A low-residue, low-extractable-content, highly safe, and highly absorbent resin and its preparation method thereof.
By using bifunctional mesoporous silicate encapsulation to contain a reducing agent and controlling its release in the preparation of superabsorbent resin, combined with staged polymerization and washing techniques, the problem of difficult diffusion of redox initiators inside the gel was solved, achieving the preparation of a highly safe resin with low residue and extractability, suitable for hygiene products and medical dressings.
Patent Information
- Application Number
- CN202611262576.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
During the polymerization process of existing superabsorbent resins, the redox initiator inside the gel is difficult to diffuse, resulting in high content of residual monomers and extractables, which makes it difficult to meet high safety requirements.
A bifunctional mesoporous silicate encapsulates the reducing agent, and its release timing is controlled by a temperature-responsive gating material. Combined with staged polymerization and ionic strength oscillation washing, redox pairs are formed inside the gel, reducing the content of residual monomers and extractables.
It improves the monomer conversion rate in the later stage of polymerization, reduces the content of residual monomers and extractables, and enhances the safety and water absorption properties of the resin, making it suitable for hygiene products and medical dressings.
Smart Images

Figure CN123106976A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of preparation technology of superabsorbent resins, specifically to a low-residue, low-extractable-content, highly safe superabsorbent resin and its preparation method. Background Technology
[0002] Superabsorbent polymers (SAPs) are widely used in hygiene products, medical dressings, and other fields. Their residual monomer and extractable content directly affect safety. The key to reducing residual monomer and extractable content lies in improving the monomer conversion rate within the gel during the later stages of polymerization. However, externally added initiators after gelation have difficulty diffusing into the gel, resulting in persistently high levels of residual monomer and extractable content.
[0003] Invention patent ZL200710043081.3 (authorization announcement number CN100554292C) discloses a rapid preparation method for superabsorbent resin. This method uses acrylic acid as a monomer and an ion-exchange membrane alkali as a neutralizing agent. After heating the monomer solution to 50–80°C using neutralization heat, a crosslinking agent and a redox initiator (such as potassium persulfate / sodium bisulfite) are added in a single step. The polymerization reaction is completed within 2–15 minutes in a reaction pan at 60–90°C. This method achieves rapid polymerization through a redox initiation system, which shortens the production cycle to some extent.
[0004] However, the aforementioned patent has a core flaw: its redox initiator is added to the monomer solution all at once, and is consumed in large quantities in the early stages of polymerization due to the rapid initiation reaction. When the system enters the gelation stage, on the one hand, the concentration of the residual reducing agent in the solution has significantly decreased; on the other hand, the externally added oxidant is also blocked from penetrating the gel interior by the gel network diffusion barrier. This results in a severe lack of effective redox initiators inside the gel in the later stages of polymerization, and the content of residual monomers and soluble oligomers (extractables) remains high (the residual monomer content in its examples is 180–420 ppm), making it difficult to meet the stringent requirements of high-safety SAP. Summary of the Invention
[0005] The purpose of this invention is to provide a low-residue, low-extractable-content, highly safe, and highly absorbent resin and its preparation method.
[0006] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing a low-residue, low-extractable-content, highly safe, and highly absorbent resin includes the following steps: (a) Prepare an aqueous monomer solution containing acrylic monomers, an internal crosslinking agent and a bifunctionalized mesoporous silicate; the inner surface of the mesoporous channels of the bifunctionalized mesoporous silicate is grafted with mercapto groups, the mesoporous pores and the outer surface are grafted with amino groups, the mesoporous channels are encapsulated with an internal reducing agent, and the mesoporous pore openings are sealed by a temperature-responsive gating material. (b) The monomer aqueous solution is polymerized in stages: in the first stage, the polymerization is initiated at low temperature with a redox initiator pair; in the second stage, the temperature is increased and a thermal initiator is added, and the polymerization continues until gelation; in the third stage, the temperature is increased to not lower than the opening temperature of the gate material, an additional oxidant is added and the temperature is maintained, the gate material is opened, the encapsulated reducing agent is released in situ inside the gel, and forms a redox pair with the additional oxidant. (c) The resulting hydrogel was subjected to ionic strength shaking wash, with alternating washing with dilute salt solution and pure water; (d) The washed gel is dried, crushed and sieved to obtain resin. The resin is then subjected to surface crosslinking treatment to obtain a highly absorbent resin.
[0007] By adopting the above technical solution, bifunctional mesoporous silicates can encapsulate the internal reducing agent in the early stage of polymerization, preventing the reducing agent from participating in the reaction and being consumed prematurely. After heating to the gate material opening temperature in the third stage, the internal reducing agent can be released in situ inside the gel and form a redox pair with the added oxidant, thereby overcoming the problem that the external initiator is difficult to diffuse into the gel after gelation and improving the monomer conversion rate in the later stage of polymerization. Staged polymerization can balance polymerization rate and gel structure stability. Ionic strength shaking washing can promote the precipitation of residual monomers, soluble oligomers and auxiliary agent residues. Surface crosslinking treatment is beneficial to improving the gel strength and absorption performance of the resin, so that the resulting resin has low residual monomers, low extractables, high safety and good water absorption properties.
[0008] Preferably, the matrix of the bifunctional mesoporous silicate includes MCM-41 or SBA-15, with a pore size of 2-10 nm and a specific surface area of 500-1000 m² / g; the grafting density of thiol groups is 0.2-1.0 mmol / g, and the grafting density of amino groups is 0.5-2.0 mmol / g; both the thiol grafting density and the amino grafting density are based on the mass of the dried functionalized mesoporous silica before the encapsulation of the reducing agent and the formation of the gate layer; the amount of bifunctional mesoporous silica used is 0.1-1.0 wt% of the mass of the acrylic monomer.
[0009] By adopting the above technical solutions, MCM-41 or SBA-15 possesses a regular mesoporous structure and a high specific surface area, providing ample space for reducing agent encapsulation and functional group grafting. Limiting the pore size, specific surface area, and grafting density of thiol and amino groups facilitates differentiated functionalization of the inner surface of the pores and the pore openings and outer surfaces. Specifically, amino groups grafted onto the pore openings and outer surfaces improve the dispersibility of mesoporous silicates in monomer aqueous solutions and polymer matrices; thiol groups grafted onto the inner surface of the pores form hydrogen bonds and weak polar interactions with the encapsulated reducing agent molecules, anchoring the encapsulated reducing agent and reducing leakage before gate closure. Furthermore, it suppresses instantaneous release after gate opening, allowing the encapsulated reducing agent to be released smoothly and continuously into the surrounding gel aqueous phase, achieving stable encapsulation and controllable release. Controlling the amount of bifunctionalized mesoporous silicate reduces residual monomers and extractables while avoiding excessive inorganic components that could negatively impact the resin's water absorption ratio, gel strength, and processing performance.
[0010] The differentiated functionalization of the aforementioned bifunctional mesoporous silicates is achieved through the sequence of preparation steps. Thiolization modification is performed before encapsulation with the reducing agent. At this stage, the mesoporous channels are open, allowing mercaptopropylsilane to enter the channels and graft onto the inner surface. Since the specific surface area of mesoporous silicates such as MCM-41 and SBA-15 is primarily contributed by the inner surface of the channels, with the outer surface typically accounting for less than 5%, the majority of thiol groups are located on the inner surface of the channels, and the small number of thiol groups on the outer surface have no substantial impact on the encapsulation and controlled release behavior of the reducing agent. Aminolation modification is performed after encapsulation with the reducing agent and temperature-gated sealing. At this stage, the mesoporous channels are filled and sealed by the reducing agent and gating material, making it difficult for aminopropylsilane to enter the channels. It can only react with the silanol groups at the pore openings and on the outer surface; therefore, the amino groups are mainly grafted onto the pore openings and the outer surface. Therefore, without additional selective protection or deprotection steps, a spatial distribution can be achieved in which thiol groups are mainly located on the inner surface of the pores, and amino groups are mainly located on the pore openings and outer surfaces.
[0011] Preferably, the temperature-responsive gating material includes fatty acid phase change materials, which are selected from one or more of stearic acid, arachidic acid, and behenic acid; the opening temperature of the temperature-responsive gating material is 5-15°C higher than the highest processing temperature of the second stage and 5-15°C lower than the heat preservation temperature of the third stage.
[0012] By adopting the above technical solution, fatty acid-based phase change materials can undergo phase change at a set temperature, thereby achieving temperature-responsive sealing and opening of mesoporous channels. Setting the opening temperature between the highest processing temperature of the second stage and the holding temperature of the third stage ensures that the gated material remains sealed in the first and second stages, preventing premature release of the encapsulated reducing agent. After entering the third stage, the gated material can reliably open, allowing the encapsulated reducing agent to be released promptly within the gel, thereby improving the accuracy of the release timing, reducing premature consumption of the reducing agent, and enhancing the redox initiation efficiency within the gel during the later stages of polymerization.
[0013] Preferably, the inner reducing agent includes ascorbic acid, sodium bisulfite, and sodium metabisulfite; the amount of the inner reducing agent is 5-20 wt% of the mass of the bifunctional mesoporous silicate; the supplementary oxidant includes one or more of potassium persulfate, sodium persulfate, ammonium persulfate, and hydrogen peroxide; the amount of supplementary oxidant is 0.02-0.20 mol based on the total molar amount of acrylic monomers.
[0014] By employing the above technical solutions, ascorbic acid, sodium bisulfite, and sodium metabisulfite can form an effective redox initiation system with the added oxidant, promoting the continued polymerization of residual monomers within the gel in the third stage. Limiting the amount of encapsulated reducing agent ensures sufficient reducing components within the gel while avoiding excessive reducing agent leading to increased residues or polymerization imbalance. Limiting the type and amount of added oxidant facilitates a continuous and appropriate supply of free radicals after gelation, improving the subsequent monomer conversion rate while reducing initiator residues and their impact on resin safety.
[0015] Preferably, the first stage is carried out at 5–15°C; the redox initiator pair includes an oxidant and a reductant, the oxidant includes ammonium persulfate, potassium persulfate, and sodium persulfate, and the reductant includes sodium bisulfite, sodium metabisulfite, and sodium sulfite; based on the total molar amount of acrylic monomers, the amount of oxidant is 0.005–0.03 mol%, the amount of reductant is 0.005–0.06 mol%, and the molar ratio of oxidant to reductant is 1:0.5–1:2; the second stage is heated to 40–70°C at a rate of 0.5–2°C / min and held for 30–120 min; the third stage is heated to 80–95°C at a rate of 0.5–2°C / min and held for 60–180 min.
[0016] By adopting the above technical solution, the low-temperature first stage can slow down the initial polymerization rate, reduce localized burst polymerization and uneven gel structure; limiting the amount and molar ratio of oxidant and reducing agent is beneficial for forming a stable and controllable initial initiation process. The second stage uses gradient heating and holding, which allows the polymerization reaction to continue while forming a stable gel network; the third stage further heats and holds, which can improve polymer chain activity and the conversion degree of residual monomers. The coordination of temperature and time in each stage is beneficial for balancing polymerization stability, gel structure uniformity, residual monomer reduction effect, and production efficiency.
[0017] Preferably, the thermal initiator is selected from one or more of 2,2′-azobis(2-amidinylpropane) dihydrochloride, 2,2′-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, ammonium persulfate, and potassium persulfate; the amount of thermal initiator is 0.01 to 0.20 mol based on the total molar amount of acrylic monomers.
[0018] By adopting the above technical solution, the thermal initiator can decompose and generate free radicals during the second stage of heating, which, together with the polymer active centers formed in the first stage, synergistically promote the continued polymerization reaction. Selecting a thermal initiator suitable for the waterborne acrylic monomer polymerization system is beneficial to improving the initiation efficiency and polymerization uniformity during the heating stage. Controlling the amount of thermal initiator can ensure sufficient monomer conversion before gelation while avoiding excessively high free radical concentrations that could lead to uncontrolled polymerization rate, excessively short polymer chains, or increased initiator residue.
[0019] Preferably, the dilute salt solution in the ionic strength shaking wash includes an aqueous solution of sodium chloride or sodium sulfate with a concentration of 0.05–0.5 wt%. The ionic strength shaking wash consists of one wash with dilute salt solution followed by one wash with pure water as a cycle, and is performed for 3–6 cycles, with the last wash using pure water. The liquid-to-solid mass ratio of the ionic strength shaking wash is 5:1 to 10:1, where the liquid-to-solid mass ratio is the ratio of the mass of the washing solution used in a single wash to the total mass of the hydrogel. The washing time for a single wash is 10–30 min, and the washing temperature is 40–60 °C. After the ionic strength shaking wash, a gradient washing step is also included: first washing with an aqueous solution containing 5–20 vol% ethanol, then washing with pure water containing 0.005–0.05 wt% citric acid, and finally washing with pure water until neutral.
[0020] By employing the above technical solution, the alternating action of dilute salt solution and pure water causes the hydrogel to repeatedly shrink and swell during changes in ionic strength, enhancing mass transfer between the gel interior and the washing solution. This promotes the migration of residual monomers, soluble oligomers, salts, and initiator residues from the gel interior to the exterior. Limiting the number of washing cycles, liquid-to-solid ratio, time, and temperature helps to improve elution efficiency while minimizing damage to the gel structure. Ethanol-water solution further elutes weakly polar extractable components, citric acid solution complexes or promotes the migration of metal ions and some polar impurities, and final washing with pure water restores the resin to a neutral state, thereby improving product safety and hygienic suitability.
[0021] Preferably, a microwave treatment step is included between step (b) and step (c): the obtained hydrogel is broken into particles with a particle size of 2-8 mm and treated with microwave power of 300-500 W for 1-3 min.
[0022] By employing the above-mentioned technical solution, breaking the hydrogel into suitable particle sizes can shorten the migration path of soluble components from the gel's interior to the exterior. Microwave treatment enables rapid overall heating of the gel particles, enhancing molecular thermal motion and water migration within the gel, and promoting the diffusion of residual monomers, soluble oligomers, and other extractables to the gel surface. Controlling the microwave power and treatment time can improve subsequent washing efficiency while avoiding over-treatment that could damage the gel network or reduce resin absorption performance.
[0023] Preferably, the drying in step (d) is vacuum-nitrogen pulse drying, specifically including: placing the washed gel in a vacuum drying device and maintaining a vacuum for 10-20 minutes under an absolute pressure of 5-20 kPa and a temperature of 60-80°C; then purging with nitrogen for 2-5 minutes, restoring to normal pressure, and completing one pulse cycle; repeating the pulse cycle 3-6 times; the surface crosslinking treatment includes: spraying a surface crosslinking agent onto the pulverized and sieved resin, followed by heat treatment of the resin; the surface crosslinking agent includes one or more of polyols, cyclic carbonates, polyglycidyl ethers, and polyvalent metal salts.
[0024] By adopting the above technical solutions, the vacuum environment can reduce the temperature and time required for moisture removal, while nitrogen pulse purging can promptly remove moisture from gel pores and between particles. The cyclical combination of vacuum and nitrogen purging can reduce surface crusting and internal moisture retention during the drying process, resulting in resin particles with a more uniform structure and better water absorption. The surface crosslinking agent, after spraying and heat treatment, can form a structure with a high crosslinking density on the surface of the resin particles, thereby improving gel strength, pressure absorption performance, and anti-caking properties. Simultaneously, it reduces the outward migration of soluble components from within the particles, which is beneficial for balancing absorption performance and safety in use.
[0025] The present invention also provides a low-residue, low-extractable, high-safety, and highly absorbent resin prepared by any of the above preparation methods, comprising a cross-linked polymer matrix formed by polymerizing acrylic monomers, and a bifunctionalized mesoporous silicate uniformly dispersed in the cross-linked polymer matrix.
[0026] By employing the above technical solution, the cross-linked polymer matrix formed by the polymerization of acrylic monomers endows the resin with excellent water absorption and retention capabilities. The uniformly dispersed bifunctionalized mesoporous silicate provides a controllable release of reducing agent during polymerization and promotes further conversion of residual monomers within the gel. The resulting resin can simultaneously reduce the content of residual monomers and extractables, minimizing potential skin irritation and migration risks, while maintaining high water absorption capacity, gel strength, and stability. It is suitable for applications with high safety requirements, such as hygiene products and medical dressings.
[0027] In summary, the present invention has at least the following beneficial effects: 1. Constructing an in-situ delayed initiation mechanism within the gel: The reducing agent is encapsulated using bifunctional mesoporous silicate, and its release timing is controlled by a temperature-responsive gating material. This allows the reducing agent to be released in situ within the gel after gelation, forming a redox pair with the added oxidant, effectively solving the problem of external initiators being difficult to diffuse into the gel.
[0028] 2. Reduce the content of residual monomers and extractables: Improve the monomer conversion rate in the later stage of polymerization by staged polymerization through low-temperature redox initiation, thermal initiation and high-temperature in-situ redox initiation; combined with ionic strength oscillation washing and gradient washing, further promote the elution of soluble oligomers, residual monomers and auxiliary agent residues.
[0029] 3. Improve the overall performance of the resin: Vacuum-nitrogen pulse drying reduces surface crusting and internal moisture retention during the drying process, and surface crosslinking treatment improves the gel strength, pressure absorption performance and anti-caking performance of the resin particles.
[0030] 4. Improve product safety: Ascorbic acid, sodium bisulfite, sodium metabisulfite and other encapsulated reducing agents participate in the later polymerization stage after mesoporous encapsulation and controlled release, reducing free reducing agents and system residues; finally, washing to neutral makes the resin more suitable for fields with high safety requirements such as hygiene products and medical dressings. Attached Figure Description
[0031] Figure 1 This is a process flow diagram of the method for preparing a low-residue, low-extractable-content, high-safety, and highly absorbent resin according to the present invention. Detailed Implementation
[0032] like Figure 1As shown, the overall process flow of the preparation method of the low-residue, low-extractable, high-safety, and highly absorbent resin of the present invention is as follows: preparing an aqueous monomer solution containing acrylic monomers, an internal crosslinking agent, and bifunctionalized mesoporous silicate; polymerizing the aqueous monomer solution in stages; washing the resulting hydrogel with ionic strength shaking; drying, pulverizing, and sieving the washed gel, and then performing surface crosslinking treatment to obtain the highly absorbent resin.
[0033] The present invention will be further illustrated by the following examples. Example 1 uses the median values of the main parameters, Example 2 uses the lower limit values of the main raw materials and dosage parameters, Example 3 uses the upper limit values of the main raw materials and dosage parameters, Example 4 is used to investigate the effect of not performing microwave treatment on the resin properties, and Example 5 is used to investigate the effect of the composite surface crosslinking system on the resin properties. Comparative Examples 1-6 are used to investigate the effects of mesoporous silicate encapsulation structure, temperature-responsive gated material, third-stage in-situ redox initiation, ion strength oscillation washing, and vacuum-nitrogen pulse drying, respectively. Comparative Example 7 is used to investigate the effects of initial gelation disruption and atomized spraying of oxidant.
[0034] In the following examples, unless otherwise specified, the amount of acrylic acid used was 100.0g, the degree of neutralization was 75mol%, the internal crosslinking agent was polyethylene glycol diacrylate, and the amount used was 0.20wt% of the mass of acrylic acid; the particle size of the resin after crushing and sieving was 150-850μm.
[0035] Example 1
[0036] This embodiment uses intermediate parameters to prepare a low-residue, low-extractable-content, high-safety, and highly absorbent resin.
[0037] 1. Preparation of bifunctional mesoporous silicates Commercially available MCM-41 was used as the mesoporous silicate matrix. The pore size of MCM-41 was determined to be 3.2 nm and the specific surface area was 850 m² / g using a nitrogen adsorption analyzer.
[0038] (1) Thiolization modification 50.0 g of MCM-41 was placed in a vacuum drying oven and dried at 120 °C for 4 h to remove adsorbed water. The dried MCM-41 was then added to a 1 L three-necked flask equipped with a mechanical stirrer, a reflux condenser, and a nitrogen inlet tube. 500 mL of anhydrous toluene was added, and the mixture was ultrasonically dispersed for 20 min. Subsequently, 5.9 g of 3-mercaptopropyltrimethoxysilane was added, and the mixture was heated to 110 °C under nitrogen protection and a stirring rate of 300 r / min, and refluxed for 12 h.
[0039] After the reaction was completed, the mixture was filtered using a sintered glass funnel, washed three times each with toluene and anhydrous ethanol, and then extracted with anhydrous ethanol using a Soxhlet extractor for 12 hours to remove unreacted silane coupling agent. The resulting solid was dried under vacuum at 60°C for 12 hours to obtain mercaptolated MCM-41. The sulfur content was determined using an elemental analyzer, and the mercapto grafting density was calculated to be 0.60 mmol / g.
[0040] (2) Inner encapsulation of reducing agent Add 30.0 g of mercapto-modified MCM-41 to a 250 mL round-bottom flask, then add 100 mL of a water / ethanol mixture containing 4.5 g of ascorbic acid (water to ethanol volume ratio 1:1). Connect the flask to a vacuum apparatus and maintain the pressure at 25 °C and 10 kPa for 30 min, then restore atmospheric pressure to allow the ascorbic acid solution to enter the mesoporous channels. Repeat the vacuum impregnation process three times.
[0041] After impregnation, the solid was removed and quickly rinsed with a small amount of cold ethanol to remove the ascorbic acid adhering to the outer surface of the particles. Then, it was vacuum dried to constant weight at 35°C under nitrogen protection to obtain thiolized MCM-41 encapsulated with ascorbic acid.
[0042] (3) Temperature-gated closure Stearic acid and arachidic acid were mixed in a 1:1 mass ratio to obtain a fatty acid-based phase change material. The turn-on temperature of this fatty acid-based phase change material was determined to be 70℃ using differential scanning calorimetry.
[0043] 3.0 g of fatty acid phase change material was melted in an oil bath at 76 °C, and the above-mentioned thiolated MCM-41 encapsulating ascorbic acid was added. The mixture was stirred at 100 r / min for 10 min to seal the mesoporous pore openings of the molten fatty acid phase change material. It was then rapidly cooled to 25 °C to obtain gated mesoporous silicate.
[0044] (4) Aminoation modification The gated mesoporous silicate was added to a 500 mL three-necked flask, followed by 150 mL of an ethanol / water mixture (95:5 volume ratio). At 25 °C and a stirring rate of 200 rpm, 8.0 g of 3-aminopropyltriethoxysilane was slowly added dropwise. After the addition was complete, the reaction continued for 4 h.
[0045] After the reaction was completed, the mixture was filtered, washed three times with anhydrous ethanol, and dried under vacuum at 40°C for 12 h to obtain bifunctionalized mesoporous silica. The nitrogen content was determined using an elemental analyzer, and the amino grafting density was calculated to be 1.20 mmol / g. Both the thiol grafting density and amino grafting density were based on the mass of the dried functionalized mesoporous silica before encapsulation of the reducing agent and formation of the gate layer. Thermogravimetric analysis and extraction-titration were used to verify that the ascorbic acid encapsulation amount was 12 wt% of the mass of the bifunctionalized mesoporous silica.
[0046] 2. Preparation of monomer aqueous solution A 1L jacketed glass reactor was used as the polymerization equipment. The reactor was equipped with an anchor stirrer, thermometer, nitrogen inlet pipe, condenser and metering pump.
[0047] Add 100.0g of acrylic acid and 80.0g of deionized water to the reactor, start stirring and introduce a refrigeration circulating medium to maintain the system temperature below 15℃. Under a stirring rate of 200r / min, slowly add 166.5g of a 25wt% sodium hydroxide aqueous solution over a time of 40min until the acrylic acid reaches a neutralization degree of 75mol%. During the addition process, control the system temperature to not exceed 25℃.
[0048] After neutralization, add 0.20 g of polyethylene glycol diacrylate and stir for 15 min to dissolve it completely. Then add 0.50 g of the above bifunctionalized mesoporous silicate and disperse it at 2000 r / min for 10 min using a high-speed disperser, followed by ultrasonic treatment for 5 min to obtain a homogeneous monomer aqueous solution.
[0049] 3. Phased aggregation Nitrogen gas was bubbled into the monomer aqueous solution for 30 minutes to remove dissolved oxygen from the system. The temperature of the reactor was controlled at 10℃.
[0050] Stage 1: Weigh out 0.0475 g of ammonium persulfate and 0.0433 g of sodium bisulfite, and dissolve each in 5.0 g of deionized water. Based on the total molar amount of acrylic acid, the amount of ammonium persulfate is 0.015 mol%, and the amount of sodium bisulfite is 0.030 mol%, with a molar ratio of 1:2. Add the ammonium persulfate solution first, followed by the sodium bisulfite solution, at 10°C, and stir for 20 min.
[0051] Second stage: Weigh 0.188 g of 2,2′-azobis(2-amidinepropane) dihydrochloride, dissolve it in 10.0 g of deionized water, and add it to the reaction vessel. The amount of thermal initiator is 0.050 mol% based on the total molar amount of acrylic acid. Then, the system is heated from 10 °C to 55 °C at a rate of 1 °C / min, and held at 55 °C for 60 min to allow the system to reach the initial stage of gelation, resulting in a gel that still has a water-containing soft gel state.
[0052] After the second stage is completed, while the gel is still hot, it is shredded into gel particles with a diameter of about 5 mm through a perforated plate, and the gel particles are then placed back into a reaction vessel with a jacket and a low-speed stirring device.
[0053] Stage 3: The gel particles were heated from 55°C to 85°C at a rate of 1°C / min. 0.375 g of potassium persulfate was weighed and dissolved in 10.0 g of deionized water to obtain a supplementary oxidant solution. At 85°C, the supplementary oxidant solution was sprayed evenly onto the surface of the gel particles in three applications using an atomizing nozzle. After each spray, the particles were stirred at a low speed of 30 r / min for 2 min to ensure that the potassium persulfate was evenly distributed between the gel particles and diffused into the interior along the continuous aqueous phase of the gel particles. The amount of potassium persulfate used was 0.100 mol based on the total molar amount of acrylic acid.
[0054] During the heating process, when the system temperature reaches 70℃, the fatty acid phase change material activates, and ascorbic acid is released from the mesoporous channels to the channel openings, the outer surface of the mesoporous silicate, and the surrounding aqueous gel phase. Potassium persulfate diffuses along the continuous aqueous phase of the gel particles to the vicinity of the mesoporous silicate, comes into contact with the released ascorbic acid, and forms a redox pair. After the oxidant solution is added and sprayed, the system is kept at 85℃ for 120 min to allow the residual monomers inside the gel to continue to polymerize, resulting in hydrous gel particles.
[0055] 4. Microwave processing The obtained hydrogel was removed and crushed into particles with a diameter of approximately 5 mm using a gel crusher. The gel particles were then spread evenly in a microwave-safe tray, with a layer thickness controlled at 15 mm. The tray was then processed using a 2450 MHz microwave oven at 400 W for 2 minutes. The particles were turned over every minute during processing to ensure even heating.
[0056] 5. Ion strength shaking wash and gradient wash The microwave-treated hydrogel was placed in a washing vessel equipped with a stirrer and temperature control. It was washed alternately with a 0.20 wt% sodium chloride aqueous solution and pure water, with one wash of dilute salt solution followed by one wash of pure water constituting one cycle, for a total of four cycles.
[0057] The liquid-to-solid mass ratio for each wash was 8:1, the washing temperature was 50℃, the washing time was 20 minutes, and the stirring rate was 100 r / min. The final wash used pure water.
[0058] After the ionic strength shaking wash is completed, a gradient wash is continued: first, an aqueous solution containing 10 vol% ethanol is used to wash for 20 min at a liquid-to-solid mass ratio of 8:1 and 50℃; then, pure water containing 0.02 wt% citric acid is used to wash for 20 min at the same liquid-to-solid mass ratio and temperature; finally, pure water is used to wash until the pH of the wash solution is 6.8–7.2.
[0059] 6. Vacuum-nitrogen pulse drying The washed gel particles were evenly spread on a tray in a vacuum drying oven, with a layer thickness controlled at 10 mm. The vacuum drying oven was heated to 70°C, and a vacuum was drawn to an absolute pressure of 12 kPa, which was maintained for 15 min. Then, nitrogen gas was introduced to purge for 3 min, and the pressure was restored to normal, completing one pulse cycle. The above pulse cycle was repeated 4 times to obtain dried resin blocks.
[0060] The dried resin blocks were crushed using a pulverizer and then sieved using a standard sieve to collect resin particles with a diameter of 150–850 μm.
[0061] 7. Surface crosslinking treatment The sieved resin particles were placed in a horizontal mixer equipped with an atomizing nozzle, and the stirring speed was controlled at 300 r / min. 0.30 wt% of 1,4-butanediol diglycidyl ether was weighed based on the dry resin mass and dispersed in a water / ethanol mixed solvent with a water to ethanol mass ratio of 1:1. The total amount of surface crosslinking treatment solution used was 3.0 wt% of the dry resin mass.
[0062] The surface crosslinking treatment liquid was uniformly sprayed onto the surface of the resin particles through an atomizing nozzle for 10 minutes, followed by 10 minutes of mixing. The resin particles were then placed in a 150°C hot air circulating drying oven for 30 minutes for heat treatment. After cooling, a low-residue, low-extractable-content, highly safe, and highly absorbent resin was obtained.
[0063] Example 2
[0064] This embodiment uses the lower limit values of the main raw materials and dosage parameters. The only difference from Embodiment 1 is: 1. SBA-15 was used as the mesoporous silicate matrix with a pore size of 6.5 nm and a specific surface area of 550 m² / g.
[0065] 2. The thiol grafting density was 0.20 mmol / g, and the amino grafting density was 0.50 mmol / g.
[0066] 3. The amount of bifunctional mesoporous silicate used is 0.10 wt% of the mass of acrylic acid.
[0067] 4. The reducing agent inside is sodium bisulfite, and the packaging amount is 5 wt% of the mass of the bifunctional mesoporous silicate.
[0068] 5. The temperature-responsive gating material is stearic acid, and the opening temperature is 70℃.
[0069] 6. The temperature of the first stage is 5℃; based on the total molar amount of acrylic acid, the amount of ammonium persulfate is 0.005 mol%, the amount of sodium bisulfite is 0.005 mol%, and the molar ratio of the two is 1:1.
[0070] 7. In the second stage, the temperature is increased to 60℃ at a rate of 0.5℃ / min and held for 120min; the thermal initiator is ammonium persulfate, and the amount is 0.010mol.
[0071] 8. After the second stage ends and the system reaches the initial stage of gelation, while it is still hot, break the soft gel into particles with a diameter of about 5 mm and put it back into the reaction vessel with a jacket and a low-speed stirring device.
[0072] 9. In the third stage, the gel particles were heated from 60℃ to 80℃ at a rate of 0.5℃ / min. Sodium persulfate was added as the oxidant, at a dosage of 0.020 mol% based on the total molar amount of acrylic acid. The sodium persulfate was dissolved in 10.0 g of deionized water and sprayed evenly onto the surface of the gel particles in three applications using an atomizing nozzle. After each spray, the particles were stirred at a low speed of 30 r / min for 2 min. After spraying, the mixture was kept at 80℃ for 180 min.
[0073] 10. Ionic strength shaking washing uses 0.05wt% sodium chloride aqueous solution, for a total of 3 cycles, with a liquid-to-solid mass ratio of 5:1, a single washing time of 10 min, and a washing temperature of 40℃.
[0074] 11. In the gradient washing process, the concentration of the ethanol aqueous solution was 5 vol%, and the concentration of citric acid was 0.005 wt%.
[0075] 12. The gel particles obtained in the third stage do not need to be crushed into large pieces again. They can be directly processed using a microwave processing device with a frequency of 2450MHz at a power of 300W for 1 minute.
[0076] 13. The vacuum-nitrogen pulse drying conditions are: absolute pressure 20 kPa, temperature 60℃, vacuum hold for 10 min, nitrogen purging for 2 min, repeated 3 times.
[0077] 14. The surface crosslinking agent is glycerol, the amount of which is 0.20 wt% of the dry resin mass, the heat treatment temperature is 140℃, and the heat treatment time is 40 min.
[0078] The remaining raw materials, operating steps and preparation conditions are the same as in Example 1.
[0079] Example 3
[0080] This embodiment uses the upper limit values of the main raw materials and dosage parameters. The only difference from Embodiment 1 is: 1. MCM-41 was used as the mesoporous silicate matrix with a pore size of 2.5 nm and a specific surface area of 980 m² / g.
[0081] 2. The thiol grafting density was 1.00 mmol / g, and the amino grafting density was 2.00 mmol / g.
[0082] 3. The amount of bifunctional mesoporous silicate used is 1.0 wt% of the mass of acrylic acid.
[0083] 4. The reducing agent inside is sodium metabisulfite, and the packaging amount is 20 wt% of the mass of the bifunctional mesoporous silicate.
[0084] 5. The temperature-responsive gating material is a mixture of arachidic acid and behenic acid in a 1:1 mass ratio, with an opening temperature of 82℃.
[0085] 6. The temperature of the first stage is 15℃; based on the total molar amount of acrylic acid, the amount of potassium persulfate is 0.030 mol%, the amount of sodium bisulfite is 0.060 mol%, and the molar ratio of the two is 1:2.
[0086] 7. In the second stage, the temperature is increased to 70℃ at a rate of 2℃ / min and held for 30min; the thermal initiator is potassium persulfate, and the amount used is 0.200mol.
[0087] 8. After the second stage ends and the system reaches the initial stage of gelation, while it is still hot, break the soft gel into particles with a particle size of 2-5 mm and put it back into the reaction vessel with a jacket and a low-speed stirring device.
[0088] 9. In the third stage, the gel particles were heated from 70°C to 95°C at a rate of 2°C / min. Ammonium persulfate was added as the oxidant, at a dosage of 0.200 mol% based on the total molar amount of acrylic acid. The ammonium persulfate was dissolved in 10.0 g of deionized water and sprayed evenly onto the surface of the gel particles in three applications using an atomizing nozzle. After each spray, the particles were stirred at a low speed of 30 r / min for 2 min. After spraying, the mixture was kept at 95°C for 60 min.
[0089] 10. Ionic strength shaking washing uses a 0.50wt% sodium sulfate aqueous solution, for a total of 6 cycles, with a liquid-to-solid mass ratio of 10:1, a single washing time of 30 min, and a washing temperature of 60℃.
[0090] 11. In the gradient washing, the concentration of the ethanol aqueous solution was 20 vol%, and the concentration of citric acid was 0.05 wt%.
[0091] 12. The microwave processing power is 500W, and the processing time is 3 minutes.
[0092] 13. The vacuum-nitrogen pulse drying conditions are: absolute pressure 5 kPa, temperature 80℃, vacuum holding for 20 min, nitrogen purging for 5 min, repeated 6 times.
[0093] 14. The surface crosslinking agent is polyglycidyl ether, the amount of which is 0.50 wt% of the dry resin mass, the heat treatment temperature is 160℃, and the heat treatment time is 25 min.
[0094] The remaining raw materials, operating steps and preparation conditions are the same as in Example 1.
[0095] Example 4
[0096] This example is used to investigate the effect of microwave treatment on resin properties. The only difference from Example 1 is that after the third stage of heat preservation and obtaining hydrogel particles, they are crushed into particles with a particle size of approximately 5 mm, but microwave treatment is not performed; subsequent ionic strength shaking washing and gradient washing are performed directly. All other raw materials, operating steps, and preparation conditions are the same as in Example 1.
[0097] Example 5
[0098] This example is used to investigate the effect of the composite surface crosslinking system on resin properties. The only difference from Example 1 is: 1. MCM-41 was used as the mesoporous silicate matrix with a pore size of 3.8 nm and a specific surface area of 780 m² / g.
[0099] 2. The thiol grafting density was 0.80 mmol / g, and the amino grafting density was 1.50 mmol / g.
[0100] 3. The amount of bifunctional mesoporous silicate used is 0.80 wt% of the mass of acrylic acid.
[0101] 4. The reducing agent inside is sodium bisulfite, and the packaging amount is 15 wt% of the mass of the bifunctional mesoporous silicate.
[0102] 5. The temperature-responsive gate material is arachidic acid, and the opening temperature is 75℃.
[0103] 6. The temperature of the first stage is 12℃; based on the total molar amount of acrylic acid, the amount of sodium persulfate is 0.020 mol%, the amount of sodium sulfite is 0.010 mol%, and the molar ratio of the two is 1:0.5.
[0104] 7. In the second stage, the temperature was increased to 65℃ at a rate of 1.5℃ / min and held for 50min; the thermal initiator was 2,2′-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, and the amount used was 0.100mol.
[0105] 8. After the second stage ends and the system reaches the initial stage of gelation, while it is still hot, break the soft gel into particles with a diameter of about 5 mm and put it back into the reaction vessel with a jacket and a low-speed stirring device.
[0106] 9. In the third stage, the gel particles were heated from 65℃ to 90℃ at a rate of 1.5℃ / min. The added oxidant consisted of potassium persulfate and hydrogen peroxide in a 1:1 molar ratio, with a total added oxidant amount of 0.150 mol% based on the total molar amount of acrylic acid. The added oxidant was dispersed or dissolved in 10.0 g of deionized water and sprayed evenly onto the surface of the gel particles in three applications using an atomizing nozzle. After each spray, the particles were stirred at a low speed of 30 r / min for 2 min. After spraying, the mixture was kept at 90℃ for 90 min.
[0107] 10. Ionic strength shaking washing uses a 0.30wt% sodium chloride aqueous solution, for a total of 5 cycles, with a liquid-to-solid mass ratio of 9:1, a single washing time of 25 min, and a washing temperature of 55℃.
[0108] 11. In the gradient washing, the concentration of the ethanol aqueous solution was 15 vol%, and the concentration of citric acid was 0.04 wt%.
[0109] 12. The microwave processing power is 400W, and the processing time is 2 minutes.
[0110] 13. The vacuum-nitrogen pulse drying conditions are: absolute pressure 10 kPa, temperature 75℃, vacuum holding for 18 min, nitrogen purging for 4 min, repeated 5 times.
[0111] 14. The surface crosslinking agent is ethylene carbonate and aluminum sulfate, with a mass ratio of ethylene carbonate to aluminum sulfate of 3:1. The total amount of surface crosslinking agent is 0.40 wt% of the dry resin mass. The heat treatment temperature is 155℃ and the heat treatment time is 30 min.
[0112] The remaining raw materials, operating steps and preparation conditions are the same as in Example 1.
[0113] Comparative Example 1
[0114] The only difference from Example 1 is that bifunctional mesoporous silicates are not added to the monomer aqueous solution, and encapsulated ascorbic acid is not introduced into the system.
[0115] After the second stage ends and the system reaches the initial stage of gelation, the soft gel is broken into particles with a diameter of about 5 mm while it is still hot, and then placed back into a reaction vessel with a jacket and a low-speed stirring device. In the third stage, after the temperature is raised to 85°C, only 0.375 g of potassium persulfate is dissolved in 10.0 g of deionized water and added in three portions using the same atomized spraying method as in Example 1.
[0116] The remaining polymerization, washing, microwave treatment, drying and surface crosslinking conditions were the same as in Example 1.
[0117] Comparative Example 2
[0118] The only difference from Example 1 is that an equal amount of ascorbic acid is encapsulated in mesoporous silicate, but fatty acid phase change materials are not used to seal the mesoporous pore openings, so that ascorbic acid is released and consumed in advance during the preparation of monomer aqueous solution and the first and second stage polymerization processes.
[0119] After the second stage reaches the initial stage of gelation, the soft gel is broken into particles with a diameter of about 5 mm. In the third stage, potassium persulfate solution is sprayed in the same way as in Example 1.
[0120] All other conditions are the same as in Example 1.
[0121] Comparative Example 3
[0122] The only difference from Example 1 is that unencapsulated ascorbic acid-gated mesoporous silicate is used, and the amount of mesoporous silicate added is the same as in Example 1.
[0123] After the second stage reaches the initial stage of gelation, the soft gel is also broken into particles with a diameter of about 5 mm. In the third stage, after heating to 85℃, 0.06 g of ascorbic acid and 0.375 g of potassium persulfate are dissolved together in 10.0 g of deionized water, and sprayed onto the surface of the gel particles in 3 times using an atomizing nozzle. After each spray, the mixture is stirred at a low speed of 30 r / min for 2 min.
[0124] All other conditions are the same as in Example 1.
[0125] Comparative Example 4
[0126] The only difference from Example 1 is that the ion strength oscillation washing and gradient washing are replaced with pure water washing.
[0127] The washing process was repeated 8 times with pure water, each time with a liquid-to-solid mass ratio of 8:1, a washing temperature of 50°C, and a washing time of 20 minutes, ensuring that the total washing water consumption and total washing time remained consistent with Example 1. After the pure water washing, ethanol-water solution washing and citric acid-water solution washing were not performed; instead, subsequent vacuum-nitrogen pulse drying was carried out directly.
[0128] The remaining conditions for initial gelation disruption, atomized spraying to replenish oxidant, microwave treatment, drying, and surface crosslinking were the same as in Example 1.
[0129] Comparative Example 5
[0130] The only difference from Example 1 is that vacuum-nitrogen pulse drying is replaced with conventional hot air drying.
[0131] Specifically, the washed gel particles were evenly spread in a stainless steel tray with a layer thickness of 10 mm, and then dried in a 70°C hot air circulating drying oven for 8 hours. After drying, the particles were crushed, sieved, and surface crosslinked in the same manner as in Example 1.
[0132] The remaining conditions for initial gelation disruption, atomized spraying to replenish oxidant, ionic strength shaking washing, gradient washing, and microwave treatment were the same as in Example 1.
[0133] Comparative Example 6
[0134] The only difference from Example 1 is that the third stage of heating, gate opening, oxidant spraying, and high-temperature insulation treatment are not performed.
[0135] Specifically, in the second stage, the system is kept at 55℃ for 60 minutes to reach the initial stage of gelation. While still hot, the soft gel is broken into particles with a diameter of about 5 mm. Then, it is directly subjected to microwave treatment, ion strength shaking washing, gradient washing, vacuum-nitrogen pulse drying and surface crosslinking treatment.
[0136] All other conditions are the same as in Example 1.
[0137] Comparative Example 7
[0138] The only difference from Example 1 is that in the second stage, after holding the gel at 55°C for 60 min and reaching the initial stage of gelation, the blocky soft gel was kept intact and heated directly from 55°C to 85°C at a rate of 1°C / min. 0.375 g of potassium persulfate was dissolved in 10.0 g of deionized water and poured onto the surface of the blocky gel at 85°C in one go, without atomization spraying or stirring. The gel was then held at 85°C for 120 min. After the third stage of holding, the resulting gel was broken into particles with a diameter of approximately 5 mm, and then subjected to microwave treatment, ionic strength shaking washing, gradient washing, vacuum-nitrogen pulse drying, and surface crosslinking treatment in the same manner as in Example 1. All other raw materials, operating steps, and preparation conditions were the same as in Example 1.
[0139] Performance testing
[0140] The superabsorbent resins prepared in Examples 1-5 and Comparative Examples 1-7 were subjected to performance tests. Each group of samples was tested in triplicate, and the average value was taken as the test result.
[0141] 1. Residual monomer content Weigh 1.000 g of resin sample and add 100 mL of 0.9 wt% sodium chloride aqueous solution. Extract by shaking at 25 °C and 180 r / min for 60 min. After extraction, filter through a 0.45 μm aqueous filter membrane and perform high performance liquid chromatography analysis on the filtrate.
[0142] The chromatographic conditions were as follows: C18 column; mobile phase: 0.01 mol / L potassium dihydrogen phosphate aqueous solution, pH adjusted to 2.5 with phosphoric acid; flow rate: 1.0 mL / min; column temperature: 30℃; UV detection wavelength: 210 nm. A standard curve was plotted using acrylic acid standards, and acrylates were converted to acrylic acid. Test results are expressed in ppm (mass of acrylic acid as a percentage of the dry resin).
[0143] 2. Extractable content Weigh 1.000 g of resin sample and add 200 mL of deionized water. Extract by shaking at 25 °C and 180 r / min for 2 h. After extraction, filter through a 0.45 μm filter membrane. Accurately measure 50 mL of the filtrate into a pre-weighed evaporating dish and evaporate to constant weight at 105 °C. After subtracting the blank, calculate the mass of soluble substances. The extractable content is expressed as a percentage of the mass of soluble substances to the mass of dried resin.
[0144] 3. Absorption rate of physiological saline Weigh 0.500g of resin sample and place it in a pre-weighed nonwoven bag. Immerse the nonwoven bag in 500mL of 0.9wt% sodium chloride aqueous solution and allow it to absorb freely at 25℃ for 30min. After removal, let it stand for 10min to drain the liquid. Weigh the total mass of the nonwoven bag after water absorption, subtract the mass of the nonwoven bag and the blank absorption volume, and calculate the mass of physiological saline absorbed per gram of dry resin, in g / g.
[0145] 4. Pressure absorption capacity Weigh 0.160 g of resin sample and spread it evenly in a test tube with a sieve. Apply a load of 0.7 psi above the resin. Contact the resin with a 0.9 wt% sodium chloride aqueous solution and absorb at 25 °C for 60 min. After the test, weigh the mass of absorbed liquid and calculate the absorption capacity per unit mass of resin under pressure, expressed in g / g.
[0146] 5. Absorption rate Add 50 mL of 0.9 wt% sodium chloride aqueous solution to a 100 mL beaker and stir at 25 °C and 300 rpm to form a stable vortex. Add 2.000 g of resin sample at once and start timing simultaneously. Record the time required for the vortex to disappear and the system to transform into a homogeneous gel. The shorter the time required, the faster the resin absorption rate.
[0147] 6. Performance Test Results
[0148] 7. Results Analysis (1) The role of breaking up gels in the early stage of gelation and adding oxidant by atomized spraying Comparative Example 7 maintained its blocky soft gel without breaking after reaching the initial stage of gelation in the second stage. In the third stage, potassium persulfate solution was directly poured onto the surface of the blocky gel. The residual monomer content was 185 ppm and the extractable content was 7.0 wt%, both significantly higher than the 45 ppm and 3.2 wt% of Example 1, respectively. This is because the blocky gel has a small specific surface area, and potassium persulfate can only act on the surface and shallow areas of the gel. The diffusion distance from the gel surface to the interior is long, and the diffusion is blocked by the gel network, making it difficult to reach the interior of the gel. In the later stage of polymerization, the interior of the gel still lacks effective redox initiators, resulting in insufficient conversion of residual monomers.
[0149] In Example 1, after the initial gelation stage, the soft gel was broken into particles with a diameter of approximately 5 mm, and potassium persulfate solution was added in stages using a mist spraying method. Compared to the intact block gel, the specific surface area of the gel particles was significantly increased, and the distance that potassium persulfate diffused from the particle surface to the particle center was significantly shortened. This facilitated the entry of potassium persulfate into the gel interior along the continuous aqueous phase of the gel particles, where it formed a redox pair with the ascorbic acid released after the gate was opened, thereby initiating the continued polymerization of residual monomers inside the gel. Therefore, the residual monomer content and extractable content of Example 1 were significantly lower than those of Comparative Example 7.
[0150] (2) The role of bifunctional mesoporous silicates and the third-stage in-situ redox initiation Comparative Example 1 did not include bifunctional mesoporous silicate, and only potassium persulfate was added via spraying in the third stage. Although potassium persulfate could diffuse into the gel interior after the gel particles were broken, the gel interior lacked a reducing agent to cooperate with it. Potassium persulfate mainly relied on thermal decomposition to generate free radicals, resulting in limited initiation efficiency in the later stages of polymerization. Therefore, the residual monomer content of Comparative Example 1 reached 365 ppm, and the extractable content reached 10.5 wt%.
[0151] The residual monomer content in Example 1 was 45 ppm, and the extractable content was 3.2 wt%. Compared with Comparative Example 1, the residual monomer content in Example 1 was reduced by approximately 87.7%, and the extractable content was reduced by approximately 69.5%. These results indicate that the mesoporous silicate pre-dispersed within the gel can provide a reducing agent release point for the later stages of polymerization, allowing the added oxidant and the released reducing agent to form a redox pair within the gel, thereby significantly improving the conversion degree of the residual monomer.
[0152] Comparative Example 6 did not undergo the third-stage heating, gating, and oxidant replenishment treatment. Ascorbic acid within the mesoporous channels was not released, and a late-stage redox initiation system was not formed inside the gel. Therefore, its residual monomer content was 168 ppm, and its extractable content was 7.2 wt%, both significantly higher than that of Example 1, further demonstrating that the third-stage in-situ redox initiation plays a crucial role in reducing the residual monomer and extractable content.
[0153] (3) The role of temperature-responsive gating materials Comparative Example 2 did not use fatty acid-based phase change materials to seal the mesoporous channels, resulting in the premature release of ascorbic acid during the preparation of the monomer aqueous solution and the first and second stages of polymerization. This prematurely released ascorbic acid participates in the initial redox reaction and is consumed; it also tends to form additional residues before washing. Upon entering the third stage, the amount of usable ascorbic acid within the gel significantly decreased; therefore, Comparative Example 2 had a residual monomer content of 210 ppm and an extractable content of 8.3 wt%.
[0154] Example 1 uses a fatty acid-based phase change material with an opening temperature of 70°C to maintain stable encapsulation of ascorbic acid in the first and second stages. When the temperature in the third stage exceeds the opening temperature of the gating material, ascorbic acid is released concentratedly inside the gel. Thus, Example 1 avoids premature consumption of the reducing agent, allowing more reducing agent to play its role in the later stages of polymerization, and its residual monomer and extractable content are significantly lower than those of Comparative Example 2.
[0155] (4) Advantages of in-situ release within the gel compared to simultaneous external supplementation In Comparative Example 3, ascorbic acid and potassium persulfate were co-prepared into a solution in the third stage and added to the gel particles via atomized spraying. While this method improved the distribution of the added components among the gel particles, ascorbic acid still needed to diffuse from the surface of the gel particles inwards. The gel network hindered the diffusion of the reducing agent, and ascorbic acid and potassium persulfate preferentially reacted upon contact at the gel surface, further reducing the effective amount of reducing agent that could penetrate into the gel. Therefore, Comparative Example 3 had a residual monomer content of 225 ppm and an extractable content of 8.8 wt%.
[0156] In Example 1, ascorbic acid was pre-encapsulated within mesoporous silicate channels uniformly dispersed in the polymerization system, ensuring its distribution throughout the system before gelation. After gelation, the ascorbic acid was released outward from multiple release points located within the gel, eliminating the need for long-distance migration from the gel particle surface. Therefore, the residual and extractable content of Example 1 was significantly lower than that of Comparative Example 3.
[0157] (5) The effect of ionic strength shaking washing and gradient washing Comparative Example 4 used pure water for washing with the same total water volume and total washing time. Its residual monomer content was 118 ppm and the extractable content was 7.8 wt%, both higher than those of Example 1. This is because pure water washing mainly relies on concentration difference to promote the migration of soluble components, while the release rate of soluble oligomers, residual monomers, and additive residues inside the gel is relatively slow.
[0158] Example 1 used alternating washing with dilute salt solution and pure water, causing the gel particles to repeatedly shrink and swell during changes in ionic strength, thus enhancing mass transfer between the gel and the washing solution. Ethanol-water solution further eluted weakly polar extractable components, while citric acid solution promoted the migration of metal ions and some polar impurities. Therefore, the extractable content in Example 1 was significantly lower than in Comparative Example 4.
[0159] Example 4 was identical to Example 1 except that it did not undergo microwave treatment. Its residual monomer content was 82 ppm and extractable content was 4.8 wt%, which, while still significantly lower than Comparative Examples 1-4, were higher than Example 1. This result indicates that microwave treatment can promote the migration of water and soluble components from the gel interior to the gel surface, improving the efficiency of subsequent ionic strength shaking and gradient washing.
[0160] (6) The effect of vacuum-nitrogen pulse drying Comparative Example 5, dried using conventional hot air, had a residual monomer content of 58 ppm, which was not significantly different from Example 1, indicating that the drying method was not the main factor affecting the residual monomer content. However, the saline absorption rate of Comparative Example 5 was only 43 g / g, the absorption capacity under 0.7 psi pressure was 19.1 g / g, and the absorption time was extended to 55 s, showing significantly worse absorption performance than Example 1.
[0161] The reason is that during conventional hot air drying, the surface of gel particles loses water and shrinks first, easily forming a dense layer that hinders further removal of internal moisture, leading to uneven internal structure and partial pore collapse. Example 1 uses vacuum-nitrogen pulse drying. The vacuum stage reduces resistance to moisture removal, while the nitrogen purging stage promptly removes moisture from gel pores and between particles. This cyclical combination reduces surface crusting and internal moisture retention, maintaining a more uniform particle structure in the resin. Therefore, the absorption rate, pressure absorption capacity, and absorption rate of Example 1 are significantly better than those of Comparative Example 5.
[0162] (7) Effect of different parameter ranges on resin properties Example 2, using the lower limits of the amounts of bifunctional mesoporous silicate, reducing agent encapsulation, and oxidant supplementation, had a residual monomer content of 65 ppm and an extractable content of 4.0 wt%, which were still significantly lower than those of Comparative Examples 1-4. Meanwhile, due to the lower amounts of inorganic components and surface crosslinking agents, the physiological saline absorption rate reached 55 g / g, indicating that a lower dosage range can achieve a significant reduction in residual monomers while maintaining a high absorption rate.
[0163] Example 3 used the upper limit of the main dosage, with a residual monomer content of 70 ppm and an extractable content of 4.5 wt%, which remained at a low level. However, due to the higher dosage of mesoporous silicate, initiation system, and surface crosslinking agent, the proportion of inorganic components and the degree of crosslinking in the resin particles increased, and the physiological saline absorption rate decreased to 49 g / g. This result indicates that further increasing the dosage of functional components and initiator does not continuously reduce the residual monomer and extractable content; on the contrary, it may affect the swelling space of the resin.
[0164] Example 5 uses a composite surface crosslinking system composed of ethylene carbonate and aluminum sulfate, with an absorption capacity of 26.4 g / g under 0.7 psi pressure, which is higher than that of Example 1. This indicates that the composite surface crosslinking system is beneficial for improving the surface strength of resin particles and their absorption capacity under pressure. Considering the residual monomer content, extractable content, absorption ratio, pressure absorption capacity, and absorption rate, Example 1 has the most balanced overall performance and is the preferred embodiment of this invention.
[0165] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any ordinary changes and substitutions made by those skilled in the art within the scope of the technical solution of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a low-residue, low-extractable-content, highly safe, and highly absorbent resin, characterized in that, Includes the following steps: (a) Prepare an aqueous monomer solution containing acrylic monomers, an internal crosslinking agent and a bifunctional mesoporous silicate; wherein the inner surface of the mesoporous channels of the bifunctional mesoporous silicate is grafted with mercapto groups, the mesoporous pores and the outer surface are grafted with amino groups, the mesoporous channels are encapsulated with an internal reducing agent, and the openings of the mesoporous channels are sealed by a temperature-responsive gating material. (b) The monomer aqueous solution is polymerized in stages: in the first stage, polymerization is initiated at low temperature with a redox initiator pair; in the second stage, the temperature is increased and a thermal initiator is added, and polymerization continues until gelation; in the third stage, the temperature is increased to not lower than the opening temperature of the gate material, an additional oxidant is added and the temperature is maintained, the gate material is opened, the encapsulated reducing agent is released in situ inside the gel, and forms a redox pair with the additional oxidant; (c) The resulting hydrogel is subjected to ionic strength shaking wash, wherein the ionic strength shaking wash is performed by alternating washing with dilute salt solution and pure water; (d) The washed gel is dried, pulverized and sieved to obtain resin, and the resin is subjected to surface crosslinking treatment to obtain the superabsorbent resin.
2. The preparation method according to claim 1, characterized in that, The matrix of the bifunctional mesoporous silicate includes MCM-41 or SBA-15, with a pore size of 2–10 nm and a specific surface area of 500–1000 m² / g; the grafting density of the thiol groups is 0.2–1.0 mmol / g, and the grafting density of the amino groups is 0.5–2.0 mmol / g; both the thiol grafting density and the amino grafting density are based on the mass of the dried functionalized mesoporous silica before encapsulation of the reducing agent and formation of the gate layer; the amount of the bifunctional mesoporous silicate used is 0.1–1.0 wt% of the mass of the acrylic monomer.
3. The preparation method according to claim 1, characterized in that, The temperature-responsive gating material includes a fatty acid phase change material, which is selected from one or more of stearic acid, arachidic acid, and behenic acid. The opening temperature of the temperature-responsive gating material is 5-15°C higher than the highest processing temperature of the second stage, and the opening temperature of the temperature-responsive gating material is 5-15°C lower than the heat preservation temperature of the third stage.
4. The preparation method according to claim 1, characterized in that, The inner reducing agent includes ascorbic acid, sodium bisulfite, and sodium metabisulfite, and the amount of the inner reducing agent is 5-20 wt% of the mass of the bifunctional mesoporous silicate; the supplementary oxidant includes one or more of potassium persulfate, sodium persulfate, ammonium persulfate, and hydrogen peroxide, and the amount of the supplementary oxidant is 0.02-0.20 mol based on the total molar amount of the acrylic monomers.
5. The preparation method according to claim 1, characterized in that, The first stage is carried out at 5–15°C; the redox initiator pair includes an oxidant and a reductant, the oxidant includes ammonium persulfate, potassium persulfate, and sodium persulfate, and the reductant includes sodium bisulfite, sodium metabisulfite, and sodium sulfite; based on the total molar amount of the acrylic monomers, the amount of oxidant is 0.005–0.03 mol%, the amount of reductant is 0.005–0.06 mol%, and the molar ratio of oxidant to reductant is 1:0.5–1:2; the second stage is heated to 40–70°C at a rate of 0.5–2°C / min and held for 30–120 min; the third stage is heated to 80–95°C at a rate of 0.5–2°C / min and held for 60–180 min.
6. The preparation method according to claim 1, characterized in that, The thermal initiator is selected from one or more of 2,2′-azobis(2-amidinylpropane) dihydrochloride, 2,2′-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, ammonium persulfate, and potassium persulfate; the amount of the thermal initiator is 0.01 to 0.20 mol based on the total molar amount of the acrylic monomers.
7. The preparation method according to claim 1, characterized in that, In the ionic strength agitation washing, the dilute salt solution includes a sodium chloride or sodium sulfate aqueous solution with a concentration of 0.05–0.5 wt%. The ionic strength agitation washing consists of one wash with the dilute salt solution followed by one wash with pure water as one cycle. The ionic strength agitation washing is performed for 3–6 cycles, with the final wash using pure water. The liquid-to-solid mass ratio of the ionic strength agitation washing is 5:1 to 10:1, where the liquid-to-solid mass ratio is the ratio of the mass of the washing solution used in a single wash to the total mass of the hydrogel. The single wash time of the ionic strength agitation washing is 10–30 min, and the washing temperature is 40–60 °C. Following the ionic strength agitation washing, a gradient washing step is included: first washing with an aqueous solution containing 5–20 vol% ethanol, then washing with pure water containing 0.005–0.05 wt% citric acid, and finally washing with pure water until neutral.
8. The preparation method according to claim 1, characterized in that, Between step (b) and step (c), a microwave treatment step is also included: the obtained hydrogel is broken into particles with a particle size of 2-8 mm and treated with microwave power of 300-500 W for 1-3 min.
9. The preparation method according to claim 1, characterized in that, The drying in step (d) is vacuum-nitrogen pulse drying, specifically including: placing the washed gel in a vacuum drying device and maintaining a vacuum for 10-20 minutes under an absolute pressure of 5-20 kPa and a temperature of 60-80°C; then purging with nitrogen for 2-5 minutes, restoring to normal pressure, and completing one pulse cycle; repeating the pulse cycle 3-6 times; the surface crosslinking treatment includes: spraying a surface crosslinking agent onto the pulverized and sieved resin, followed by heat treatment of the resin; the surface crosslinking agent includes one or more of polyols, cyclic carbonates, polyglycidyl ethers, and polyvalent metal salts.
10. A low-residue, low-extractable-content, highly safe, and highly absorbent resin prepared by the preparation method according to any one of claims 1 to 9, characterized in that, It includes a cross-linked polymer matrix formed by the polymerization of acrylic monomers, and a bifunctionalized mesoporous silicate uniformly dispersed in the cross-linked polymer matrix.
Citation Information
Patent Citations
Method for fast preparing for high water absorption resin
CN100554292C
Method for fast preparing high water absorption resin
CN101100493A