Polyethylene copolymers, their products and methods
By polymerizing ethylene, branched vinyl esters, and vinyl acetate copolymers, the problem of controlling the molecular weight and molecular weight distribution of polyolefin materials has been solved, and the preparation of polymer compositions with optimized performance has been achieved.
Patent Information
- Application Number
- CN202611219153.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-04
- Filing Date
- 2020-10-05
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polyolefin materials have difficulty in effectively controlling molecular weight and molecular weight distribution during the preparation process, resulting in poor performance in different applications.
By preparing copolymers of ethylene, branched vinyl ester monomers, and vinyl acetate, polymer compositions with specific molecular weights and molecular weight distributions are formed under different pressure and temperature conditions using free radical initiators.
Precise control of the molecular weight and molecular weight distribution of polymer compositions has been achieved, improving their performance in various applications, including the adjustment of physical properties such as crystallinity, hardness, and melting temperature.
Smart Images

Figure CN123106969A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to polyethylene copolymers, their products, and methods. Background Technology
[0002] The production of polyolefin materials (such as polyethylene (PE) and polypropylene (PP)) boasts the highest production volumes of any synthetic polymer invented to date. This success is largely attributed to the low production costs, energy efficiency, low greenhouse gas emissions, versatility in producing a wide range of polymers with varying properties, and high polymer processing performance. A broad range of products made using polyolefin materials include films, molded products, foams, pipes, textiles, and more. These products are also attractive for recycling via pyrolysis into gases and oils or by incineration into energy. The physical and chemical properties of polyolefin compositions can vary depending on factors such as molecular weight, molecular weight distribution; the content, properties, and distribution of comonomers (or multiple comonomers); the presence and distribution of short-chain and / or long-chain branches; thermal and shear processes; and similar factors defining their feasibility in certain applications. To further enhance their applications, polyolefins can be formulated with a range of possible comonomers into random and block copolymers, as well as with a range of possible additives into mixtures. Summary of the Invention
[0003] This overview is provided to introduce the selection of concepts further described in the following detailed description. This overview is not intended to identify key or essential features of the subject matter for which protection is sought, nor is it intended to help limit the scope of the subject matter for which protection is sought.
[0004] In one or more aspects, the embodiments disclosed herein relate to a polymer composition comprising a polymer prepared from ethylene, one or more branched vinyl ester monomers, and optionally vinyl acetate, wherein said polymer has a number-average molecular weight in the range of 5 to 10,000 kDa and a molecular weight distribution in the range of 1 to 60, as obtained by GPC.
[0005] In another aspect, the embodiments disclosed herein relate to an article prepared from a polymer composition comprising a polymer prepared from ethylene, one or more branched vinyl ester monomers, and optionally vinyl acetate, wherein the polymer has a number-average molecular weight in the range of 5 to 10,000 kDa and a molecular weight distribution in the range of 1 to 60, as obtained by GPC.
[0006] Other aspects and advantages of the claimed subject matter will become apparent from the following description and the appended claims. Attached Figure Description
[0007] Figure 1 Showing some samples according to embodiments of this disclosure13 C NMR spectrum.
[0008] Figure 2 Showing some samples according to embodiments of this disclosure 1 H NMR spectrum.
[0009] Figure 3 It is a graphical depiction of viscometer gel permeation chromatography (GPC) chromatograms obtained from some samples according to embodiments of this disclosure.
[0010] Figures 4A-4C It is a graphical depiction of two-dimensional liquid chromatography (2D-LC) chromatograms of some samples according to embodiments of this disclosure.
[0011] Figures 5A-5C It is a graphical depiction of differential scanning calorimetry (DSC) results for some samples according to embodiments of this disclosure.
[0012] Figures 6A-6B It is a graphical depiction of the dynamic mechanical analysis (DMA) results of some samples according to the embodiments of this disclosure.
[0013] Figures 7A-7B It is a graphical depiction of thermogravimetric analysis (TGA) thermal spectra of some samples according to embodiments of this disclosure.
[0014] Figures 8A-8B It is a graphical depiction of the continuous self-nucleation and annealing (SSA) results of some samples according to embodiments of this disclosure. Detailed Implementation
[0015] In one aspect, the embodiments disclosed herein relate to a polymer composition comprising a copolymer prepared from ethylene and one or more branched vinyl ester monomers, and a ternary polymer prepared from ethylene, branched vinyl esters, and vinyl acetate. In one or more embodiments, the polymer composition may be prepared by reacting ethylene with one or more branched vinyl esters and optionally vinyl acetate (which modifies various properties of the resulting copolymer, particularly including crystallinity, hardness, melting temperature, and glass transition temperature).
[0016] The polymer compositions according to this disclosure may include copolymers incorporating ethylene and one or more branched vinyl esters in multiple ratios. In some embodiments, the polymer composition may be prepared by reacting ethylene with branched vinyl esters in the presence of additional comonomers and one or more free radical initiators to form a copolymer. In other embodiments, a ternary polymer may be prepared by reacting ethylene with a first comonomer to form a polymer resin or prepolymer, and then reacting it with a second comonomer to prepare the final polymer composition, wherein the first and second comonomers may be added in the same reactor or in different reactors. In one or more embodiments, the copolymer may be prepared by reacting ethylene with one or more comonomers in one or more polymerization stages to obtain multiple repeating unit microstructures. In one or more embodiments, the polymer composition may include a polymer derived from monomers derived from petroleum and / or renewable resources.
[0017] Branched vinyl ester monomers
[0018] In one or more embodiments, the branched vinyl ester may comprise a branched vinyl ester produced from a mixture of isomers of a branched alkyl acid. The branched vinyl ester according to this disclosure may have a general chemical formula (I):
[0019] (I)
[0020] Where R 1 R 2 and R 3 It has a combination of carbon numbers in the range of C3 to C20. In some embodiments, R 1 R 2 and R 3 It can be entirely alkyl chains, and in some embodiments, it has different degrees of branching; or in some embodiments, R 1 R 2 and R 3 A subset of can be independently selected from groups consisting of hydrogen, alkyl, or aryl groups.
[0021] In one or more embodiments, the vinyl carbonyl monomer may comprise a vinyl ester having a branch of the general chemical formula (II):
[0022] (II)
[0023] Where R 4 and R 5 Having a combined carbon number of 6 or 7, and the polymer composition having a number-average molecular weight (Mn) in the range of 5 kDa to 10000 kDa obtained by GPC. nIn one or more implementations, R 4 and R 5 It can have a combined carbon number of less than 6 or greater than 7, and the polymer composition can have an M value of up to 10,000 kDa. n In other words, when M n When R is less than 5kDa, 4 and R 5 It can have a combination of carbon numbers less than 6 or greater than 7; however, if M n Greater than 5 kDa, such as in the range of 5 to 10000 kDa, R 4 and R 5 It can include combinations of 6 or 7 carbons. In a particular embodiment, R 4 and R 5 It has a combination of 7 carbons and M n It can be in the range of 5 to 10,000 kDa. Furthermore, in one or more particular embodiments, the vinyl carbonyl group according to formula (II) can be used in combination with vinyl acetate.
[0024] Examples of branched vinyl esters may include monomers having the following chemical structures, including their derivatives:
[0025]
[0026]
[0027] In one or more embodiments, the polymer composition may include a polymer derived from monomers derived from petroleum and / or renewable resources.
[0028] In one or more embodiments, the branched vinyl ester may comprise a mixture of monomers and comonomers comprising vinyl esters such as neononanoic acid and neodecanoic acid. In some embodiments, the branched vinyl ester may comprise tertiary carboxylic acids from the Versatic™ acid series, including Versatic™ acid EH, Versatic™ acid 9, and Versatic™ acid 10 synthesized by Koch and commercially available from Hexion™ Chemicals. In one or more embodiments, the polymer composition may comprise a polymer derived from monomers derived from petroleum and / or renewable resources.
[0029] The polymer composition according to this disclosure may include ethylene, the weight percentage of which is determined by proton nuclear magnetic resonance (NMR). 1 H NMR) and carbon-13 NMR ( 13C NMR) measurements are taken within a range from a lower limit selected from one of 10 wt%, 20 wt%, or 30 wt% to an upper limit selected from one of 60 wt%, 70 wt%, 80 wt%, 90 wt%, 95 wt%, 99.9 wt%, and 99.99 wt%, where any lower limit may be paired with any upper limit.
[0030] The polymer compositions according to this disclosure may include vinyl ester monomers, such as vinyl ester monomers of formulas (I) and (II) above, wherein the weight percentage of the vinyl ester monomer is determined by... 1 H NMR and 13 C NMR measurements are taken from a lower limit selected from one of 0.01 wt%, 0.1 wt%, 1 wt%, 5 wt%, 10 wt%, 20 wt%, or 30 wt% to an upper limit selected from 50 wt%, 60 wt%, 70 wt%, 80 wt%, 89.99 wt%, or 90 wt%, where any lower limit may be paired with any upper limit.
[0031] In some embodiments, the polymer composition according to this disclosure may optionally include vinyl acetate, the weight percentage of which is determined by... 1 H NMR and 13 C NMR measurements are taken within a range from a lower limit selected from one of 0.01 wt%, 0.1 wt%, 1 wt%, 5 wt%, 10 wt%, 20 wt%, or 30 wt% to an upper limit selected from 50 wt%, 60 wt%, 70 wt%, 80 wt%, or 89.99 wt%, where any lower limit may be paired with any upper limit.
[0032] The polymer compositions according to this disclosure can have a number-average molecular weight (Mn) in kilodaltons (kDa). n The value is measured by gel permeation chromatography (GPC) within a range from a lower limit selected from one of 1 kDa, 5 kDa, 10 kDa, 15 kDa, and 20 kDa to an upper limit selected from one of 40 kDa, 50 kDa, 100 kDa, 300 kDa, 500 kDa, 1000 kDa, 5000 kDa, and 10000 kDa, where any lower limit can be paired with any upper limit.
[0033] The polymer compositions according to this disclosure can have such a weight-average molecular weight (M) in kilodaltons (kDa). wThe lower limit of the value is measured by GPC within a range from a lower limit selected from one of 1 kDa, 5 kDa, 10 kDa, 15 kDa, and 20 kDa to an upper limit selected from one of 40 kDa, 50 kDa, 100 kDa, 200 kDa, 300 kDa, 500 kDa, 1000 kDa, 2000 kDa, 5000 kDa, 10000 kDa, and 20000 kDa, where any lower limit can be paired with any upper limit.
[0034] According to this disclosure, polymer compositions can have a molecular weight distribution (MWD, defined as M...). w For M n The ratio, which is measured by GPC, has a lower limit of any one of 1, 2, 5 or 10 and an upper limit of any one of 20, 30, 40, 50 or 60, wherein any lower limit can be paired with any upper limit.
[0035] Initiators for free radical polymerization
[0036] The polymer compositions according to this disclosure may include one or more initiators for free radical polymerization, which are capable of generating free radicals in the reactant mixture that initiate the chain polymerization of comonomers and prepolymers. In one or more embodiments, the free radical initiator may include chemical species that spontaneously release free radicals or that release free radicals through degradation by stimulation of temperature, pH or other triggers.
[0037] In one or more embodiments, the free radical initiator may include peroxides and bifunctional peroxides, such as benzoyl peroxide, dicumyl peroxide, di-tert-butane peroxide, tert-butyl peroxide, tert-butyl-peroxy-2-ethylhexanoate, tert-butyl peroxypentanoate, tert-butyl peroxyneodecanate, tert-butyl-peroxy-benzoate, tert-butyl-peroxy-2-ethylhexanoate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxybenzoate, and tert-butyl-2-ethylhexanoate. Examples of compounds include basal carbonates, 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, 1,1-di(tert-butylperoxide)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tert-butylperoxide)hexyn-3, 3,3,5,7,7-pentamethyl-1,2,4-trioxacycloheptane, butyl valerate 4,4-di(tert-butylperoxide) ester, bis(2,4-dichlorobenzoyl peroxide), bis(4-methylbenzoyl peroxide), and bis(tert-butylperoxyisopropyl)benzene peroxide.
[0038] Free radical initiators may also include benzoyl peroxide, 2,5-di(isopropylphenylperoxy)-2,5-dimethylhexane, 2,5-di(isopropylphenylperoxy)-2,5-dimethylhexyn-3,4-methyl-4-(tert-butylperoxy)-2-pentanol, 4-methyl-4-(tert-pentylperoxy)-2-pentanol, 4-methyl-4-(isopropylphenylperoxy)-2-pentanol, 4-methyl-4-(tert-butylperoxy)-2-pentanone, 4-methyl-4-(tert-pentylperoxy)-2-pentanone, 4-methyl-4-(isopropylphenylperoxy)-2-pentanone, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-pentylperoxy)-2-pentanone, and 2,5-dimethyl-2,5-di(tert-pentylperoxy)-2-pentanone. 2,5-Dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(tert-pentylperoxy)hexyne-3, 2,5-dimethyl-2-tert-butylperoxy-5-hydroperoxyhexane, 2,5-dimethyl-2-isopropylphenylperoxy-5-hydroperoxyhexane, 2,5-dimethyl-2-tert-pentylperoxy-5-hydroperoxyhexane, m / p-α,α-di[(tert-butylperoxy)isopropyl]benzene, 1,3,5-tris(tert-butylperoxyisopropyl)benzene, 1,3,5-tris(tert-pentylperoxyisopropyl)benzene, 1,3,5-tris(isopropylphenylperoxyisopropyl)benzene, di[1,3-dimethyl-3-]carbonate [(tert-butylperoxy)butyl] ester, di[1,3-dimethyl-3-(tert-pentylperoxy)butyl] ester, di[1,3-dimethyl-3-(isopropylphenylperoxy)butyl] ester, ditert-pentane peroxide, tert-pentylisopropylbenzene peroxide, tert-butyl-isopropylbenzene peroxide, 2,4,6-tris(butylperoxy)-triazine, 1,3,5-tris[1-(tert-butylperoxy)-1-methylethyl]benzene, 1,3,5-tris-[(tert-butylperoxy)-isopropyl]benzene, 1,3-dimethyl-3-(tert-butylperoxy)butanol, 1,3-dimethyl-3-(tert-pentylperoxy)butanol, peroxydicarbonate di(2-phenoxyethyl) ester, peroxydicarbonate Di(4-tert-butylcyclohexyl) ester, peroxydimethylmyristate, peroxydibenzyl dicarbonate, peroxydicarbonate di(isoborneol) ester, 3-isopropylphenylperoxy-1,3-dimethylbutyl methacrylate, 3-tert-butylperoxy-1,3-dimethylbutyl methacrylate, 3-tert-pentylperoxy-1,3-dimethylbutyl methacrylate, tris(1,3-dimethyl-3-tert-butylperoxybutoxy)vinylsilane, N-[1-{3-(1-methylvinyl)-phenyl)-1-methylethyl]carbamate 1,3-dimethyl-3-(tert-butylperoxy)butyl ester, N-[1-{3-(1-methylvinyl)-phenyl}-1-methylethyl]carbamate 1,3-dimethyl-3-(tert-butylperoxy)butyl ester, N-[1-{3-(1-methylvinyl)-phenyl}-1-methylethyl]carbamate 1,3-Dimethyl-3-(tert-amylperoxy)butyl ester, N-[1-{3-(1-methylvinyl)-phenyl}-1-methylethyl]carbamate 1,3-dimethyl-3-(isopropylphenylperoxy)butyl ester, 1,1-di(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(tert-butylperoxy)cyclohexane, 4,4-di(tert-amylperoxy)valerate n-butyl ester, 3,3-di(tert-butylperoxy)butyrate ethyl ester, 2,2-di(tert-amylperoxy)propane, 3,6,6,9,9-pentamethyl-3-ethoxycarbonylmethyl-1,2,4,5-tetraoxane, n-butyl-4,4-bis(tert-butylperoxy)valerate, Ethyl-3,3-di(tert-amylperoxy)butyrate, benzoyl peroxide, OO-tert-butyl-O-hydro-monoperoxy-succinate, OO-tert-amyl-O-hydro-monoperoxy-succinate, 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane (or cyclic terpolymer of methyl ethyl ketone peroxide), cyclic dimer of methyl ethyl ketone peroxide, 3,3,6,6,9,9-hexamethyl-1,2,4,5-tetraoxecyclononane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, tert-butyl perbenzoate, tert-butylperoxyacetic acid, tert-butylperoxy-2-ethyl hexanoate, tert-amyl perbenzoate, tert-amyl... 3-Hydroxyperoxyacetic acid ester, tert-butylperoxyisobutyrate, 3-hydroxy-1,1-dimethyl-tert-butylperoxy-2-ethyl hexanoate, OO-tert-pentyl-O-hydro-monoperoxysuccinate, OO-tert-butyl-O-hydro-monoperoxysuccinate, di-tert-butyl dipperoxyphthalate, tert-butylperoxy(3,3,5-trimethylhexanoate), 1,4-bis(tert-butylperoxycarbon)cyclohexane, tert-butylperoxy-3,5,5-trimethylhexanoate, tert-butyl-peroxy-(cis-3-carboxyl)propionate, allyl 3-methyl-3-tert-butylperoxybutyrate, OO-tert-butyl-O-isopropyl monoperoxycarbonate, OO-tert-butyl-O-(2-ethylhexyl) Monoperoxycarbonates, 1,1,1-tris[2-(tert-butylperoxy-carbonyloxy)ethoxymethyl]propane, 1,1,1-tris[2-(tert-pentylperoxy-carbonyloxy)ethoxymethyl]propane, 1,1,1-tris[2-(isopropylphenylperoxy-carbonyloxy)ethoxymethyl]propane, OO-tert-pentyl-O-isopropyl monoperoxycarbonate, di(4-methylbenzoyl) peroxide, di(3-methylbenzoyl) peroxide, di(2-methylbenzoyl) peroxide, didecanoyl peroxide, dilauroyl peroxide, 2,4-dibromobenzoyl peroxide, succinic acid peroxide, dibenzoyl peroxide, di(2,4-dichlorobenzoyl) peroxide, and combinations thereof.
[0039] In one or more embodiments, the free radical initiator may include an azo compound, such as azobisisobutyronitrile (AIBN), 2,2'-azobis(amidinylpropyl) dihydrochloride, etc.; an azo-peroxide initiator comprising a mixture of a peroxide and an azodiacetonitrile compound (such as 2,2'-azobis(2-methyl-valerate), 2,2'-azobis(2-methyl-butyronitrile), 2,2'-azobis(2-ethyl-valerate), 2-[(1-cyano-1-methylpropyl)azo]-2-methyl-valerate, 2-[(1-cyano-1-ethylpropyl)azo]-2-methyl-butyronitrile, 2-[(1-cyano-1-methylpropyl)azo]-2-ethyl, etc.).
[0040] In one or more embodiments, the radical initiator may include a carbon-carbon (“CC”) radical initiator, such as 2,3-dimethyl-2,3-diphenylbutane, 3,4-dimethyl-3,4-diphenylhexane, 3,4-diethyl-3,4-diphenylhexane, 3,4-dibenzyl-3,4-dimethylhexane, 2,7-dimethyl-4,5-diethyl-4,5-diphenyloctane, 3,4-dibenzyl-3,4-diphenylhexane, etc.
[0041] In one or more embodiments, the polymer according to this disclosure can be formed from one or more free radical initiators present as a weight percentage (wt%) of the total polymeric mixture, said weight percentage being in the range of a lower limit selected from one of 0.000001 wt%, 0.0001 wt%, 0.01 wt%, 0.1 wt%, 0.15 wt%, 0.4 wt%, 0.6 wt%, 0.75 wt%, and 1 wt% to an upper limit selected from one of 0.5 wt%, 1.25 wt%, 2 wt%, 4 wt%, and 5 wt%, wherein any lower limit can be used in conjunction with any upper limit. Furthermore, it is contemplated that the concentration of the free radical initiator may be more or less depending on the application of the final material.
[0042] stabilizer
[0043] The polymer compositions according to this disclosure can be formed from one or more stabilizers present in a certain weight percentage of the total polymer mixture, which are capable of preventing polymerization in the feed lines of monomers and comonomers but not hindering polymerization at the reactor.
[0044] In one or more embodiments, the stabilizer may include nitroyl derivatives such as 2,2,6,6-tetramethyl-1-piperidinyloxy, 2,2,6,6-tetramethyl-4-hydroxy-1-piperidinyloxy, 4-oxo-2,2,6,6-tetramethyl-1-piperidinyloxy, 2,2,6,6-tetramethyl-4-amino-piperidinyloxy, etc.
[0045] In one or more embodiments, the polymer composition may be formed from one or more stabilizers, said stabilizers being present in a weight percentage (wt%) of the total polymeric mixture, said weight percentage being in the range from a lower limit selected from one of 0.000001 wt%, 0.0001 wt%, 0.01 wt%, 0.1 wt%, 0.15 wt%, 0.4 wt%, 0.6 wt%, 0.75 wt%, and 1 wt% to an upper limit selected from one of 0.5 wt%, 1.25 wt%, 2 wt%, 4 wt%, and 5 wt%, wherein any lower limit may be used in conjunction with any upper limit. Furthermore, it is contemplated that the concentration of the stabilizer may be more or less depending on the application of the final material.
[0046] additive
[0047] The polymer compositions according to this disclosure may include fillers and additives that modify a variety of physical and chemical properties when added to the polymer composition during blending. These include one or more polymer additives such as kickers, processing aids, lubricants, antistatic agents, clarifying agents, nucleating agents, β-nucleating agents, slip agents, antioxidants, anti-acid agents, light stabilizers (such as HALS), IR absorbers, whitening agents, organic and / or inorganic dyes, anti-caking agents, processing aids, flame retardants, plasticizers, biocides, and adhesion promoters.
[0048] The polymer compositions according to this disclosure may include one or more inorganic fillers, such as talc, glass fiber, marble dust, cement dust, clay, carbon black, feldspar, silica or glass, calcined silica, silicates, calcium silicate, silica powder, glass microspheres, mica; metal oxide particles and nanoparticles, such as magnesium oxide, antimony oxide, zinc oxide; inorganic salt particles and nanoparticles, such as barium sulfate, wollastonite, alumina, aluminum silicate, titanium oxide, calcium carbonate, polyhedral oligomeric silsesquioxanes (POSS).
[0049] In one or more embodiments, the polymer composition according to this disclosure may contain one or more additives and / or fillers, wherein the weight percentage (wt%) of the total composition of the one or more additives and / or fillers is in the range of a lower limit selected from one of 0.01 wt%, 0.02 wt%, 0.05 wt%, 1.0 wt%, 5.0 wt%, 10.0 wt%, 15.0 wt%, and 20.0 wt% to an upper limit selected from one of 25 wt%, 30 wt%, 40 wt%, 50 wt%, 60 wt%, and 70 wt%, wherein any lower limit may be used in conjunction with any upper limit.
[0050] Method for preparing polymer compositions
[0051] In one or more embodiments, the polymer composition according to this disclosure can be prepared in a reactor by polymerizing ethylene and one or more branched vinyl ester monomers. The method of reacting the comonomers in the presence of a radical initiator can include any suitable method in the art, including solution-phase polymerization, pressure radical polymerization, bulk polymerization, emulsion polymerization, and suspension polymerization. In some embodiments, the reactor can be a batch or continuous reactor at a pressure below 500 bar, known as a low-pressure polymerization system. In one or more embodiments, the reaction is carried out by a low-pressure polymerization method, wherein ethylene and one or more vinyl ester monomers are polymerized in an inert solvent and / or in the liquid phase of one or more liquid monomers. In one embodiment, the polymerization comprises an initiator for radical polymerization in an amount of about 0.0001 to about 0.01 mmol, the amount being calculated as the total amount of one or more initiators for radical polymerization per liter of polymerization zone volume. The amount of ethylene in the polymerization zone will depend primarily on the total reactor pressure in the range of about 20 bar to about 500 bar and the temperature in the range of about 20 °C to about 300 °C. In one or more embodiments, the pressure in the reactor may have a lower limit of any one of 20, 30, 40, 50, 75, or 100 bar and an upper limit of any one of 100, 150, 200, 250, 300, 350, 400, 450, or 500 bar. The liquid phase of the polymerization method according to this disclosure may include ethylene, one or more vinyl ester monomers, an initiator for free radical polymerization, and optionally one or more inert solvents such as tetrahydrofuran (THF), chloroform, dichloromethane (DCM), dimethyl sulfoxide (DMSO), dimethyl carbonate (DMC), hexane, cyclohexane, ethyl acetate (EtOAc), acetonitrile, toluene, xylene, ether, dioxane, dimethylformamide (DMF), benzene, or acetone. Copolymers and terpolymers prepared under low-pressure conditions may exhibit number-average molecular weights of 1 to 300 kDa, weight-average molecular weights of 1 to 1000 kDa, and MWDs of 1 to 60.
[0052] In some embodiments, the comonomer and one or more free radical polymerization initiators are polymerized in a continuous or batch manner at temperatures greater than 70 °C and pressures greater than 1000 bar, known as high-pressure polymerization systems. For example, pressures greater than 1000, 1100, 1200, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500, 3000, 5000, or 10000 bar can be used. Copolymers and terpolymers prepared under high-pressure conditions can have number-average molecular weights (Mn) from 1 to 10000 kDa. n Weight-average molecular weight (M) from 1 to 20,000 kDa w Molecular weight distribution (MWD) is determined by weight-average molecular weight (M).w ) and the number-average molecular weight (M) obtained by GPC n The ratio of ) is obtained. Copolymers and terpolymers prepared under high pressure conditions can have MWD from 1 to 60.
[0053] In some embodiments, in low-pressure polymerization and high-pressure polymerization systems, the conversion rate during polymerization can have a lower limit of any one of 0.01%, 0.1%, 1%, 2%, 5%, 7%, 10% and an upper limit of any one of 15%, 17%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 60%, 70%, 80%, 90%, 99%, or 100%, wherein the conversion rate is defined as the weight or mass flow rate of the polymer being prepared divided by the weight or mass flow rate of the monomer and comonomer.
[0054] Physical properties
[0055] In one or more embodiments, the polymer composition may have a melt flow rate (MFR) in the range of 190 °C / 2.16 kg according to ASTM D1238, said range having a lower limit selected from any one of 0.01 g / 10 min, 0.5 g / 10 min, 1 g / 10 min, and 10 g / 10 min to an upper limit selected from any one of 50 g / 10 min, 350 g / 10 min, 450 g / 10 min, 550 g / 10 min, 1000 g / 10 min, and 2000 g / 10 min, wherein any lower limit may be paired with any upper limit.
[0056] In one or more embodiments, the polymer composition may have a crystallinity in the range of ASTM D3418 by differential scanning calorimetry (DSC) or wide-angle X-ray diffraction (WAXD), said range having a lower limit selected from any one of 0.1%, 1%, 10%, and 20% to an upper limit selected from any one of 60%, 70%, and 80%, wherein any lower limit may be paired with any upper limit.
[0057] In one or more embodiments, the polymer composition may have a glass transition temperature (Tg) within the range measured by dynamic mechanical analysis (DMA) or by DSC according to ASTM D3418. g The range has an upper limit selected from any one of 100 °C, 90 °C and 80 °C to a lower limit selected from any one of -50 °C, -60 °C and -70 °C, wherein any lower limit can be paired with any upper limit.
[0058] In one or more embodiments, the polymer composition may have a melting temperature (T) within the range measured by DSC according to ASTM D3418. m The range has a lower limit selected from any one of 20 °C, 30 °C, and 40 °C to an upper limit selected from any one of 100 °C, 110 °C, 120 °C, 130 °C, 140 °C, and 150 °C, wherein any lower limit can be paired with any upper limit. In some embodiments, the polymer composition may be free of T. m It is characterized as a completely amorphous polymer composition.
[0059] In one or more embodiments, the polymer composition may have a crystallization temperature (T) within the range measured by DSC according to ASTM D3418. c The range has a lower limit selected from any one of 0 °C, 5 °C, 10 °C, 20 °C and 30 °C to an upper limit selected from any one of 80 °C, 90 °C, 100 °C, 110 °C, 120 °C, 130 °C, 140 °C and 150 °C, wherein any lower limit can be paired with any upper limit.
[0060] In one or more embodiments, the polymer composition may have a heat of crystallization measured by DSC according to ASTM D3418 within the range having a lower limit of any one of 0, 10, 20, 30, 40, 50 and 60 J / g and an upper limit of any one of 140, 180, 200, 240 and 280 J / g, wherein any lower limit may be paired with any upper limit.
[0061] Polymerization conditions result in polymers with a wide range of molecular weight distributions (MWD). In one embodiment, the polymer obtained by this polymerization method has an MWD of about 1 to about 60, having a lower limit of any one of 1, 1.5, 3, 5, or 10 and an upper limit of any one of 10, 20, 30, 40, 50, or 60, wherein any lower limit can be used in combination with any upper limit. However, depending on the amount of comonomer incorporated, samples prepared under high pressure conditions exhibit a wide range of MWDs from about 1 to 60. Copolymers and ternary polymers prepared under low pressure conditions can exhibit number-average molecular weights of 1 to 300 kDa, weight-average molecular weights of 1 to 1000 kDa, and MWDs from 1 to 60. On the other hand, copolymers and ternary polymers prepared under high pressure conditions can exhibit number-average molecular weights of 1 to 10000 kDa, weight-average molecular weights of 1 to 20000 kDa, and MWDs from 1 to 60.
[0062] In one or more embodiments, the polymer composition may have a hardness as determined according to ASTM D2240 within a range having a lower limit selected from any one of 25, 35, and 45 Shore A to an upper limit selected from any one of 80, 90, and 100 Shore A, wherein any lower limit may be paired with any upper limit.
[0063] In one or more embodiments, the polymer composition may have a hardness as determined according to ASTM D2240 within a range having a lower limit selected from any one of 10, 20, and 30 Shore D to an upper limit selected from any one of 50, 60, and 70 Shore D, wherein any lower limit may be paired with any upper limit.
[0064] In one or more embodiments, the polymer composition may have elongation percentage, tensile strength, and modulus in the ranges determined according to ASTM D368, said range having a lower limit selected from any one of 10, 50, and 100 elongation percentages to an upper limit selected from any one of 500, 1000, and 2000 elongation percentages; a lower limit selected from any one of 1, 5, and 10 MPa tensile strengths to an upper limit selected from any one of 15, 30, 70, 100, and 500 MPa tensile strengths; and a lower limit selected from any one of 0.1, 1, 5, 20, and 40 MPa modulus to an upper limit selected from any one of 100, 200, 300, 1000, and 5000 MPa modulus, wherein any lower limit may be paired with any upper limit.
[0065] In one or more embodiments, the polymer composition may have a density within the range selected from 0.75 g / cm³ according to ASTM D792. 3 0.85 g / cm 3 and 0.89 g / cm 3 The lower limit of any of them is selected from 1.1 g / cm³. 3 1.2 g / cm 3 and 1.3 g / cm 3 The upper limit of any one of them, where any lower limit can be paired with any upper limit.
[0066] In one or more embodiments, the polymer composition may have a bio-based carbon content in the range determined by ASTM D6866-18 Method B, said range having a lower limit selected from any one of 1%, 5%, 10%, and 20% to an upper limit selected from any one of 60%, 80%, 90%, and 100%, wherein any lower limit may be paired with any upper limit.
[0067] In one or more embodiments, the polymer may have a long chain branching frequency in the range of 0 to 10, such as a lower limit from any one of 1, 0.5, 1 or 1.5 to an upper limit from any one of 2, 4, 6, 8 or 10, wherein any lower limit may be paired with any upper limit.
[0068] In one or more implementations, the long chain branches average Calculations can be performed using a GPC instrument equipped with an IR5 infrared detector and a four-capillary viscometer detector, both from PolymerChar. Data collection is performed using PolymerChar software. The concentration measured by the IR5 detector is calculated, assuming the entire area of the chromatogram is equivalent to 100% elution of the injected mass. The average concentration is then calculated according to the following formula. :
[0069]
[0070] Where R is the molar mass of the repeating unit and is calculated based on the molar percentage of each as determined by NMR, taking into account the contributions of the monomer and comonomer. w It is the weight-average molecular weight and is calculated using the following formula with general correction:
[0071]
[0072] Average B n The constant is calculated according to the following formula:
[0073]
[0074] The average g' and g constant are calculated according to the following formula:
[0075]
[0076] ε is known to be the viscosity shielding ratio and is assumed to be a constant and equal to 0.7.
[0077] Intrinsic viscosity (IV) of branched samples 分支 ) can use the specific viscosity (η) from the viscometer detector sp The calculation is performed as follows.
[0078]
[0079] Where SA is the sample amount, KIV is the viscosity detector constant, and the volume increment (ΔV) is a constant determined by the difference between consecutive retention volumes (ΔV = RV). i+1 -RV i ).
[0080] The intrinsic viscosity (IV) of the linear counterpart 线型 The Mark-Houwink equation can be used for calculation, and considering the concentration from the Stacy-Haney method, the Mark-Houwink constant is obtained from the intrinsic viscosity as follows. Stacy-Haney IV (IV) SH Based on Stacy-Haney concentration, via Perform calculations, where C SH Obtained from the following formula:
[0081]
[0082] And η rel It is the relative viscosity (η) rel =η sp +1), (hν) i It is the hydrodynamic volume at each elution volume plate derived from the universal calibration curve; and the Mark-Houwink exponent α is defined as 0.725, which is a reference value for linear polyethylene homopolymers; and the constant K is calculated according to the following formula:
[0083]
[0084] Also according to IV Shi ,according to Obtain the molecular weight (M) on each elution volume of the tablet. SH ).
[0085] Relative to M SHi Drawing IV SHi Both were expressed as logarithmic units, yielding the Mark-Houwink constants k and α for linear polymers. Finally, IV 线型 The calculation can be performed as follows:
[0086]
[0087] Where M ν It is the viscosity-average molecular weight obtained through universal correction and concentration via an IR5 infrared detector, and is calculated according to the following formula:
[0088]
[0089] Where N i It has a molecular weight M i The number of the i-th molecule. M i This was obtained taking into account the concentration obtained through the IR5 infrared detector and the hydrodynamic volume from the universal correction. M iThis is done by plotting the volume, removing noisy extrema from the curve, and then extrapolating using a third-order fitting polynomial. M is then calculated as a function of the volume being preserved using equations derived from this third-order fitting polynomial. i In one or more embodiments, the polymer may have a long-chain branching frequency calculated by GPC analysis in the range of 0 to 10, such as a lower limit from any one of 1, 0.5, 1 or 1.5 to an upper limit from any one of 2, 4, 6, 8 or 10, wherein any lower limit may be paired with any upper limit.
[0090] In one or more embodiments, the polymer may have the properties of passing through... 13 C NMR measures the content of long chain branches in the range of 0 to 10, from a lower limit of any one of 0, 0.2, 0.4, 0.6, 0.8 or 1 to an upper limit of any one of 2, 4, 6, 8 or 10, wherein any lower limit can be paired with any upper limit.
[0091] exist 13 In C10 NMR analysis, long-chain branching (LCB) is defined as any branch having six or more carbons. 13 C10 NMR spectra, LCB content in branched polymers (B10 NMR spectra) 6+ ) Calculated by the following formula:
[0092] B 6+ =S 3,聚合物 -S 3,乙烯基酯单体
[0093] The S3 peak is located at 13 At 32.2 ppm in the C10 NMR spectrum. This method takes into account the branching of the main chain (B10). 6+ Both the chain ends and the long branches in the vinyl ester monomer have an effect using their 13 C NMR spectral corrections were made, and the effects at the chain ends could also be corrected using GPC data.
[0094] In one or more embodiments, the polymer may have a heat flow-to-temperature profile following a heat staged process of continuous self-nucleation and annealing (SSA) having 0 to 20 minimum values, such as a lower limit of any one of 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 minimum values and an upper limit of any one of 12, 14, 16, 18, or 20 minimum values, wherein any lower limit may be paired with any upper limit, and wherein these minimum values may be assigned within the following temperature ranges: 140-150 °C, 130-140 °C, 120-130 °C, 110-120 °C, 100-110 °C, 90-100 °C, 80-90 °C, 70-80 °C, 60-70 °C, 50-60 °C, 40-50 °C, 30-40 °C, 20-30 °C, 10-20 °C, and / or 0-10 °C. °C. Such thermal grading can be performed using a temperature scheme (a series of heating and cooling cycles) to produce a lamellar distribution, the size of which reflects the distribution of methyl sequence lengths in the copolymer and terpolymer. Thermal grading can be performed under nitrogen in a TA Instruments Discovery DSC2500. All cooling cycles can be performed at 5 °C / min and heating cycles at 20 °C / min. The sample can be heated from 25 °C to 150 °C, held at 150 °C for 5 minutes, cooled to 25 °C, and held at that temperature for 3 minutes. Subsequently, the sample can be heated to a first annealing temperature (140 °C), held at that temperature for 5 minutes, and cooled to 25 °C. The sample can then be heated again to the next annealing temperature (130 °C), held at that temperature for 5 minutes, and cooled to 25 °C. This procedure can be repeated in 10 °C steps until the final annealing temperature (such as, but not limited to, 0 °C) is reached. The sample can then be heated to 150 °C at 20 °C / min to obtain a melt profile.
[0095] In one or more embodiments, the polymer may have thermal stability measured by thermogravimetric analysis (TGA), wherein the ratio of weight loss at 250 to 400 °C to the total polymonomer content is in the range of 0 to 2, such as a lower limit of any one of 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 and 1 and an upper limit of any one of 1.2, 1.4, 1.6, 1.8 or 2, wherein any lower limit may be paired with any upper limit.
[0096] In one or more embodiments, the polymer may have a storage modulus of 1 to 10 GPa at 0 °C, such as a lower limit of any one of 0.1, 1, 2, 5, 10, 20, 40, 60, 80 or 100 MPa and an upper limit of any one of 200 MPa, 300 MPa, 400 MPa, 500 MPa, 700 MPa, 1 GPa, 5 GPa or 10 GPa, wherein any lower limit may be paired with any upper limit.
[0097] In one or more embodiments, the polymer may have one or two relaxation maxima in a tan δ versus temperature plot from -75 to 75 °C, wherein the peak at the higher temperature is labeled α and the peak at the lower temperature is labeled β. In one or more embodiments, T α The temperature (corresponding to the α peak) can vary between -75 and 75 °C, with a lower limit such as any of -75, -60, -50, -40, -30, -20, -10, or 0 °C and an upper limit such as any of 10, 20, 30, 40, 50, 60, or 75 °C, wherein any lower limit can be paired with any upper limit. In one or more embodiments, T β The temperature (corresponding to the β peak) can vary between -75 and 50 °C, with a lower limit of any one of -75, -60, -50, -40, -30, -20, -10 or 0 °C and an upper limit of any one of 10, 20, 30, 40 or 50 °C, where any lower limit can be paired with any upper limit.
[0098] application
[0099] In one or more embodiments, the polymer composition can be used in a variety of molding methods to produce articles, including extrusion molding, injection molding, thermoforming, casting extrusion, blown film extrusion, foaming, extrusion blow molding, ISBM (injection stretch blow molding), 3D printing, rotational molding, pultrusion, etc.
[0100] The polymer compositions according to this disclosure can also be formulated for use in a variety of polymer articles, including the preparation of sealants, hoses, shoe insoles, shoe midsoles, shoe outsoles, automotive parts and bumpers, sealing systems, hot melt adhesives, films, conveyor belts, sporting articles, rotationally molded articles, primers, linings in civil engineering, industrial flooring, sound insulation, etc.
[0101] In one or more embodiments, a polymer composition may be included in a polymer blend with one or more polymer resins. In some embodiments, the polymer composition may be formulated as a masterbatch and added to the polymer resin at a weight percentage of 1% to 99% by weight.
[0102] The following embodiments are merely exemplary and should not be construed as limiting the scope of this disclosure.
[0103] Example 1
[0104] Ethylene vinyl acetate (EVA) copolymers account for a large portion of the ethylene copolymer market and possess a range of properties dependent on the vinyl acetate content. Increasing the incorporation of vinyl acetate results in decreased crystallinity, glass transition temperature, melting temperature, and chemical resistance, while simultaneously increasing optical transparency, impact and stress fracture resistance, elasticity, and adhesion. In this example, ethylene-based polymers incorporating varying amounts of vinyl acetate and the vinyl ester monomer VeoVa™ 10 from Hexion™ (a mixture of isomers of vinyl esters of branched alkane carboxylic acids with 10 carbon atoms) were prepared to analyze some polymer properties of the resulting compositions.
[0105] Ethylene (99.95%, Air Liquide, 1200 psi), VeoVa™ 10 (Hexion), and 2,2'-azobisisobutyronitrile (AIBN, 98% Sigma Aldrich) are used as received. Dimethyl carbonate (DMC, anhydrous 99%, Sigma Aldrich) and vinyl acetate (99%, Sigma Aldrich) are distilled before use and stored under nitrogen.
[0106] Synthesis of a ternary polymer using ethylene, vinyl acetate, and VeoVa™ 10 (samples A1-A5)
[0107] A polymer composition was prepared by free radical polymerization of a comonomer mixture in solution by combining 80 g of dimethyl carbonate (DMC), 9.97 or 14.98 g of vinyl acetate, 13.5 or 11.48 g of VeoVa™ 10, and 0.1 g of azobisisobutyronitrile (AIBN) in a Parr reactor. The reactor was sealed and flushed three times with ethylene at 1000 psi while stirring. The system was then heated at 70 °C under ethylene pressure of 1200 psi and stirred for 2 hours. The reaction mixture was collected and the reactor was washed with THF at 60 °C. The solvent in the reaction mixture and washing solution was removed by rotary evaporation. The resulting polymer was dissolved in THF and precipitated into cold methanol, followed by vacuum filtration.
[0108] Example 2
[0109] Ethylene-based polymers containing varying amounts of vinyl tert-pentanoate, vinyl laurate, and vinyl 4-tert-butylbenzoate were prepared to analyze some polymeric properties of the resulting compositions.
[0110] Ethylene (99.95%, Air Liquide, 1200 psi) and azobisisobutyronitrile (AIBN, 98%, Sigma-Aldrich) are used as received. Dimethyl carbonate (DMC, anhydrous 99%, Sigma-Aldrich), vinyl acetate (99%, Sigma-Aldrich), vinyl tert-valerate (99%, Sigma-Aldrich), vinyl laurate (99%, Sigma-Aldrich), and vinyl 4-tert-butylbenzoate (99%, Sigma-Aldrich) are distilled and stored under nitrogen before use.
[0111] Synthesis of ternary polymers using ethylene, vinyl acetate and vinyl pentanoate, vinyl laurate and vinyl 4-tert-butylbenzoate (samples B1-B3)
[0112] A polymer composition was prepared by free radical polymerization of a comonomer mixture in solution by combining 80 g of dimethyl carbonate (DMC), 9.3 g of vinyl acetate, and 13.9 g of vinyl tert-pentanoate or 24.4 g of vinyl laurate or 22 g of 4-tert-butylbenzoate, along with 0.1 g of azobisisobutyronitrile (AIBN), in a Parr reactor. The reactor was sealed and flushed three times with ethylene at 1000 psi while stirring. The system was then heated at 70 °C and stirred at 1200 psi for 2 hours. The reaction mixture was collected and the reactor was washed with THF at 60 °C. The solvent in the reaction mixture and washing solution was removed by rotary evaporation. The resulting polymer was dissolved in THF and precipitated into cold methanol, followed by vacuum filtration.
[0113] Example 3
[0114] Ethylene-based polymers incorporating varying amounts of vinyl acetate and the vinyl ester monomer VeoVa™ 10 from Hexion™ were prepared under high pressure to analyze some polymer properties of the resulting compositions, wherein VeoVa™ 10 is a mixture of isomers of vinyl esters of branched alkane carboxylic acids having 10 carbon atoms.
[0115] Ethylene, VeoVa™ 10 (Hexion), tert-butylperoxy-2-ethylhexanoate, heptane (99%, Sigma-Aldrich), and vinyl acetate (99%, Sigma-Aldrich) are used as received.
[0116] The synthesis of ternary polymers using ethylene, vinyl acetate, and VeoVa™ 10 was carried out under high pressure conditions (samples D1-D15).
[0117] Polymer compositions were prepared by continuous free radical polymerization of a comonomer mixture by combining different streams of ethylene, vinyl acetate, VeoVa™ 10, heptane, and tert-butylperoxy-2-ethylhexanoate in a high-pressure reactor. Prior to each polymerization round, the reactor was purged five times with ethylene at 2200–2300 bar. Each reaction was initiated by heating the reactor to 200 °C and feeding ethylene to a pressure of 1900–2000 bar. A continuous ethylene stream was then fed into the reactor at a rate of 2000 g / h. Once the target pressure and a stable ethylene stream were achieved, the comonomers were added to the reactor. A mixture of initiator and heptane was introduced into the system at a flow rate of 2 mL / h. The reaction mixture was collected, and the reactor was washed with xylene at 145 °C. The resulting polymer was dissolved in xylene and precipitated into cold methanol, followed by vacuum filtration.
[0118] Polymer characterization
[0119] Twenty ethylene-based polymer samples (indicated as A1-A5, B1-B3, and D1-D15) were purified and characterized. The ethylene-based polymers contained varying amounts of both vinyl acetate and vinyl carbonyl monomers.
[0120]
[0121]
[0122] Table 1 provides a summary of gel permeation chromatography (GPC) and nuclear magnetic resonance (NMR) data for all synthetic polymers and two comparative commercial EVA samples, M1 and M2.
[0123] For polymer samples containing vinyl carbonyl monomers, quantitative methods are used. 13 C NMR is used to determine the inclusion, because accurate integration is required. 1 The H NMR spectrum showed significant overlap between the carbonyl and alkyl regions. In pure EVA... 13 The carbonyl peak not observed in the C NMR was identified as originating from the branched vinyl carbonyl monomer unit and used to calculate the weight percentage of the comonomer.
[0124] Especially for Figure 1 It shows the complete VeoVa™ acid 10 monomer and representative samples A2 and M1. 13 C10 NMR spectrum (TCE-D2, 393.1 K, 125 MHz). Evidence of branched vinyl esters was found in both the carbonyl (170–180 ppm) and alkyl (0–50 ppm) regions. The spectrum showed a significant increase in peaks for the carbonyl carbon and long alkyl chain within the branched vinyl esters. Further... Figure 1The spectrum shows general peak assignments. When comparing the spectra of VeoVa™ acid 10 monomer and polymer A2, the polymer spectrum shows the disappearance of the vinyl peak and the appearance of peaks corresponding to all three comonomers studied (ethylene, vinyl acetate, and VeoVa™ acid 10). The abundance of peaks in both regions can be attributed to the mixture of isomers in the VeoVa™ acid 10 monomer, and the presence of these peaks in the polymer sample confirms the formation of the respective ternary polymers.
[0125] Further evidence regarding the incorporation of the VeoVa™ acid 10 monomer clarifies that... Figure 2 The image shows polymer samples A2 and M1. 1 1H NMR spectrum (TCE-D2, 393.2 K, 500 MHz). The spectrum shows peaks for vinyl acetate and ethylene, and additional peaks in the alkyl region (0.5–1.5 ppm) of the long alkyl chain on the branched vinyl ester monomer.
[0126] A2 and M1 1 The H NMR spectrum (TCE-D2, 393.2 K, 500 MHz) shows some relevant peak assignments. Figure 2 The results show overlap near the peak at a slightly higher magnetic field of 5 ppm between vinyl acetate and branched vinyl ester monomer units. If these peaks were purely methines of ethyl acetate, the integration ratio between the 5 ppm peak and the peak near 2 ppm (from the methyl group of vinyl acetate) would be 1:3. However, the integration ratio is 1:1, indicating overlap of methines from both vinyl acetate and branched vinyl esters, resulting in a broadened peak near 5 ppm. (Using...) 1 H NMR and 13 The relative intensities of the measured peaks in the C NMR spectrum were used to calculate the inclusion of vinyl esters and VeoVa™ 10 monomers in the copolymer / terpolymer.
[0127] Specifically, for Table 1, a wide range of conversion rates were obtained for each polymer. The degree of conversion during polymerization will affect the branching and topology of the chains, and alter the properties of the polymer.
[0128] Especially for Figure 3The gel permeation chromatogram of the sample was displayed, from which the molecular weight and distribution were derived. GPC experiments were performed using gel permeation chromatography coupled with triple detection, employing an IR5 infrared detector and a four-bridge capillary viscometer, both from PolymerChar; and an eight-angle light scattering detector from Wyatt. A 13-micron four-tube mixed bed from Tosoh was used at 140 °C. Experimental conditions were: a concentration of 1 mg / mL, a flow rate of 1 mL / min, a dissolution temperature and time of 160 °C and 90 min, respectively, and an injection volume of 200 μL. The solvent used was TCB (trichlorobenzene) stabilized with 100 ppm BHT.
[0129] Polymers A1-A5 containing VeoVa™ 10 exhibit a molecular weight range of 10 to 30 kDa and a molecular weight distribution (MWD) of approximately 2. Polymers B1-B3 show similar MWDs. While the patterns of the ternary polymers are similar to those of the comparative commercial samples (M1 and M2), their molecular weight distributions differ, with the commercial grades showing a wider molecular weight range and MWDs in the range of 4–6. However, depending on the amount of comonomers incorporated, samples prepared under high-pressure conditions (polymers D1–D15) show a wide range of MWDs from approximately 2 to 18. Copolymers and ternary polymers prepared under low-pressure conditions typically exhibit number-average molecular weights of 1 to 300 kDa, weight-average molecular weights of 1 to 1000 kDa, and MWDs of 1 to 60. On the other hand, copolymers and ternary polymers prepared under high-pressure conditions typically show number-average molecular weights of 1 to 10000 kDa, weight-average molecular weights of 1 to 20000 kDa, and MWDs of 1 to 60. Due to the presence of high molecular weight chains in these polymers, they can exhibit unique properties (such as higher melt strength, ESCR, impact strength, etc.) compared to their low MWD counterparts.
[0130] Especially for Figures 4A-4CThe figures show two-dimensional liquid chromatography (2D-LC) chromatograms of polymers D13-D15. The 2D-LC system uses high-performance liquid chromatography (HPLC) and GPC instruments to analyze these copolymers and terpolymers. 2D-LC measurements were performed using a PolymerChar 2D-LC high-temperature chromatogram (Valencia, Spain). This instrument is equipped with a Hypercarb™ HPLC column (100 x 4.5 mm L x ID, 5 μm particle size) and a PLgel Olexis GPC column (300 x 7.5 mm L x ID, 13 μm particle size). The sample loop used for 2D-LC contained a volume of 200 μL. All experiments were performed at 160 °C. Detection was achieved using a fixed-wavelength infrared (IR) detector (IR6, PolymerChar) with bandpass filter, capable of detecting overall polymer concentration, CH2, CH3, and C=O. GPC elution times were corrected for polystyrene (EasiCal PS-1, Agilent, Waldbronn, Germany). Calibration was performed in GPC mode and applied similarly to the 2D-LC results. The HPLC mobile phase was 1-decyl alcohol (Merk, Darmstadt, Germany) / 1,2-dichlorobenzene (ODCB, Acros Organics, Schwerte, Germany) at a flow rate of 0.01 mL / min. Gradient conditions: 0–200 min: pure 1-decyl alcohol; 200–700 min: linear gradient from 1-decyl alcohol to ODCB; 700–1100 min: pure ODCB. The column was then flushed with 1-decyl alcohol at 0.8 mL / min for 40 min to re-establish adsorption equilibrium. The GPC mobile phase was 1,2-dichlorobenzene (ODCB, Acros Organics, Schwerte, Germany) at a flow rate of 1.5 mL / min. HPLC eluent (100 μL) from the fractionating valve sample loop was injected into the GPC every 10 min. The sample concentration was approximately 8 mg / mL. 6 mL of mobile phase (containing the weighed polymer) was automatically added to sample vials using an autosampler, while simultaneously rinsing them with nitrogen. The samples were dissolved under shaking for 1 hour prior to injection. To correct for HPLC elution times of EVA, samples with average vinyl acetate contents of 70, 50, 30, 14, and 5% by weight were used. All samples were mixed in a single 2D-LC wheel (at similar concentrations, approximately 2 mg) and analyzed. To correct for HPLC elution times of VeoVa, a method similar to that used for samples D1-D6 was employed. Except for the low molecular weight fractions, all polymers showed a uniform molar distribution of vinyl acetate and VeoVa™ 10. In these polymers, the concentrations of vinyl acetate and VeoVa™ 10 in the polymer chains varied between 10 and 65% by weight.
[0131] In order to analyze the branching frequency of long chains ( The samples were analyzed using a GPC instrument equipped with an IR5 infrared detector and a four-capillary viscometer detector, and the results are shown in Table 2.
[0132]
[0133] The content of long-chain branches in several polymer samples was used. 13 Measurements were performed using C NMR and the methods described in this paper, and the results are summarized in Table 3 below.
[0134]
[0135] Differential scanning calorimetry (DSC) and dynamic mechanical analysis (DMA) were used to analyze the thermal properties of the polymers. Specifically, for... Figures 5A-5C DSC analysis of EVA and ternary polymer samples showed Figure 5A Among them Figures 5B-5C supply Figure 5A A magnified view of the peaks. During DSC analysis, these samples were equilibrated at 140 °C for 5 minutes and measured at a cooling rate of 10 °C / min, followed by equilibration at -50.0 °C and heating back to a maximum of 140 °C at a heating rate of 10 °C / min.
[0136] Table 4 summarizes the DSC and DMA experiments. When comparing polymers containing branched vinyl ester comonomers with comparative samples, the crystallization temperature showed the greatest influence from the incorporation of branched vinyl ester comonomers. This trend is expected to stem from the crystallization disruption caused by the branching groups introduced into the polymer from the vinyl ester comonomer. Introducing vinyl carbonyl comonomers into copolymers of ethylene and vinyl acetate can produce ternary polymers with morphology different from EVA copolymers. This monomer can disrupt structural regularity and the polymer's ability to form a crystalline state. Therefore, by increasing the amorphous phase region, the Tc of the obtained polymer can be reduced. g T m and T c .
[0137] The heat of crystallization (ΔH), crystallization temperature, and melting temperature of the polymers and commercial EVA samples prepared in Examples 1 to 3 are shown in Table 4. Analysis was performed under nitrogen atmosphere in a TA Q2000 instrument. Samples were heated to 160 °C at 10 °C / min and held at that temperature for 1 minute, then cooled downwards to -20 °C at 10 °C / min and held at that temperature for 1 minute. The samples were then heated back to a maximum of 160 °C at 10 °C / min. Cooling and heating curves were recorded, and analysis was performed by setting baseline endpoints to obtain the crystallization peak temperature, melting peak temperature, and ΔH.
[0138]
[0139] The glass transition temperature (T0) of the sample was determined based on the maximum value of the tan δ peak measured in tension mode using a TA 800 DMA instrument during DMA measurements. g The films prepared from each sample were cooled to -150 °C and temperature scanned at a rate of 3 °C / min, while a preload of 0.01 N was applied at a frequency of 1 Hz and an amplitude of 30 μm to evaluate their viscoelastic response. Storage modulus, loss modulus, and tan δ (storage modulus to loss modulus ratio) were recorded as a function of temperature. A reference temperature of 0 °C was selected for comparison of the storage modulus of the samples. In the tan δ versus temperature plot, the samples showed one or two maxima in the range of -75 °C to 75 °C. The presence of a single peak in the range of -75 °C to 75 °C was labeled as an α peak. The presence of two peaks in the range of -75 °C to 75 °C was indicated by the maxima at the higher temperature as α relaxation and the maxima at the lower temperature as β relaxation. Different polymer morphologies can also be identified in the DMA results. Specifically for... Figures 6A-6B The samples exhibited DMA for D2-D7, D9, and D11. D2-D6 showed broad relaxation from -50 to 75 °C. Increasing the amount of branched vinyl ester comonomer decreased the intensity of the α-relaxation peak while increasing the intensity of the β-relaxation peak. D4 showed the broadest relaxation in this region. Similar to commercial EVA samples, samples D7, D9, and D11 showed a single relaxation within this range.
[0140] Specifically, for Table 4, the copolymers and terpolymers prepared in the examples also exhibit a wide range of MFRs and densities. Table 5 summarizes the storage modulus results of Example 3 at 0 °C, which covers a wide range of values depending on the different morphologies.
[0141]
[0142] Thermogravimetric analysis (TGA) was used to study the thermal degradation of polymers under a nitrogen atmosphere. Samples were placed in a TA Q500 TGA instrument and heated from 25 °C to 700 °C at a heating rate of 20 °C / min. Weight loss was recorded as a function of temperature. Specifically for… Figures 7A-7B The results show TGA values from D7 to D10. All of these polymers contain approximately 30% by weight of comonomers. In the thermograms of these polymers, the first weight loss (at lower temperatures) is associated with the separation of acidic groups (acetic acid or branched alkane carboxylic acids) from the polymer. The second weight loss at higher temperatures corresponds to the degradation of the polymer backbone. Replacing vinyl acetate with VeoVa™ 10 during high-pressure polymerization resulted in more stable polymers and showed less weight loss at lower temperatures. Figure 7B The results show that as the amount of VeoVa™ 10 in the copolymers (circular) and terpolymers (triangular) increases, the strength of the first weight loss (the amount of the first weight loss divided by the ratio of the total polymonomer content) decreases and the copolymers and terpolymers become more thermally stable. A second degradation occurs after 400 °C, in which the carbon-carbon bonds in the polymer backbone begin to degrade.
[0143] The samples were also subjected to thermal grading. Thermal grading used a temperature scheme (a series of heating and cooling cycles) to produce a lamellar distribution, the size of which reflected the distribution of methyl sequence lengths in the copolymers and terpolymers. Thermal grading was performed under nitrogen in a TA Instruments Discovery DSC2500. All cooling cycles were performed at 5 °C / min and heating cycles at 20 °C / min. The sample was heated from 25 °C to 150 °C, held at 150 °C for 5 minutes, cooled to 25 °C, and held at that temperature for 3 minutes. Subsequently, the sample was heated to the first annealing temperature (140 °C), held at that temperature for 5 minutes, and cooled to 25 °C. The sample was then heated again to the next annealing temperature (130 °C), held at that temperature for 5 minutes, and cooled to 25 °C. This procedure was repeated in 10 °C steps until the final annealing temperature (70 °C). The sample was then heated to 150 °C at 20 °C / min to obtain a melt profile. Annealing temperatures include: 140 °C, 130 °C, 120 °C, 110 °C, 100 °C, 90 °C, 80 °C, and 70 °C. These are produced through SSA thermal grading. Figures 8A-8B .
[0144] While only a few embodiments have been described in detail above, those skilled in the art will readily recognize that many modifications can be made to the embodiments without substantially departing from the invention. Therefore, it is intended that all such modifications be included within the scope of this disclosure as defined in the following claims. In the claims, the means plus function clause is intended to cover the structure described herein when performing the stated function, and not only structural equivalents but also equivalent structures. Thus, in the case of fastening wooden parts, while nails and screws may not be structural equivalents, where nails use a cylindrical surface to secure the wooden parts together and screws use a helical surface, nails and screws can be equivalent structures. The applicant expressly intends not to invoke any limitation of 35 USC §112(f) in any of the claims herein, except for those claims in which the phrase “means for…” is expressly used with the associated function.
Claims
1. A polymer composition comprising: Polymers prepared from ethylene, one or more branched vinyl ester monomers, and optionally vinyl acetate; The polymer has a number-average molecular weight in the range of 5 to 10,000 kDa and a molecular weight distribution in the range of 1.5 to 60, obtained by GPC.
2. The polymer composition according to claim 1, wherein the one or more branched vinyl ester monomers have a general structure (II): (II) Where R 4 and R 5 It has a combination of 7 carbon atoms.
3. The polymer composition according to claim 1, wherein the polymer is a copolymer of ethylene and one or more branched vinyl esters.
4. The polymer composition according to claim 1, wherein the polymer has a vinyl ester content of vinyl branches in the range of 0.01 to 90% by weight.
5. The polymer composition according to claim 1, wherein the polymer is a ternary polymer composed of ethylene, one or more branched vinyl esters, and vinyl acetate.
6. The polymer composition according to claim 5, wherein the polymer has a branched vinyl ester content in the range of 0.01 to 89.99% by weight.
7. The polymer composition according to claim 5, wherein the polymer has a vinyl acetate content in the range of 0.01 to 89.99% by weight.
8. The polymer composition of claim 1, wherein the polymer is polymerized under conditions including a reactor pressure greater than 40 bar and a reactor temperature greater than 50 °C.
9. The polymer composition of claim 1, wherein the polymer is polymerized under conditions including a reactor pressure greater than 1000 bar and a reactor temperature greater than 50 °C.
10. The polymer composition of claim 1, wherein the polymer has an ethylene content in the range of 10 to 99.99% by weight.
11. The polymer composition of claim 1, wherein the long chain branching frequency, as measured by GPC, is in the range of 0 to 10.
12. The polymer composition according to claim 1, wherein the polymer is obtained by means of... 13 The long-chain branch content measured by C NMR ranged from 0 to 10.
13. The polymer composition of claim 1, wherein the polymer according to ASTM D3418 has a melting temperature in the range of 0 to 150 °C.
14. The polymer composition of claim 1, wherein the crystallization temperature of the polymer according to ASTM D3418 is in the range of 0 to 150 °C.
15. The polymer composition according to claim 1, wherein the heat of crystallization according to ASTM D3418 is in the range of 0 to 280 J / g.
16. The polymer composition of claim 1, wherein the heat flow to temperature profile of the polymer has 0 to 20 minimum values measured by thermal grading via continuous self-nucleation and annealing in 10°C steps.
17. The polymer composition of claim 16, wherein the minimum value is in the temperature range of 0 to 150 °C.
18. The polymer composition of claim 1, wherein the ratio of the first weight loss at 250 to 400 °C to the total polymonomer content is in the range of 0 to 2.
19. The polymer composition of claim 1, wherein the polymer has a storage modulus in the range of 0.1 MPa to 10 Gpa at 0 °C.
20. The polymer composition of claim 1, wherein the polymer has 1 to 2 relaxation maximum values in a tan δ versus temperature plot at -75 to 75 °C.
21. The polymer composition according to claim 20, wherein T α Temperature varies between -75 and 75 °C.
22. The polymer composition according to claim 20, wherein T β Temperature varies between -75 and 50 °C.
23. The polymer composition of claim 1, wherein the MFR at 190 °C / 2.16 kg according to ASTM D1238 is in the range of 0.01 g / 10 min to 1000 g / 10 min.
24. The polymer composition according to claim 1, wherein the density according to ASTM D792 is 0.85 g / cm³. 3 Up to 1.3 g / cm 3 Within the range.
25. The polymer composition of claim 1, wherein the bio-based carbon content according to ASTM D6866-18 is in the range of 1% to 100%.
26. An article prepared from the polymer composition according to claim 1.
27. The article of claim 26, wherein the article is a sealant, hose, insole, midsole, outsole, automotive bumper, sealing system, hot melt adhesive, film, conveyor belt, sporting article, rotationally molded article, primer, lining, industrial flooring, and sound insulation.