A photothermal stabilizing agent, its preparation method and application
By introducing polyacrylate copolymers with covalently bonded long-chain alkyl, benzotriazole, and epoxy groups into photovoltaic module encapsulation materials, the problems of light transmittance and interfacial adhesion of photovoltaic modules under high and low temperature cycling and ultraviolet irradiation are solved, thereby improving the long-term stability of the encapsulation materials and the power generation efficiency of the modules.
Patent Information
- Application Number
- CN202611414500.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing photovoltaic module encapsulation materials, under conditions of high and low temperature cycling and UV irradiation coupled aging, cannot simultaneously maintain transmittance, interfacial adhesion, and long-term stability, leading to decreased module transmittance, failure of encapsulation protection performance, and degradation of cell efficiency.
Polyacrylate copolymers are used as photothermal stabilizers. By covalently bonding long-chain alkyl, benzotriazole and epoxy groups on the molecular chain, the compatibility with the encapsulating resin is improved, the migration and precipitation of the additives are inhibited, and the interfacial adhesion and weather resistance are enhanced.
Under high and low temperature cycling and ultraviolet irradiation conditions, the film maintains light transmittance and interfacial adhesion reliability, thus extending the long-term power generation stability and outdoor service life of photovoltaic modules.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photovoltaic module encapsulation material modification technology, and particularly relates to a photothermal stabilizing agent, its preparation method and application. Background Technology
[0002] During the long-term service of outdoor photovoltaic (PV) modules, the coupled and synergistic aging effect of high and low temperature cycling and ultraviolet (UV) irradiation is the core degradation factor that distinguishes it from single damp heat aging, single UV aging, and single thermal aging. It is also a key pain point in the industry that restricts the medium- and long-term power generation efficiency of PV modules and causes significant power degradation in the later stages. In major PV application bases such as deserts and plateaus, the service environment is harsh, with diurnal temperature differences reaching 40°C to 60°C, and the modules undergo more than 3,000 high and low temperature cycles per year. The continuous alternating temperature stress will continuously induce micro-cracking, interface debonding, and molecular chain aging and breakage of the encapsulation material. At the same time, the photo-oxidative degradation effect of high-intensity UV irradiation exacerbates and synergistically damages the module, ultimately leading to a decrease in the light transmittance of the PV module, failure of the encapsulation protection performance, and degradation of the cell efficiency, significantly shortening the outdoor service life of the module.
[0003] Currently, crystalline silicon photovoltaic module encapsulation mainly uses EVA or EPE film systems, typically improving the film's outdoor service stability by adding weather-resistant modifiers. However, existing film modification technologies are mostly optimized for single properties such as heat resistance, UV resistance, or toughening, without being designed for high and low temperature cycling and UV-coupled aging conditions, making it difficult to meet the comprehensive weather resistance requirements of complex outdoor environments. Furthermore, conventional weather-resistant additives have poor compatibility with polyolefin and EVA resin matrices, easily migrating and precipitating during long-term service. This not only leads to a gradual decrease in film transmittance and interfacial adhesion but also significantly reduces the long-term weather resistance reliability of the module, failing to simultaneously achieve optical transmittance, interfacial adhesion stability, and resistance to coupled photothermal aging.
[0004] Therefore, how to improve the long-term stability of photovoltaic encapsulation films under photothermal coupling service conditions while taking into account both optical performance and interface reliability has become a technical problem that needs to be solved. Summary of the Invention
[0005] This invention provides a photothermal stabilizing agent, its preparation method, and its application. This photothermal stabilizing agent can be used in photovoltaic encapsulation films to improve compatibility and stability under photothermal coupling and temperature cycling conditions, reduce the risk of migration, agglomeration, and microcracks, and maintain the film's light transmittance, interfacial adhesion reliability, and long-term power generation stability of the module.
[0006] This invention provides a photothermal stabilizing agent comprising a polyacrylate copolymer, wherein the main molecular chain of the polyacrylate copolymer is covalently bonded with side chain groups, the side chain groups including long-chain alkyl groups, benzotriazole groups and epoxy groups; the long-chain alkyl groups have C12-C18 carbon atoms.
[0007] As described above, the photothermal stabilizing agent comprises at least one of 2-(2H-benzotriazole-2-yl)-4-methylphenyl and 2-(2H-benzotriazole-2-yl)-4,6-di-tert-butylphenyl; the epoxy group comprises at least one of glycidyl ether group and glycidyl ester group; and / or, the number average molecular weight of the polyacrylate copolymer is 1800~2200.
[0008] This invention also provides a method for preparing the above-mentioned photothermal stabilizing agent, comprising the following steps: a first material containing an initiator, an epoxy-containing acrylate monomer, and a first organic solvent is added dropwise to a second material containing a long-chain alkyl acrylate monomer and a benzotriazole acrylate monomer to carry out a polymerization reaction; after the polymerization reaction is completed, the solvent is removed, and the material is washed and dried to obtain the photothermal stabilizing agent.
[0009] The preparation method of the photothermal stabilizer described above, based on the total mass of the monomers participating in the polymerization reaction, has the following mass percentages: long-chain alkyl acrylate monomers: 35%-50%; benzotriazole acrylate monomers: 20%-30%; and epoxy-containing acrylate monomers: 15%-25%.
[0010] In the preparation method of the photothermal stabilizing agent as described above, the first material is added dropwise within 2 hours; after the dropwise addition is completed, the temperature is raised to 75~80℃ for a constant-temperature polymerization reaction for 4~5 hours; and / or, the epoxy-containing acrylate monomer includes glycidyl methacrylate and / or glycidyl acrylate ether; and / or, the first organic solvent includes butyl acetate; and / or, the long-chain alkyl acrylate monomer includes dodecyl methacrylate; and / or, the benzotriazole acrylate monomer is a copolyacrylate-modifying monomer containing a carbon-carbon double bond, including at least one of 2-(2H-benzotriazole-2-yl)-4-methylphenyl acrylate and 2-(2H-benzotriazole-2-yl)-4,6-di-tert-butylphenyl acrylate.
[0011] This invention also provides an EPE photovoltaic encapsulation film, comprising ethylene-vinyl acetate copolymer resin, polyolefin elastomer resin, and the above-mentioned photothermal stabilizing agent or photothermal stabilizing agent prepared by the above-mentioned preparation method.
[0012] The EPE photovoltaic encapsulating film as described above further includes one or more of the following: crosslinking agent, silane coupling agent, and antioxidant auxiliaries.
[0013] The EPE photovoltaic encapsulating film as described above comprises, by weight, the following components: 62-68 parts ethylene-vinyl acetate copolymer resin, 27-33 parts polyolefin elastomer resin, 1.2-2.5 parts photothermal stabilizer, 0.3-0.6 parts crosslinking agent, 0.1-0.3 parts silane coupling agent, and 0.2-0.4 parts antioxidant auxiliaries; and / or, the crosslinking agent comprises one or more of 2-ethylhexyl tert-butyl carbonate peroxide, dicumyl peroxide, and tert-butyl cumyl peroxide; and / or, the silane coupling agent comprises one or more of KH-550, KH-560, and KH-570; and / or, the antioxidant auxiliaries comprise one or more of antioxidant 1010, antioxidant 168, antioxidant 1076, and tris(2,4-di-tert-butylphenyl) phosphite.
[0014] This invention also provides a method for preparing the above-mentioned EPE photovoltaic encapsulating film, comprising the following steps: mixing a third material containing ethylene-vinyl acetate copolymer resin, polyolefin elastomer resin and photothermal stabilizer, and sequentially performing melt extrusion, casting molding and cooling winding to obtain the EPE photovoltaic encapsulating film.
[0015] In the preparation method of EPE photovoltaic encapsulating film as described above, the third material further includes one or more of crosslinking agent, silane coupling agent, and antioxidant auxiliary agent; and / or, the extrusion temperature of melt extrusion is 110~130℃, the melt extrusion is carried out using a screw extruder, and the screw speed of the screw extruder is 250~300r / min; and / or, the roll temperature of casting is 25~35℃.
[0016] This invention also provides a photovoltaic laminated module, including the above-described EPE photovoltaic encapsulating film or the EPE photovoltaic encapsulating film prepared by the above-described preparation method.
[0017] This invention also provides a photovoltaic module, including the photovoltaic laminated module described above.
[0018] This invention provides a photothermal stabilizing agent, its preparation method, and its application. By employing a photothermal stabilizing agent comprising polyacrylate copolymers, and covalently bonding long-chain alkyl, benzotriazole, and epoxy groups to the molecular chain of the polyacrylate copolymers, it is possible to achieve compatibility with the encapsulating resin, UV protection, and interfacial stability within the same agent molecule. This inhibits the migration and precipitation of the agent during long-term service, thereby improving the long-term stability of the photovoltaic encapsulation film under high and low temperature cycling and UV irradiation conditions, and is beneficial for maintaining light transmittance, adhesion, and encapsulation durability. Detailed Implementation
[0019] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0020] Existing photovoltaic encapsulation films mostly use EVA or EPE resin as the matrix, adding heat-resistant agents, UV absorbers, or inorganic fillers to improve weather resistance. The basic principle lies in using cross-linking to enhance high-temperature dimensional stability, or using UV absorption and shielding to slow polymer aging, or using fillers to improve deformation resistance. However, these modification paths are mostly single-function additives, and the compatibility between different additives and the resin matrix is limited. After long-term use, migration, precipitation, and aggregation easily occur, leading to increased film haze, decreased light transmittance, and weakened interfacial adhesion. When high and low temperature cycling and UV irradiation coexist, the resin chains repeatedly contract and extend, undergoing photo-oxidation. Microcracks and micropores easily form inside the film, making problems such as interlayer delamination and increased water vapor permeation more pronounced. These defects continue to affect the overall reliability of the module, leading to encapsulation failure around the cells, corrosion of metal electrodes, and power output degradation, making it difficult to meet the requirements of low degradation and high stability for long-term outdoor service.
[0021] Based on the aforementioned technical problems, traditional phenolic benzotriazole UV additives lack polymerization activity and can only be physically blended into the film matrix. Under long-term service conditions, they are prone to migration and precipitation, leading to a gradual loss of protective performance. Furthermore, multi-component additive formulations suffer from compatibility conflicts, making it difficult to simultaneously achieve toughening, UV resistance, and interfacial adhesion properties. Therefore, this invention abandons the phenolic benzotriazole small molecule without double bonds and selects a double-bond modified polyacrylate benzotriazole monomer. This monomer has carbon-carbon double bonds and can undergo one-step free radical copolymerization with long-chain alkyl acrylate monomers and epoxy-containing acrylate monomers, covalently attaching benzotriazole functional groups to the polyacrylate molecular backbone, achieving molecular-level bonding of functional groups, and completely solving the inherent defects of traditional small molecule additives.
[0022] In view of this, embodiments of the present invention provide a photothermal stabilizing agent comprising a polyacrylate copolymer, wherein the main molecular chain of the polyacrylate copolymer is covalently bonded with side chain groups, the side chain groups including long-chain alkyl groups, benzotriazole groups and epoxy groups; the long-chain alkyl groups have C12-C18 carbon atoms.
[0023] This invention integrates flexible long-chain side groups, benzotriazole UV-stabilizing structures, and epoxy reactive structures onto the same polyacrylate copolymer molecular chain, enabling the photothermal stabilizing agent to possess thermal stress buffering, UV aging resistance, and network anchoring capabilities. It can maintain a stable dispersion and interfacial bonding state under photothermal coupling and humid heat cycling conditions, ensuring the optical performance and reliability of the material. The specific analysis is as follows: 1) Long-chain alkyl flexible toughening groups can significantly improve the low-temperature elasticity of the film, inhibit the generation of micro-cracks under high and low temperature cycling, and improve the film's toughness over a wide temperature range; 2) Benzotriazole groups, as UV stabilizers, can achieve full-band UV absorption and efficiently capture polymeric free radicals generated by UV aging, fundamentally inhibiting film yellowing, degradation, and transmittance decay; 3) Epoxy groups can undergo covalent cross-linking reactions with active end groups (such as hydroxyl, carboxyl, and amino groups) generated by the thermal degradation of EVA resin under high-temperature lamination conditions, while improving interfacial compatibility with POE resin, anchoring the additive molecules in the resin matrix network, and alleviating problems of additive migration, precipitation, and failure. This photothermal stabilizer replaces the traditional multi-component compound additive system, integrating the triple functions of temperature-sensitive toughening, UV free radical capture, and high-temperature oxidation resistance through molecular structure design. Furthermore, the molecular end groups contain cross-linkable active groups that can covalently bond with the EPE resin matrix, effectively reducing the risk of precipitation and making it suitable for all-condition photovoltaic module encapsulation applications.
[0024] In this embodiment of the invention, if the carbon chain of the long-chain alkyl group in the photothermal stabilizer is too short, the flexible buffering effect will be insufficient; if the carbon chain is too long, it may increase the tendency of the copolymer to crystallize and affect the dispersion uniformity with the resin matrix. Long-chain alkyl groups with C12-C18 carbon atoms can play a dispersing role in local stress concentration areas without significantly sacrificing the light transmittance and processing fluidity of the material.
[0025] In some embodiments, polyacrylate copolymers can be prepared by polymerization to obtain copolymers with long-chain alkyl, benzotriazole, and epoxy groups covalently bonded to the molecular chain. These groups can also be introduced into the polyacrylate copolymer molecular chain through other methods capable of covalent bonding, as long as a stable intramolecular covalent bond structure is ultimately formed on the polyacrylate copolymer chain.
[0026] In this embodiment of the invention, the benzotriazole group includes at least one of 2-(2H-benzotriazole-2-yl)-4-methylphenyl and 2-(2H-benzotriazole-2-yl)-4,6-di-tert-butylphenyl. This allows for the adjustment of absorption bands, steric hindrance effects, and thermal stability through substituent differences, thereby suppressing UV-induced chain scission and photo-oxidation.
[0027] In this embodiment of the invention, the epoxy groups include at least one of glycidyl ether groups and glycidyl ester groups. During the lamination and heating process, they can undergo a ring-opening reaction with the active groups in the resin system, allowing the additives to be covalently fixed in the film network, preventing migration and precipitation.
[0028] In some embodiments, the number average molecular weight of the polyacrylate copolymer is 1800-2200. Limiting the number average molecular weight within this range allows the copolymer to have both appropriate chain length and good flowability and dispersibility, making it easier to spread evenly and maintain a stable distribution in the EVA or EPE encapsulation matrix. This avoids migration, precipitation, and additive loss caused by excessively low molecular weight, as well as decreased compatibility, difficulty in melt dispersion, and local agglomeration caused by excessively high molecular weight.
[0029] In this embodiment of the invention, the number-average molecular weight of the polyacrylate copolymer can be determined by conventional methods in the art, such as gel permeation chromatography.
[0030] This invention provides a method for preparing the above-mentioned photothermal stabilizing agent, comprising the following steps: a first material containing an initiator, an epoxy acrylate monomer, and a first organic solvent is added dropwise to a second material containing a long-chain alkyl acrylate monomer and a benzotriazole acrylate monomer to carry out a polymerization reaction; after the polymerization reaction is completed, the solvent is removed, and the material is washed and dried to obtain the photothermal stabilizing agent.
[0031] Specifically, the first material is pre-dissolved in a first organic solvent. The second material is placed in a reactor and heated to a temperature suitable for free radical polymerization under stirring. The first material is then added dropwise to the second material to carry out the polymerization reaction. During the dropwise addition, the concentration of active monomers in the system can be kept relatively stable by controlling the dropwise rate, thereby inhibiting localized overly rapid polymerization and component segregation. After the dropwise addition is completed, the reaction continues, allowing the initiator to continuously generate free radicals and promote the copolymerization of long-chain alkyl acrylate monomers, benzotriazole acrylate monomers, and epoxy acrylate monomers. After polymerization, the solvent is removed from the reaction system, and the system is washed with an appropriate solvent to remove unreacted monomers, oligomers, and residual initiator. Finally, the system is dried to obtain the target photothermal stabilizer.
[0032] In some embodiments, based on the total mass of monomers participating in the polymerization reaction, the mass percentage of long-chain alkyl acrylate monomers is 35%-50%, the mass percentage of benzotriazole acrylate monomers is 20%-30%, and the mass percentage of epoxy-containing acrylate monomers is 15%-25%. Because the proportions of the three types of functional groups are limited within a matching range, the three effects of flexibility, UV resistance, and reaction fixation are balanced and synergistic, allowing the film to maintain low haze and high light transmittance even under continuous exposure to light, heat, and humidity, thereby ensuring stable interfacial adhesion, improved lamination reliability, and delayed component power decay.
[0033] In this embodiment of the invention, the first material is added dropwise at a uniform rate within 2 hours; after the addition is completed, the temperature is raised to 75-80°C and a constant temperature polymerization reaction is carried out for 4-5 hours. The first material is added dropwise at a uniform rate within 2 hours, allowing the initiator and glycidyl methacrylate to gradually enter the reaction environment formed by the second material, thereby controlling the free radical generation rate and the instantaneous monomer concentration, reducing local overheating and component segregation; after the addition is completed, the system is heated to 75-80°C and maintained for 4-5 hours, which allows epoxy-containing acrylate monomers, long-chain alkyl acrylate monomers, and benzotriazole acrylate monomers to fully copolymerize, forming polyacrylate copolymers with long-chain alkyl, benzotriazole, and epoxy groups simultaneously introduced into the molecular chain.
[0034] In some embodiments, the epoxy-containing acrylate monomers include glycidyl methacrylate and / or glycidyl acrylate ether.
[0035] In some embodiments, the first organic solvent includes butyl acetate.
[0036] In some embodiments, long-chain alkyl acrylate monomers include dodecyl methacrylate.
[0037] In some embodiments, the benzotriazole acrylate monomers are copolyacrylate-modifying monomers containing carbon-carbon double bonds, including at least one of 2-(2H-benzotriazole-2-yl)-4-methylphenyl acrylate and 2-(2H-benzotriazole-2-yl)-4,6-di-tert-butylphenyl acrylate.
[0038] This invention also provides an EPE photovoltaic encapsulation film, comprising ethylene-vinyl acetate copolymer resin, polyolefin elastomer resin, and the above-mentioned photothermal stabilizing agent or photothermal stabilizing agent prepared by the above-mentioned preparation method.
[0039] In this embodiment of the invention, the EPE photovoltaic encapsulating film is a polymer film system suitable for the lamination and encapsulation of crystalline silicon photovoltaic modules. Ethylene-vinyl acetate copolymer resin and polyolefin elastomer resin together form a continuous matrix to balance melt flowability, wetting ability on glass and cell surfaces, and compatibility with lamination processes. The polyolefin elastomer resin supplements the low-temperature flexibility and resilience of the matrix. Considering the outdoor service conditions of the encapsulating film, which simultaneously withstands solar heating, nighttime cooling, high and low temperature cycling, and damp heat intrusion, the use of the above-mentioned resin components in the EPE system allows the matrix to possess both the processing and bonding properties provided by the ethylene-vinyl acetate copolymer resin and the low-temperature deformation resistance provided by the polyolefin elastomer resin. This provides a suitable polymer environment for the subsequent dispersion, grafting, or embedding of photothermal stabilizing agents into the network.
[0040] In this embodiment of the invention, the EPE photovoltaic encapsulating film further includes one or more of a crosslinking agent, a silane coupling agent, and an antioxidant auxiliary agent. This allows the film to form a more stable network structure and interface state during melt extrusion, lamination curing, and long-term outdoor service.
[0041] In some embodiments, the crosslinking agent includes peroxide-based crosslinking agents, such as one or more of 2-ethylhexyl tert-butyl carbonate peroxide, dicumyl peroxide, or tert-butyl cumyl peroxide, which decompose and release free radicals under heating conditions, thereby initiating crosslinking reactions between resin molecular chains and improving the thermal deformation stability, dimensional retention, and creep resistance of the film.
[0042] In some embodiments, the silane coupling agent includes one or more of KH-550, KH-560, and KH-570, or other silane coupling agents with amino, epoxy, vinyl, or methacryloxy functional groups. The silane end can form a chemical bond with the glass, the surface of the solar cell, or inorganic components, while the other end can couple or react with the resin matrix, thereby enhancing the interfacial adhesion strength between the encapsulated film and the encapsulated component and reducing the risk of delamination under thermal cycling and humid conditions.
[0043] In some embodiments, the antioxidant auxiliary agent preferably includes one or more of antioxidant 1010, antioxidant 168, antioxidant 1076, and tris(2,4-di-tert-butylphenyl) phosphite, and can be used in combination with a primary antioxidant and an auxiliary antioxidant. By capturing free radicals and decomposing peroxides, this process inhibits the thermo-oxidative aging chain reaction, thereby slowing down yellowing, embrittlement, and molecular chain breakage, and improving the long-term stability of the film under photothermal coupling and alternating high and low temperature conditions.
[0044] Through the synergistic effect of the crosslinking agent, silane coupling agent, antioxidant auxiliaries, and photothermal stabilizers described above, the film achieves more complete crosslinking curing and higher network integrity on the one hand, and enhances the interfacial bonding with glass, battery cells, and backsheet on the other hand, while simultaneously inhibiting thermo-oxidative degradation and auxiliaries migration, thereby significantly improving the light transmittance retention rate, interlayer bonding reliability, and outdoor service life.
[0045] In this embodiment of the invention, the EPE photovoltaic encapsulating film comprises the following components by weight: 62-68 parts ethylene-vinyl acetate copolymer resin, 27-33 parts polyolefin elastomer resin, 1.2-2.5 parts photothermal stabilizer, 0.3-0.6 parts crosslinking agent, 0.1-0.3 parts silane coupling agent, and 0.2-0.4 parts antioxidant. The ethylene-vinyl acetate copolymer resin and polyolefin elastomer resin are blended in a ratio of 62-68 parts and 27-33 parts, respectively. This blending ensures hot-melt processability while introducing sufficient flexibility and low-temperature impact resistance, allowing the film to adhere to the solar cell and glass surface after lamination, while also buffering stress caused by thermal expansion and contraction. A crosslinking agent, added at 0.3–0.6 parts, can form a suitable crosslinking density during melt extrusion or lamination curing, making the film less prone to flow and deformation at high temperatures and improving its heat shrinkage resistance. The use of 2-ethylhexyl tert-butyl carbonate peroxide and its complex allows for control of decomposition temperature and free radical release rate, ensuring the crosslinking process matches the processing window. A silane coupling agent, added at 0.1–0.3 parts, can build a more stable chemical bridge between the film and the glass, battery cell, and resin interfaces, enhancing interfacial adhesion and reducing the risk of delamination under humid and hot conditions. An antioxidant auxiliary agent, added at 0.2–0.4 parts, can synergistically scavenge free radicals and peroxides with the main antioxidant system, inhibiting thermo-oxidative degradation and thus maintaining the mechanical strength and optical stability of the film. Therefore, through the synergistic effects of matrix toughening, photothermal stabilization, moderate crosslinking, interfacial coupling, and antioxidant protection, this formulation enables the encapsulant film to maintain low haze, high light transmittance, and more stable interfacial bonding reliability under photothermal coupling and high and low temperature cycling conditions, thereby improving the long-term service life of crystalline silicon photovoltaic modules.
[0046] This invention also provides a method for preparing the above-mentioned EPE photovoltaic encapsulating film, comprising the following steps: mixing a third material containing ethylene-vinyl acetate copolymer resin, polyolefin elastomer resin, and photothermal stabilizer, and sequentially performing melt extrusion, casting molding, and cooling and winding to obtain the EPE photovoltaic encapsulating film. During melt extrusion, the material can be gradually plasticized by segmented heating to avoid resin thermal degradation and promote uniform dispersion of each component; during casting molding, the film can be spread after extrusion through a die to ensure the continuity of the film and its compatibility with subsequent lamination; during cooling and winding, the molded film is cooled and wound to obtain an EPE photovoltaic encapsulating film with uniform thickness and a smooth surface.
[0047] In some embodiments, the third material also includes one or more of a crosslinking agent, a silane coupling agent, and an antioxidant auxiliary agent.
[0048] In some embodiments, the crosslinking agent may be an organic peroxide or other thermal crosslinking system, the silane coupling agent may be a coupling component containing an alkoxysilane structure, and the antioxidant auxiliary agent may be a hindered phenol or phosphite-assisted antioxidant system. The above components are used in combination with ethylene-vinyl acetate copolymer resin, polyolefin elastomer resin and photothermal stabilizing agent to form a more stable blend network structure.
[0049] In some embodiments, the extrusion temperature of melt extrusion is 110~130°C, which is beneficial for the ethylene-vinyl acetate copolymer resin and polyolefin elastomer resin to be fully melted and coated with photothermal stabilizing additives; melt extrusion is carried out using a screw extruder with a screw speed of 250~300 r / min.
[0050] In some implementations, the roller temperature for casting is 25~35°C.
[0051] This invention also provides a photovoltaic laminated module, comprising the EPE photovoltaic encapsulating film described above or the EPE photovoltaic encapsulating film prepared by the above method. This photovoltaic laminated module has advantages corresponding to the aforementioned EPE photovoltaic encapsulating film, which will not be elaborated upon here.
[0052] This invention also provides a photovoltaic module, including the aforementioned photovoltaic laminated module. This photovoltaic module uses an EPE photovoltaic encapsulating film to laminate and encapsulate the solar cells, glass, and backsheet. The polyacrylate additive carrier in the film simultaneously introduces long-chain alkyl, benzotriazole, and epoxy groups onto its molecular chain, concentrating flexible buffering, UV stability, and interfacial reaction bonding capabilities within the same molecular system. This reduces migration, precipitation, and aggregation caused by insufficient compatibility of multi-component additives. Because the film maintains high light transmittance, low haze, and stable adhesion under conditions of light exposure, heat, alternating hot and cold temperatures, and moisture intrusion, it is less prone to microcracks, micropores, and delamination between layers, thereby inhibiting water vapor penetration and metal electrode corrosion. Therefore, it is beneficial for maintaining the encapsulation reliability, power generation efficiency, and low power degradation performance of the module during long-term outdoor operation.
[0053] Preparation Example 1
[0054] This preparation example provides a photothermal stabilizing agent, wherein the raw materials are in the following proportions by weight: 40 parts of dodecyl methacrylate, 25 parts of 2-(2H-benzotriazol-2-yl)-4-methylphenyl acrylate, 20 parts of glycidyl methacrylate, 1.20 parts of azobisisobutyronitrile, and 90 parts of butyl acetate.
[0055] The preparation method of the photothermal stabilizing agent includes the following steps: 2-(2H-benzotriazol-2-yl)-4-methylphenyl acrylate and dodecyl methacrylate in the above proportions are added to a reaction vessel, heated to 68℃ and stirred until fully dissolved, and kept at this temperature for 30 min; azobisisobutyronitrile and glycidyl methacrylate are dissolved in butyl acetate to prepare a mixed solution, which is added dropwise to the reaction vessel at a uniform rate over 2 h; after the addition is completed, the temperature is raised to 78℃ and polymerized at a constant temperature for 4.5 h; after the polymerization reaction is completed, the butyl acetate solvent is completely removed by vacuum distillation, and the product is purified by washing with anhydrous ethanol multiple times, vacuum dried, and then ground to obtain a powdered photothermal stabilizing agent. The number average molecular weight of the photothermal stabilizing agent is measured to be 2030.
[0056] Preparation Example 2
[0057] Compared to Preparation Example 1, the difference lies in the following: by mass, the raw materials are: 48 parts of dodecyl methacrylate, 22 parts of 2-(2H-benzotriazol-2-yl)-4-methylphenyl acrylate, 18 parts of glycidyl methacrylate, 1.10 parts of azobisisobutyronitrile, and 95 parts of butyl acetate.
[0058] The preparation method of the photothermal stabilizing agent includes the following steps: 2-(2H-benzotriazol-2-yl)-4-methylphenyl acrylate and dodecyl methacrylate in the above proportions are added to a reaction vessel, heated to 68℃ and stirred until fully dissolved, and kept at this temperature for 30 min; azobisisobutyronitrile and glycidyl methacrylate are dissolved in butyl acetate to prepare a mixed solution, and added dropwise to the reaction vessel at a uniform rate over 2 h; after the dropwise addition is completed, the temperature is raised to 78℃ and polymerized at a constant temperature for 4.5 h; after the polymerization reaction is completed, the butyl acetate solvent is completely removed by vacuum distillation, and the product is purified by washing with anhydrous ethanol multiple times, vacuum dried, and then ground to obtain a powdered photothermal stabilizing agent. The number average molecular weight of the photothermal stabilizing agent is measured to be 1960.
[0059] Preparation Example 3
[0060] Compared to Preparation Example 1, the difference lies in the following: by mass, the raw materials are: 42 parts of dodecyl methacrylate, 29 parts of 2-(2H-benzotriazol-2-yl)-4-methylphenyl acrylate, 19 parts of glycidyl methacrylate, 1.30 parts of azobisisobutyronitrile, and 100 parts of butyl acetate.
[0061] The preparation method of the photothermal stabilizing agent includes the following steps: 2-(2H-benzotriazol-2-yl)-4-methylphenyl acrylate and dodecyl methacrylate in the above proportions are added to a reaction vessel, heated to 70℃ and stirred until fully dissolved, and kept at this temperature for 30 min; azobisisobutyronitrile and glycidyl methacrylate are dissolved in butyl acetate to prepare a mixed solution, and added dropwise to the reaction vessel at a uniform rate for 2 h; after the dropwise addition is completed, the temperature is raised to 80℃ and polymerized at a constant temperature for 5 h; after the polymerization reaction is completed, the butyl acetate solvent is completely removed by vacuum distillation, and the product is purified by washing with anhydrous ethanol multiple times, vacuum dried and ground to obtain a powdered photothermal stabilizing agent. The number average molecular weight of the photothermal stabilizing agent is measured to be 2080.
[0062] Preparation Example 4
[0063] Compared to Preparation Example 1, the raw materials, by mass, are: 36 parts of dodecyl methacrylate, 23 parts of 2-(2H-benzotriazol-2-yl)-4-methylphenyl acrylate, 24 parts of glycidyl methacrylate, 1.25 parts of azobisisobutyronitrile, and 88 parts of butyl acetate.
[0064] The preparation method of the photothermal stabilizing agent includes the following steps: 2-(2H-benzotriazol-2-yl)-4-methylphenyl acrylate and dodecyl methacrylate in the above proportions are added to a reaction vessel, heated to 68℃ and stirred until fully dissolved, and kept at this temperature for 30 min; azobisisobutyronitrile and glycidyl methacrylate are dissolved in butyl acetate to prepare a mixed solution, and added dropwise to the reaction vessel at a uniform rate over 2 h; after the dropwise addition is completed, the temperature is raised to 78℃ and polymerized at a constant temperature for 4.5 h; after the polymerization reaction is completed, the butyl acetate solvent is completely removed by vacuum distillation, and the product is purified by washing with anhydrous ethanol multiple times, vacuum dried, and then ground to obtain a powdered photothermal stabilizing agent. The number average molecular weight of the photothermal stabilizing agent is measured to be 2140.
[0065] Preparation Example 5
[0066] Compared to Preparation Example 1, the difference lies in the following: by mass, the raw materials are: 35 parts of dodecyl methacrylate, 20 parts of 2-(2H-benzotriazol-2-yl)-4-methylphenyl acrylate, 15 parts of glycidyl methacrylate, 1.20 parts of azobisisobutyronitrile, and 82 parts of butyl acetate.
[0067] The preparation method of the photothermal stabilizing agent includes the following steps: 2-(2H-benzotriazol-2-yl)-4-methylphenyl acrylate and dodecyl methacrylate in the above proportions are added to a reaction vessel, heated to 70℃ and stirred until fully dissolved, and kept at this temperature for 30 min; azobisisobutyronitrile and glycidyl methacrylate are dissolved in butyl acetate to prepare a mixed solution, and added dropwise to the reaction vessel at a uniform rate for 2 h; after the dropwise addition is completed, the temperature is raised to 80℃ and polymerized at a constant temperature for 5 h; after the polymerization reaction is completed, the butyl acetate solvent is completely removed by vacuum distillation, and the product is purified by washing with anhydrous ethanol multiple times, vacuum dried and ground to obtain a powdered photothermal stabilizing agent. The number average molecular weight of the photothermal stabilizing agent is measured to be 2100.
[0068] Comparative Preparation Example 1
[0069] The difference from Preparation Example 1 is that 2-(2H-benzotriazol-2-yl)-4-methylphenylacrylate was not added, while the remaining steps and conditions were basically the same as in Preparation Example 1.
[0070] Comparative Preparation Example 2
[0071] The difference from Preparation Example 1 is that no dodecyl methacrylate was added, while the remaining steps and conditions are basically the same as those in Preparation Example 1.
[0072] Examples 1-5 and Comparative Examples 1-2
[0073] This embodiment provides an EPE photovoltaic encapsulation film, the components of which, by weight, are: 65 parts of EVA resin (VA content 28%), 30 parts of POE polyolefin resin, 1.8 parts of photothermal stabilizing agent prepared in Preparation Examples 1-5 and Comparative Preparation Examples 1-2, 0.45 parts of crosslinking agent (2-ethylhexyl tert-butyl carbonate peroxide), 0.2 parts of silane coupling agent, and 0.3 parts of antioxidant auxiliary agent.
[0074] The preparation process is as follows:
[0075] 1) Premixing treatment: EVA resin and POE resin are put into a high-speed mixer and stirred at room temperature for 10 minutes at a stirring speed of 800 r / min to ensure that the resin matrix is fully and uniformly mixed; then photothermal stabilizer and antioxidant are added and stirred for another 6 minutes to ensure that the additives are evenly dispersed and that there are no obvious agglomerated particles in the system.
[0076] 2) Melt extrusion: The premixed material is fed into a co-rotating twin-screw extruder. The extrusion temperature is 120℃ and the screw speed is 275r / min to ensure that the material is fully melted and plasticized, and to control the shear heat to avoid local overheating and degradation of the resin.
[0077] 3) Uniform dispersion modification of additives: During the extrusion process, crosslinking agent and silane coupling agent are added simultaneously through the side feed port. Under the shearing action of the screw, the crosslinking agent, silane coupling agent, resin matrix, and photothermal stabilizing additives are fully mixed and dispersed. The epoxy groups carried by the additives retain their reactivity and can form covalent bonds with the resin matrix.
[0078] 4) Casting, cooling and winding: Casting is used for forming, the temperature of the cooling roller is controlled at 30℃, and the material is wound up after cooling and shaping to obtain an EPE photovoltaic encapsulation film with a thickness of 0.5mm. The obtained EPE photovoltaic encapsulation film can be directly used for photovoltaic module lamination and encapsulation.
[0079] Comparative Example 3
[0080] Commercially available conventional EPE film (without modified additives) was used as the EPE photovoltaic encapsulation film.
[0081] Comparative Example 4
[0082] EPE encapsulant film with single UV resistance modification by adding small molecule benzotriazole UV absorber was used as EPE photovoltaic encapsulant film.
[0083] Comparative Example 5
[0084] An EPE encapsulant film with single temperature-dependent modification by adding long-chain alkyl acrylate toughening agent was used as an EPE photovoltaic encapsulant film.
[0085] The following performance tests were performed on the EPE photovoltaic encapsulation films in the above embodiments and comparative examples:
[0086] 1) Test method for maximum power degradation rate after aging: The encapsulant film, solar cells, glass and backsheet are encapsulated to prepare a simulated photovoltaic module. The UV pretreatment test and 200 high and low temperature cycle test are carried out in sequence according to IEC61215:2021 standard to complete the light-heat coupling accelerated aging. After aging, the maximum power of the module is tested using a solar simulator. The maximum power of the module before and after aging is compared and the maximum power of the module before and after aging is calculated according to the formula.
[0087] Calculation formula: Maximum power attenuation rate (%) = ((Maximum power before aging - Maximum power after aging) / Maximum power before aging) × 100%. The smaller the value, the better the component's anti-coupling aging performance.
[0088] 2) Film transmittance retention rate
[0089] Test method: Take a 0.5 mm thick film sample and use a UV-Vis spectrophotometer to test the average transmittance of the film in the 400-800 nm visible light band before and after aging.
[0090] Calculation formula: Light transmittance retention rate (%) = (Average visible light transmittance after aging / Average visible light transmittance before aging) × 100%. The higher the value, the better the film's resistance to photoaging and yellowing.
[0091] 3) Interfacial adhesion retention rate
[0092] Test method: Prepare glass-adhesive film-backsheet laminated samples, and test the 180° peel strength between the adhesive film and glass using a universal tensile testing machine in accordance with GB / T2791 standard; test the peel strength before aging and after coupling aging respectively.
[0093] Calculation formula: Interfacial adhesion retention rate (%) = (Peel strength after aging / Peel strength before aging) × 100%. The higher the value, the less likely the interface is to debond under high and low temperature cycling, and the better the encapsulation reliability.
[0094] 4) Film haze increase rate
[0095] Test method: The haze value of the film before and after aging was tested using a haze meter according to the GB / T2410 standard.
[0096] Calculation formula: Haze increase rate (%) = ((Haze after aging - Haze before aging) / Haze before aging) × 100%. The smaller the value, the less likely the film is to develop microcracks, whitening, or fogging after aging, and the better its optical performance is maintained.
[0097] Table 1
[0098]
[0099] As shown in Table 1, compared with Comparative Examples 1-5, the EPE photovoltaic encapsulating films prepared in Examples 1-5 have better resistance to photothermal aging, high and low temperature cycling stability, light transmittance retention and interfacial adhesion reliability. At the same time, they can effectively inhibit the migration and aggregation of additives, reduce the risk of microcracks in the film, and their overall performance is more suitable for the long-term service requirements of photovoltaic modules.
[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A photothermal stabilizing aid, characterized in that, The invention includes polyacrylate copolymers, wherein the main molecular chain of the polyacrylate copolymer is covalently bonded with side chain groups, the side chain groups including long-chain alkyl groups, benzotriazole groups and epoxy groups; the long-chain alkyl groups have C12-C18 carbon atoms.
2. The photothermal stabilizing aid according to claim 1, characterized in that The benzotriazole group includes at least one of 2-(2H-benzotriazole-2-yl)-4-methylphenyl and 2-(2H-benzotriazole-2-yl)-4,6-di-tert-butylphenyl; And / or, the epoxy group includes at least one of glycidyl ether group and glycidyl ester group; And / or, the number average molecular weight of the polyacrylate copolymer is 1800~2200.
3. A process for the preparation of the photothermal stabilisation aid according to claim 1 or 2, characterised in that Includes the following steps: A first material containing an initiator, an epoxy-containing acrylate monomer, and a first organic solvent is added dropwise to a second material containing a long-chain alkyl acrylate monomer and a benzotriazole acrylate monomer to carry out a polymerization reaction. After the polymerization reaction is completed, the solvent is removed, and the mixture is washed and dried to obtain the photothermal stabilizer.
4. The method of preparing a photothermal stabilisation aid according to claim 3, characterised in that, Based on the total mass of monomers participating in the polymerization reaction, the mass percentage of long-chain alkyl acrylate monomers is 35%-50%, the mass percentage of benzotriazole acrylate monomers is 20%-30%, and the mass percentage of epoxy-containing acrylate monomers is 15%-25%.
5. The method of preparing a photothermal stabilisation aid according to claim 4, characterised in that, The first material is added dropwise within 2 hours; after the addition is complete, the temperature is raised to 75~80℃ for constant temperature polymerization reaction for 4~5 hours. And / or, the epoxy-containing acrylate monomers include glycidyl methacrylate and / or glycidyl acrylate ether; And / or, the first organic solvent includes butyl acetate; And / or, the long-chain alkyl acrylate monomer includes dodecyl methacrylate; And / or, the benzotriazole acrylate monomer is a copolyacrylate-modifying monomer containing a carbon-carbon double bond, including at least one of 2-(2H-benzotriazole-2-yl)-4-methylphenyl acrylate and 2-(2H-benzotriazole-2-yl)-4,6-di-tert-butylphenyl acrylate.
6. An EPE photovoltaic encapsulant film, characterized by, It includes ethylene-vinyl acetate copolymer resin, polyolefin elastomer resin, and the photothermal stabilizing agent as described in claim 1 or 2, or the photothermal stabilizing agent prepared by any one of claims 3-5.
7. The EPE photovoltaic encapsulant film of claim 6, wherein, The EPE photovoltaic encapsulation film also includes one or more of the following: crosslinking agent, silane coupling agent, and antioxidant auxiliaries.
8. The EPE photovoltaic encapsulant film of claim 7, wherein, The EPE photovoltaic encapsulating film comprises the following components by weight: 62-68 parts ethylene-vinyl acetate copolymer resin, 27-33 parts polyolefin elastomer resin, 1.2-2.5 parts photothermal stabilizer, 0.3-0.6 parts crosslinking agent, 0.1-0.3 parts silane coupling agent, and 0.2-0.4 parts antioxidant auxiliaries. And / or, the crosslinking agent includes one or more of 2-ethylhexyl tert-butyl carbonate peroxide, dicumyl peroxide, and tert-butyl cumyl peroxide; And / or, the silane coupling agent includes one or more of KH-550, KH-560, and KH-570; And / or, the antioxidant adjuvant includes one or more of antioxidant 1010, antioxidant 168, antioxidant 1076, and tris(2,4-di-tert-butylphenyl) phosphite.
9. A method of producing the EPE photovoltaic encapsulant film according to any one of claims 6 to 8, characterized by, Includes the following steps: A third material containing ethylene-vinyl acetate copolymer resin, polyolefin elastomer resin and photothermal stabilizer is mixed and then sequentially melt-extruded, cast, cooled and wound to obtain the EPE photovoltaic encapsulation film.
10. The method for preparing the EPE photovoltaic encapsulating film according to claim 9, characterized in that, The third material also includes one or more of the following: crosslinking agent, silane coupling agent, and antioxidant auxiliary agent; And / or, the extrusion temperature of the melt extrusion is 110~130℃, and the melt extrusion is carried out using a screw extruder with a screw speed of 250~300 r / min; And / or, the roller temperature for casting is 25~35℃.
11. A photovoltaic laminate assembly, characterized by Includes the EPE photovoltaic encapsulating film according to any one of claims 6-8 or the EPE photovoltaic encapsulating film prepared by the preparation method according to claim 9 or 10.
12. A photovoltaic module, characterized by, Including the photovoltaic laminated module as described in claim 11.