A glass precursor material with self-healing properties and its application

By using self-healing glass precursor materials and supporting processes, the problem of balancing high silica doping levels with functional properties in existing technologies has been solved, enabling the fabrication of large-size, irregularly shaped structures, improving the optical and mechanical properties of glass devices, and expanding their application scenarios.

CN123106980APending Publication Date: 2026-11-17UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611268397.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing glass additive manufacturing technologies cannot simultaneously achieve high silica doping levels and functional properties. Equipment forming width and process limitations prevent the fabrication of large-size, irregularly shaped, and partitioned functional structures. Glass splicing technology suffers from low interfacial bonding strength and poor optical consistency. Debinding and sintering processes have poor adaptability, leading to defects in highly silica-filled precursors during sintering.

Method used

By employing a glass precursor material with self-healing properties, including reactive monomers, crosslinking agents, dynamic crosslinking solvents, photoinitiators, and sintering aids, and through a multi-step mixing method and a stepwise debinding-two-step sintering process, a balance between high silica doping and stable self-healing is achieved, thus solving the defects in seamless splicing at room temperature and high-temperature sintering.

Benefits of technology

It achieves a balance between high silica doping and self-healing properties, overcomes molding limitations, improves process stability and product yield, and produces glass devices with excellent optical and mechanical properties, as well as zoned light emission and self-bending capabilities, making them suitable for optical devices, consumer electronics and aerospace fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention belongs to the field of special glass materials and advanced additive manufacturing technology, specifically relating to a glass precursor material with self-healing properties and its applications. Addressing the core deficiencies of existing glass additive manufacturing technologies and precursor materials, the core objective of this invention is to provide a glass precursor material that combines high silica doping content with room-temperature self-healing properties. Simultaneously, it establishes a complete glass preparation method based on the self-healing splicing of this precursor, solving the industry pain point that existing technologies cannot simultaneously achieve high filler content, self-healing, sinterability, and high performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of special glass materials and advanced additive manufacturing technology, specifically relating to a glass precursor material with self-healing properties and its application. Background Technology

[0002] Glass, as an indispensable basic functional material, boasts excellent optical transparency, chemical stability, thermal stability, and mechanical properties, making it irreplaceable in key fields such as architecture, optics, electronics, and aerospace. In recent years, the rapid development of additive manufacturing technology has brought revolutionary breakthroughs to glass manufacturing. Based on layer-by-layer deposition, glass additive manufacturing technology possesses core advantages of high efficiency, flexibility, and customizability, providing a new path for the fabrication of complex geometric structures and high-precision glass devices. Currently, mainstream glass additive manufacturing technologies are mainly divided into two categories: direct melt molding and indirect photopolymerization. Direct melt molding technology requires high-temperature melting of silica (>1600℃) through a high-energy heat source, demanding sophisticated equipment and high energy consumption. Furthermore, its molding precision can only reach the millimeter level, making it unsuitable for fabricating high-precision micro / nano glass devices. Indirect photopolymerization technology first prepares a silica / organic composite glass precursor green body through photopolymerization, then obtains transparent glass through debinding and sintering. It offers high molding precision and a gentler process, making it the mainstream technology route for high-precision glass manufacturing. However, existing indirect photopolymerization glass additive manufacturing technologies still face four major insurmountable industry bottlenecks: First, existing glass precursor materials cannot simultaneously achieve high silica doping levels and functional properties. Silica doping levels directly determine the shrinkage rate and structural integrity of the glass after sintering. High doping levels can significantly reduce sintering shrinkage and cracking defects. However, in existing precursor systems, high silica filling significantly degrades the formability and functionality of the material, making it impossible to achieve additional performance enhancements. Second, existing additive manufacturing technologies are limited by the forming area of ​​equipment (micrometer level) and processes, making it impossible to efficiently prepare large-size, irregularly shaped, and functionally partitioned complex glass structures. The overall forming is difficult and the scrap rate is high, which cannot meet the needs of personalized and customized glass device preparation. Third, existing glass splicing / assembly technologies (such as organic bonding, high-temperature hot welding, etc.) have fatal flaws: organic bonding interfaces cannot withstand the subsequent high-temperature debinding and sintering process, and are prone to debonding, cracking, and carbonization contamination; high-temperature hot welding is prone to glass structure deformation and optical performance degradation, and cannot achieve precise splicing of heterogeneous precursors, with low interface bonding strength and poor optical consistency. Fourth, existing debinding and sintering processes for high-filled silica precursors have poor adaptability. During the debinding process, precursors with high organic content are prone to defects such as uneven shrinkage, deformation, cracking, and delamination due to the rapid decomposition of organic matter. Moreover, these defects only appear after sintering and cannot be repaired. Traditional one-step sintering processes are prone to crystallization, high porosity, and insufficient density, making it impossible to simultaneously achieve high transparency, high density, and no crystallization in glass. Furthermore, it cannot guarantee the structural integrity and performance consistency of the splicing interface after high-temperature treatment.

[0003] Self-healing materials, as an important branch of smart materials, possess the unique properties of autonomously repairing damage at room temperature and achieving seamless interface bonding. They have already been applied in flexible electronics, coatings, and composite materials. However, a mature technical solution for introducing self-healing systems into glass additive manufacturing is still lacking, and achieving a balance between "high silica doping content + stable self-healing ability + suitable debinding and sintering process + high-performance interface retention after sintering" remains elusive. Therefore, developing a glass precursor material with both high silica content and excellent self-healing properties, and establishing a corresponding debinding and sintering process, are core technical challenges that urgently need to be addressed in the current glass additive manufacturing field. Summary of the Invention

[0004] To address the aforementioned problems, this invention provides a glass precursor with self-healing properties, comprising the following components: a reactive monomer, a crosslinking agent, a dynamic crosslinking solvent, a photoinitiator, a sintering aid, and an inorganic filler; wherein the reactive monomer is hydroxyethyl methacrylate (HEMA), the crosslinking agent is acrylic acid (AAc), the dynamic crosslinking solvent is polyethylene glycol 400 (PEG400), the photoinitiator is phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide 819, the sintering aid is phenoxyethanol (POE), and the inorganic filler is silica nanoparticles.

[0005] The present invention also provides a method for preparing the above-mentioned glass precursor with self-healing properties, comprising the following steps: 1) Take a brown, light-proof container and add 6 mL of HEMA monomer; 2) Add silica nanoparticle powder to HEMA in batches, 1 gram each time. After each addition, mix thoroughly with a shaker to ensure that the silica powder is well dispersed in the solution. Continue this process until the fifth addition, when the powder shows obvious agglomeration. 3) Add 1 mL of POE sintering aid to the solution and shake it thoroughly with a shaker. The agglomeration phenomenon was found to have disappeared. Then add 1 g of silica and shake to verify the dispersion stability. 4) Alternately add 1 mL of acrylic acid and 1 g of silica to the solution, shaking thoroughly with a shaker each time, until 6 mL of acrylic acid is added. While ensuring that no agglomeration occurs, a total of 12 g of silica powder is added. The solution is then sonicated to obtain a clear and transparent solution. 5) Add 8 mL of PEG400 in two portions, 4 mL each time, and mix thoroughly with a shaker after each addition; 6) Add 0.21g of photoinitiator 819, stir and mix thoroughly with an oscillator, and finally sonicate to obtain a transparent glass precursor solution.

[0006] This shipment also provides the application of the aforementioned glass precursor in the preparation of zoned controllable light-emitting functional glass.

[0007] This shipment also provides the application of the aforementioned glass precursor in the preparation of moldless, self-bending irregularly shaped glass.

[0008] The present invention has the following beneficial effects: 1) Breakthrough in material performance: For the first time in the field of glass additive manufacturing, it achieves a balance between high silica doping of over 30% and stable room temperature self-healing, solving a core pain point in the industry and providing a brand-new approach for the development of functional glass precursors.

[0009] 2) Significantly improved process flexibility: The room temperature adhesive-free splicing process can produce large-size, complex three-dimensional glass structures at low cost without the need for large additive manufacturing equipment, breaking through the forming limitations of existing technologies.

[0010] 3) Significantly improved process stability and yield: The supporting step-by-step debinding-two-step sintering process completely solves the problems of deformation, cracking and crystallization in the debinding and sintering process of high-filled precursors, and the product yield is greatly improved.

[0011] 4) Excellent product performance: The optical and mechanical properties of the prepared quartz glass are consistent with those of commercial products, the splicing interface is integrated, and there are no optical or mechanical defects.

[0012] 5) Wide range of applications: It can realize the preparation of customized functional glass such as zoned light emission and self-bending, and has excellent industrialization prospects in the fields of optical devices, consumer electronics, aerospace and other fields. Attached Figure Description

[0013] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0014] Figure 1. Schematic diagram of the multi-step mixing process for preparing self-healing glass precursors; Figure 2. Comparison of the formability and performance of precursors with different ratios; Figure 3. Schematic diagram of the glass precursor splicing and assembly process based on self-healing properties; Figure 4. TG-DTA thermal analysis curves of the precursor material; Figure 5. Temperature rise curve of the step-by-step degreasing process; Figure 6. Temperature rise curve of the two-step vacuum sintering process; Figure 7. Physical image showing the evolution of the sample's appearance throughout the entire degreasing and sintering process; Figure 8. SEM microstructure of the degreased green body; Figure 9. Comparison of shrinkage rate of samples before and after sintering and SEM morphology of glass cross section; Figure 10. Ultraviolet-visible-near-infrared transmittance spectrum of sintered quartz glass; Figure 11. Comparison of partitioned light-emitting glass under natural light and ultraviolet light irradiation; a. Directly doped with rare earth ions; b. Physical image of three-color spliced ​​glass under natural light. c. Actual image of tri-color spliced ​​glass under ultraviolet light Figure 12 Schematic diagram of the directional bending mechanism of self-bending glass; Figure 13 Comparison of the actual objects before and after the self-bending glass was sintered. Detailed Implementation

[0015] Various exemplary embodiments of the present invention are now described in detail. Unless otherwise specified, the methods used in the embodiments are conventional methods, and the reagents used are commercially available reagents or reagents prepared using conventional methods. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, characteristics, and embodiments of the present invention.

[0016] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0017] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0018] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be readily apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0019] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0020] Example 1: I. Glass precursor materials with self-healing properties and their preparation method The glass precursor material of this invention is based on a UV curing system with dynamic cross-linking of multivalent hydrogen bonds. It can achieve uniform dispersion of high silica content and room temperature self-healing function, and is also compatible with subsequent high-temperature debinding and sintering processes.

[0021] 1. Composition of the material system The core components and functions of this precursor material are as follows: 1) Reactive monomer: Hydroxyethyl methacrylate (HEMA), which combines the excellent dispersibility of silica nanoparticles with photopolymerization reactivity. The vinyl functional groups in its molecule can undergo free radical polymerization under ultraviolet light, and at the same time can form a stable solvent layer on the surface of silica nanoparticles to prevent nanoparticle aggregation. 2) Crosslinking agent: Acrylic acid (AAc), which can copolymerize with HEMA to form a P (HEMA-co-AAc) copolymer matrix, providing hydrogen bonding sites for the system; 3) Dynamic crosslinking solvent: Polyethylene glycol 400 (PEG400) molecules can form multivalent hydrogen bonds with P (HEMA-co-AAc) copolymer molecules. It serves as both a solvent and a dynamic crosslinking agent in the system. At room temperature, it achieves rapid self-healing of materials through the reversible breaking and reconstruction of hydrogen bonds. 4) Photoinitiator: Phenylene bis(2,4,6-trimethylbenzoyl)phosphine oxide (819), a high-efficiency photoinitiator for UV curing systems, which can efficiently initiate the free radical copolymerization reaction of HEMA and AAc; 5) Sintering aid: Phenoxyethanol (POE) can improve the dispersibility of silica nanoparticles and promote the densification and fusion of nanoparticles during subsequent sintering, thereby reducing sintering defects. 6) Inorganic filler: Silica nanoparticles provide the glass phase matrix for subsequent sintering, enabling the preparation of glass with low defects and high density.

[0022] 2. Optimal proportioning optimization of the material system 1) Optimization of the basic self-healing system formulation: With a fixed HEMA to AAc volume ratio of 1:1, both were cured under 365nm UV light for 30 min to form a P(HEMA-co-AAc) copolymer matrix. Five gradient formulations were set with P(HEMA-co-AAc) to PEG400 volume ratios of 2:1, 3:2, 1:1, 2:3, and 1:2. Moldability verification, tensile performance testing (tensile rate 10 mm / min), and self-healing efficiency calculation after 2 h of room temperature healing were performed. The comparison of moldability and performance of different formulations is shown in Figure 2. The results show that the 2:3, 1:2, and 1:1 formulations could not form a stable solid molded body; only the 2:1 and 3:2 formulations could be completely cured. Among them, the 3:2 formulation achieved a self-healing efficiency of 60% (better than the 55.2% of the 2:1 formulation) and also possessed superior flexibility, thus being determined as the optimal basic formulation for the system.

[0023] 2) Optimization of high silica doping process:  Based on the optimal basic ratio of 3:2, the doping upper limit of single-step mixing method and multi-step alternating mixing method was compared. The results showed that the single-step mixing method could only achieve a maximum of 8g of silica uniform doping, while the multi-step alternating mixing method could achieve 12g of silica uniform doping, which increased the doping amount by 50%, and the system had no obvious agglomeration. Even with a doping amount of 30%, it still retained 12.8% of the self-healing ability.

[0024] 3. Core process for precursor preparation (multi-step alternating mixing method) In order to maximize the amount of silicon dioxide doping while ensuring the material has healing properties and reducing subsequent sintering shrinkage and defects, this invention adopts a multi-step alternating mixing method. The specific material preparation process is shown in Figure 1.

[0025] 1) Take a brown, light-proof container and add 6 mL of HEMA monomer; 2) Add silica nanoparticle powder to HEMA in batches, 1 gram each time. After each addition, mix thoroughly with a shaker to ensure that the silica powder is well dispersed in the solution. Continue this process until the fifth addition, when the powder shows obvious agglomeration. 3) Add 1 mL of POE sintering aid to the solution, shake thoroughly with a shaker to mix, and find that the agglomeration phenomenon disappears. Then add 1 g of silica and shake to verify the dispersion stability. 4) Alternately add 1 mL of acrylic acid and 1 g of silica to the solution, shaking thoroughly with a shaker each time, until 6 mL of acrylic acid is added. While ensuring that no agglomeration occurs, a total of 12 g of silica powder is added. The solution is then sonicated to obtain a clear and transparent solution. 5) Add 8 mL of PEG400 in two portions, 4 mL each time, and mix thoroughly with a shaker after each addition; 6) Add 0.21g of photoinitiator 819, stir and mix thoroughly with a shaker, and finally sonicate to obtain a transparent glass precursor solution with very good flowability.

[0026] The final glass precursor solution contained over 30% silica by mass, representing the highest silica content without agglomeration. Testing showed that even with a 30% doping level, the precursor retained 12.8% self-healing capability after curing, meeting the requirements for subsequent assembly processes.

[0027] Example 2: Glass precursor splicing and assembly process based on self-healing properties 1. Precursor unit molding: Inject the precursor solution into a custom silicone mold and cure it with 365nm ultraviolet light for 30 minutes to obtain a complete self-healing precursor block, which is then cut into precursor units of a preset shape according to design requirements; 2. Seamless splicing at room temperature: After cleaning the cross-section of the unit to be spliced, it is directly bonded without additional adhesive. It is allowed to stand and heal for more than 2 hours at room temperature and normal pressure. Seamless splicing is achieved through the dynamic reconstruction of multivalent hydrogen bonds, resulting in an integrated precursor green body with a complex structure. The whole process is shown in Figure 3.

[0028] Example 3: Stepwise degreasing-two-step vacuum sintering process adapted to self-healing splicing precursors 1. Step-by-step degreasing process Based on TG-DTA thermal analysis (heating rate 10℃ / min, air atmosphere, room temperature - 1000℃), the precursor thermal decomposition was divided into three stages, and the thermogravimetric-differential thermal analysis curves are shown in Figure 4: room temperature - 300℃ (small molecule escape, weight loss 16.5%), 300℃-450℃ (main organic phase decomposition, weight loss 45%, high defect incidence stage), 450℃-610℃ (residual organic matter decomposition, weight loss 6%).

[0029] To avoid deformation, cracking, and delamination defects during the degreasing process, a step-by-step process of vacuum pre-degreasing + air final degreasing is adopted. The degreasing temperature rise curve is shown in Figure 5. The specific procedure is as follows: 1) Vacuum degreasing: The assembled green blanks are placed in a vacuum degreasing furnace and pre-degreasing is completed according to the air degreasing heating program. In a low-oxygen environment, structural defects caused by rapid decomposition of organic matter are avoided. 2) Air degreasing: The sample is transferred into a box-type muffle furnace and processed according to the following procedure: room temperature 3℃ / min, raise to 200℃ and hold for 2h → 0.5℃ / min, raise to 300℃ and hold for 2h → 0.5℃ / min, raise to 400℃ and hold for 5h → 0.5℃ / min, raise to 550℃ and hold for 2h → 0.5℃ / min, raise to 610℃ and hold for 3h. The sample is then cooled to room temperature in the furnace to obtain a green blank with silica powder.

[0030] FTIR and SEM verification showed that the organic components were completely removed after degreasing. The sample state changes during the entire degreasing and sintering process are shown in Figure 7, and the microstructure of the green blank is shown in Figure 8. The green blank had no cracks, delamination, or deformation defects.

[0031] 2. Two-step vacuum sintering process Sintering was carried out in a vacuum tube furnace using a two-step sintering method: high-temperature densification at 1310℃ followed by low-temperature holding at 1100℃. This method avoided crystallization and improved density. The final sintering program was determined through parameter optimization, and the sintering temperature rise curve is shown in Figure 6. The temperature was increased from 50℃ to 875℃ at 5℃ / min, then increased to 1100℃ at 1℃ / min and held for 2 hours, then increased to 1310℃ at 10℃ / min, then immediately decreased to 1100℃ at 10℃ / min and held for 2 hours. The temperature was then cooled to room temperature in the furnace to obtain transparent quartz glass. The changes in the state of the sample throughout the debinding and sintering process are shown in Figure 7.

[0032] The comparison of shrinkage rate and cross-sectional morphology of the samples before and after sintering is shown in Figure 9. The UV-Vis-NIR transmittance spectrum of the sintered glass is shown in Figure 10. The visible light transmittance is >90%. The nanoindentation test shows an average hardness of 10.90 GPa and an elastic modulus of 68.95 GPa, which are consistent with the performance of commercial quartz glass. The shrinkage rates in the diameter and thickness directions are 43.3% and 43.5%, respectively, which shows excellent isotropic shrinkage characteristics. The fracture stress at the splicing interface reaches 61.9% of the bulk, and the interface integration effect is excellent.

[0033] Example 4: Core Functional Application Expansion 1. Zoned Controllable Light Emitting Functional Glass: Eu³⁺, Ce³⁺, and Tb³⁺ rare earth ions are in-situ doped into silica nanoparticles to prepare a self-healing precursor with corresponding light-emitting properties. After photopolymerization, self-healing splicing, and debinding sintering, a functional glass that is fully transparent under natural light and emits red, blue, and green primary colors in zones under 254nm ultraviolet light is obtained. A physical comparison is shown below. Figure 11 As shown, there is no interface optical mismatch and no color bleeding.

[0034] Moldless self-bending irregular-shaped glass: Utilizing the differential shrinkage characteristics of precursors with different silica contents during sintering, precursor units with different contents are spliced ​​into a double-layer structure through self-healing. After sintering, the whole structure is directionally bent along the side with low silica content. The directional bending mechanism is shown in Figure 12. The preparation process and the actual object are compared in Figure 13. Irregular curved glass can be prepared without molds, external force and subsequent hot bending treatment.

[0035] Processing Examples I. Example 1: Preparation of Transparent Quartz Glass Based on Self-Healing Splicing 1) Precursor preparation: Take a brown light-proof reagent bottle and add 6 mL of HEMA; add silica nanopowder in 5 portions (1 g each time, shake at 3000 r / min for 5 min), stop adding when agglomeration occurs after adding 5 g; add 1 mL of POE and shake until the agglomeration disappears, then add 1 mL of AAc and 1 g of silica alternately until 6 mL of AAc is added, with a total of 12 g of silica added, and sonicate for 30 min to obtain a clear dispersion; add 8 mL of PEG400 in 2 portions (4 mL each time, shake for 5 min), add 0.21 g of photoinitiator 819, shake for 10 min, and sonicate for 20 min to obtain a self-healing precursor solution with a silica mass fraction of 32%.

[0036] 2) Splicing and molding: The precursor solution was injected into the dumbbell-shaped mold of GB / T 1040.2 standard and cured under ultraviolet light for 30 min to obtain 2 sets of standard samples; 1 set of samples was cut in the middle and the cross-sections were glued together and cured at room temperature for 2 h to obtain spliced ​​samples; the other set of complete samples served as the control group.

[0037] 3) Stepwise degreasing: The two groups of samples were first pre-degreased under vacuum, and then transferred to a muffle furnace for processing according to the established degreasing procedure. The raw blanks were obtained by cooling in the furnace.

[0038] 4) Two-step sintering: The green blank is placed in a vacuum tube furnace, the vacuum is drawn to below 10 Pa, and it is processed according to the established sintering procedure. The transparent quartz glass sample is obtained by cooling with the furnace.

[0039] 5) Performance verification: The average visible light transmittance of the sample was 91.2%, the hardness was 10.90 GPa, and the elastic modulus was 68.95 GPa; the fracture stress of the control group was 9.16 MPa, and the fracture stress of the spliced ​​sample was 5.67 MPa, indicating excellent interfacial bonding performance. II. Example 2: Preparation of Tri-color Localized Light Emitting Glass 1) Preparation of rare earth-doped silica: Prepare 0.1 mol / L ethanol solutions of europium nitrate, cerium nitrate, and terbium nitrate respectively; take 3 portions of 12g silica nanoparticles, mix them with the above rare earth solutions at a solid-liquid ratio of 1g:5mL, stir at 3000r / min for 30min, dry at 80℃, and grind to obtain Eu³⁺, Ce³⁺, and Tb³⁺-doped silica nanoparticles.

[0040] 2) Preparation of light-emitting precursors: Red, blue and green light-emitting self-healing precursors were prepared using the above-mentioned doped silicon dioxide according to the process in Example 1.

[0041] 3) Splicing and sintering: The three precursors were cured into 10mm×10mm×2mm units, which were then sequentially bonded together and cured at room temperature for 3 hours to obtain spliced ​​green bodies. These green bodies were then processed using the debinding and sintering process described in Example 1 to obtain partitioned luminescent glass. 4) Effect verification: The sample is colorless and completely transparent under natural light, with no visible splicing interface; under 254nm ultraviolet light, the three zones emit uniform red, blue and green light respectively, without color mixing.

[0042] II. Example 3: Preparation of Moldless Self-Bending Irregularly Shaped Glass 1) Precursor preparation: Precursor A with a silica mass fraction of 30% and precursor B with a silica mass fraction of 0% were prepared according to the process in Example 1.

[0043] 2) Unit molding and splicing: Precursor A and B are cured into thin film units of 30mm×5mm×0.5mm and 20mm×5mm×0.5mm respectively; Precursor B is attached to the middle area of ​​precursor A, with a 5mm single-layer area reserved at each end, and allowed to stand at room temperature for 2 hours to heal, thus obtaining a double-layer composite green body.

[0044] 3) Degreasing and sintering: The glass is processed according to the stepwise degreasing-two-step sintering process in Example 2 to finally obtain self-bending transparent glass.

[0045] 4) Effect verification: The sample is completely transparent and has no crack defects; the middle double-layer area is directionally bent along one side of the original precursor B, and the single-layer areas at both ends maintain horizontal extension, which is completely consistent with the theoretical design. No mold or hot bending process is required to achieve the precise preparation of irregular curved glass.

[0046] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A glass precursor having self-healing properties, characterized in that, It includes the following components: reactive monomer, crosslinking agent, dynamic crosslinking solvent, photoinitiator, sintering aid, and inorganic filler; wherein, the reactive monomer is hydroxyethyl methacrylate (HEMA), the crosslinking agent is acrylic acid (AAc), the dynamic crosslinking solvent is polyethylene glycol 400 (PEG400), the photoinitiator is phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide 819, the sintering aid is phenoxyethanol (POE), and the inorganic filler is silica nanoparticles.

2. The method for preparing a glass precursor with self-healing properties as described in claim 1, characterized in that, Includes the following steps: 1) Take a brown, light-proof container and add 6 mL of HEMA monomer; 2) Add silica nanoparticle powder to HEMA in batches, 1 gram each time. After each addition, mix thoroughly with a shaker to ensure that the silica powder is well dispersed in the solution. Continue this process until the fifth addition, when the powder shows obvious agglomeration. 3) Add 1 mL of POE sintering aid to the solution and shake it thoroughly with a shaker. The agglomeration phenomenon was found to have disappeared. Then add 1 g of silica and shake to verify the dispersion stability. 4) Alternately add 1 mL of acrylic acid and 1 g of silica to the solution, shaking thoroughly with a shaker each time, until 6 mL of acrylic acid is added. While ensuring that no agglomeration occurs, a total of 12 g of silica powder is added. The solution is then sonicated to obtain a clear and transparent solution. 5) Add 8 mL of PEG400 in two portions, 4 mL each time, and mix thoroughly with a shaker after each addition; 6) Add 0.21g of photoinitiator 819, stir and mix thoroughly with an oscillator, and finally sonicate to obtain a transparent glass precursor solution.

3. The application of the glass precursor as described in claim 1 in the preparation of zoned controllable light-emitting functional glass.

4. The application of the glass precursor as described in claim 1 in the preparation of moldless self-bending irregularly shaped glass.