SAN resin and its preparation method, flame-retardant and heat-resistant materials and flame-retardant products

By introducing α-methylstyrene, acrylonitrile, and monoacrylate monophosphate monomers into SAN resin via free radical copolymerization, an intrinsically flame-retardant modified SAN resin is formed, which solves the problem of insufficient heat resistance and flame retardancy of the SAN/ABS resin system and achieves high heat resistance and flame retardancy of UL94 V-1 level or higher.

CN123106972APending Publication Date: 2026-11-17WANHUA CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611553854.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing SAN/ABS resin systems cannot simultaneously meet the requirements of high heat resistance and UL94 V-1~V-0 flame retardancy. Added flame retardants are prone to migration and precipitation during high-temperature processing and long-term use, leading to a decline in material performance.

Method used

Free radical copolymers, including α-methylstyrene, acrylonitrile monomers and monoacrylate monophosphate monomers, are used to permanently bind phosphorus-containing flame-retardant groups to the polymer chain through covalent bonds, forming intrinsically flame-retardant modified SAN resins. Diacrylate monophosphate monomers are combined to improve impact performance.

Benefits of technology

It achieves high heat resistance and flame retardancy rating of SAN resin above UL94 V-1, while solving the problem of migration and precipitation of flame retardants during high-temperature processing and long-term use, thus maintaining the mechanical and processing properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

This application relates to SAN resin and its preparation method, flame-retardant and heat-resistant materials, and flame-retardant articles. The SAN resin comprises: a free radical copolymer comprising a first structural unit, a second structural unit, and a third structural unit in a mass ratio of (60-70):(25-35):(1.5-8); wherein the comonomer of the first structural unit is α-methylstyrene, the comonomer of the second structural unit is an acrylonitrile monomer, and the comonomer of the third structural unit is a monoacrylate monophosphate monomer. In the above-mentioned SAN resin, the phosphorus-containing flame-retardant groups are permanently bonded to the side chains of the polymer chain in the form of covalent bonds, achieving intrinsic flame-retardant modification and solving the migration and precipitation problem of added flame retardants during high-temperature processing and long-term use. This results in the SAN resin of this application not only being heat-resistant but also achieving a UL94 flame retardant rating of V-1 or higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of polymer materials technology, and in particular to SAN resin and its preparation methods, flame-retardant and heat-resistant materials and flame-retardant articles. Background Technology

[0002] Styrene-acrylonitrile copolymer (SAN resin) is an important type of thermoplastic polymer material that combines the excellent processing flow and good mechanical strength of styrene resin with the chemical resistance provided by the acrylonitrile component. It is widely used in electronic and electrical appliance housings, automotive interior parts, food packaging containers, and optical lenses. Furthermore, SAN resin can also be used as a base material to co-extrude with polybutadiene rubber particles to prepare ABS resin. ABS resin possesses excellent physical and mechanical properties, excellent low-temperature impact resistance, electrical properties, abrasion resistance, dimensional stability, chemical resistance, dyeability, and ease of molding and machining. It is widely used in electronics and large appliances, small appliances, transportation (such as dashboards and wheel covers), and light industry (such as bags, toys, and sheet materials).

[0003] As downstream applications increasingly demand higher material performance, especially in high-temperature environments such as electronic component packaging and automotive engine peripheral parts, higher standards are being set for the heat resistance of SAN and ABS resins. The Vicat softening point of ordinary SAN resin is typically between 80℃ and 100℃, which is insufficient to meet the heat resistance requirements of these applications.

[0004] Meanwhile, the SAN / ABS resin system itself does not possess flame-retardant properties. In applications such as electronics and electrical engineering, where specific flame-retardant ratings are required, additional flame retardants are typically necessary. However, added flame retardants have poor compatibility with the polymer matrix and are prone to migration and exudation during high-temperature processing and long-term use, leading to exudates on the material surface and a decrease in the material's mechanical properties and heat resistance.

[0005] Therefore, the field faces the technical challenge of how to maintain the high heat resistance of the SAN / ABS resin system while simultaneously meeting the UL94 V-1 to V-0 flame retardant requirements. Summary of the Invention

[0006] Therefore, it is necessary to provide SAN resins that can achieve both high heat resistance and flame retardancy, as well as their preparation methods, flame-retardant and heat-resistant materials, and flame-retardant products.

[0007] One aspect of this application provides a SAN resin comprising a free radical copolymer, the free radical copolymer comprising a first structural unit, a second structural unit, and a third structural unit in a mass ratio of (60-70):(25-35):(1.5-8); wherein the comonomer of the first structural unit is α-methylstyrene, the comonomer of the second structural unit is an acrylonitrile monomer, and the comonomer of the third structural unit is a monoacrylate monophosphate monomer.

[0008] In some embodiments, the free radical copolymer further includes a fourth structural unit, wherein the comonomer of the fourth structural unit is a diacrylate monophosphate monomer;

[0009] Optionally, the mass of the fourth structural unit accounts for 1000ppm to 5000ppm of the total mass of the free radical copolymer.

[0010] In some embodiments, the mass ratio of the first structural unit, the second structural unit and the third structural unit in the free radical copolymer is (65~70):(25~30):(3~6).

[0011] In some embodiments, the SAN resin includes one or more of the following characteristics:

[0012] (1) The weight average molecular weight of the SAN resin is 90,000 g / mol to 120,000 g / mol.

[0013] (2) The glass transition temperature of the SAN resin is greater than or equal to 127°C;

[0014] (3) The melt flow rate of the SAN resin at 220℃ and 10kg is ≥10g / 10min;

[0015] (4) The limiting oxygen index (LOI) of the SAN resin is greater than or equal to 25%;

[0016] (5) The flame retardancy rating of the SAN resin is UL94 V-1 or V-0;

[0017] (6) The unnotched impact strength of the simply supported beam of the SAN resin is greater than or equal to 26 kJ / m. 2 .

[0018] In a second aspect, this application provides a method for preparing SAN resin, comprising the following steps: mixing the components of a raw material composition for SAN resin, carrying out a polymerization reaction, and after the reaction is complete, removing the light components to obtain the SAN resin; wherein, by weight, the raw material composition comprises 60-70 parts of α-methylstyrene, 25-35 parts of acrylonitrile monomers, 1.5-8 parts of monoacrylate monophosphate monomers, 0.1-0.5 parts of initiator, and 5-20 parts of solvent.

[0019] In some embodiments, the method for preparing SAN resin includes one or more of the following features:

[0020] (1) The acrylonitrile monomers include one or more of acrylonitrile, methacrylonitrile, phenylacrylonitrile or α-chloroacrylonitrile;

[0021] (2) The monoacrylate monophosphate monomers include one or more of the following: 2-methyl-2-acrylate-2-(phosphonoyloxy)ethyl ester, 2-hydroxyethyl methacrylate phosphate, hydroxypropyl methacrylate phosphate, 2-(phosphonoyloxy)ethyl acrylate, dimethyl methacrylate-2-hydroxyethyl phosphate, 2-[(diethoxyphosphono)oxy]ethyl methacrylate, and diphenyl methacrylate-2-hydroxyethyl phosphate;

[0022] (3) The initiator is one or more of organic peroxide initiators and azo initiators; optionally, the organic peroxide initiator includes one or more of 1,1-bis(tert-butylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)-2-methylcyclohexane, and tert-butyl peroxide-3,5,5-trimethylhexanoate; optionally, the azo initiator is one or more of azobisisobutyronitrile and azobisisoheptanenitrile.

[0023] (4) The solvent includes one or more of benzene, toluene, xylene, and ethylbenzene;

[0024] (5) By weight, the raw material composition comprises: 65-70 parts of α-methylstyrene, 25-30 parts of acrylonitrile monomers, 3-6 parts of monoacrylate monophosphate monomers and 0.1-0.3 parts of initiator;

[0025] (6) The total weight of the raw material composition is 100 parts.

[0026] In some embodiments, the method for preparing the SAN resin includes one or more of the following features:

[0027] (1) The raw material composition further includes diacrylate monophosphate monomers; optionally, the mass of the diacrylate monophosphate monomers accounts for 1000ppm-5000ppm of the total mass of monomers in the raw material composition; optionally, the diacrylate monophosphate monomers include one or more of di(methacryloyloxyethyl) hydrogen phosphate, di(acryloyloxyethyl) hydrogen phosphate, 2-(phosphoryloxy)propane-1,3-dimethyldimethacrylate, and 2-(phosphoryloxy)propane-1,3-dimethyldiacrylate.

[0028] (2) The polymerization reaction temperature is 110℃~130℃;

[0029] (3) The polymerization reaction includes a first polymerization stage and a second polymerization stage carried out sequentially. The monomer conversion rate of the first polymerization stage is 30%~40%, and the monomer conversion rate of the second polymerization stage is 55%~65%.

[0030] In some embodiments, the step of removing light components includes a first removal stage and a second removal stage performed sequentially, wherein the first removal stage removes 70wt% to 80wt% of the light components and the second removal stage removes the remaining 20wt% to 30wt% of the light components.

[0031] Optionally, the melt temperature in the first removal stage is 150℃~180℃, the absolute pressure during processing is 40kPa~60 kPa, and the removal time is 1min~15min;

[0032] Optionally, the melt temperature in the second removal stage is 210℃~260℃, the absolute pressure during processing is 1kPa~15kPa, and the removal time is 1~15min.

[0033] In a third aspect, this application provides a flame-retardant and heat-resistant material, comprising at least one of the SAN resins described above and SAN resins prepared by the methods described above.

[0034] Optionally, by weight percentage, the flame-retardant and heat-resistant material comprises 60% to 80% flame-retardant and heat-resistant SAN resin and 20% to 40% ABS resin, wherein the flame-retardant and heat-resistant SAN resin is at least one of the above-mentioned SAN resins and SAN resins prepared by the above-mentioned SAN resin preparation methods.

[0035] In a fourth aspect, this application provides a flame-retardant article, including a flame-retardant structure, wherein the flame-retardant structure comprises the aforementioned flame-retardant and heat-resistant material;

[0036] Optionally, the flame-retardant structure includes at least one of electronic device housings, electrical appliance housings, and tubular equipment.

[0037] The aforementioned SAN resin comprises a free radical copolymer with α-methylstyrene as the main comonomer. The steric hindrance effect of the α-methyl group on the benzene ring enhances the rigidity and thermal stability of the polymer backbone, resulting in a high glass transition temperature and Vicat softening point, and excellent heat resistance. The SAN resin contains structural units formed by acrylate phosphate monomers, which permanently bind phosphorus-containing flame-retardant groups to the side chains of the polymer chain via covalent bonds, achieving intrinsic flame-retardant modification. This solves the migration and precipitation problem of added flame retardants during high-temperature processing and long-term use, making the SAN resin of this application not only heat-resistant but also achieving a UL94 flame retardant rating of V-1 or higher. Detailed Implementation

[0038] To facilitate understanding of this application, a more complete description will be provided below. However, this application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the disclosure of this application.

[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application.

[0040] the term

[0041] Unless otherwise stated or in case of contradiction, the terms or phrases used herein shall have the following meanings:

[0042] As used herein, the term "and / or" includes any and all combinations of one or more of the related listed items.

[0043] In this invention, the terms "multiple" or "various" are used unless otherwise specified, referring to a quantity greater than or equal to 2. For example, "one or more" means one or more types.

[0044] In this invention, terms such as "further" and "particularly" are used for descriptive purposes and to indicate differences in content, but should not be construed as limiting the scope of protection of this invention.

[0045] In this invention, the technical features described in an open-ended manner include both closed-ended technical solutions composed of the listed features and open-ended technical solutions that include the listed features.

[0046] In this invention, numerical intervals (i.e., numerical ranges) are involved. Unless otherwise specified, the distribution of selectable values ​​within a numerical interval is considered continuous, and includes the two endpoints of the numerical interval (i.e., the minimum and maximum values), as well as every value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints, which is equivalent to directly listing every integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be merged. In other words, unless otherwise specified, the numerical ranges disclosed herein should be understood to include any and all subranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, percentage, ratio, etc. The term "numerical interval" can be broadly included to include numerical interval types such as percentage intervals, ratio intervals, and proportion intervals.

[0047] In this invention, the term "room temperature" generally refers to 4℃~35℃, and preferably 20℃±5℃. In some embodiments of this invention, room temperature refers to 20℃~30℃.

[0048] In this invention, unless otherwise specified, the temperature parameters are allowed to be either constant temperature or vary within a certain temperature range. It should be understood that the constant temperature treatment allows temperature fluctuations within the precision range controlled by the instrument. Fluctuations are permitted within ranges such as ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C.

[0049] In this invention, if the unit of a data range is only followed by the right endpoint, it indicates that the units of the left and right endpoints are the same. For example, 2~25h means that the units of the left endpoint "2" and the right endpoint "25" are both h (hours).

[0050] The existing SAN / ABS resin system has difficulty in simultaneously achieving high heat resistance and flame retardancy. To solve this problem, this application provides at least one SAN resin and its preparation method, flame-retardant and heat-resistant material, and flame-retardant article.

[0051] According to a typical embodiment of this application, a SAN resin is provided, comprising: a free radical copolymer, the free radical copolymer comprising a first structural unit, a second structural unit, and a third structural unit in a mass ratio of (60-70):(25-35):(1.5-8); wherein the comonomer of the first structural unit is α-methylstyrene, the comonomer of the second structural unit is an acrylonitrile monomer, and the comonomer of the third structural unit is a monoacrylate monophosphate monomer.

[0052] The aforementioned SAN resin comprises a free radical copolymer with α-methylstyrene as the main comonomer. The steric hindrance effect of the α-methyl group on the benzene ring enhances the rigidity and thermal stability of the polymer backbone, resulting in a high glass transition temperature and Vicat softening point, and excellent heat resistance. The SAN resin contains structural units formed by acrylate phosphate monomers, which permanently bind phosphorus-containing flame-retardant groups to the side chains of the polymer chain via covalent bonds, achieving intrinsic flame-retardant modification. This solves the migration and precipitation problem of added flame retardants during high-temperature processing and long-term use, making the SAN resin of this application not only heat-resistant but also achieving a UL94 flame retardancy rating of V-1 or higher. The copolymerization of acrylate phosphate monomers into the α-methylstyrene-acrylonitrile copolymer (AMSAN) molecular chain weakens the van der Waals forces between molecular chains, reduces chain segment movement resistance, and improves resin flowability, which is beneficial for subsequent processing and production.

[0053] In this application, unless otherwise specified, "monoacrylate monophosphate monomer" refers to a compound comprising one acrylate group and one phosphate group, wherein the ester group of the phosphate group is formed by coupling an alcohol hydroxyl group attached to the acrylate group and a hydroxyl group of the phosphoric acid, and the P atom of the phosphate group is also attached to two -OR groups, where R can be hydrogen, alkyl, or aromatic. It is understood that the acrylate group includes, but is not limited to, acrylate groups and methacrylate groups.

[0054] In some embodiments, the monoacrylate monophosphate monomers include one or more of 2-methyl-2-acrylate-2-(phosphonooxy)ethyl acrylate (CAS No. 24599-21-1), 2-hydroxyethyl methacrylate phosphate (CAS No. 52628-03-2), hydroxypropyl methacrylate phosphate (CAS No. 82427-01-8), 2-(phosphonooxy)ethyl acrylate (CAS No. 32120-16-4), dimethyl methacrylate-2-hydroxyethyl phosphate (CAS No. 61393-58-6), 2-[(diethoxyphosphono)oxy]ethyl methacrylate (CAS No. 814-35-7), and diphenyl methacrylate-2-hydroxyethyl phosphate (CAS No. 16069-23-1).

[0055] In this application, unless otherwise specified, "acrylonitrile monomers" refers to compounds having the following structures:

[0056] In this embodiment, R1, R2, and R3 are each independently hydrogen, alkyl, aromatic, or halogen. In some embodiments, at least one of R1 and R2 is H; more specifically, both R1 and R2 are H. In some embodiments, R3 is H or C. 1-3Alkyl group, further optionally H or methyl. In some embodiments, R3 is H, methyl, phenyl or Cl.

[0057] In some embodiments, the acrylonitrile monomer includes one or more of acrylonitrile, methacrylonitrile, phenylacrylonitrile, or α-chloroacrylonitrile.

[0058] In some embodiments, the free radical copolymer further includes a fourth structural unit, the comonomer of which is a diacrylate monophosphate monomer. The fourth structural unit formed by the diacrylate monophosphate monomer in the SAN resin forms a branched structure in the free radical copolymer, thereby improving the SAN resin's impact resistance while also providing it with good flame retardant and processability properties.

[0059] In this application, unless otherwise specified, "diacrylate monophosphate monomer" refers to a compound containing two acrylate groups and one phosphate group, wherein the ester group of the phosphate group is formed by coupling the two hydroxyl groups of the phosphate group with the alcohol hydroxyl groups attached to the acrylate group, and the P atom of the phosphate group is also attached to an -OR group, wherein R can be hydrogen, alkyl or aromatic.

[0060] In some embodiments, the diacrylate monophosphate monomers include one or more of di(methacryloyloxyethyl) hydrogen phosphate (CAS No. 32435-46-4), di(acryloyloxyethyl) hydrogen phosphate (CAS No. 40074-34-8), 2-(phosphoryloxy)propane-1,3-dimethyldimethacrylate (CAS No. 67829-13-4), and 2-(phosphoryloxy)propane-1,3-dimethyldiacrylate (CAS No. 1338644-02-2).

[0061] In some embodiments, the mass of the fourth structural unit accounts for 1000ppm-5000ppm of the total mass of the free radical copolymer, and is not limited to 1000ppm, 1500ppm, 2000ppm, 4000ppm, 5000ppm, etc. Wherein, "ppm" means parts per million.

[0062] In some embodiments, the mass ratio of the first structural unit, the second structural unit and the third structural unit in the free radical copolymer is (65~70):(25~30):(3~6).

[0063] In some embodiments, the mass fractions of the first structural unit, the second structural unit, and the third structural unit in the free radical copolymer are 65%~70%, 25%~30%, and 3%~6%, respectively.

[0064] In some embodiments, the weight-average molecular weight of the SAN resin is 90,000 to 120,000 g / mol. Non-limitingly, the weight-average molecular weight of the SAN resin can be 90,000, 95,000, 100,000, 105,000, 110,000, 115,000, 120,000 g / mol, etc.

[0065] In some embodiments, the glass transition temperature of the SAN resin is greater than or equal to 127°C; alternatively, the glass transition temperature of the SAN resin is 127°C to 130°C.

[0066] In some embodiments, the melt flow rate of the SAN resin at 220°C and 10 kg is ≥10 g / 10 min. Non-limitingly, the melt flow rate of the SAN resin at 220°C and 10 kg can be 10 g / 10 min, 12 g / 10 min, 14 g / 10 min, 16 g / 10 min, 18 g / 10 min, or 20 g / 10 min. Optionally, the melt flow rate of the SAN resin at 220°C and 10 kg is 10 g / 10 min to 18 g / 10 min.

[0067] In some embodiments, the limiting oxygen index (LOI) of the SAN resin is greater than or equal to 25%, and can be selected as 25% to 30%.

[0068] In some embodiments, the SAN resin has a UL94 flame retardancy rating of V-1 or V-0.

[0069] In some embodiments, the unnotched impact strength of a simply supported beam of SAN resin is greater than or equal to 26 kJ / m. 2 .

[0070] According to yet another typical embodiment, a method for preparing SAN resin is provided, which can be used to prepare the aforementioned SAN resin.

[0071] In some embodiments, a method for preparing SAN resin is provided, comprising the following steps: mixing the components of a raw material composition for SAN resin, carrying out a polymerization reaction, and after the reaction is complete, removing the light components to obtain SAN resin; in some embodiments, the raw material composition comprises, by weight, 60-70 parts of α-methylstyrene, 25-35 parts of acrylonitrile monomers, 1.5-8 parts of monoacrylate monophosphate monomers, 0.1-0.5 parts of initiator, and 5-20 parts of solvent.

[0072] SAN resin prepared by the above method contains acrylate phosphate monomers that can polymerize carbon-carbon double bonds. These monomers can undergo free radical copolymerization with α-methylstyrene and acrylonitrile monomers, so that phosphorus-containing flame-retardant groups are permanently bonded to the side chains of the polymer chain in the form of covalent bonds, thereby achieving intrinsic flame-retardant modification. This solves the problem of migration and precipitation of added flame retardants during high-temperature processing and long-term use. The prepared SAN resin is not only heat-resistant, but also has a flame retardant rating of UL94 V-1 or higher.

[0073] In some embodiments, the acrylonitrile monomer includes one or more of acrylonitrile, methacrylonitrile, phenylacrylonitrile, or α-chloroacrylonitrile.

[0074] In some embodiments, the monoacrylate monophosphate monomers include one or more of 2-methyl-2-acrylate-2-(phosphonoyloxy)ethyl ester, 2-hydroxyethyl methacrylate phosphate, hydroxypropyl methacrylate phosphate, 2-(phosphonoyloxy)ethyl acrylate, dimethyl methacrylate-2-hydroxyethyl phosphate, 2-[(diethoxyphosphono)oxy]ethyl methacrylate, and diphenyl methacrylate-2-hydroxyethyl phosphate.

[0075] In some embodiments, the initiator is one or more of organic peroxide initiators and azo initiators; optionally, the organic peroxide initiator includes one or more of 1,1-bis(tert-butylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)-2-methylcyclohexane, and tert-butyl peroxide-3,5,5-trimethylhexanoate; optionally, the azo initiator is one or more of azobisisobutyronitrile and azobisisoheptanenitrile.

[0076] In some embodiments, the solvent includes one or more of benzene, toluene, xylene, and ethylbenzene.

[0077] In some embodiments, the raw material composition comprises, by weight, 65-70 parts of α-methylstyrene, 25-30 parts of acrylonitrile monomers, 3-6 parts of monoacrylate monophosphate monomers, 0.1-0.3 parts of initiator, and 5-10 parts of solvent.

[0078] In some embodiments, the raw material composition further includes diacrylate monophosphate monomers. Diacrylate monophosphate monomers can form branched structures in free radical copolymers, thereby improving the impact resistance of SAN resin while giving it good flame retardant and processability properties.

[0079] Optionally, the mass of the diacrylate monophosphate monomer accounts for 0.1%-0.5% of the total mass of monomers in the raw material composition; optionally, the diacrylate monophosphate monomer includes one or more of di(methacryloyloxyethyl) hydrogen phosphate, di(acryloyloxyethyl) hydrogen phosphate, 2-(phosphoryloxy)propane-1,3-dimethyldimethacrylate, and 2-(phosphoryloxy)propane-1,3-dimethyldiacrylate.

[0080] In some embodiments, the raw material composition comprises, by weight, 65-70 parts of α-methylstyrene, 25-30 parts of acrylonitrile monomers, 3-6 parts of monoacrylate monophosphate monomers, 0.1-0.3 parts of initiator, 5-10 parts of solvent, and 1000ppm-5000ppm of diacrylate monophosphate monomers by weight of total monomer mass.

[0081] In some embodiments, the polymerization temperature is 110°C to 130°C, and non-limitingly, it can be 110°C, 115°C, 120°C, 125°C, 130°C, etc. Optionally, the polymerization temperature is 120°C to 130°C.

[0082] In some embodiments, the polymerization reaction includes a first polymerization stage and a second polymerization stage, wherein the monomer conversion rate in the first polymerization stage is 30% to 40%, and the monomer conversion rate in the second polymerization stage is 55% to 65%. This facilitates the use of continuous bulk polymerization processes, with mild and controllable process conditions, and good uniformity in monomer conversion rate and product composition.

[0083] The monomer conversion rate was measured and calculated as follows: 1g of the reaction solution was placed in aluminum foil (the foil was weighed beforehand), placed in a 220℃ vacuum oven, and the absolute pressure was controlled to be <1kPa. After vacuuming for 0.5h, the solution was removed, cooled to room temperature, and the weight of the dried resin was measured. The monomer conversion rate was calculated using the following formula: Monomer conversion rate = Weight of dried resin / (Mass of reaction solution × Mass fraction of monomer in total feed) × 100%; where, the mass fraction of monomer in total feed = (Mass of α-methylstyrene + Mass of acrylonitrile + Mass of acrylate monophosphate monomers) / Total mass of raw material solution.

[0084] Without limitation, the monomer conversion rate in the first polymerization stage can be 30%, 32%, 34%, 36%, 38%, 40%, etc.

[0085] Without limitation, the monomer conversion rate in the second polymerization stage (representing the cumulative total conversion rate of monomers in the system after the second polymerization stage) can be 55%, 57%, 59%, 60%, 62%, 64%, 65%, etc.

[0086] In the above steps for removing light components, light components refer to solvents and unreacted α-methylstyrene, acrylonitrile monomers, monoacrylate monophosphate monomers, and optionally diacrylate monophosphate monomers.

[0087] In some embodiments, the method for preparing SAN resin includes: mixing the components of the raw material composition of SAN resin, carrying out a free radical polymerization reaction at 110°C to 130°C, removing the light components at 150°C to 260°C after the reaction is complete, granulating, and preparing the SAN resin.

[0088] In some embodiments, the step of removing light components includes a first removal stage and a second removal stage performed sequentially, wherein the first removal stage removes 70wt% to 80wt% of the light components and the second removal stage removes the remaining 20wt% to 30wt% of the light components.

[0089] Optionally, the melt temperature in the first removal stage is 150℃~180℃, the absolute pressure during treatment is 40 kPa~60 kPa, and the removal time is 1 min~15 min;

[0090] Optionally, the melt temperature in the second removal stage is 210℃~260℃, the absolute pressure during treatment is 1 kPa~15 kPa, and the removal time is 1~15 min.

[0091] In some embodiments, the above-described SAN resin is provided for use in the preparation of flame-retardant and heat-resistant ABS materials. The SAN resin can act as a flame-retardant and heat-resistant modifier, improving the heat resistance and flame-retardant properties of ABS resin.

[0092] In some embodiments, the SAN resin described above is provided for use in the manufacture of electronic device housings, electrical appliance housings, and tubing equipment. The SAN resin described above can be used as a main material in the manufacture of equipment housings, electrical appliance housings, and tubing equipment, giving them good heat resistance and flame retardancy.

[0093] According to another typical embodiment of this application, a flame-retardant and heat-resistant material is provided, comprising at least one of the above-mentioned SAN resin and SAN resin prepared by the above-mentioned method. The above-mentioned SAN resin can be used as a heat-resistant modifier to prepare flame-retardant and heat-resistant ABS resin compositions, achieving a synergistic balance between flame-retardant and heat-resistant properties. It is widely applicable to applications in electronics, electrical appliances, and home appliances where both flame-retardant ratings and heat resistance are clearly required.

[0094] In some embodiments, the flame-retardant and heat-resistant material comprises, by weight percentage, 60% to 80% flame-retardant and heat-resistant SAN resin and 20% to 40% ABS resin, wherein the flame-retardant and heat-resistant SAN resin is at least one of the above-mentioned SAN resin and SAN resin prepared by the above-mentioned SAN resin preparation method. The flame-retardant and heat-resistant material having this composition not only has good flame-retardant and heat-resistant properties but also good mechanical properties.

[0095] According to another typical embodiment of this application, a flame-retardant article is provided, including a flame-retardant structure comprising the aforementioned flame-retardant and heat-resistant material. The flame-retardant article containing the aforementioned flame-retardant and heat-resistant material exhibits good heat resistance and flame retardancy, and also possesses good mechanical properties.

[0096] For example, the aforementioned flame-retardant products include, but are not limited to, electronic devices, electrical equipment, and tubing.

[0097] Optionally, the flame-retardant structure includes at least one of electronic device housings, electrical appliance housings, and tubular equipment.

[0098] To further illustrate this application, the technical solution of this application is described in detail below with reference to specific embodiments. Where specific techniques or conditions are not specified in the embodiments, they are performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.

[0099] The main raw material information involved in the examples and comparative examples is shown in Table 1:

[0100] Table 1

[0101]

[0102] The formulations of the SAN resin compositions prepared in the examples and comparative examples are shown in Table 2 below. The amounts of each component in Table 2 are expressed as parts by weight, where "ppm" means parts per million by weight.

[0103] Table 2

[0104]

[0105] The SAN resin compositions in the above examples and comparative examples were prepared into SAN resins according to the following methods:

[0106] α-Methylstyrene was mixed with acrylonitrile, 2-methyl-2-acrylate-2-(phosphonooxy)ethyl ester, toluene, initiator 1,1-bis(tert-butylperoxy)cyclohexane, and di(methacryloyloxyethyl) hydrogen phosphate in a certain proportion and then pumped into a 500L reactor at a feed rate of 100kg / h. The temperature of the first reactor was controlled at about 120℃, and the monomer conversion rate of the reaction liquid in the reactor was controlled at about 30% (first polymerization stage).

[0107] The slurry from the first reactor is pumped into the second reactor, which has a volume of 500 L, at a feed rate of 100 kg / h. The temperature of the second reactor is controlled at about 120°C, and the monomer conversion rate of the reaction liquid in the reactor is controlled at about 60% (second polymerization stage).

[0108] The reaction liquid from the second reactor is fed into the first devolatilizer D101. The melt temperature inside the devolatilizer is controlled at 160℃, the pressure at 50Kpa, and the devolatilization time at 10min, removing approximately 75% of the light components.

[0109] The polymer melt after devolatilization in the first devolatilizer is fed into the second devolatilizer D102. The melt temperature in the devolatilizer is controlled at 220°C, the pressure is 2 kPa, and the devolatilization time is 10 min. The remaining light components of about 25% are removed. The devolatilized polymer melt is then water-cooled and pelletized to obtain granular SAN products.

[0110] The SAN resins prepared in the above examples and comparative examples were tested according to the following methods, and the test results are listed in Table 3.

[0111] The weight-average molecular weight was measured using a Shimadzu LC-20AD instrument (Japan), and the unit is g / mol.

[0112] Phosphorus (P): The P element in the obtained resin was determined using an elemental analyzer, in wt%.

[0113] Glass transition temperature (Tg): 1g of sample was dissolved in 10g of tetrahydrofuran, flocculated with 50g of ethanol, dried in a vacuum oven at 80℃ under negative pressure for 30min, and measured using a Swiss METTLER instrument. The unit is °C.

[0114] Melt Flow Index (MFR): Tested using a CEAST MF30 melt flow indexer, unit: g / 10min;

[0115] Heat distortion temperature (HDT): Tested according to ISO 75-2:2013. The sample was injection molded into a piece with a length of 80 mm, a width of 10 mm, and a thickness of 4 mm. A bending stress of 1.8 MPa was applied along the thickness direction.

[0116] Unnotched / notched impact strength of simply supported beams: tested according to ASTM D256, unit kJ / m 2 .

[0117] Limiting oxygen index (LOI) was determined according to GB / T 2406.2 standard.

[0118] The flame retardancy rating is determined according to the UL94 standard. The lower the rating number, the better the flame retardancy.

[0119] Table 3 SAN Resin Performance Test Table

[0120]

[0121] In Table 3, "P element content" refers to the mass percentage of P element in SAN resin.

[0122] The SAN resins prepared in the above examples and comparative examples were used to prepare ABS resins according to the following methods:

[0123] 1.5 parts by weight of vinyl bis-stearamide (EBS), 0.1 parts by weight of antioxidant 1076, 0.2 parts by weight of antioxidant 618, and 0.2 parts by weight of magnesium stearate were added to a mixture of 30 parts by weight of HR181 and 70 parts by weight of SAN resin and blended. Particle resin was prepared at 220°C using a twin-screw extruder. Specimens were then injection molded at 220°C using an injection molding machine to test the physical properties of the heat-resistant ABS resin. The test methods were the same as those for SAN resin.

[0124] The performance results of the prepared ABS resin are shown in Table 4.

[0125] Table 4 Performance Test Table for Blended ABS Resin

[0126]

[0127] The comparison of the above experimental results shows that, as can be seen from the comparison between Examples 1-5 and Comparative Examples 1-4, this invention achieves intrinsic flame retardant modification by introducing acrylate phosphate flame retardant monomers, allowing phosphorus-containing flame retardant groups to be covalently bonded to the polymer backbone. The resulting flame-retardant and heat-resistant SAN resin has a limiting oxygen index (LOI) of over 25%, a flame retardant rating of UL94V-0, and an impact strength of 26 kJ / m. 2 Of the above, the SAN resin in Example 6, which did not contain a bifunctional phosphorus-containing monomer, had impact properties close to those of ordinary heat-resistant SAN resin, at 23 kJ / m. 2Comparative Examples 1 and 2, SAN resins without added monofunctional phosphorus-containing monomers, had an LOI below 19% and a flame retardant rating of HB, failing to meet flame retardant requirements. Comparative Example 4, SAN resin with only 0.5 parts by weight of flame-retardant monomer, had an LOI of only 19.2% and a flame retardant rating of HB, also failing to meet flame retardant requirements. Comparative Example 5, SAN resin with 10 parts by weight of monoacrylate monophosphate monomer, achieved an LOI of 30.4% and a flame retardant rating of V-0. However, the excessive addition of monoacrylate monophosphate monomer led to a significant decrease in the impact performance of the SAN resin, with an impact performance of only 19 kJ / m. 2 Meanwhile, the flame-retardant and heat-resistant SAN resin obtained by this invention maintains a glass transition temperature above 127°C, exhibiting excellent heat resistance and impact resistance.

[0128] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0129] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims, and the specification can be used to interpret the content of the claims.

Claims

1. A SAN resin, characterized in that, The invention includes a free radical copolymer comprising a first structural unit, a second structural unit, and a third structural unit in a mass ratio of (60-70):(25-35):(1.5-8); wherein the comonomer of the first structural unit is α-methylstyrene, the comonomer of the second structural unit is an acrylonitrile monomer, and the comonomer of the third structural unit is a monoacrylate monophosphate monomer.

2. The SAN resin according to claim 1, characterized in that, The free radical copolymer further includes a fourth structural unit, wherein the comonomer of the fourth structural unit is a diacrylate monophosphate monomer; Optionally, the mass of the fourth structural unit accounts for 1000ppm to 5000ppm of the total mass of the free radical copolymer.

3. The SAN resin according to claim 1 or 2, characterized in that, In the free radical copolymer, the mass ratio of the first structural unit, the second structural unit and the third structural unit is (65~70):(25~30):(3~6).

4. The SAN resin according to claim 1 or 2, characterized in that, Includes one or more of the following features: (1) The weight-average molecular weight of the SAN resin is 90,000 g / mol to 120,000 g / mol; (2) The glass transition temperature of the SAN resin is greater than or equal to 127°C; (3) The melt flow rate of the SAN resin at 220℃ and 10kg is ≥10g / 10min; (4) The limiting oxygen index (LOI) of the SAN resin is greater than or equal to 25%; (5) The flame retardancy rating of the SAN resin is UL94 V-1 or V-0; (6) The unnotched impact strength of the simply supported beam of the SAN resin is greater than or equal to 26 kJ / m. 2 .

5. A method for preparing SAN resin, characterized in that, The steps include the following: The components of the raw material composition for SAN resin are mixed and subjected to a polymerization reaction. After the reaction is completed, the light components are removed to obtain the SAN resin. The raw material composition comprises, by weight, 60-70 parts of α-methylstyrene, 25-35 parts of acrylonitrile monomers, 1.5-8 parts of monoacrylate monophosphate monomers, 0.1-0.5 parts of initiator, and 5-20 parts of solvent.

6. The method for preparing SAN resin according to claim 5, characterized in that, Includes one or more of the following features: (1) The acrylonitrile monomers include one or more of acrylonitrile, methacrylonitrile, phenylacrylonitrile or α-chloroacrylonitrile; (2) The monoacrylate monophosphate monomers include one or more of the following: 2-methyl-2-acrylate-2-(phosphonoyloxy)ethyl ester, 2-hydroxyethyl methacrylate phosphate, hydroxypropyl methacrylate phosphate, 2-(phosphonoyloxy)ethyl acrylate, dimethyl methacrylate-2-hydroxyethyl phosphate, 2-[(diethoxyphosphono)oxy]ethyl methacrylate, and diphenyl methacrylate-2-hydroxyethyl phosphate; (3) The initiator is one or more of organic peroxide initiators and azo initiators; optionally, the organic peroxide initiator includes one or more of 1,1-bis(tert-butylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)-2-methylcyclohexane, and tert-butyl peroxide-3,5,5-trimethylhexanoate; optionally, the azo initiator is one or more of azobisisobutyronitrile and azobisisoheptanenitrile. (4) The solvent includes one or more of benzene, toluene, xylene, and ethylbenzene; (5) By weight, the raw material composition comprises: 65-70 parts of α-methylstyrene, 25-30 parts of acrylonitrile monomers, 3-6 parts of monoacrylate monophosphate monomers and 0.1-0.3 parts of initiator; (6) The total weight of the raw material composition is 100 parts.

7. The method for preparing SAN resin according to claim 5 or 6, characterized in that, Includes one or more of the following features: (1) The raw material composition further includes diacrylate monophosphate monomers; optionally, the mass of the diacrylate monophosphate monomers accounts for 1000ppm-5000ppm of the total mass of monomers in the raw material composition; optionally, the diacrylate monophosphate monomers include one or more of di(methacryloyloxyethyl) hydrogen phosphate, di(acryloyloxyethyl) hydrogen phosphate, 2-(phosphoryloxy)propane-1,3-dimethyldimethacrylate, and 2-(phosphoryloxy)propane-1,3-dimethyldiacrylate. (2) The polymerization reaction temperature is 110℃~130℃; (3) The polymerization reaction includes a first polymerization stage and a second polymerization stage carried out sequentially. The monomer conversion rate of the first polymerization stage is 30%~40%, and the monomer conversion rate of the second polymerization stage is 55%~65%.

8. The method for preparing SAN resin according to claim 5 or 6, characterized in that, The steps for removing light components include a first removal stage and a second removal stage performed sequentially. The first removal stage removes 70wt% to 80wt% of the light components, and the second removal stage removes the remaining 20wt% to 30wt% of the light components. Optionally, the melt temperature in the first removal stage is 150℃~180℃, the absolute pressure during processing is 40 kPa~60 kPa, and the removal time is 1 min~15 min; Optionally, the melt temperature in the second removal stage is 210℃~260℃, the absolute pressure during processing is 1 kPa~15 kPa, and the removal time is 1~15 min.

9. A flame-retardant and heat-resistant material, characterized in that, It includes at least one of the SAN resins according to any one of claims 1 to 4 and the SAN resins prepared by the preparation methods according to any one of claims 5 to 8; Optionally, by weight percentage, the flame-retardant and heat-resistant material comprises 60% to 80% flame-retardant and heat-resistant SAN resin and 20% to 40% ABS resin, wherein the flame-retardant and heat-resistant SAN resin is at least one of the SAN resin of claim 4 or 5 and the SAN resin prepared by the preparation method of the SAN resin of claims 6 to 8.

10. A flame-retardant product, characterized in that, Includes a flame-retardant structure, wherein the flame-retardant structure comprises the flame-retardant and heat-resistant material as described in claim 9; Optionally, the flame-retardant structure includes at least one of electronic device housings, electrical appliance housings, and tubular equipment.