A functional wax and its preparation method

High-purity functional waxes are prepared by catalytic copolymerization or oxidation of ethylene with polar monomers, which solves the problems of insufficient stability and processing performance of existing functional waxes and achieves the effects of controllable melting point, high purity and low energy consumption.

CN123106968APending Publication Date: 2026-11-17SHANGHAI INST OF ORGANIC CHEM CHINESE ACAD OF SCI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510635751.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing functional waxes suffer from defects such as poor stability, poor processing performance, and limited functionality. There is a lack of high-purity functional waxes with excellent performance and a narrow melting point range on the market.

Method used

High-purity functional waxes with narrow melting point ranges can be prepared by catalyzing the copolymerization of ethylene and polar monomers with a bidentate Ni ligand catalyst of a specific structure, or by oxidizing or dihydroxylating polyolefins containing double bonds.

Benefits of technology

It achieves high purity and good compatibility of functional waxes, with melting points between 80-100℃, melting enthalpy ≥180J/g, and oxygen content of 0.1-6.0%, simplifying the process and reducing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005406603550000021
    Figure BDA0005406603550000021
  • Figure BDA0005406603550000022
    Figure BDA0005406603550000022
  • Figure BDA0005406603550000061
    Figure BDA0005406603550000061
Patent Text Reader

Abstract

This invention discloses a functional wax and its preparation method. Specifically, the functional wax disclosed in this invention has the following characteristics: (a) a white or pale yellow solid, free from visible mechanical impurities; inorganic content <100ppm; metal content <10ppm; (b) a high melting peak temperature (T0). pm (c) Number-average molecular weight is 600-4000 g / mol, and molecular weight distribution PDI < 3; (d) Temperature T for 5% thermal weight loss d5 ≥200℃; (e) oxygen content of 0.1-6.0%; and / or (f) solubility in alkanes: ≥10g / 100mL at >90℃.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of petrochemical and fine chemical technology. Specifically, this invention relates to a functional wax and its preparation method. Background Technology

[0002] Functional waxes are wax materials with specific functions prepared through chemical modification, physical compounding, or special processes. They possess new properties compared to traditional waxes, such as increased viscosity, hardening, lubrication, antistatic properties, and antioxidant properties, and are widely used in coatings, inks, plastics, cosmetics, and pharmaceuticals. Traditional waxes are derived from natural waxes (such as beeswax, carnauba wax, and paraffin wax) and synthetic waxes (such as polyethylene wax and Fischer-Tropsch wax). Traditional waxes generally have low melting points and low viscosity. Existing functional waxes on the market may have drawbacks such as poor stability, poor processing performance, and limited functionality.

[0003] Therefore, developing functional waxes with comprehensive functions and excellent performance is of great significance. Summary of the Invention

[0004] The purpose of this invention is to provide a high-purity functional wax with a narrow melting point range and its preparation method.

[0005] In a first aspect of the present invention, a functional wax is provided, the functional wax having the following characteristics:

[0006] (a) White or pale yellow solid, free from visible mechanical impurities; inorganic content <100ppm; metal content <10ppm;

[0007] (b) Peak melting temperature (T) pm The temperature is 80-100℃, and the enthalpy of melting is ≥180J / g;

[0008] (c) Number-average molecular weight is 600-4000 g / mol, and molecular weight distribution PDI < 3;

[0009] (d) Temperature T at which thermal weight loss is 5% d5 ≥200℃;

[0010] (e) The oxygen content is 0.1-6.0%; and / or

[0011] (f) Solubility in alkanes: >90℃, solubility ≥10g / 100mL.

[0012] In another preferred embodiment, the alkane is selected from the group consisting of high-boiling-range petroleum ether, heptane, and octane.

[0013] In another preferred embodiment, the peak melting temperature (T) of the functional wax is... pm The temperature is 90-100℃.

[0014] In another preferred embodiment, the number-average molecular weight of the functional wax is 600-2000 g / mol.

[0015] In another preferred embodiment, the number-average molecular weight is 700-1500 g / mol; more preferably, it is 700-1250 g / mol.

[0016] In another preferred embodiment, the functional wax exhibits a 5% thermal weight loss at temperature T. d5 ≥210℃; preferably, T d5 ≥220℃.

[0017] In another preferred embodiment, the oxygen content of the functional wax is 0.5-5.0%.

[0018] In another preferred embodiment, the oxygen content is 2.0-5.0%.

[0019] In another preferred embodiment, the oxygen element is present in the form selected from the group consisting of -OH, OR, epoxy group, carbonyl group, and COOH, wherein R is selected from the group consisting of methyl and ethyl.

[0020] In a second aspect of the present invention, a method for preparing the functional wax described in the first aspect of the present invention is provided, comprising the following steps:

[0021] The functional wax is obtained by copolymerizing ethylene with a polar monomer in the presence of a catalyst and a co-catalyst at 30-80℃ and 0.5-2.0MPa ethylene pressure.

[0022] The catalyst has the structure shown in Formula I:

[0023]

[0024] Among them, R 1 H, methyl, ethyl; R 2 It is a C1-C4 alkyl group.

[0025] In another preferred embodiment, R 2 Selected from the following group: methyl, ethyl, n-propyl, isopropyl.

[0026] In another preferred embodiment, the catalyst is selected from the group consisting of:

[0027]

[0028] In another preferred embodiment, the ethylene pressure is 0.5-1.0 MPa.

[0029] In another preferred embodiment, the temperature of the copolymerization reaction is 30-50°C.

[0030] In another preferred embodiment, the copolymerization reaction is carried out in an inert solvent.

[0031] In another preferred embodiment, the inert solvent is selected from the group consisting of aromatic solvents, alkane solvents, or combinations thereof; more preferably, the inert solvent is selected from the group consisting of toluene and hexane.

[0032] In another preferred embodiment, the polar monomer is a C3-C6 olefin having a polar group selected from the group consisting of carboxyl and hydroxyl groups.

[0033] In another preferred embodiment, the polar monomer is a C3-C6 olefin substituted with hydroxyl and / or carboxyl groups.

[0034] In another preferred embodiment, the polar monomer is selected from the group consisting of acrylic acid and 3-butenoic acid.

[0035] In another preferred embodiment, the molar ratio of the polar monomer to the catalyst is (2000-8000):1.

[0036] In another preferred embodiment, the co-catalyst is an alkylaluminum.

[0037] In another preferred embodiment, the co-catalyst is selected from the group consisting of: dichloroethylaluminum, diethylaluminum chloride, triethylaluminum, triisobutylaluminum, sesquichlorinated ethylaluminum, sesquichlorinated butylaluminum, aluminoxane, or methylaluminoxane.

[0038] In another preferred embodiment, the molar ratio of the co-catalyst to the catalyst is (1000-4000):1.

[0039] In a third aspect of the present invention, a method for preparing the functional wax described in the first aspect of the present invention is provided, comprising the following steps:

[0040] Polyolefins containing double bonds are obtained by oxidation with an oxidizing agent; or

[0041] Polyolefins containing double bonds are obtained by dihydroxylation reaction using a dihydroxylating agent.

[0042] In another preferred embodiment, the double-bonded polyolefin is polyethylene.

[0043] In another preferred embodiment, the molecular weight of the polyolefin containing double bonds is 600-2000.

[0044] In another preferred embodiment, the oxidizing agent is selected from the group consisting of m-chlorobenzoic acid peroxide, peracetic acid, and hydrogen peroxide.

[0045] In another preferred embodiment, the oxidation reaction takes 4-10 hours, more preferably 6-8 hours.

[0046] In another preferred embodiment, the oxidation reaction is carried out at a temperature of 50-100°C; more preferably, at 60-80°C.

[0047] In another preferred embodiment, the oxidation and dihydroxylation reactions are carried out in an aromatic solvent.

[0048] In another preferred embodiment, after the oxidation reaction is completed, the product is post-treated with an alcohol solvent to precipitate a solid, i.e., the oxidation product.

[0049] In another preferred embodiment, the molar amount of the oxidizing agent or the dihydroxylating agent is 1-3 times, more preferably 1.1-2 times, the molar amount of the polyolefin containing the double bond.

[0050] In another preferred embodiment, the dihydroxylating agent is selected from the group consisting of osmium tetroxide (OsO4), potassium permanganate (KMnO4), and peroxyacid / hydrogen peroxide systems.

[0051] In a fourth aspect of the invention, a use of the functional wax described in the first aspect of the invention is provided, for use as a lubricant, dispersant, release agent, additive, and desensitizer.

[0052] It should be understood that, within the scope of this invention, the above-described technical features of this invention and the technical features specifically described below (such as in the embodiments) can be combined with each other to form new or preferred technical solutions. Due to space limitations, they will not be described in detail here. Detailed Implementation

[0053] Through extensive and in-depth research, the inventors have provided a high-purity functional wax with a narrow melting point range. This functional wax is prepared by catalyzing ethylene and polar monomers containing oxygen groups using a bidentate Ni ligand catalyst with a specific structure, or by oxidizing or hydroxylating polyolefins containing double bonds. The functional wax of this invention exhibits good compatibility and adhesion, with a melting point between 80-100°C, a melting enthalpy ≥180 J / kg, and an oxygen content of 0.1-6.0%. It allows for precise control of the melting point, improving product purity, simplifying the process, and reducing energy consumption. Based on these characteristics, the inventors completed this invention.

[0054] Functional wax

[0055] Functional waxes are materials that, through chemical modification, compounding, or the addition of functional ingredients, impart special physicochemical properties or functional characteristics to traditional waxes (such as paraffin wax, beeswax, and microcrystalline wax). Compared with ordinary waxes, functional waxes possess superior heat resistance, lubricity, adhesion, wear resistance, conductivity, optical properties, and environmental adaptability, and are widely used in chemical, pharmaceutical, electronics, textile, coating, and food industries. They appear as white or pale yellow lumps, flakes, or powdery solids with a relative molecular mass of 1000–5000; their molecular chains contain polar groups such as hydroxyl and carboxyl groups, exhibiting good compatibility with polymers, making them suitable as heat stabilizers and internal / external lubricants in PVC processing; through esterification or hydrogenation modification, their adhesion is improved, leading to their use in pharmaceutical ointments, cosmetic lipsticks, and wax-based coatings. Functional waxes are developing towards low toxicity, high efficiency, and multifunctional composites, and will have broader application prospects in fields such as bio-based materials and new energy in the future.

[0056] Currently, there are three methods for producing functional waxes. The first method is oxidation, which uses ordinary PE wax as raw material and introduces oxygen-containing groups through an oxidation reaction under certain conditions. Air or oxygen is typically used as the oxidant, and under the action of a catalyst, some carbon-hydrogen bonds in the PE wax molecule are oxidized into oxygen-containing groups such as hydroxyl and carboxyl groups. The second method is transesterification, which utilizes PE wax to undergo a transesterification reaction with ester compounds containing oxygen-containing groups, introducing these groups into the PE wax molecule. For example, fatty acid esters can be used to undergo transesterification with PE wax under the action of a catalyst, causing some segments of the PE wax molecule to be replaced by oxygen-containing groups from the fatty acid ester. Transesterification is usually a reversible reaction, and to achieve a high conversion rate, a long reaction time is often required, which reduces production efficiency and increases production cycle and cost. Moreover, this method may cause various side reactions, such as intramolecular transesterification and polymer chain degradation, which can affect the structure and properties of the product. The third method is graft copolymerization, which utilizes monomers containing oxygen-containing groups to undergo a graft copolymerization reaction with PE wax, introducing these groups into the PE wax molecular chain. For example, monomers containing double bonds and oxygen-containing groups, such as acrylic acid and maleic anhydride, can be selected. Under the action of an initiator, the double bonds of the monomers undergo an addition reaction with the active sites on the PE wax molecular chain, thereby achieving graft copolymerization. However, the grafting rate is difficult to control in this method; too high or too low a grafting rate may lead to unsatisfactory product performance, failing to meet specific application requirements.

[0057] This invention provides a method for preparing functional waxes by copolymerizing ethylene and polar monomers via metal complex catalysis. This method is simple, allows for precise control of the product structure, resulting in functional waxes with good compatibility and adhesion, a melting point between 80-100℃, a melting enthalpy ≥180J / g, and an oxygen content of 0.1-6.0%. Optimizing the reaction conditions can achieve precise control of the melting point, improved product purity, simplified process, and reduced energy consumption.

[0058] The testing methods for all characteristics of the functional wax of the present invention are conventional testing methods well known to those skilled in the art, as detailed below:

[0059] (1) The oxygen and metal content of the polymer can be obtained through elemental analysis.

[0060] (2) The content of inorganic matter can be obtained by ash content determination or thermogravimetric analysis;

[0061] (3) The peak melting temperature T of the polymer was obtained by DSC testing. pm and enthalpy of fusion;

[0062] (4) The temperature at which the polymer loses 5% of its thermal weight is obtained by TGA test; the temperature is controlled to rise from room temperature to 600.0℃ while maintaining a heating rate of 10.0℃ / min; nitrogen flow rate: 50.0mL / min and nitrogen is maintained for 1-2 hours before the test begins.

[0063] (5) The number-average molecular weight and molecular weight distribution of the polymer were obtained by GPC testing;

[0064] (6) Solubility test method: Weigh a certain amount of polymer sample and add it to petroleum ether with a boiling range of (90~120)℃. Heat and reflux with stirring until the sample is completely dissolved in petroleum ether and the system is visually clear. Record the amount of sample dissolved and the volume of solvent at this time, in g / 100mL.

[0065] Preparation method of functional wax

[0066] The present invention also provides a method for preparing a functional wax, which uses a specific catalyst and a co-catalyst to cause ethylene and a polar monomer to undergo a copolymerization reaction to obtain the functional wax.

[0067] Specifically, the preparation method of the functional wax of the present invention includes the following steps:

[0068] The functional wax is obtained by copolymerizing ethylene with a polar monomer in the presence of a catalyst and a co-catalyst at 30-80℃ and 0.5-2.0MPa ethylene pressure.

[0069] The catalyst described herein is prepared using a method disclosed in the applicant's earlier application CN 112390904A, which is incorporated herein by reference. In particular, the catalyst suitable for the preparation method of this invention has the following structure:

[0070]

[0071] Among them, R 1 H, methyl, ethyl; R2 It is a C1-C4 alkyl group.

[0072] Preferably, the catalyst is selected from the group consisting of:

[0073]

[0074] The reaction conditions for the copolymerization reaction can be the conventional reaction conditions for this type of reaction in the art; for example, the following reaction conditions:

[0075] Any conventional technique in the field can be used, such as slurry polymerization, loop polymerization, gas-phase polymerization, or other forms of conventional polymerization reaction processes.

[0076] The copolymerization reaction is generally carried out in an inert solvent, such as hydrocarbons, cyclic hydrocarbons, or aromatic hydrocarbons. To facilitate reactor operation and polymerization products, the type of inert solvent is not particularly limited; hydrocarbons with fewer than 12 carbon atoms can be used, such as one or more of propane, isobutane, n-pentane, 2-methylbutane, hexane, toluene, and chlorobenzene.

[0077] The temperature of the copolymerization reaction is not particularly limited and is selected according to the equipment used in the polymerization reaction and the target product. Preferably, the temperature of the copolymerization reaction can be maintained between 20 and 100°C, and to achieve good catalytic activity and production capacity, it can be maintained between 30 and 80°C.

[0078] The copolymerization reaction time is not particularly limited and can vary from 0.5 h to 12 h, preferably from 0.5 h to 4 h, depending on the equipment used and the target product. In a preferred embodiment of the invention, operating within 0.5 h to 2 h yields better reactor operating parameters and polymer.

[0079] The pressure of the copolymerization reaction is not particularly limited and can vary from 0.1 to 10 MPa, preferably from 0.1 to 5 MPa, depending on the equipment used in the copolymerization reaction and the target product. In a preferred embodiment of the invention, better reactor operating parameters and polymers can be obtained by operating within the range of 0.1 to 3 MPa.

[0080] In the copolymerization reaction described herein, the cocatalyst may be a conventional cocatalyst in this type of reaction in the art, such as alkyl aluminum compounds (e.g., one or more of AlEt3, AlEt2Cl, AlEtCl2, AlMe2Cl, AlMe3 and Al(iBu)3), alkyl aluminum oxanes [e.g., methyl aluminum oxane (e.g., a product purchased from AkzoNobel, 1.5 M (mol / L) toluene solution), modified / modified methyl aluminum oxane (e.g., a product purchased from AkzoNobel, 2.0 M (mol / L) n-heptane solution), ethyl aluminum oxane and butyl aluminum oxane], and one or more metal salts containing weakly coordinating anions (e.g., Na[B(3,5-(CF3)2C6H3)4] and / or AgOSO2CF3).

[0081] Before the copolymerization reaction, the polar monomer may be pretreated with conventional reagents or without pretreatment {e.g., one or more of the following: tert-butyldimethylsilyl (TBS) reagents (e.g., tert-butyldimethylsilyltrifluoromethanesulfonate, tert-butyldimethylchlorosilane), trimethylolaminoethanesulfonic acid (TES), tert-butyldiphenylsilyl (TBDPS) reagents, trimethylsilyl reagents (TMS, trimethylchlorosilane), alkylaluminum compounds (e.g., AlEt3, AlEt2Cl, AlEtCl2, AlMe2Cl, AlMe3, Al(iBu)3), and alkylaluminoxanes (e.g., methylaluminoxane, ethylaluminoxane, butylaluminoxane, modified methylaluminoxane)}. However, regardless of whether pretreatment is performed, the catalyst and the co-catalyst can effectively catalyze the copolymerization of ethylene and the polar monomer.

[0082] In the method of the present invention, the molar ratio of the polar monomer to the catalyst is (2000-8000):1; preferably (3000-6000):1; more preferably (4500-5500):1.

[0083] In this invention, an equivalent or slightly larger amount of alkylaluminum is pre-contacted with the polar monomer to form a protective layer for the catalyst; and a large amount of alkylaluminum is added as a co-catalyst during the polymerization process.

[0084] In the method of the present invention, the molar ratio of the co-catalyst to the catalyst is (1000-4000):1; preferably (2000-4000):1; and more preferably (3000-4000):1.

[0085] Alternatively, the functional wax of the present invention can also be obtained by oxidizing or dihydroxylating a polyolefin containing double bonds. There are no particular limitations on the reaction time and temperature, as long as the reaction can be completed conveniently. Specifically, the oxidizing agent used in the oxidation reaction is a commonly used oxidizing agent in the art, without particular limitations, such as m-chlorobenzoic acid peroxide, peracetic acid, or hydrogen peroxide; the dihydroxylating agent used in the dihydroxylating reaction is a commonly used dihydroxylating agent in the art, without particular limitations, such as osmium tetroxide (OsO4), potassium permanganate (KMnO4), or a peroxyacid / hydrogen peroxide system. There are no particular limitations on the reaction solvent for the oxidation or dihydroxylating reaction; it can be carried out in an inert solvent, such as an aromatic solvent. After the reaction is complete, an alcohol reagent can be added to precipitate the product, which, after filtration, washing, and drying, yields the functional wax.

[0086] The preparation method of the functional wax of the present invention also includes adding silica gel or diatomaceous earth, heating and refluxing for 1-2 hours, filtering while hot to remove inorganic matter or metal, and drying to obtain ethylene copolymer, i.e., the functional wax.

[0087] application

[0088] The functional wax of this invention incorporates oxygen-containing polar groups, enhancing its internal lubrication while maintaining a certain level of external lubrication, thus achieving a balance between internal and external lubrication performance. Therefore, it can be used as a lubricant. The introduction of polar groups improves the dispersibility of the functional wax with inorganic pigments and fillers, reducing agglomeration and improving coating uniformity; therefore, it can be used as a dispersant and additive. Furthermore, it exhibits better compatibility with polar resins, enhancing coating functionality. Due to its high thermal decomposition temperature, the functional wax demonstrates enhanced stability and is suitable for high-temperature extrusion or injection molding processes.

[0089] Furthermore, due to the introduction of oxygen-containing groups, the functional wax has higher degradability and can be used in food packaging and medical fields.

[0090] In summary, the functional wax of the present invention can be used as a lubricant, dispersant, release agent, additive, desensitizer, etc.

[0091] Compared with the prior art, the main advantages of the present invention include:

[0092] (1) The functional wax provided by the present invention has high purity, is a white or light yellow solid, and has no visible mechanical impurities; the inorganic content is <100ppm; and the metal content is <10ppm.

[0093] (2) The present invention uses a bidentate Ni ligand catalyst with a specific structure to catalyze the preparation of the functional wax from ethylene and polar monomers.

[0094] (3) The functional wax of the present invention has good compatibility and adhesion, and has a melting point between 80-100℃, a melting enthalpy ≥180J / kg, and an oxygen content of 0.1-6.0%.

[0095] (4) The functional wax of the present invention can achieve precise control of melting point, improve product purity, simplify process and reduce energy consumption.

[0096] (5) The functional wax of the present invention can be used as a lubricant, dispersant, release agent, additive, desensitizer, etc.

[0097] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods in the following embodiments, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. Percentages and parts are by weight unless otherwise stated.

[0098] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as are familiar to those skilled in the art. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to the methods of this invention. The preferred embodiments and materials described herein are for illustrative purposes only.

[0099] Example 1: Copolymerization of ethylene and acrylic acid

[0100] Under a nitrogen atmosphere, toluene (50 mL) and Et2AlCl solution (molar ratio of Et2AlCl to catalyst of 3000) were sequentially added to a 300 mL autoclave that had been dried by vacuum heating. The mixture was stirred for 5 min at an oil bath temperature of 50 °C. Then, 50 mmol of acrylic acid was added. The reaction was exothermic and violent. After stirring for 5-10 min, the temperature was lowered to 50 °C, and then the catalyst solution (I-1, 10 μmol) was added. Immediately after the addition, ethylene was introduced (1.0 MPa). After reacting for 30 min, the ethylene was cut off. After cooling to room temperature, the autoclave was opened, and the reaction was terminated with 5% acidified ethanol. The polymer was obtained by precipitation and filtration. The polymer was then mixed with silica gel or diatomaceous earth and heated under reflux for 1-2 h. The mixture was then filtered while hot to remove inorganic or metallic impurities. After drying, the ethylene copolymer was obtained. The polymer test results are shown in Table 1.

[0101] Example 2: Copolymerization of ethylene and acrylic acid

[0102] Example 1 was repeated, except that the catalyst was I-2, and the polymer test results are shown in Table 1.

[0103] Example 3: Copolymerization of ethylene and acrylic acid

[0104] Example 1 was repeated, except that the catalyst was I-3, and the polymer test results are shown in Table 1.

[0105] Example 4: Copolymerization of ethylene and 3-butenoic acid

[0106] Example 1 was repeated, except that the polar monomer was 3-butenoic acid, and the polymer test results are shown in Table 1.

[0107] Example 5: Copolymerization of ethylene and 3-butenoic acid

[0108] Example 1 was repeated, except that the catalyst was I-2 and the polar monomer was 3-butenoic acid. The polymer test results are shown in Table 1.

[0109] Example 6: Copolymerization of ethylene and 3-butenoic acid

[0110] Example 1 was repeated, except that the catalyst was I-3 and the polar monomer was 3-butenoic acid. The polymer test results are shown in Table 1.

[0111] Example 7: Copolymerization of ethylene and acrylic acid

[0112] Example 1 was repeated, except that the solvent was hexane, and the polymer test results are shown in Table 1.

[0113] Example 8: Copolymerization of ethylene and acrylic acid

[0114] Example 1 was repeated, except that the ethylene pressure was 0.5 MPa, and the polymer test results are shown in Table 1.

[0115] Example 9: Epoxidation reaction

[0116] 6 g of polyethylene containing double bonds was added to a 500 mL flask, dissolved in 250 mL of toluene, and then 9 g of m-chloroperoxybenzoic acid was added. The mixture was heated to 60 °C and reacted for 6 h. After the reaction was completed by NMR spectroscopy, the product was poured into 600 mL of anhydrous methanol, and a solid precipitated. After filtration, washing, and drying, 5.98 g of the epoxidized product was obtained. The test results are shown in Table 1.

[0117] Table 1

[0118]

[0119] In summary, as shown in Table 1 above, the functional wax provided by this invention has a narrow melting temperature range of 80-100℃, a metal content of <10ppm and an inorganic content of <100ppm; a solubility in alkanes of ≥10g / 100mL, and an oxygen content of 3-4.5%.

[0120] Test Example 1: Solubility Test

[0121] The functional waxes prepared in Examples 1-9 of this invention were subjected to solubility tests in high-boiling-range petroleum ether (the test method is as described above), and the results are shown in Table 1. It can be seen that the high-melting-point polyethylene wax of this invention has a solubility ≥10 g / 100 mL in alkane solvents, indicating that the functional wax of this invention has high solubility and can form a uniform dispersion system in alkane solvents, making it suitable for applications in plastics processing, coatings, inks, hot melt adhesives, cosmetics, and other fields.

[0122] All documents mentioned in this invention are incorporated herein by reference as if each document were individually incorporated by reference. Furthermore, it should be understood that after reading the foregoing teachings of this invention, those skilled in the art can make various alterations or modifications to this invention, and these equivalent forms also fall within the scope defined by the appended claims.

Claims

1. A functional wax, characterized in that, The functional wax described above has the following characteristics: (a) White or pale yellow solid, free from visible mechanical impurities; inorganic content <100ppm; metal content <10ppm; (b) a melting peak temperature (T pm ) of 80 to 100 °C and a melting enthalpy > 180 J / g; (c) Number-average molecular weight is 600-4000 g / mol, and molecular weight distribution PDI < 3; (d) temperature T at which 5% thermal weight loss d5 ≥ 200 °C; (e) The oxygen content is 0.1-6.0%; and / or (f) Solubility in alkanes: >90℃, solubility ≥10g / 100mL.

2. The functional wax of claim 1, wherein, The melting peak temperature (T pm ) of the functional wax is 90-100°C.

3. The functional wax of claim 1, wherein The number-average molecular weight of the functional wax is 600-2000 g / mol.

4. The functional wax as described in claim 1, characterized in that, The functional wax has a temperature T at which 5% of the wax is lost by thermal degradation d5 ≥ 210°C; preferably, T d5 ≥ 220°C.

5. The functional wax as described in claim 1, characterized in that, The oxygen content of the functional wax is 0.5-5.0%.

6. A method for preparing the functional wax according to claim 1, characterized in that, Includes the following steps: The functional wax is obtained by copolymerizing ethylene with a polar monomer in the presence of a catalyst and a co-catalyst at 30-80℃ and 0.5-2.0MPa ethylene pressure. The catalyst has the structure shown in Formula I: wherein R 1 is H, methyl, ethyl; R 2 is C1-C4 alkyl.

7. The preparation method according to claim 6, characterized in that, The polar monomer is selected from the group consisting of C3-C6 olefins substituted with hydroxyl and / or carboxyl groups; preferably acrylic acid or 3-butenoic acid.

8. The preparation method according to claim 6, characterized in that, The molar ratio of the polar monomer to the catalyst is (2000-8000):

1.

9. A method for preparing the functional wax according to claim 1, characterized in that, Includes the following steps: Polyolefins containing double bonds are obtained by oxidation with an oxidizing agent; or Polyolefins containing double bonds are obtained by dihydroxylation reaction using a dihydroxylating agent.

10. The use of the functional wax according to claim 1, characterized in that, It is used as a lubricant, dispersant, release agent, additive, and desensitizer.

Citation Information

Patent Citations

  • Polyethylene containing polar functional groups, and preparation method thereof

    CN112390904A