by volume changes. This leads to the active material gradually losing contact with the binder ("debonding"), a sharp increase in interfacial contact resistance, and a rapid decrease in the actual usable capacity of the battery.
[0005] Therefore, developing polymer binders with high tensile strength and strong stress dissipation function, which are different from traditional binder structures, is of great significance for the commercial application of high energy density sulfide solid-state batteries. Summary of the Invention
[0006] This application provides a stress-dissipating polymer binder, its preparation method, and its application, aiming to solve the problem that existing binders cannot meet the requirements for preparing composite electrodes and electrolyte membranes for sulfide solid-state batteries with excellent mechanical robustness and electrochemical stability.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A stress-dissipating polymer adhesive, wherein the adhesive is formed by self-polymerization of a monomer containing a bicyclic structure force-sensitive group or by copolymerization with other functional monomers; The general structural formula of the monomer containing the bicyclic mechanosensitive group is as follows: ; In the formula, n takes the value of a natural number from 1 to 6, and R1 is taken from the bonds, NH, and (CH2). x (x takes values from 1 to 4), R2 is taken from an unsubstituted or substituted C2-C6 alkenyl group, C1-C 10 Alkyl, C1-C 10 The alkoxy group, wherein the following groups are cyano, C1-C5 alkyl, or C1-C5 acyl.
[0008] Preferably, the structural formula of the monomer containing the bicyclic mechanosensitive group is: where n is 2, R1 is taken from the bond, and R2 is taken from the methyl group; the specific structural formula is: .
[0009] When the adhesive is obtained by copolymerizing monomers containing bicyclic mechanosensitive groups with other functional monomers, the other functional monomers include acrylonitrile, lithium acrylate, lithium methacrylate, alkyl acrylate, alkyl methacrylate, aryl acrylate, and aryl methacrylate. , One or more of the following; The molar ratio of the monomer containing the bicyclic mechanosensitive group to other functional monomers is (1-99):(1-99).
[0010] The molar ratio of the monomer containing the bicyclic structure mechanosensitive group to the other functional monomers is (5-10):(95-90).
[0011] The self-polymerization or copolymerization is completed in the presence of an initiator, wherein the amount of initiator added is 0.5%-1.0% of the total mass of the monomers.
[0012] The initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, and azobiscyclohexylformitrile.
[0013] A method for preparing the stress-dissipating polymer adhesive involves dissolving the raw material monomer in an organic solvent and polymerizing it at 60-80°C for 5-24 h in the presence of an initiator; the raw material monomer is a monomer with a bicyclic structure and a force-sensitive group, or other functional monomers.
[0014] The organic solvent is one or more of toluene, xylene, and isobutyl isobutyrate.
[0015] An application of the stress-dissipating polymer binder, wherein the stress-dissipating polymer binder is used in one or more of the preparation of sulfide solid lithium / sodium battery electrodes and electrolyte membranes.
[0016] The binder is used to prepare one or more of the positive and negative electrode sheets and sulfide electrolyte membranes of sulfide solid lithium / sodium batteries through wet or dry processes.
[0017] A sulfide solid-state battery includes positive and negative electrode sheets and an electrolyte membrane, wherein the binder is added to one or more of the positive and negative electrode sheets and the electrolyte membrane respectively.
[0018] The positive or negative electrode sheet is formed by coating a mixture of electrode active material, sulfide electrolyte, conductive agent and stress dissipation polymer binder onto a current collector; wherein the mass ratio of electrode active material, sulfide electrolyte, conductive agent and stress dissipation polymer binder according to claim 1 is (50-85):(10-20):(2-5):(3-25). The electrolyte membrane is formed of a sulfide electrolyte and a stress-dissipating polymer binder; wherein the mass ratio of the sulfide electrolyte to the stress-dissipating polymer binder is (70-99):(1-30).
[0019] The positive electrode active material includes one or more of lithium cobalt oxide, lithium iron manganese phosphate, lithium manganese oxide, lithium iron phosphate, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, sodium vanadium phosphate, lithium-rich manganese-based materials, sodium vanadium fluorinated phosphate, sodium iron pyrophosphate, and sodium nickel iron manganese oxide. The negative electrode active material includes one or more of the following: lithium metal alloy, graphite, nano-silicon, silicon suboxide, and hard carbon. The conductive agent includes one or more of Super P conductive agent, Ketjen Black, acetylene black, and carbon nanotubes.
[0020] The sulfide electrolytes include Li6PS5X (where X is one or more of Cl, Br, and I), Li2S-P2S5 glass-ceramic type, thio-LISICON type, and anion-doped Li2S-P2S5 solid electrolytes, Na3XS4 (where X is one or more of P and Sb), and Na 10 N x P 3-x S 12 One or more of the following: (where 0 ≤ x ≤ 2, N = Si, Ge or Sn) and Na2S: (1-x)P2S5 (where x = 0.7~0.8). Advantages of this invention: The bicyclic force-sensitive groups in the binder of this invention can undergo specific ring-opening reactions and trigger in-situ chain growth under the mechanical stress caused by the volume change of the active material during battery cycling. This effectively dissipates interfacial stress, avoids the generation and propagation of microcracks, and simultaneously achieves local reconstruction and reinforcement of the polymer network in stress concentration areas, maintaining the integrity of the electrode structure and the stability of the ion / electron transport network.
[0021] Compared to polymer binders without stress-sensitive groups obtained solely from the self-polymerization of functional monomers, the stress-dissipating polymer binder prepared in this invention exhibits a 100%–150% increase in elongation at break and a 150%–300% increase in toughness. Using the stress-dissipating polymer binder prepared in this invention, composite electrode and electrolyte membranes with excellent mechanical robustness and electrochemical stability can be constructed, significantly alleviating the capacity decay and shortened lifespan problems caused by interfacial contact failure and stress accumulation in sulfide solid-state batteries, thereby greatly improving the battery's cycle life and rate performance. Attached Figure Description
[0022] Figure 1 The graph shows the cycle performance of the battery prepared using the binder described in Example 1 of this invention. Figure 2 The graph shows the cycle performance of the battery prepared using the binder described in Example 2 of this invention. Figure 3 The graph shows the cycle performance of the battery prepared using the binder described in Example 3 of this invention. Figure 4 The graph shows the cycle performance of the battery prepared using the binder described in Example 4 of this invention. Figure 5 The graph shows the cycle performance of the battery prepared using the binder described in Example 5 of this invention. Figure 6 The graph shows the cycle performance of the battery prepared using SBR binder.
[0023] Figure 7The spectrum of the monomer containing a bicyclic mechanosensitive group was obtained in Example 1 of this invention. Detailed Implementation
[0024] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0025] The stress-dissipating polymer binder of this invention undergoes a specific ring-opening reaction and triggers in-situ chain growth under the mechanical stress generated by the volume change of active materials during battery cycling. This effectively dissipates interfacial stress, preventing the generation and propagation of microcracks. Simultaneously, it achieves local reconstruction and reinforcement of the polymer network in stress concentration areas, maintaining the integrity of the electrode structure and the stability of the ion / electron transport network. Compared to polymer binders without force-sensitive groups obtained solely from the self-polymerization of functional monomers, the stress-dissipating polymer binder prepared in this invention exhibits a 100%–150% increase in elongation at break and a 150%–300% increase in toughness. Using the stress-dissipating polymer binder prepared in this invention, composite electrodes and electrolyte membranes with excellent mechanical robustness and electrochemical stability can be constructed, significantly alleviating the capacity decay and shortened lifespan problems caused by interfacial contact failure and stress accumulation in sulfide solid-state batteries, thereby greatly improving the battery's cycle life and rate performance.
[0026] The binder of this invention can be used to prepare electrodes and electrolyte membranes for solid-state lithium / sodium batteries using wet or dry processes in a roll-to-roll manner. The specific preparation methods are as follows: Dry-process all-solid-state battery module fabrication: (1) Preparation of sulfide electrolyte membrane: i. Premix the binder polymer monomers for 10-20 min, then add the sulfide electrolyte particles to a twin-screw extruder at a certain mass ratio, mix and extrude, and then hot press to form a sulfide electrolyte membrane of a certain thickness; (2) Preparation of positive electrode: i. Premix the binder polymer monomers for 10-20 min, then add the positive electrode active material, conductive additives, and sulfide electrolyte particles into a twin-screw extruder at a certain mass ratio, mix and extrude, and then hot press to form an electrode film of a certain thickness. ii. The dry positive electrode film obtained in the previous step is uniformly coated onto aluminum foil by means of transfer printing, etc. First, it is heat-treated at 60~80℃ for 4~6 hours, then dried in a vacuum oven at 120℃, rolled, punched, weighed, and then dried in a vacuum oven at 120℃ for later use. (3) Preparation of negative electrode: i. Premix the binder polymer monomers for 10-20 min, then add the negative electrode active material (excluding lithium and its alloys), conductive additives, and sulfide electrolyte particles into a twin-screw extruder at a certain mass ratio, mix and extrude, and then hot press to form an electrode film of a certain thickness. ii. The dry positive electrode film obtained in the previous step is uniformly coated onto copper foil or thin steel sheet by means of transfer printing, etc. First, it is heat-treated at 60~80℃ for 4~6 hours, then dried, rolled, punched, and weighed in a vacuum oven at 120℃, and then dried in a vacuum oven at 120℃ for later use. Wet-process all-solid-state battery module fabrication: (1) Preparation of sulfide electrolyte membrane: i. Dissolve the binder monomer in toluene or isobutyl isobutyrate solvent (solution concentration 0.1 g / mL), stir at room temperature for 1-2 h, then add sulfide electrolyte particles and mix thoroughly; ii. The above slurry is coated onto the substrate and then dried at 50-70°C for 6-8 hours. After drying in a vacuum drying oven at 120°C for 6-8 hours, a sulfide electrolyte membrane is obtained. Further, it is rolled and stamped, and then placed in a low dew point drying room for later use.
[0027] (2) Preparation of positive electrode: i. Dissolve the binder monomer in toluene or isobutyl isobutyrate solvent (solution concentration 0.1 g / mL), stir at room temperature for 1-2 h, then add the positive electrode active material, conductive additive, and sulfide electrolyte particles, and mix thoroughly. ii. The above slurry is coated onto aluminum foil and dried at 50-70°C for 6-8 hours, followed by drying in a vacuum drying oven at 120°C for 6-8 hours to obtain the electrode film. After further rolling, stamping, and weighing, it is placed in a low dew point drying room for later use.
[0028] (3) Preparation of negative electrode: i. Dissolve the binder monomer in toluene or isobutyl isobutyrate solvent (solution concentration 0.1 g / mL), stir at room temperature for 1-2 h, then add the negative electrode active material (excluding lithium and its alloys), conductive additives, and sulfide electrolyte particles, and mix thoroughly. ii. The above slurry is coated onto copper foil or thin steel sheet and dried at 50~70℃ for 6~8 h, followed by drying in a vacuum drying oven at 120℃ for 6~8 h to obtain the electrode film. After further rolling, stamping, and weighing, it is placed in a low dew point drying room for later use.
[0029] When preparing battery modules using the aforementioned wet or dry methods, each module may incorporate hyperbranched components at different times during fabrication. A chain-structured polymer binder, i.e., a stress-dissipating polymer binder added to one or more of the positive electrode, negative electrode and sulfide electrolyte membrane.
[0030] Example 1 Preparation of a stress-dissipating polymer binder solution A1: Under an argon atmosphere, 11.2 g of cyclooctene and 8.1 g of methyl propynate were added to 150 mL of toluene and stirred at 25 °C for 12 hours to obtain a monomer containing a bicyclic mechanosensitive group, denoted as P1. (See) Figure 7 ).
[0031] Weigh 12.0 g of monomer P1 containing a bicyclic mechanosensitive group and dissolve it in 200 mL of toluene. Then add 0.12 g of azobisisobutyronitrile to the toluene to obtain a reaction solution. Stir the above reaction solution at 65 °C for 12 hours to obtain a homogeneous and stable polymer binder solution, denoted as A1.
[0032] Example 2 Preparation of a stress-dissipating polymer binder solution A2: Under an argon atmosphere, 0.6 g of monomer P1 containing a bicyclic mechanosensitive group and 11.4 g of... (Referring to F1, purchased from Bidepharm, CAS: 82200-53-1) Dissolve in 200 mL toluene, then add 0.12 g of azobisisobutyronitrile to the toluene to obtain a reaction solution; stir the above reaction solution at 65°C for 12 hours to obtain a uniform and stable polymer binder solution, denoted as A2.
[0033] Example 3 Preparation of a stress-dissipating polymer binder solution A3: Under an argon atmosphere, 0.9 g of monomer P1 containing a bicyclic mechanosensitive group and 11.1 g of... (Referring to F2, purchased from Tianyuan Aviation Materials, POLYVEST® EP MAT) was dissolved in 200 mL of toluene, and then 0.12 g of azobisisobutyronitrile was added to the toluene to obtain a reaction solution; the above reaction solution was stirred at 65°C for 12 hours to obtain a uniform and stable polymer binder solution, denoted as A3.
[0034] Example 4 Preparation of a stress-dissipating polymer binder solution A4: Under an argon atmosphere, 2.6 g of monomer P1 containing a bicyclic mechanosensitive group and 9.4 g of lithium acrylate (denoted as F3) were weighed and dissolved in 200 mL of toluene. Then, 0.12 g of azobisisobutyronitrile was added to the toluene to obtain a reaction solution. The above reaction solution was stirred at 65 °C for 12 hours to obtain a homogeneous and stable polymer binder solution, denoted as A4.
[0035] Example 5 Preparation of a stress-dissipating polymer binder solution A5: Under an argon atmosphere, 1.7 g of monomer P1 containing a bicyclic mechanosensitive group and 10.3 g of butyl acrylate (denoted as F4) were weighed and dissolved in 200 mL of toluene. Then, 0.12 g of azobisisobutyronitrile was added to the toluene to obtain a reaction solution. The above reaction solution was stirred at 65 °C for 12 hours to obtain a homogeneous and stable polymer binder solution, denoted as A5.
[0036] Example 6 Preparation of a stress-dissipating polymer binder solution B2: Under an argon atmosphere, 0.3 g of monomer P1 containing a bicyclic mechanosensitive group and 11.7 g of monomer F1 were weighed and dissolved in 200 mL of toluene. Then, 0.12 g of azobisisobutyronitrile was added to the toluene to obtain a reaction solution. The above reaction solution was stirred at 65 °C for 12 hours to obtain a homogeneous and stable polymer binder solution, denoted as B2.
[0037] Example 7 Preparation of a stress-dissipating polymer binder solution C2: Under an argon atmosphere, 1.3 g of monomer P1 containing a bicyclic mechanosensitive group and 10.7 g of monomer F1 were weighed and dissolved in 200 mL of toluene. Then, 0.12 g of azobisisobutyronitrile was added to the toluene to obtain a reaction solution. The above reaction solution was stirred at 65 °C for 12 hours to obtain a homogeneous and stable polymer binder solution, denoted as C2.
[0038] Example 8 Preparation of a stress-dissipating polymer binder solution D2: Under an argon atmosphere, 2.1 g of monomer P1 containing a bicyclic mechanosensitive group and 9.9 g of monomer F1 were weighed and dissolved in 200 mL of toluene. Then, 0.12 g of azobisisobutyronitrile was added to the toluene to obtain a reaction solution. The above reaction solution was stirred at 65 °C for 12 hours to obtain a homogeneous and stable polymer binder solution, denoted as D2.
[0039] Example 9 Preparation of a stress-dissipating polymer binder solution E2: Under an argon atmosphere, 0.05 g of monomer P1 containing a bicyclic mechanosensitive group and 11.95 g of monomer F1 were weighed and dissolved in 200 mL of toluene. Then, 0.12 g of azobisisobutyronitrile was added to the toluene to obtain a reaction solution. The above reaction solution was stirred at 65 °C for 12 hours to obtain a homogeneous and stable polymer binder solution, denoted as E2.
[0040] Example 10 Preparation of a stress-dissipating polymer binder solution F2: Under an argon atmosphere, 11.74 g of monomer P1 containing a bicyclic mechanosensitive group and 0.26 g of monomer F1 were weighed and dissolved in 200 mL of toluene. Then, 0.12 g of azobisisobutyronitrile was added to the toluene to obtain a reaction solution. The above reaction solution was stirred at 65 °C for 12 hours to obtain a homogeneous and stable polymer binder solution, denoted as F2.
[0041] Performance study of the adhesives prepared in the above embodiments: The tensile strength of the adhesive is determined according to the tensile test method; the sample is prepared according to the national standard GB / T 1040, with a parallel section size > 20 mm, an aspect ratio of 5:1, and a thickness greater than 1 mm. A static tensile load is applied to the sample to determine the tensile strength. The elongation at break of the adhesive was determined according to the tensile test method. Samples were prepared according to the national standard GB / T 1040, with a parallel section >20mm, an aspect ratio of 5:1, and a thickness greater than 1mm. A static tensile load was applied to the sample to determine the elongation at break. The test results are shown in Table 1. Table 1
[0042] As shown in Table 1, the adhesive exhibits superior elongation at break and tensile strength. The monomers used in preparing the adhesive contain bicyclic, force-sensitive groups, which, under mechanical stress, undergo specific ring-opening reactions and trigger in-situ chain growth or the formation of new cross-linked structures, thereby significantly improving the tensile strength of the polymer adhesive. Furthermore, Table 1 shows that the adhesive prepared in Example 2 exhibits even better elongation at break. This is because the polymer adhesive prepared using F1 monomer contains a liquid crystal phase; local stress induces orientation rearrangement or even phase transformation of the liquid crystal phase, thus dissipating stress and significantly increasing the elongation at break.
[0043] Table 2
[0044] As shown in Table 2, the adhesive exhibits significantly improved mechanical properties, such as toughness, elongation at break, and tensile strength, compared to current polymer adhesives obtained solely from the self-polymerization of functional monomers and lacking stress-sensitive groups. This is because, under stress, the stress-sensitive groups undergo a specific ring-opening reaction, releasing hidden chain lengths and significantly enhancing elongation at break and toughness by extending the polymer network.
[0045] The performance of the adhesives prepared under different molar ratios of P1 and F1 was compared, and the results are shown in Table 3: Table 3
[0046] As can be seen from Table 3, the adhesives obtained under different P1 and F1 molar ratios all have excellent tensile strength and elongation at break, while the adhesives obtained under a P1 and F1 molar ratio of 10:90 have particularly outstanding mechanical properties.
[0047] Further research was conducted on the application performance of the stress-dissipating polymer binder described in Examples 1-5 above in the preparation of sulfide solid lithium / sodium battery electrodes and electrolyte membranes.
[0048] Lithium nickel cobalt manganese oxide (LCM), sulfide electrolyte, and conductive agent were added to a glass bottle at a mass ratio of 0.7:0.25:0.02:0.03 to the stress-dissipating polymer binder described in Examples 1-5. Simultaneously, 1.1 mL of toluene was added as a dispersant. The mixture was stirred at room temperature for 6 hours to obtain a uniform slurry. This slurry was then uniformly coated onto aluminum foil, which was subsequently dried in a 60°C oven for 6 hours and then in a 120°C vacuum drying oven for 6 hours to obtain the electrode film. After further rolling, stamping, and weighing, the film was placed in a dew point drying room for later use.
[0049] The sulfide electrolyte and the stress-dissipating polymer binder (pure binder) described in Examples 1-5 were added to a glass bottle at a mass ratio of 0.97:0.03, with 1.1 mL of toluene added as a dispersant. The mixture was stirred at room temperature for 1 hour to obtain a uniform slurry. This slurry was then uniformly coated onto a polyester film, which was subsequently dried at 50-70°C for 6 hours and then dried in a vacuum drying oven at 120°C for 6 hours to obtain the sulfide electrolyte membrane. After further rolling and stamping, the membrane was placed in a dew point drying room for later use.
[0050] Meanwhile, the binder used in the above-mentioned positive electrode and electrolyte prepared in the example was replaced with the SBR binder, and a control electrode was obtained by assembly.
[0051] The sulfide electrolyte used in the above-mentioned preparation of the positive electrode and electrolyte is Li6PS5Cl.
[0052] Using the electrolyte membrane and positive electrode obtained above, and with lithium-silicon alloy as the negative electrode, a lithium nickel cobalt manganese oxide / sulfide electrolyte / lithium-silicon battery was assembled. The long-cycle performance and capacity retention of the battery at 0.2 C and 40℃ were tested, and the results are as follows: Figures 1-6 As shown in Table 4.
[0053] Table 4
[0054] From Table 4 and Figure 1-6 It can be seen that the binder prepared in the examples, when applied to the electrodes and electrolyte membranes of sulfide solid-state batteries, can significantly improve the cycle stability of sulfide solid-state batteries. Among them, the lithium nickel cobalt manganese oxide / / sulfide electrolyte / / lithium silicon battery assembled based on the lithium nickel cobalt manganese oxide composite cathode and electrolyte membrane prepared in Example 2 exhibits the best long-cycle performance.
[0055] Although the above embodiments have been shown and described, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Any changes, modifications, substitutions and variations made to the above embodiments by those skilled in the art are within the protection scope of the present invention.
Claims
1. A stress-dissipating polymer adhesive, characterized in that, The adhesive is made by self-polymerization of monomers containing bicyclic mechanical sensitive groups or copolymerization with other functional monomers; The general structural formula of the monomer containing the bicyclic mechanosensitive group is as follows: ; In the formula, n takes the value of a natural number from 1 to 6, and R1 is taken from the bonds, NH, and (CH2). x (x takes values from 1 to 4), R2 is taken from an unsubstituted or substituted C2-C6 alkenyl group, C1-C 10 Alkyl, C1-C 10 The alkoxy group, wherein the following groups are cyano, C1-C5 alkyl, or C1-C5 acyl.
2. The stress-dissipating polymer binder according to claim 1, characterized in that, When the adhesive is obtained by copolymerizing monomers containing bicyclic mechanosensitive groups with other functional monomers, the other functional monomers include acrylonitrile, lithium acrylate, lithium methacrylate, alkyl acrylate, alkyl methacrylate, aryl acrylate, and aryl methacrylate. , One or more of the following; The molar ratio of the monomer containing the bicyclic mechanosensitive group to other functional monomers is (1-99):(1-99).
3. The stress-dissipating polymer binder according to claim 2, characterized in that, The molar ratio of the monomer containing the bicyclic structure mechanosensitive group to the other functional monomers is (5-10):(95-90).
4. The stress-dissipating polymer adhesive according to any one of claims 1-3, characterized in that, The self-polymerization or copolymerization is completed in the presence of an initiator, wherein the amount of initiator added is 0.5%-1.0% of the total mass of the monomers.
5. The stress-dissipating polymer adhesive according to claim 4, characterized in that, The initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, and azobiscyclohexylformitrile.
6. A method for preparing the stress-dissipating polymer adhesive according to claim 1, characterized in that, The raw material monomer is dissolved in an organic solvent and polymerized at 60-80℃ for 5-24 h in the presence of an initiator; wherein the raw material monomer is a monomer with a bicyclic structure and a mechanosensitive group, or other functional monomers.
7. The application of the stress-dissipating polymer adhesive according to claim 1, characterized in that: The stress-dissipating polymer binder is used in one or more of the preparation of sulfide solid lithium / sodium battery electrodes and electrolyte membranes.
8. The application of the stress-dissipating polymer binder according to claim 7, characterized in that: The binder is used to prepare one or more of the positive and negative electrode sheets and sulfide electrolyte membranes of sulfide solid lithium / sodium batteries through wet or dry processes.
9. A sulfide solid-state battery, comprising positive and negative electrode plates and an electrolyte membrane, characterized in that: The binder described in claim 1 is added to one or more of the positive and negative electrode sheets and the electrolyte membrane.
10. The sulfide solid-state lithium / sodium battery according to claim 9, characterized in that: The positive or negative electrode sheet is formed by coating a mixture of electrode active material, sulfide electrolyte, conductive agent and stress dissipation polymer binder as described in claim 1 onto a current collector; wherein the mass ratio of electrode active material, sulfide electrolyte, conductive agent and stress dissipation polymer binder as described in claim 1 is (50-85):(10-20):(2-5):(3-25). The electrolyte membrane is formed of a sulfide electrolyte and the stress-dissipating polymer binder of claim 1; wherein the mass ratio of the sulfide electrolyte to the stress-dissipating polymer binder is (70-99):(1-30).
Citation Information
Patent Citations
Sulfide solid electrolyte film based on self-healing binder, preparation method of sulfide solid electrolyte film and all-solid-state lithium battery
CN116190767A
Sulfide solid electrolyte membrane, preparation method thereof and all-solid-state battery