A raw fluororubber and its preparation method
By repeatedly adding pH buffer and vulcanization point monomer, the problem of uneven dispersion of vulcanization point monomer in the preparation of peroxyfluororubber was solved, which improved product performance and production efficiency and reduced costs.
Patent Information
- Application Number
- CN202611488792.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing technology, the vulcanizing point monomers are difficult to disperse uniformly during the preparation of peroxyfluororubber, resulting in poor product performance and high cost. The vulcanizing point monomers are easily lost, affecting the polymerization reaction effect.
The polymerization process was optimized by repeatedly adding pH buffer, chain transfer agent and sulfidation point monomer. The pH buffer was used to maintain the stability of the reaction system and ensure uniform dispersion of sulfidation point monomer. The use of surfactant and salt compound was also combined to optimize the polymerization process.
This method achieves efficient and uniform incorporation of monomers at vulcanization points, improving the overall performance and production efficiency of peroxyfluororubber and reducing product costs.
Smart Images

Figure SMS_2 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This invention relates to the field of fluororubber technology, and in particular to a peroxyfluororubber raw rubber and its preparation method. Background Technology
[0002] Fluororubber is one of the most widely used materials in aerospace, automotive, and petrochemical industries. Among them, peroxyfluororubber has attracted attention from various industries due to its excellent high-temperature resistance and outstanding tolerance to harsh media conditions, especially its unique electrolyte resistance, which has garnered significant interest in lithium batteries and energy storage. Peroxyfluororubber is mainly copolymerized from vinylidene fluoride (VDF), tetrafluoroethylene (TFE), hexafluoropropylene (HFP), and vulcanizing point monomer (CSM) under specific process conditions. While the proportion of vulcanizing point monomer is relatively small, the cross-linking structure formed at this site after vulcanization is initiated by peroxides and vulcanization accelerators endows peroxyfluororubber with excellent comprehensive properties. Therefore, the amount of vulcanizing point monomer incorporated is a crucial factor to consider during the preparation of peroxyfluororubber.
[0003] In the preparation of fluororubber, the vulcanizing point monomer, due to its unique molecular structure, often exhibits poor compatibility with fluorinated monomers or significant steric hindrance, making it difficult for it to uniformly embed into the fluororubber molecular chain during polymerization. Currently, the mainstream method disclosed in domestic patents such as CN121136312A, CN 118184852A, CN 116162199A, and CN115466344A involves directly injecting the vulcanizing point monomer into the reactor, allowing it to copolymerize with VDF, TFE, and HFP during dispersion. However, this method also has certain drawbacks: firstly, the vulcanizing point monomer is difficult to disperse uniformly in the polymerization system; secondly, the vulcanizing point monomer is easily lost and may even cause side reactions, making it difficult to obtain the desired product.
[0004] Patent CN121824819 A discloses a peroxyfluororubber raw rubber, peroxyfluororubber, and its preparation method. The preparation method of the peroxyfluororubber raw rubber includes the following steps: using water as the reaction medium, adding a pH buffer and emulsifier to a reaction vessel under a protective gas atmosphere, and heating to the polymerization temperature; injecting initial polymerization monomer components into the reaction vessel to the polymerization pressure, followed by adding a chain transfer agent, a vulcanizing point monomer, and an initiator; injecting additional polymerization monomer components into the reaction vessel to maintain the reaction pressure, and obtaining a fluororubber emulsion after the reaction is completed; adding salt compounds to the fluororubber emulsion to coagulate, and finally obtaining the peroxyfluororubber raw rubber after washing and drying; wherein the emulsifier is composed of a compound of a fluorinated emulsifier and a hydrocarbon emulsifier. This invention can produce peroxyfluororubber with excellent vulcanization performance and comprehensive mechanical properties. However, its vulcanizing point monomer is difficult to disperse uniformly in the polymerization reaction system, thus making it difficult to ensure that the product achieves optimal physical properties.
[0005] In summary, the vulcanizing point monomer, as a special type of polymerizing monomer, is a crucial component in fluororubber. However, existing processes increase the cost of fluororubber and present technical challenges in copolymerizing with VDF, TFE, and HFP. This leads to insufficient actual vulcanizing point monomer input or losses during polymerization, affecting product performance and ultimately impacting the final cost and profit of fluororubber products. Therefore, it is necessary to develop more suitable new polymerization processes to address existing technical problems, ensuring efficient and uniform incorporation of the vulcanizing point monomer and optimizing the performance of fluororubber to its maximum using the minimum required amount of vulcanizing point monomer. Summary of the Invention
[0006] The purpose of this invention is to provide a peroxyfluorinated rubber raw rubber and its preparation method, which enables the vulcanization point monomer to be efficiently and uniformly incorporated into the molecular chain, thereby obtaining a peroxyfluorinated rubber with excellent performance.
[0007] The objective of this invention can be achieved through the following technical solution: a method for preparing peroxyfluororubber raw rubber, comprising the following steps: (1) Add pH buffer and surfactant to the polymerization reactor to remove oxygen from the polymerization reactor, and heat to the polymerization temperature; (2) After adding the initial polymerization monomer components to the polymerization reactor to the polymerization pressure, add the chain transfer agent, sulfurization point monomer and initiator; (3) After the pressure in the polymerization reactor drops, add the monomer components to maintain the pressure in the polymerization reactor and continue the reaction. During the reaction, pH buffer, chain transfer agent and vulcanization point monomer are added multiple times. After the reaction ends, peroxyfluorinated rubber emulsion is obtained. (4) Add salt compounds and surfactants to the peroxyfluorinated rubber emulsion, and carry out coagulation, washing and drying to finally obtain the peroxyfluorinated rubber raw rubber.
[0008] Preferably, the pH buffer solution contains an alkali, a salt, and a solvent.
[0009] More preferably, the mass ratio of the alkali, salt, and solvent is (0.1-5):(0.1-5):100.
[0010] More preferably, the alkali includes at least one of ammonia, sodium hydroxide, and potassium hydroxide.
[0011] More preferably, the salt includes at least one of ammonium nitrate, ammonium sulfite, ammonium bisulfite, ammonium bicarbonate, ammonium carbonate, ammonium sulfite, ammonium chloride, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium borate tetradecylhydrate, sodium tetraborate, potassium dihydrogen phosphate, and dipotassium hydrogen phosphate.
[0012] More preferably, the solvent includes deionized water.
[0013] Preferably, the pH buffer solution contains a compound inorganic salt and a solvent.
[0014] More preferably, the mass ratio of the compounded inorganic salt to the solvent is (0.1-10):100.
[0015] More preferably, the compound inorganic salt includes at least one of sodium dihydrogen phosphate / disodium hydrogen phosphate, potassium dihydrogen phosphate / disodium hydrogen phosphate, sodium bicarbonate / sodium carbonate, ammonium carbonate / ammonium bicarbonate, and sodium tetraborate / sodium tetradecyl borate.
[0016] More preferably, the mass ratio of the two components in the compound inorganic salt is (0.1-5):1.
[0017] More preferably, the solvent includes deionized water.
[0018] Preferably, the pH buffer solution is an alkali-salt-solvent composite system or a compound inorganic salt-solvent composite system.
[0019] More preferably, the alkali-salt-solvent composite system includes one of the following: ammonia-ammonium nitrate-deionized water, ammonia-ammonium sulfite-deionized water, ammonia-ammonium bisulfite-deionized water, ammonia-ammonium bicarbonate-deionized water, ammonia-ammonium carbonate-deionized water, ammonia-ammonium sulfite-deionized water, ammonia-ammonium chloride-deionized water, sodium hydroxide-sodium dihydrogen phosphate-deionized water, sodium hydroxide-disodium hydrogen phosphate-deionized water, sodium hydroxide-sodium borate tetradecylhydrate-deionized water, sodium hydroxide-sodium tetraborate-deionized water, potassium hydroxide-potassium dihydrogen phosphate-deionized water, and potassium hydroxide-dipotassium hydrogen phosphate-deionized water.
[0020] More preferably, the compounded inorganic salt-solvent composite system includes one of sodium dihydrogen phosphate / disodium hydrogen phosphate-deionized water, potassium dihydrogen phosphate / disodium hydrogen phosphate-deionized water, sodium bicarbonate / sodium carbonate-deionized water, ammonium carbonate / ammonium bicarbonate-deionized water, and sodium tetraborate / sodium tetradecyl borate-deionized water.
[0021] Preferably, the chain transfer agent has the following general formula: A-(C Y 2) s -A; in, Y It can be a fluorine atom or a carbon atom, s = 2, 4, 6 or 8, and A can be a halogen atom.
[0022] More preferably, the halogen atom includes bromine and iodine atoms.
[0023] Preferably, the chain transfer agent includes diiodomethane, 1,4-diiodoperfluorobutane, 1,6-diiodohexane, and 1,4-diiodobutane.
[0024] Preferably, the sulfurization point monomer has the following general formula: R 1 R 2 -C=CR 3 -(CF2) m -(CH2) u -O f -(CF2) v -A; Among them, R 1 R 2 and R 3 For hydrogen or fluorine atoms, 0 ≤ m + u + v ≤ 6, 0 ≤ f ≤1, A is a halogen atom.
[0025] More preferably, the halogen atom includes bromine and iodine atoms.
[0026] Preferably, the sulfidation point monomer includes trifluoroiodoethylene, 3,3,4,4-tetrafluoro-1-butene-difluoro-6-bromo-ether, 3,3,4,4,5,5,6-6-octafluoro-6-iodo-1-hexene, 3,3,4,4-tetrafluoro-4-iodo-1-butene, 3,3,4,4-tetrafluoro-6-bromo-1-hexene, and perfluoro-1-iodo(4-hexene).
[0027] Preferably, the initiator is a group or combination of potassium persulfate and ammonium persulfate.
[0028] Preferably, in step (1), pH buffer and surfactant are added to the polymerization reactor, vacuum is drawn, nitrogen is injected and then evacuated, and the process is repeated several times to remove oxygen from the polymerization reactor. Then, stirring is turned on and the temperature is raised to the polymerization temperature.
[0029] Preferably, the polymer monomer component is a mixture of vinylidene fluoride, tetrafluoroethylene and hexafluoropropylene.
[0030] More preferably, in the initial polymerization monomer components described in step (2), the molar ratio of vinylidene fluoride, tetrafluoroethylene, and hexafluoropropylene is (16-40): (12-29): (34-58).
[0031] More preferably, in step (3), the molar ratio of vinylidene fluoride, tetrafluoroethylene, and hexafluoropropylene in the added polymer monomer components is (28-60): (16-40): (20-55).
[0032] Preferably, the surfactant in step (1) is a fluorinated compound and / or a hydrocarbon.
[0033] More preferably, the fluorinated compound includes one or more mixtures of perfluoropolyether-polyethylene glycol-perfluoropolyether triblock copolymer, perfluoropolyether ammonium carboxylate, perfluoropolyether ammonium sulfonate, linear perfluoropolyether ammonium fluorocarbonate, perfluoroalkyl phosphate, and perfluoropolyether amide sulfonate sodium.
[0034] More preferably, the hydrocarbon includes one or more of the following: sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium lauryl ether sulfate, polyoxyethylene sorbitan fatty acid ester, cocamidopropyl betaine, sodium lignin sulfonate, sodium dibutylnaphthalene sulfonate, sodium diisopropylnaphthalene sulfonate, ethoxyethanesulfonate, and sodium oleoyl methyl taurate.
[0035] More preferably, the surfactant in step (1) is a fluorinated compound and a hydrocarbon (i.e., a surfactant complex).
[0036] More preferably, when the surfactant contains two or more compounds, the mass ratio of any two compounds is (0.1-10):(0.1-10). That is, when it contains two compounds, the mass ratio of the two compounds is (0.1-10):(0.1-10); when it contains three compounds, the mass ratio of the three compounds is (0.1-10):(0.1-10):(0.1-10); when it contains four compounds, the mass ratio of the four compounds is (0.1-10):(0.1-10):(0.1-10):(0.1-10), and so on.
[0037] Preferably, the amount of surfactant used in step (1) is 0.1 wt.%-0.5 wt.% of the amount of solvent used in the pH buffer solution in step (1).
[0038] Preferably, the polymerization temperature in step (1) is 60~80℃.
[0039] Preferably, the polymerization pressure in step (2) is 1.2 MPa to 2.6 MPa.
[0040] Preferably, the amount of chain transfer agent used in step (2) is 0.04 wt.%-0.30 wt.% of the amount of solvent used in the pH buffer solution in step (1).
[0041] Preferably, the amount of the sulfur point monomer used in step (2) is 0.1 wt.%-3.0 wt.% of the amount of solvent used in the pH buffer solution in step (1).
[0042] Preferably, the amount of initiator used in step (2) is 0.1 wt.%-0.8 wt.% of the amount of solvent used in the pH buffer solution in step (1).
[0043] Preferably, in step (3), the monomer components are continuously added during the reaction to maintain the pressure inside the polymerization reactor.
[0044] Preferably, the amount of pH buffer added in step (3) is 1 wt.% to 10 wt.% of the amount of pH buffer used in step (1).
[0045] More preferably, the amount of pH buffer added in step (3) is 2 wt.%-8 wt.% of the amount of pH buffer used in step (1).
[0046] Preferably, the amount of chain transfer agent added in step (3) in a single step is 1 wt.% to 60 wt.% of the amount of chain transfer agent used in step (2).
[0047] More preferably, the amount of chain transfer agent added in step (3) in a single step is 1 wt.% to 40 wt.% of the amount of chain transfer agent used in step (2).
[0048] Preferably, the amount of sulfur point monomer added in step (3) in a single step is 10 wt.%-150 wt.% of the amount of sulfur point monomer used in step (2).
[0049] More preferably, the amount of sulfur point monomer added in step (3) in a single step is 20 wt.%-100 wt.% of the amount of sulfur point monomer used in step (2).
[0050] Preferably, the number of times the replenishment is performed in step (3) does not exceed 35 times.
[0051] More preferably, the number of times to replenish in step (3) is 1 to 30.
[0052] Preferably, the salt compound in step (4) is one or more of sulfates and chlorides.
[0053] More preferably, the sulfate includes one or more of magnesium sulfate, aluminum sulfate, and potassium aluminum sulfate dodecahydrate.
[0054] More preferably, the chloride salt includes one or more of magnesium chloride, aluminum chloride, and calcium chloride.
[0055] Preferably, the amount of salt compound used in step (4) is 0.3 wt.%-3.0 wt.% of the amount of pH buffer solvent used in step (1).
[0056] Preferably, the surfactant in step (4) is a hydrocarbon.
[0057] More preferably, the hydrocarbon includes one or more of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, and sodium lauryl ether sulfate.
[0058] More preferably, when the surfactant in step (4) is a mixture of two hydrocarbons, the mass ratio of the two is (0.1-10):1.
[0059] Preferably, the amount of surfactant used in step (4) is 0.01 wt.%-0.2 wt.% of the amount of pH buffer solvent used in step (1).
[0060] Preferably, the drying temperature in step (4) is 75-105 °C.
[0061] A type of peroxyfluororubber raw rubber is prepared by the above-described preparation method.
[0062] A peroxyfluororubber includes the above-mentioned peroxyfluororubber raw rubber, and also includes carbon black, zinc oxide, vulcanizing agent and crosslinking agent.
[0063] Preferably, the peroxyfluorinated rubber is obtained by mixing and pressing the following raw materials in parts by weight: 380-420 parts of peroxyfluorinated rubber raw rubber, 90-110 parts of carbon black, 7-9 parts of zinc oxide, 9-11 parts of vulcanizing agent and 20-24 parts of crosslinking agent.
[0064] More preferably, the vulcanizing agent is 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.
[0065] More preferably, the crosslinking agent is triallyl isocyanurate.
[0066] The mainstream method in existing publicly available technologies involves directly injecting the sulfur point monomer into the reactor, which has the following drawbacks: First, the sulfur point monomer is highly hydrophobic and has a much greater specific gravity than water. When injected into the aqueous phase in one go, it easily agglomerates, and cannot be uniformly dispersed in the polymerization system solely through rapid stirring and the adsorption of surfactants and fluorinated monomers in the polymerization system. Second, the sulfur point monomer contains post-sulfurization active components, and its residence time should not be too long in the presence of the initiating system; otherwise, it will cause loss of the sulfur point monomer and may even lead to side reactions, failing to obtain the desired product. Compared to existing publicly available technologies, this invention uses a pH buffer solution instead of a pH buffer agent. The pH buffer solution maintains the pH value of the reaction system within the target range, preventing fluctuations during the polymerization reaction. Furthermore, compared to the polymerization process in existing publicly available technologies that involves a single addition of the sulfur point monomer, chain transfer agent, and pH buffer solution, this invention replenishes the pH buffer solution, sulfur point monomer, and chain transfer agent multiple times during the reaction.
[0067] Compared with the prior art, the present invention has the following technical advantages: 1) The present invention can resist pH fluctuations caused by repeated addition of pH buffer during the polymerization reaction, and keep the polymerization reaction stable within the target pH range. This also plays an important role in stabilizing the initiation rate of the initiation system in the polymerization reaction, so that the number of free radicals in the reaction system remains stable and the overall reaction proceeds smoothly.
[0068] 2) The present invention can ensure that the concentration of the vulcanizing point monomer in the liquid phase of the polymerization reactor remains consistent throughout the reaction, so that it can be uniformly incorporated into the molecular chain. This avoids the loss caused by the excessive concentration of the vulcanizing point monomer and its prolonged residence time due to a one-time addition at the beginning of the reaction. At the same time, the multiple additions of the chain transfer agent can ensure that its concentration in the liquid phase of the polymerization reactor remains uniform, maximizing the role of controlling the molecular weight and making the molecular weight of the peroxyfluororubber more uniform.
[0069] 3) This invention uses a vulcanization point monomer with high efficiency polymerization and vulcanization and a standard compounding formula to obtain a peroxyfluororubber with excellent vulcanization performance and comprehensive mechanical properties.
[0070] 4) The peroxyfluororubber prepared by this invention has better comprehensive mechanical properties, especially compression set and media resistance.
[0071] 5) By adding chain transfer agents and sulfurization point monomers in multiple batches during the polymerization process, this invention enables the process to have the potential for high single-batch production in industrial production, which can effectively reduce product costs.
[0072] 6) This invention enables the chain transfer agent and vulcanization point monomer to maintain a uniform dispersion state from the beginning to the end of the reaction and to be uniformly integrated into the molecular chain, thereby obtaining high-performance peroxyfluororubber. Detailed Implementation
[0073] The present invention will now be described in detail with reference to specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.
[0074] This invention provides a method for preparing perfluororubber raw rubber, comprising the following steps: (1) Add pH buffer and surfactant complex to the polymerization reactor, evacuate, inject nitrogen and then evacuate again. Repeat this process several times to remove oxygen from the polymerization reactor. Then turn on the stirrer and heat to the specified polymerization temperature. (2) After injecting the first polymerization monomer component into the polymerization reactor to the specified polymerization pressure, a certain amount of chain transfer agent, sulfurization point monomer and initiator are added; (3) After the pressure inside the reactor drops, the second polymerization monomer is added to maintain the pressure inside the polymerization reactor. The reaction continues. During the reaction, a certain amount of pH buffer, chain transfer agent and sulfurization point monomer are added. The above operation is repeated several times. The reaction continues until the specified reaction amount is reached and the reaction ends to obtain peroxyfluorinated rubber emulsion. (4) Add salt compounds and surfactants to the emulsion, and carry out coagulation, washing and drying to finally obtain fluoropolymer raw rubber, and test its performance using standard formulation.
[0075] Preferably, the pH buffer solution in step (1) is an alkali-salt-solvent composite system or a compound inorganic salt-solvent composite system.
[0076] More preferably, the alkali-salt-solvent composite system includes one of the following: ammonia-ammonium nitrate-deionized water, ammonia-ammonium sulfite-deionized water, ammonia-ammonium bisulfite-deionized water, ammonia-ammonium bicarbonate-deionized water, ammonia-ammonium carbonate-deionized water, ammonia-ammonium sulfite-deionized water, ammonia-ammonium chloride-deionized water, sodium hydroxide-sodium dihydrogen phosphate-deionized water, sodium hydroxide-disodium hydrogen phosphate-deionized water, sodium hydroxide-sodium borate tetradecylhydrate-deionized water, sodium hydroxide-sodium tetraborate-deionized water, potassium hydroxide-potassium dihydrogen phosphate-deionized water, and potassium hydroxide-dipotassium hydrogen phosphate-deionized water.
[0077] More preferably, the mass ratio of alkali, salt and solvent is (0.1-5):(0.1-5):100.
[0078] More preferably, the compound inorganic salt-solvent composite system includes one of the following: sodium dihydrogen phosphate / disodium hydrogen phosphate-deionized water, potassium dihydrogen phosphate / disodium hydrogen phosphate-deionized water, sodium bicarbonate / sodium carbonate-deionized water, ammonium carbonate / ammonium bicarbonate-deionized water, or sodium tetraborate / sodium tetradecyl borate-deionized water.
[0079] More preferably, the mass ratio of the compounded inorganic salt to the solvent is (0.1-10):100.
[0080] Most preferably, the mass ratio of the two components of the compound inorganic salt is (0.1-5):1.
[0081] Preferably, the surfactant complex in step (1) is one or more fluorinated compounds and / or hydrocarbons.
[0082] More preferably, the fluorinated compound includes one or more mixtures of perfluoropolyether-polyethylene glycol-perfluoropolyether triblock copolymer, perfluoropolyether ammonium carboxylate, perfluoropolyether ammonium sulfonate, linear perfluoropolyether ammonium fluorocarbonate, perfluoroalkyl phosphate, and sodium perfluoropolyether amide sulfonate.
[0083] More preferably, the hydrocarbon includes one or more of the following: sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium lauryl ether sulfate, polyoxyethylene sorbitan fatty acid ester, cocamidopropyl betaine, sodium lignin sulfonate, sodium dibutylnaphthalene sulfonate, sodium diisopropylnaphthalene sulfonate, ethoxyethanesulfonate, and sodium oleoyl methyl taurate.
[0084] More preferably, the amount of surfactant complex used is 0.1 wt.% to 0.5 wt.% of the amount of solvent used in the pH buffer solution in step (1).
[0085] Most preferably, the mass ratio of any plurality of compounds in the surfactant complex is (0.1-10):(0.1-10), (0.1-10):(0.1-10):(0.1-10), or (0.1-10):(0.1-10):(0.1-10):(0.1-10).
[0086] Preferably, the polymerization temperature in step (1) is 60~80℃.
[0087] Preferably, the first polymerizing monomer component in step (2) is a mixture of vinylidene fluoride, tetrafluoroethylene and hexafluoropropylene.
[0088] More preferably, the molar ratio of vinylidene fluoride, tetrafluoroethylene, and hexafluoropropylene is (16-40):(12-29):(34-58).
[0089] Preferably, the polymerization pressure in step (2) is 1.2 MPa to 2.6 MPa.
[0090] Preferably, in step (2), the chain transfer agent is composed of a molecular structure such as general formula I.
[0091] The general formula I is: A-(C Y 2) s -A.
[0092] in, Y It can be a fluorine atom or a carbon atom, s = 2, 4, 6 or 8, A is a halogen atom, which can be a bromine or iodine atom.
[0093] More preferably, the amount of chain transfer agent used in step (2) is 0.04 wt.%-0.30 wt.% of the amount of solvent used in the pH buffer solution in step (1).
[0094] Preferably, in step (2), the sulfur point monomer is composed of a molecular structure such as general formula II.
[0095] The general formula II is: R 1 R 2 -C=CR 3 -(CF2)m -(CH2) u -O f -(CF2) v -A Among them, R 1 R 2 and R 3 For hydrogen atoms and / or fluorine atoms, 0 ≤ m + u + v ≤ 6, 0 ≤ f ≤1, A is a halogen atom, which can be a bromine or iodine atom.
[0096] More preferably, the amount of sulfidation point monomer used in step (2) is 0.1 wt.%-3.0 wt.% of the amount of solvent used in the pH buffer solution in step (1).
[0097] Preferably, the initiator in step (2) is a group or combination of potassium persulfate and / or ammonium persulfate.
[0098] More preferably, the amount of initiator used is 0.1 wt.%-0.8 wt.% of the amount of solvent used in the pH buffer solution in step (1).
[0099] Preferably, the second monomer component in step (3) is a mixture of vinylidene fluoride, tetrafluoroethylene and hexafluoropropylene.
[0100] More preferably, the molar ratio of vinylidene fluoride, tetrafluoroethylene, and hexafluoropropylene is (28-60):(16-40):(20-55).
[0101] Preferably, the amount of pH buffer added in step (3) is 0.01-0.1 parts of the amount of pH buffer used in step (1).
[0102] More preferably, the amount of pH buffer added in step (3) is 0.02-0.08 parts of the amount of pH buffer used in step (1).
[0103] Preferably, the amount of chain transfer agent added in step (3) is 0.01-0.6 parts of the amount of chain transfer agent used in step (2).
[0104] More preferably, the amount of chain transfer agent added in step (3) is 0.1-0.4 parts of the amount of chain transfer agent used in step (2).
[0105] Preferably, the amount of sulfur point monomer added in step (3) is 0.1-1.5 parts of the amount of sulfur point monomer used in step (2).
[0106] More preferably, the amount of sulfur point monomer added in step (3) is 0.2-1.0 parts of the amount of sulfur point monomer used in step (2).
[0107] Preferably, the number of repetitions in step (3) does not exceed 35.
[0108] More preferably, the number of repetitions in step (3) is 1 to 30 times.
[0109] Preferably, the salt compound in step (4) is one or more of sulfates and chlorides, including one or more of magnesium sulfate, aluminum sulfate, potassium aluminum sulfate dodecahydrate, magnesium chloride, aluminum chloride, and calcium chloride.
[0110] More preferably, the amount of salt compound used is 0.3-3.0 wt.% of the amount of pH buffer solvent used in step (1).
[0111] Preferably, the surfactant in step (4) is a hydrocarbon, including one or more of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, and sodium lauryl ether sulfate.
[0112] More preferably, the amount of surfactant used is 0.01-0.2 wt.% of the amount of pH buffer solvent used in step (1).
[0113] More preferably, when the surfactant in step (4) is a mixture of two hydrocarbons, the mass ratio of the two is (0.1-1):1.
[0114] Preferably, the drying temperature in step (4) is 75-105 °C.
[0115] The following detailed description is based on specific embodiments.
[0116] Unless otherwise specified, the reagents, methods, instruments, and equipment used in this invention are conventional in the art. Unless otherwise specified, the reagents and materials used in the following examples are all commercially available.
[0117] Example 1 This embodiment provides a method for preparing fluororubber raw rubber: (1) Add a pH buffer consisting of 40 kg deionized water, 0.5 kg ammonia water, and 2 kg ammonium chloride to a 100L polymerization reactor and a surfactant complex consisting of 8 g perfluoropolyether-polyethylene glycol-perfluoropolyether triblock copolymer, 23 g perfluoropolyether ammonium sulfonate, and 22 g sodium dodecyl sulfonate. Vacuum the reactor, inject nitrogen, and then evacuate again. Repeat this process several times to remove oxygen from the polymerization reactor. Then turn on the stirrer and heat the reactor to 70 °C. (2) The first polymerization monomer composed of VDF, TFE and HFP is injected into the polymerization reactor in a molar ratio of 39:21:40. The injection pressure is increased to 2 MPa, and then 0.12 kg of diiodomethane is added as a chain transfer agent, 0.04 kg of trifluoroiodoethylene as a sulfurization point monomer and 0.04 kg of ammonium persulfate as an initiator. (3) After the pressure inside the reactor drops, the second polymerization monomer composed of VDF, TFE and HFP is added. The molar ratio of the three is 42:37:21 to maintain the pressure inside the polymerization reactor. The reaction continues. During the reaction, 3.4 kg of pH buffer (with the same composition and ratio as in step 1), 24 g of diiodomethane and 0.04 kg of trifluoroiodide are added intermittently 5 times until the specified reaction amount is reached. After the reaction ends, the peroxyfluorinated rubber emulsion is obtained. (4) Add 1.2 kg magnesium chloride and 0.08 kg sodium lauryl ether sulfate to the emulsion to coagulate, filter and wash, dry at 100°C to finally obtain fluoropolymer raw rubber, and test its performance using standard formulation.
[0118] Example 2 This embodiment provides a method for preparing fluororubber raw rubber: (1) Add a pH buffer consisting of 45 kg deionized water, 3.75 kg potassium dihydrogen phosphate, and 0.75 kg dipotassium hydrogen phosphate, and a surfactant complex consisting of 17 g perfluoropolyether ammonium sulfonate and 73 g cocamidopropyl betaine to a 100L polymerization reactor. Vacuum the reactor, inject nitrogen, and then evacuate again. Repeat this process several times to remove oxygen from the polymerization reactor. Then turn on the stirrer and heat the reactor to 60 °C. (2) The first polymerization monomer composed of VDF, TFE and HFP is injected into the polymerization reactor in a molar ratio of 16:29:45. The injection pressure is increased to 2.6 MPa. Then, 0.018 kg of 1,4-diiodoperfluorobutane is added as a chain transfer agent, 1.35 kg of 3,3,4,4-tetrafluoro-1-butene-difluoro-6-bromo-ether is added as a sulfidation point monomer and 0.1215 kg of potassium persulfate is added as an initiator. (3) After the pressure inside the reactor drops, the second polymerization monomer composed of VDF, TFE and HFP is added in a molar ratio of 55:25:20 to maintain the pressure inside the polymerization reactor. The reaction continues. During the reaction, 2.475 kg of pH buffer (with the same composition and ratio as in step 1), 7.2 g of 1,4-diiodoperfluorobutane and 0.27 kg of 3,3,4,4-tetrafluoro-1-butene-difluoro-6-bromo-ether are added intermittently 10 times until the specified reaction amount is reached. After the reaction ends, peroxyfluorinated rubber emulsion is obtained. (4) Add 0.675 kg of potassium aluminum sulfate dodecahydrate, 382.5 g of sodium dodecyl sulfonate and 382.5 g of sodium lauryl ether sulfate to the emulsion to coagulate, filter and wash, dry at 75°C to finally obtain peroxyfluorinated rubber raw rubber, and test its performance using standard formulation.
[0119] Example 3 This embodiment provides a method for preparing fluororubber raw rubber: (1) Add a pH buffer consisting of 37 kg deionized water, 0.074 kg sodium hydroxide, and 0.0454 kg sodium tetraborate, and a surfactant complex consisting of 46 g linear perfluoropolyether ammonium fluorocarbonate, 28 g sodium oleoyl methyl taurate, 36 g sodium dodecylbenzene sulfonate and 75 g hydroxyethanesulfonate to a 100L polymerization reactor. Vacuum the reactor, inject nitrogen, and then evacuate again. Repeat this process several times to remove oxygen from the polymerization reactor. Then turn on the stirrer and heat the reactor to 80 °C. (2) The first polymerization monomer composed of VDF, TFE and HFP is injected into the polymerization reactor in a molar ratio of 40:12:58. The injection pressure is increased to 1.85 MPa. Then, 0.0211 kg of 1,6-diiodohexane is added as a chain transfer agent, 0.074 kg of 3,3,4,4,5,5,6-6-octafluoro-6-iodo-1-hexene is added as a sulfidation point monomer and 0.2146 kg of potassium persulfate is added as an initiator. (3) After the pressure inside the reactor drops, the second polymerization monomer composed of VDF, TFE and HFP is added in a molar ratio of 45:31:34 to maintain the pressure inside the polymerization reactor. The reaction continues. During the reaction, 1.13 kg of pH buffer (with the same composition and ratio as in step 1), 4.54 g of 1,6-diiodohexane and 0.248 kg of 3,3,4,4,5,5,6-6-octafluoro-6-iodo-1-hexene are added intermittently 30 times until the specified reaction amount is reached. After the reaction ends, the peroxyfluorinated rubber emulsion is obtained. (4) Add 0.37 kg of aluminum sulfate and 70 g of sodium dodecylbenzenesulfonate to the emulsion to coagulate, filter and wash, dry at 85°C to finally obtain peroxyfluorinated rubber raw rubber, and test its performance using standard formulation.
[0120] Example 4 This embodiment provides a method for preparing fluororubber raw rubber: (1) Add a pH buffer consisting of 30 kg deionized water, 1.2 kg ammonium carbonate, and 0.6 kg ammonium bicarbonate, and a surfactant complex consisting of 25 g sodium perfluoropolyether amide sulfonate, 40 g perfluoroalkyl phosphate, and 58 g hydroxyethanesulfonate to a 100L polymerization reactor. Vacuum the reactor, inject nitrogen, and then evacuate again. Repeat this process several times to remove oxygen from the polymerization reactor. Then turn on the stirrer and heat the reactor to 75 °C. (2) The first polymerization monomer composed of VDF, TFE and HFP is injected into the polymerization reactor in a molar ratio of 31:14:55. The injection pressure is increased to 2.1 MPa. Then, 0.039 kg of 1,4-diiodobutane is added as a chain transfer agent, 0.42 kg of 3,3,4,4-tetrafluoro-4-iodo-1-butene is added as a sulfurization point monomer and 0.135 kg of potassium persulfate is added as an initiator. (3) After the pressure inside the reactor drops, the second polymerization monomer composed of VDF, TFE and HFP is added in a molar ratio of 28:40:32 to maintain the pressure inside the polymerization reactor. The reaction continues. During the reaction, 1.272 kg of pH buffer (with the same composition and ratio as in step 1), 11.7 g of 1,4-diiodobutane and 0.126 kg of 3,3,4,4-tetrafluoro-4-iodo-1-butene are added intermittently 7 times until the specified reaction amount is reached. After the reaction ends, the peroxyfluorinated rubber emulsion is obtained. (4) Add 0.6 kg of aluminum sulfate, 30 g of sodium dodecylbenzene sulfonate and 3 g of sodium dodecyl sulfonate to the emulsion to coagulate, filter and wash, dry at 80 °C to finally obtain the raw rubber of fluoropolymer, and test its performance using the standard formula.
[0121] Example 5 This embodiment provides a method for preparing fluororubber raw rubber: (1) Add a pH buffer consisting of 50 kg deionized water, 0.3 kg ammonia water, and 1.5 kg ammonium nitrate, and a surfactant complex consisting of 45 g perfluoropolyether ammonium carboxylate, 42 g sodium dibutylnaphthalene sulfonate and 51 g sodium diisopropylnaphthalene sulfonate to a 100L polymerization reactor. Vacuum the reactor, inject nitrogen, and then evacuate again. Repeat this process several times to remove oxygen from the polymerization reactor. Then turn on the stirrer and heat the reactor to 110 °C. (2) The first polymerization monomer composed of VDF, TFE and HFP is injected into the polymerization reactor in a molar ratio of 37:29:34. The injection pressure is increased to 1.2 MPa. Then, 0.0767 kg of diiodomethane is added as a chain transfer agent, 1.5 kg of 3,3,4,4-tetrafluoro-6-bromo-1-hexene is added as a sulfidation point monomer and 0.35 kg of ammonium persulfate is added as an initiator. (3) After the pressure inside the reactor drops, the second polymerization monomer composed of VDF, TFE and HFP is added. The molar ratio of the three is 60:16:24 to maintain the pressure inside the polymerization reactor. The reaction continues. During the reaction, 4.144 kg of pH buffer (with the same composition and ratio as in step 1), 30.7 g of diiodomethane and 1.5 kg of 3,3,4,4-tetrafluoro-6-bromo-1-hexene are added intermittently once during the reaction until the specified reaction amount is reached. After the reaction ends, the peroxyfluorinated rubber emulsion is obtained. (4) Add 0.5 kg of aluminum chloride and 10 g of sodium lauryl ether sulfate to the emulsion to coagulate, filter and wash, dry at 85°C to finally obtain the raw rubber of fluoropolymer, and test its performance using the standard formula.
[0122] Example 6 This embodiment provides a method for preparing fluororubber raw rubber: (1) Add a pH buffer consisting of 40 kg deionized water, 0.2 kg sodium tetraborate, and 0.2 kg sodium tetradecyl borate and a surfactant complex consisting of 6 g perfluoropolyether ammonium sulfonate, 14 g linear perfluoropolyether ammonium fluorocarbonate, 12 g polyoxyethylene sorbitan fatty acid ester and 8 g sodium dodecyl sulfonate to a 100L polymerization reactor. Vacuum the reactor, inject nitrogen and then evacuate again. Repeat this process several times to remove oxygen from the polymerization reactor. Then turn on the stirrer and heat the reactor to 90 °C. (2) The first polymerization monomer composed of VDF, TFE and HFP is injected into the polymerization reactor in a molar ratio of 23:28:49. The injection pressure is increased to 2.5 MPa. Then, 0.0344 kg of 1,4-diiodoperfluorobutane is added as a chain transfer agent, 0.64 kg of perfluoro-1-iodo(4-hexene) is added as a sulfidation point monomer and 0.22 kg of ammonium persulfate is added as an initiator. (3) After the pressure inside the reactor drops, the second polymerization monomer composed of VDF, TFE and HFP is added in a molar ratio of 52:25:23 to maintain the pressure inside the polymerization reactor and the reaction continues. During the reaction, 1.212 kg of pH buffer (with the same composition and ratio as in step 1), 6.88 g of 1,4-diiodoperfluorobutane and 0.128 kg of perfluoro-1-iodo(4-hexene) are added intermittently 14 times until the specified reaction amount is reached. After the reaction ends, the peroxyfluorinated rubber emulsion is obtained. (4) Add 0.08 kg magnesium sulfate and 16 g sodium dodecylbenzene sulfonate to the emulsion to coagulate, filter and wash, dry at 105°C to finally obtain peroxyfluorinated rubber raw rubber, and test its performance using standard formulation.
[0123] Comparative Example 1 The difference from Example 1 is that ammonium chloride was not added to the pH buffer solution, and 3.24 kg of the aforementioned pH buffer solution was added once during the reaction. All other conditions were the same.
[0124] Comparative Example 2 The difference from Example 2 is that the surfactant complex consists of 2 g of perfluoropolyether ammonium sulfonate and 268 g of cocamidopropyl betaine. All other conditions are the same.
[0125] Comparative Example 3 The difference from Example 3 is that the chain transfer agent was changed to tribromomethane, and the number of additions during the reaction was 0. All other conditions were the same.
[0126] Comparative Example 4 The difference from Example 4 is that the initial amount of 1,4-diiodobutane added to the reaction was 1 kg. All other conditions were the same.
[0127] Comparative Example 5 The difference from Example 5 is that the amount of 3,3,4,4-tetrafluoro-6-bromo-1-hexene added is 5 g, and the amount of 3,3,4,4-tetrafluoro-6-bromo-1-hexene added subsequently is also 5 g. All other conditions are the same.
[0128] Comparative Example 6 The difference from Example 6 is that the mass of sodium tetraborate is 0.36 kg and the mass of sodium borate tetradecylate is 0.04 kg. All other conditions are the same.
[0129] Based on the successful preparation of the peroxyfluorinated rubber raw materials in the above embodiments and comparative examples, this invention further weighs the raw rubber corresponding to Examples 1-6 and Comparative Examples 1-6, along with various vulcanizing auxiliaries, according to the standard formulations in Table 1 below. After thorough mixing, the raw materials are pressed into test pieces, and the vulcanization properties, mechanical properties, and media resistance properties of the peroxyfluorinated rubber are tested. Detailed results for each peroxyfluorinated rubber sample are shown in Tables 2 and 3.
[0130] The scorch time Ts2, scorch time Ts10, scorch time Ts50, and positive vulcanization time T90 were measured using a vulcanization tester. Hardness was measured using a hardness tester. Tensile strength and elongation at break were measured using a rubber tensile testing machine. Compression set (70h) was measured. (200℃) Measured according to GB / T 7759.1.
[0131] Table 1 Standard Formulation Table Table 2. Summary of test results for Examples 1-6 Table 3. Summary of test results for comparative examples 1-6 Compared to Comparative Examples 1-6, Examples 1-6 exhibited superior mechanical properties and resistance to media. Examples 1-6 had high degrees of vulcanization, and the hardness of the vulcanized fluoropolymers was not lower than 78, classifying them as high-hardness fluoropolymers. Furthermore, the vulcanized fluoropolymers of Examples 1-6 possessed excellent tensile properties, with tensile strengths generally exceeding 20 MPa and elongation at break exceeding 169%, demonstrating excellent tensile mechanical properties. Most importantly, the vulcanized fluoropolymers of Examples 1-6 exhibited excellent compression set properties, with a compression set rate of less than 15%, compared to only 9% for Example 6, both superior to the performance of fluoropolymers in existing patents. In addition, the vulcanized fluoropolymers of Examples 1-6, after immersion in methanol at 80°C for 72 hours, showed a volume change rate of no more than 0.3%, exhibiting almost no swelling, indicating that the fluoropolymers prepared in this invention exhibit excellent methanol resistance. After being immersed in an electrolyte at 80°C for 72 hours, the vulcanized peroxyfluororubbers of Examples 1-6 showed a maximum volume change rate of only 8.5%, all exhibiting excellent electrolyte resistance. In summary, the peroxyfluororubbers of Examples 1-6, after being mixed and vulcanized using the standard formulation, exhibited excellent mechanical properties and resistance to electrolytes.
[0132] The difference between Comparative Example 1 and Example 1 lies in the fact that the vulcanization rate of Comparative Example 1 was slower and the degree of vulcanization was significantly reduced, but the hardness increased. Although the tensile strength increased, the elongation at break decreased significantly. In addition, although the compression set remained almost unchanged, the volume change rate after methanol immersion increased to 1.5%, and the volume change rate after electrolyte immersion increased to 14.6%. The main reason is that less ammonium chloride was added to the pH buffer, which changed the pH of the entire polymerization system, resulting in a significant change in the structure of the final fluoropolymer, leading to a decrease in the mechanical properties and media resistance of the fluoropolymer.
[0133] The difference between Comparative Example 2 and Example 2 lies in the fact that the vulcanization rate of Comparative Example 2 remained essentially unchanged, but the degree of vulcanization and hardness decreased significantly, with a hardness of only 76A and a tensile strength reduced to 16.2 MPa. However, its elongation at break increased to 219%, and its compression set also increased to 30%. The volume change rate after methanol immersion and electrolyte immersion increased significantly, especially after electrolyte immersion, where the volume change rate increased to 29.6%. The main reason for this is that after changing the emulsifier ratio, the dispersibility of the chain transfer agent and vulcanization point monomer in the polymerization system deteriorated, resulting in these additives not being uniformly incorporated, ultimately leading to a decrease in the performance of the peroxyfluororubber.
[0134] The difference between the results of Comparative Example 3 and Example 3 is due to the fact that when the chain transfer agent was changed to tribromoethane and not added during the reaction, the concentration of the chain transfer agent in the polymerization system was insufficient, and the chain transfer effect was not obvious. As a result, not enough vulcanizing point monomers were introduced into the peroxyfluorinated rubber, which led to an accelerated vulcanization rate but a lower degree of vulcanization. Ultimately, this resulted in a significant decrease in the mechanical properties, methanol resistance, and electrolyte resistance of the peroxyfluorinated rubber, manifested as a significant increase in the volume change rate after immersion.
[0135] The results from Comparative Example 4 and Example 4 show that, in Comparative Example 4, the addition of a larger amount of chain transfer agent resulted in a smaller molecular weight, leading to a faster vulcanization rate. However, the degree of vulcanization did not significantly improve. Furthermore, the compression set, methanol, and electrolyte tolerance also deteriorated significantly. The main reason is that the addition of a large amount of chain transfer agent caused abnormalities in the molecular chain structure of the fluoropolymer, ultimately resulting in a significant difference between the properties of the vulcanized fluoropolymer in Comparative Example 4 and those in Example 4.
[0136] The difference between Comparative Example 5 and Example 5 lies in the fact that Comparative Example 5 had a lower amount of vulcanizing point monomer added, resulting in a slower vulcanization rate and a significantly reduced degree of vulcanization. Therefore, the tensile strength of the vulcanized fluoropolymer was significantly lower than that of Example 5. Furthermore, the compression set, methanol immersion volume change rate, and electrolyte immersion volume change rate were all higher than those of Example 5, indicating a significant deterioration in the performance of the fluoropolymer in Comparative Example 5. The main reason is that the reduced amount of vulcanizing point monomer resulted in fewer vulcanizing points in the fluoropolymer molecular chain, thus leading to a significant difference in the performance of the fluoropolymer in Comparative Example 5 compared to the product in Example 5.
[0137] Based on the results of Comparative Example 6 and Example 6, the change in the ratio of the composite salt in the pH buffer caused the pH range of the polymerization system to exceed the effective polymerization pH range, which had a very adverse effect on the performance of the final raw rubber.
[0138] Compression set is a crucial property of fluororubber. Low compression set enables its widespread application in traditional and emerging fields such as chemical engineering, aerospace, and new energy, generating substantial economic benefits. Furthermore, resistance to various media is another important property of fluororubber. Excellent resistance to media means that fluororubber can be used under extremely harsh conditions, achieving very high added value. The technical solution provided by this invention allows for a stable polymerization reaction, with precise control over the polymerization rate of each monomer during the reaction, resulting in fluororubber with low compression set and excellent resistance to various media.
[0139] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.
Claims
1. A method for preparing peroxyfluororubber raw rubber, characterized in that, Includes the following steps: (1) Add pH buffer and surfactant to the polymerization reactor to remove oxygen from the polymerization reactor, and heat to the polymerization temperature; (2) After adding the initial polymerization monomer components to the polymerization reactor to the polymerization pressure, add the chain transfer agent, sulfurization point monomer and initiator; (3) After the pressure in the polymerization reactor drops, add the monomer components to maintain the pressure in the polymerization reactor and continue the reaction. During the reaction, pH buffer, chain transfer agent and vulcanization point monomer are added multiple times. After the reaction ends, peroxyfluorinated rubber emulsion is obtained. (4) Add salt compounds and surfactants to the peroxyfluorinated rubber emulsion, and carry out coagulation, washing and drying to finally obtain the peroxyfluorinated rubber raw rubber.
2. The method for preparing peroxyfluororubber raw rubber according to claim 1, characterized in that, The pH buffer solution contains alkali, salt, and solvent; The mass ratio of the alkali, salt, and solvent is (0.1-5):(0.1-5):100; Alternatively, the pH buffer solution may contain a compound inorganic salt and a solvent; The mass ratio of the compounded inorganic salt to the solvent is (0.1-10):
100.
3. The method for preparing peroxyfluororubber raw rubber according to claim 2, characterized in that, The alkali includes at least one of ammonia, sodium hydroxide, and potassium hydroxide; The salt includes at least one of ammonium nitrate, ammonium sulfite, ammonium bisulfite, ammonium bicarbonate, ammonium carbonate, ammonium sulfite, ammonium chloride, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium borate tetradecylhydrate, sodium tetraborate, potassium dihydrogen phosphate, and dipotassium hydrogen phosphate. The compound inorganic salt includes at least one of sodium dihydrogen phosphate / disodium hydrogen phosphate, potassium dihydrogen phosphate / disodium hydrogen phosphate, sodium bicarbonate / sodium carbonate, ammonium carbonate / ammonium bicarbonate, and sodium tetraborate / sodium tetradecylate. The solvent includes deionized water.
4. The method for preparing peroxyfluororubber raw rubber according to claim 1, characterized in that, The chain transfer agent has the following general formula: A-(C Y 2) s -A; in, Y It is a fluorine atom or a carbon atom, s = 2, 4, 6 or 8, and A is a halogen atom, including bromine and iodine atoms; The sulfurization point monomer has the following general formula: R 1 R 2 -C=C-R 3 -(CF2) m -(CH2) u -O f -(CF2) v -A; Among them, R 1 R 2 and R 3 For hydrogen or fluorine atoms, 0 ≤ m + u + v ≤ 6, 0 ≤ f ≤1, where A is a halogen atom, including bromine and iodine atoms; The initiator is a group or combination of potassium persulfate and ammonium persulfate.
5. The method for preparing peroxyfluororubber raw rubber according to claim 1, characterized in that, The polymer monomer components are a mixture of vinylidene fluoride, tetrafluoroethylene and hexafluoropropylene; In step (2), the molar ratio of vinylidene fluoride, tetrafluoroethylene, and hexafluoropropylene in the initial monomer components is (16-40): (12-29): (34-58). In step (3), the molar ratio of vinylidene fluoride, tetrafluoroethylene, and hexafluoropropylene in the added monomer components is (28-60): (16-40): (20-55).
6. The method for preparing peroxyfluororubber raw rubber according to claim 1, characterized in that, The surfactant mentioned in step (1) is a fluorinated compound and / or a hydrocarbon; The fluorinated compounds include one or more mixtures of perfluoropolyether-polyethylene glycol-perfluoropolyether triblock copolymer, perfluoropolyether ammonium carboxylate, perfluoropolyether ammonium sulfonate, linear perfluoropolyether ammonium fluorocarbonate, perfluoroalkyl phosphate, and sodium perfluoropolyether amide sulfonate. The hydrocarbons include one or more of the following: sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium lauryl ether sulfate, polyoxyethylene sorbitan fatty acid ester, cocamidopropyl betaine, sodium lignin sulfonate, sodium dibutylnaphthalene sulfonate, sodium diisopropylnaphthalene sulfonate, ethoxyethanesulfonate, and sodium oleoyl methyl taurate. The amount of surfactant used in step (1) is 0.1 wt.%-0.5 wt.% of the amount of solvent used in the pH buffer solution in step (1); The polymerization temperature in step (1) is 60~80℃.
7. The method for preparing peroxyfluororubber raw rubber according to claim 1, characterized in that, The polymerization pressure in step (2) is 1.2 MPa to 2.6 MPa; The amount of chain transfer agent used in step (2) is 0.04 wt.% - 0.30 wt.% of the amount of solvent used in the pH buffer solution in step (1); The amount of sulfide point monomer used in step (2) is 0.1 wt.%-3.0 wt.% of the amount of solvent used in the pH buffer solution in step (1). The amount of initiator used in step (2) is 0.1 wt.%-0.8 wt.% of the amount of solvent used in the pH buffer solution in step (1).
8. The method for preparing peroxyfluororubber raw rubber according to claim 1, characterized in that, In step (3), the amount of pH buffer added in a single step is 1 wt.% to 10 wt.% of the amount of pH buffer used in step (1). The amount of chain transfer agent added in step (3) in a single step is 1 wt.%-60 wt.% of the amount of chain transfer agent used in step (2). The amount of sulfur point monomer added in step (3) in a single step is 10 wt.%-150 wt.% of the amount of sulfur point monomer used in step (2); The number of times to replenish in step (3) shall not exceed 35.
9. The method for preparing peroxyfluororubber raw rubber according to claim 1, characterized in that, The salt compound mentioned in step (4) is one or more of sulfates and chlorides, including one or more of magnesium sulfate, aluminum sulfate, potassium aluminum sulfate dodecahydrate, magnesium chloride, aluminum chloride, and calcium chloride. The amount of salt compound used in step (4) is 0.3 wt.%-3.0 wt.% of the amount of pH buffer solvent used in step (1). The surfactant mentioned in step (4) is a hydrocarbon; The hydrocarbons include one or more of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, and sodium lauryl ether sulfate; The amount of surfactant used in step (4) is 0.01 wt.%-0.2 wt.% of the amount of pH buffer solvent used in step (1); The drying temperature in step (4) is 75-105 ℃.
10. A type of peroxyfluororubber raw rubber, characterized in that, It is prepared by any one of the preparation methods described in claims 1 to 9.
Citation Information
Patent Citations
Transparent peroxide fluororubber intelligent wearable material and preparation method thereof
CN115466344A
Raw fluororubber and preparation method thereof
CN116162199A
Peroxide vulcanized fluororubber and preparation method thereof
CN118184852A
Synergistic enhanced high-thermal-stability corrosion-resistant fluoroperoxide rubber and preparation method thereof
CN121136312A
Peroxyfluororubber raw rubber, peroxyfluororubber and preparation method of peroxyfluororubber raw rubber
CN121824819A