A random copolymer and its application

By using random copolymer modification layers and block copolymer self-assembly technology in semiconductor manufacturing, the problem of block copolymers being difficult to align vertically on the substrate has been solved, achieving high-resolution photolithography patterning and improving line density and process compatibility.

CN123106982APending Publication Date: 2026-11-17FUDAN UNIVERSITY +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510619171.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing block copolymers are difficult to form phase separation structures perpendicular to the substrate in semiconductor manufacturing, and solvent annealing processes are not compatible with existing processes, making it difficult to further reduce line size in photolithography.

Method used

Random copolymers were used as a modifying layer. Random copolymers were prepared by free radical polymerization and block copolymers were coated on their surface. The vertical orientation self-assembly of the block copolymers was achieved by thermal annealing to form high-resolution photolithographic patterns.

Benefits of technology

It achieves vertical orientation self-assembly of block copolymers, improves the resolution of photolithography, reaches a line density of sub-10nm, and the process is compatible with existing semiconductor manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005401993870000021
    Figure BDA0005401993870000021
  • Figure BDA0005401993870000023
    Figure BDA0005401993870000023
  • Figure BDA0005401993870000033
    Figure BDA0005401993870000033
Patent Text Reader

Abstract

This invention relates to a random copolymer and its applications. Specifically, the invention discloses a random copolymer that, by using the random copolymer to prepare a modifying layer for a silicon wafer, enables a subsequently coated block copolymer layer to achieve vertically oriented self-assembly after thermal annealing. The invention also discloses a silicon wafer modified with the modified layer and a silicon wafer containing a vertically oriented block copolymer self-assembled pattern.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of materials, and more specifically to a random copolymer and its applications. Background Technology

[0002] Integrated circuits can integrate tens of millions of components on an area of ​​one square centimeter. This development is made possible by the continuous improvement of semiconductor manufacturing technology, and photolithography plays an extremely important role in it.

[0003] Photolithography is a process that transfers patterns from a photomask to photoresist by irradiating it with ultraviolet light or an electron beam. These patterns can be used to define various regions in integrated circuits, such as active areas and contact holes. In short, the smaller the line size that photolithography can create, the smaller the final device size, the more devices can be accommodated in the same area, and the more functions the circuit can perform. With the continuous advancement of industrial nodes, the expectation is for photolithography dimensions to become smaller and smaller. However, 193nm immersion lithography has reached its physical limits, and extreme ultraviolet (EUV) lithography, due to its extremely high cost and low process reliability, cannot be widely applied to all stages of the photolithography process. Direct Self-Assembly (DSA) patterning technology, as an emerging photolithography technology, has significant advantages in terms of equipment cost and process requirements. Rapid annealing allows block copolymers to approach a defect-free state within the same patterning process time. Compared to EUV lithography, DSA technology can achieve comparable line sizes at a much lower cost.

[0004] The materials commonly used in DSA (Digital Substrate Altering) technology are block copolymers (BCPs). After annealing, BCPs can form different morphologies, such as layered parallel stripes or columnar porous lines. The morphology formed after annealing is determined by the properties of the BCP material itself. Typically, layered BCPs are used to form lines, and columnar BCPs are used to form holes. Layered materials can undergo phase separation in two possible ways: stacking them parallel to the substrate or aligning them perpendicular to the substrate. In photolithography, the perpendicular alignment is obviously required. Therefore, the layered structure formed by phase separation needs to be perpendicular to the substrate. However, due to the difference in surface energy between the different blocks of BCP and the substrate interface, the blocks with lower surface energy tend to aggregate at the interface to minimize the system energy. This causes the phase-separated structure formed by the block copolymer to tend to be parallel to the substrate orientation, making it unsuitable for use as a photolithography template. Furthermore, while solvent annealing can achieve vertical orientation, it involves a closed solvent atmosphere where the substrate does not directly contact the solvent, but rather the block copolymer film swells in the vapor, leading to orientation-related microphase separation. Therefore, solvent annealing typically includes the introduction and removal of solvent vapor. However, semiconductor manufacturing has stringent environmental requirements, and residual solvent vapor can affect other process steps. Consequently, solvent annealing is difficult to integrate with existing semiconductor manufacturing processes, making it impractical for industrial semiconductor production.

[0005] In the early stages of the research and development of this invention, block copolymers for DSA technology were developed, with publication numbers CN109251283A and CN107245133A. Although the polymers disclosed in these two patents can achieve rapid self-assembly and high order in a short time, and provide a means to obtain extremely high resolution photolithography, the layered phase structure of these materials is usually arranged parallel to the substrate, making it difficult to form the required vertical layered structure. Therefore, there is an urgent need to develop a guided self-assembly patterning method that enables the lines formed by the phase separation of block copolymers to be arranged perpendicular to the substrate material and is compatible with semiconductor manufacturing technology. Summary of the Invention

[0006] The purpose of this invention is to provide a random copolymer and its application in DSA technology.

[0007] In a first aspect, the present invention provides a random copolymer, said random copolymer being prepared by polymerization of a first monomer and a second monomer;

[0008] The first monomer has the structure shown in Formula I:

[0009]

[0010] R1 is selected from the following group: H, halogen, C1-C6 alkyl, halo-C1-C6 alkyl;

[0011] X1 is selected from the following group: none, O, C1-C6 alkylene, halo-C1-C6 alkylene;

[0012] R2 is selected from the following group: C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, halo-C1-C6 alkyl;

[0013] X2 is selected from the following group: O, C1-C6 alkylene groups;

[0014] The second monomer is selected from the following group: the structure shown in Formula II and the structure shown in Formula III;

[0015]

[0016] R3 is selected from the following group: H, halogens, C1-C6 alkyl, and halo-C1-C6 alkyl;

[0017] Each R4 is independently selected from the following group: halogen, halogenated C1-C20 alkyl, -CR5R6-OH, OH;

[0018] m is selected from the following groups: 1, 2, 3, 4, 5;

[0019] R5 is selected from the following group: halogens, halogenated C1-C6 alkyl groups;

[0020] R6 is selected from the following group: halogens, halogenated C1-C6 alkyl groups;

[0021] R7 is selected from the following group: halogens, halogenated C1-C20 alkyl groups.

[0022] In another preferred embodiment, R1 is selected from the group consisting of: H, halogen, C1-C3 alkyl, and halogenated C1-C3 alkyl.

[0023] In another preferred embodiment, R1 is selected from the group consisting of: H, halogen, C1-C3 alkyl, and F-substituted C1-C3 alkyl.

[0024] In another preferred embodiment, X1 is selected from the group consisting of: none, O, C1-C3 alkylene, and halogenated C1-C3 alkylene.

[0025] In another preferred embodiment, X1 is selected from the group consisting of: none, O, C1-C3 alkylene, and F-substituted C1-C3 alkylene.

[0026] In another preferred embodiment, R2 is selected from the following group: C1-C3 alkyl, C2-C3 alkenyl, C2-C3 alkynyl, halo-C1-C3 alkyl;

[0027] X2 is selected from the following group: O, C1-C3 alkylene.

[0028] In another preferred embodiment, R2 is selected from the following group: C1-C3 alkyl, C2-C3 alkenyl, C2-C3 alkynyl, F-substituted C1-C3 alkyl;

[0029] X2 is selected from the following group: O, C1-C3 alkylene.

[0030] In another preferred embodiment, R3 is selected from the group consisting of: H, halogen, C1-C3 alkyl, and halogenated C1-C3 alkyl.

[0031] In another preferred embodiment, R3 is selected from the group consisting of: H, halogens, C1-C3 alkyl, and F-substituted C1-C3 alkyl.

[0032] In another preferred embodiment, R7 is selected from the group consisting of halogens and halogenated C1-C10 alkyl groups.

[0033] In another preferred embodiment, R7 is selected from the group consisting of halogens and halogenated C1-C6 alkyl groups.

[0034] In another preferred embodiment, R7 is selected from the group consisting of halogens and halogenated C1-C3 alkyl groups.

[0035] In another preferred embodiment, R7 is selected from the group consisting of halogens and F-substituted C1-C10 alkyl groups.

[0036] In another preferred embodiment, R7 is selected from the group consisting of halogens and F-substituted C1-C6 alkyl groups.

[0037] In another preferred embodiment, R7 is selected from the group consisting of halogens and F-substituted C1-C3 alkyl groups.

[0038] In another preferred embodiment, the structure shown in Equation II is the same as the structure shown in Equation IV.

[0039]

[0040] R3 is defined as in claim 1;

[0041] R4 is selected from the following group: halogens, halogenated C1-C20 alkyl groups, -CR5R6-OH;

[0042] R5 is selected from the following group: halogens, halogenated C1-C6 alkyl groups;

[0043] R6 is selected from the following group: halogens, halogenated C1-C6 alkyl groups.

[0044] In another preferred embodiment, R4 is selected from the group consisting of halogens, halogenated C1-C10 alkyl groups, and -CR5R6-OH.

[0045] In another preferred embodiment, R4 is selected from the group consisting of halogens, halogenated C1-C6 alkyl groups, and -CR5R6-OH.

[0046] In another preferred embodiment, R4 is selected from the group consisting of halogens, halogenated C1-C3 alkyl groups, and -CR5R6-OH.

[0047] In another preferred embodiment, R4 is selected from the group consisting of halogens, F-substituted C1-C20 alkyl groups, and -CR5R6-OH.

[0048] In another preferred embodiment, R4 is selected from the group consisting of halogens, F-substituted C1-C10 alkyl groups, and -CR5R6-OH. In another preferred embodiment, R4 is selected from the group consisting of halogens, F-substituted C1-C6 alkyl groups, and -CR5R6-OH.

[0049] In another preferred embodiment, R4 is selected from the group consisting of halogens, F-substituted C1-C3 alkyl groups, and -CR5R6-OH.

[0050] In another preferred embodiment, R5 is selected from the group consisting of halogens and halogenated C1-C3 alkyl groups.

[0051] In another preferred embodiment, R5 is selected from the group consisting of halogens and F-substituted C1-C6 alkyl groups.

[0052] In another preferred embodiment, R5 is selected from the group consisting of halogens and F-substituted C1-C3 alkyl groups.

[0053] In another preferred embodiment, R6 is selected from the group consisting of halogens and halogenated C1-C3 alkyl groups.

[0054] In another preferred embodiment, R6 is selected from the group consisting of halogens and F-substituted C1-C6 alkyl groups.

[0055] In another preferred embodiment, R6 is selected from the group consisting of halogens and F-substituted C1-C3 alkyl groups.

[0056] In another preferred embodiment, R4 is -CR5R6-OH;

[0057] R5 is selected from the following group: halogens, halogenated C1-C6 alkyl groups;

[0058] R6 is selected from the following group: halogens, halogenated C1-C6 alkyl groups.

[0059] In another preferred embodiment, R4 is -CR5R6-OH;

[0060] R5 is selected from the following group: halogens, halogenated C1-C3 alkyl groups;

[0061] R6 is selected from the following group: halogens, halogenated C1-C3 alkyl groups.

[0062] In another preferred embodiment, R4 is -CR5R6-OH;

[0063] R5 is selected from the following group: halogens, F-type C1-C6 alkyl groups;

[0064] R6 is selected from the following group: halogens, F-type C1-C6 alkyl groups.

[0065] In another preferred embodiment, R4 is -CR5R6-OH;

[0066] R5 is selected from the following group: halogens, F-type C1-C3 alkyl groups;

[0067] R6 is selected from the following group: halogens, F-type C1-C3 alkyl groups.

[0068] In another preferred embodiment, the first monomer is selected from the group consisting of:

[0069]

[0070] and / or

[0071] The second monomer is selected from the following group:

[0072]

[0073] In another preferred embodiment, in the random copolymer, the molar ratio of the second segment obtained by polymerization of the second monomer to the first segment obtained by polymerization of the first monomer is 1-300:1-100 (preferably 10-250:3-60, more preferably 25-210:5-50).

[0074] In another preferred embodiment, the random copolymer contains a first fragment obtained by polymerization of the first monomer and a second fragment obtained by polymerization of the second monomer, which together account for 70-100 wt%, 80-99 wt%, 85-98 wt%, 90-97 wt%, or 93-95 wt% of the total mass of the random copolymer.

[0075] In another preferred embodiment, the weight-average molecular weight of the random copolymer is 10-200 kg / mol (preferably 15-180 kg / mol, more preferably 20-160 kg / mol).

[0076] In another preferred embodiment, the number average molecular weight of the random copolymer is 5-100 kg / mol (preferably 10-90 kg / mol, more preferably 15-85 kg / mol).

[0077] In another preferred embodiment, the first monomer and the second monomer are polymerized via a free radical polymerization reaction to obtain the random copolymer.

[0078] In another preferred embodiment, the reaction temperature of the free radical polymerization reaction is 50-120°C, more preferably 60-100°C, and even more preferably 62-80°C; and / or

[0079] The reaction time for the free radical polymerization reaction is 0.5-24 h, preferably 2-12 h, and more preferably 3-6 h.

[0080] In another preferred embodiment, the initiator for the free radical polymerization reaction is selected from the group consisting of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, azobisisobutyramidine hydrochloride, benzoyl peroxide, dialkyl peroxide, or combinations thereof.

[0081] In another preferred embodiment, the free radical polymerization reaction is carried out in an inert protective atmosphere.

[0082] In another preferred embodiment, the inert protective atmosphere is nitrogen and / or argon.

[0083] In another preferred embodiment, the weight ratio of the first monomer, the second monomer, and the initiator is (3-150):(50-150):1, more preferably (4-120):(70-120):1, and even more preferably (4-100):(75-100):1.

[0084] In another preferred embodiment, after the free radical polymerization reaction is completed, the random copolymer is obtained through post-processing.

[0085] In another preferred embodiment, the post-processing includes deposition in a precipitant, collection of the precipitate, and drying of the precipitate to obtain the random copolymer.

[0086] In another preferred embodiment, the precipitant is selected from the group consisting of dichloromethane, n-hexane, methanol, water, or combinations thereof.

[0087] A second aspect of the present invention provides a silicon wafer modified with a modification layer, comprising: a silicon wafer and a modification layer located on the surface of the silicon wafer;

[0088] The modified layer is obtained by crosslinking and curing the random copolymer described in the first aspect of the present invention.

[0089] In another preferred embodiment, the thickness of the modified layer is 5-300 nm, more preferably 10-100 nm, and even more preferably 15-50 nm.

[0090] A third aspect of the present invention provides a silicon wafer containing a vertically oriented block copolymer self-assembled pattern, comprising, in sequence:

[0091] 1) A silicon wafer modified with the modification layer described in the second aspect of the present invention; and

[0092] 2) Vertically oriented block copolymer self-assembly pattern located on the surface of the modified layer.

[0093] In another preferred embodiment, the block copolymer is an F-containing block copolymer.

[0094] In another preferred embodiment, the block copolymer comprises block A and block B;

[0095] Block A is obtained by polymerization of monomer A, which has the structure shown in formula A:

[0096]

[0097] The block B is obtained by polymerization of monomer B, wherein the monomer B is selected from the following group: the structure shown in formula B1 and the structure shown in formula B2;

[0098]

[0099] Each Ra is independently selected from the following group: H, halogen, C1-C6 alkyl, halo-C1-C6 alkyl;

[0100] Rb is selected from the following group: halogens, halogenated C1-C10 alkyl groups;

[0101] Rc is selected from the following groups: H, OH.

[0102] In another preferred embodiment, the structure shown in equation B1 is as follows:

[0103] In another preferred embodiment, the structure shown in equation B2 is as follows:

[0104] In another preferred embodiment, each Ra is independently selected from the group consisting of: H, halogen, C1-C3 alkyl, and halogenated C1-C3 alkyl.

[0105] In another preferred embodiment, Rb is selected from the group consisting of halogens and F-substituted C1-C10 alkyl groups.

[0106] In another preferred embodiment, Rb is selected from the group consisting of halogens and halogenated C1-C6 alkyl groups.

[0107] In another preferred embodiment, Rb is selected from the group consisting of halogens and F-substituted C1-C6 alkyl groups.

[0108] In another preferred embodiment, monomer A is selected from the group consisting of:

[0109] In another preferred embodiment, the monomer B is selected from the group consisting of:

[0110] In another preferred embodiment, the molar ratio of block A to block B in the block copolymer is 1-500:1-500, more preferably 3-100:3-100, and even more preferably 5-60:6-80.

[0111] In another preferred embodiment, the block copolymer has a weight-average molecular weight of 5-100 kg / mol (preferably 8-50 kg / mol, more preferably 9-20 kg / mol).

[0112] In another preferred embodiment, the number-average molecular weight of the block copolymer is 5-100 kg / mol (preferably 8-50 kg / mol, more preferably 9-20 kg / mol).

[0113] In another preferred embodiment, the thickness of the block copolymer self-assembled pattern is 5-200 nm, more preferably 10-100 nm, and even more preferably 15-50 nm.

[0114] In another preferred embodiment, the resolution of the block copolymer self-assembled pattern is ≤10nm (preferably 5-10nm, more preferably 6-9nm, and most preferably 7.5-8.5nm).

[0115] It should be understood that, within the scope of this invention, the above-described technical features of this invention and the technical features specifically described below (such as in the embodiments) can be combined with each other to form new or preferred technical solutions. Due to space limitations, they will not be described in detail here. Attached Figure Description

[0116] Figure 1 The above is the 1H NMR spectrum of the random copolymer A1 (PMS-r-PGMA) prepared in Example A1 of this invention;

[0117] Figure 2 The 1H NMR spectrum of the random copolymer B1 (P4T-r-PGMA) prepared in Example B1 of this invention;

[0118] Figure 3 The hydrogen nuclear magnetic resonance spectrum of homopolymer C1 (PGMA) obtained in Example C1 of this invention;

[0119] Figure 4 This is a process flow diagram of application example A1 of the present invention;

[0120] Figure 5 A scanning electron microscope (SEM) image of the vertical orientation of the layered block copolymer in application example A1;

[0121] Figure 6 A scanning electron microscope (SEM) image of the vertical orientation of the layered block copolymer in application example A2;

[0122] Figure 7 A scanning electron microscope (SEM) image of the layered block copolymer of application example B1;

[0123] Figure 8A scanning electron microscope (SEM) image of the layered block copolymer of application example C1;

[0124] Figure 9 A scanning electron microscope (SEM) image of the vertical orientation of the layered block copolymer of application example A11;

[0125] Figure 10 A scanning electron microscope (SEM) image of the vertical orientation of the layered block copolymer of application example A12;

[0126] Figure 11 For comparison with the process flow diagram of Application Example 1;

[0127] Figure 12 For comparison, scanning electron microscope images of the phase separation morphology of the block copolymer material in Application Example 1 on a silicon substrate, showing the planar and 45° cross-sections;

[0128] Figure 13 A planar scanning electron microscope image of the phase separation morphology of the block copolymer material on a silicon substrate for comparison with Application Example 2.

[0129] Figure 14 A planar scanning electron microscope image of the phase separation morphology of the block copolymer material in Application Example 3 on a silicon substrate. Detailed Implementation

[0130] Through long-term and in-depth research, the inventors have developed a method to prepare random copolymers by selecting specific monomer combinations. These random copolymers are then used as precursors for further crosslinking to obtain a polymer serving as a silicon wafer modification layer. In the presence of this modification layer, block polymers (especially F-containing block copolymers) are further spin-coated onto it. Following thermal annealing, phase separation and rapid self-assembly of the block polymers are achieved, resulting in a vertically oriented phase-separated structure. This phase-separated structure exhibits small pattern size and high resolution, reaching sub-10 nm resolution, thus increasing the line density per unit area. Based on this, the inventors have completed this invention.

[0131] This invention proposes a random copolymer, its preparation method and application, and a guided self-assembly patterning method. The random copolymer provided by this invention can be further used in DSA processes. First, the substrate is modified with the random copolymer, and then block copolymers are used for self-assembly on its surface. This eliminates the surface energy differences between the blocks of the block copolymer, thereby achieving low-temperature rapid self-assembly. Simultaneously, it allows for the vertical alignment of layered or columnar block polymers on the substrate template, completing high-resolution rapid DSA lithography.

[0132] The random copolymer provided by this invention has a first monomer that forms a crosslinking repeating unit for crosslinking to form an organic film, serving as a solvent-insoluble crosslinking pad (modification layer). The second monomer forms a functional repeating unit, which controls the spatial orientation of the block copolymer, making it perpendicular to the substrate. The first and second monomers form a specific random copolymer through random copolymerization. The surface energy of this type of random copolymer is between the surface energies of the two blocks in the block copolymer used, exhibiting no preferential affinity for either block. Therefore, the two parts of the block copolymer will be uniformly aligned on the surface of the film formed by this type of random copolymer, transforming the original layered structure parallel to the substrate into one perpendicular to the substrate.

[0133] The present invention also provides a guided self-assembly graphical method, comprising the following steps:

[0134] A modification layer (a crosslinked pad insoluble in solvent) is prepared on a substrate using the random copolymer, and then a block copolymer solution is coated on the surface of the modification layer to obtain a block copolymer film. The film is then annealed and optionally etched to obtain a vertically oriented pattern.

[0135] Preferably, the method for preparing the modification layer is one of physical vapor deposition (PVD), chemical vapor deposition (CVD), or spin-coating.

[0136] More preferably, the method for preparing the modified layer is spin coating, and the specific steps of spin coating include:

[0137] The random copolymer is dissolved in an organic solvent to obtain the random copolymer solution, which is then spin-coated onto the substrate surface. The solution is first spin-coated at 100-500 rpm for 5 s, and then at 2000-5000 rpm for 60 s to obtain a film with a thickness of 5-200 nm. The solvent is removed, and the film is then heat-annealed at 100-250 °C for 1-24 h to obtain the modified layer.

[0138] Preferably, the method for removing the solvent is to place it in an N2 environment and heat it at 30-80°C for 5-30 minutes until the solvent evaporates completely.

[0139] Preferably, the organic solvent is at least one of propylene glycol methyl ether acetate (PGMEA), tetrahydrofuran (THF), cyclohexanone, and toluene.

[0140] Preferably, the specific steps of coating the block copolymer solution onto the surface of the modified layer include:

[0141] The block copolymer solution was spin-coated onto the surface of the modified layer. First, the spin-coating was carried out at 100-500 rpm for 3-8 seconds, and then at 2000-5000 rpm for 50-70 seconds to obtain a film with a thickness of 30-200 nm. The solvent was then removed.

[0142] Preferably, the method for removing the solvent is to place it in an N2 environment and heat it at 30-80°C for 1-30 minutes until the solvent evaporates completely.

[0143] Preferably, the solute mass fraction of the block copolymer solution is 0.5%-6%, and / or the block copolymer solution is coated by spin coating, and / or the spin coating speed is 1500-5000 rpm, and / or the spin coating time is 30-120 s.

[0144] Preferably, the specific steps of the annealing method include:

[0145] The block copolymer film is self-assembled using a thermal annealing method, wherein the thermal annealing temperature is 60-160°C and / or the thermal annealing time is 5 min-3 h.

[0146] Preferably, the temperature of the heat annealing is 80-120°C, and / or the heat annealing time is 10-30 min.

[0147] Preferably, the substrate is one of the following: silicon wafer substrate, silicon oxide substrate, silicon nitride substrate, titanium nitride (TiN) hard mask substrate, anti-reflective coating substrate (BARC), spin-on glass substrate (SOG), glass substrate, and polymer substrate (such as polyimide substrate).

[0148] Preferably, the block copolymer is a layered fluorinated block copolymer and / or a columnar fluorinated block copolymer. Because fluorine has a very low surface energy, fluorinated layered block copolymer materials typically tend to form a layered structure parallel to the substrate surface if a modification layer is lacking. This orientation is generally unsuitable for applications in photolithography manufacturing.

[0149] More preferably, the block copolymer is poly(p-hydroxystyrene-b-poly(1H,1H-perfluorobutyl methacrylate)) (layered block copolymer, abbreviated as P4HS-b-PHFBMA).

[0150] The random copolymer provided by this invention includes a first monomer and a second monomer with a specific structure as raw materials. The random copolymer is further used in a guided self-assembly patterning process, which can directly produce a modification layer on a substrate. Then, a block copolymer is coated on the surface of the modification layer. The block copolymer can achieve phase separation and rapid self-assembly under conditions of lower annealing temperature and shorter annealing time (such as hot annealing at 60-160℃ for 5 min-3 h). The resulting vertically oriented pattern has a small size and high resolution, which can reach a sub-10 nm resolution, thereby increasing the density of lines per unit area.

[0151] Compared with the prior art, the present invention has the following main advantages:

[0152] (1) By using the modified layer prepared by further crosslinking polymerization of the random copolymer described in this invention, this invention can achieve phase separation and self-assembly of F-block copolymer to form a vertically oriented phase separation structure;

[0153] (2) In the application field of the random copolymer described in this invention, the required equipment and process flow are already mature in the semiconductor manufacturing field, so they can be integrated with existing processes and have good application prospects.

[0154] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods in the following embodiments, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. Unless otherwise stated, percentages and parts are by weight.

[0155] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as are familiar to those skilled in the art. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to the methods of this invention. The preferred embodiments and materials described herein are for illustrative purposes only.

[0156] Unless otherwise specified, the raw materials, reagents or apparatus used in the following examples are available from conventional commercial sources or can be obtained by existing known methods.

[0157] Example: Preparation of random copolymer A1

[0158] 2 g of 1,1,1,3,3,3-hexafluoro-2-(4-vinylphenyl)-2-propanol and 2 g of glycidyl methacrylate monomer were added to a reaction tube, along with 24 mg of azobisisobutyronitrile (AIB) as an initiator. Under a nitrogen atmosphere, using 10 mL of tetrahydrofuran as the reaction solvent, the reactants and tetrahydrofuran solvent were refluxed at 65 °C for 4 h to carry out free radical polymerization. After the reaction, the product was precipitated in a mixed solvent of dichloromethane and n-hexane, dried, and poly(1,1,1,3,3,3-hexafluoro-2-(4-vinylphenyl)-2-propanol-r-poly(glycidyl methacrylate) (PMS-r-PGMA), i.e., random copolymer A1.

[0159] The 1H NMR spectrum of the prepared PMS-r-PGMA product (random copolymer A1) (characterized using deuterated tetrahydrofuran as solvent) is as follows: Figure 1As shown, the peak e, representing polyglycidyl methacrylate, the peak d, representing the benzene ring in poly1,1,1,3,3,3-hexafluoro-2-(4-vinylphenyl)-2-propanol, and the peak f, representing the hydroxyl group, all appear in the spectrum, indicating that a PMS-r-PGMA random copolymer has been obtained, with the structure as follows:

[0160]

[0161] The random copolymer A1 was found to have a weight-average molecular weight of 33.4 kg / mol, a number-average molecular weight of 17.9 kg / mol, and a degree of polymerization (m:n) molar ratio of 39:47.

[0162] Example: Preparation of A2-A5 random copolymer A2-A5

[0163] The monomer type, initiator type, and reaction solvent type are the same as in Example A1. The differences and results are shown in the table below.

[0164]

[0165] Example: Preparation of random copolymer B1

[0166] 2 g of 4-trifluoromethylstyrene and 0.7 g of glycidyl methacrylate monomer were added to a reaction tube, along with 24 mg of azobisisobutyronitrile (AIB) as an initiator. Under a protective nitrogen atmosphere, 10 mL of tetrahydrofuran was used as the reaction solvent. The reactants and tetrahydrofuran solvent were refluxed at 65 °C for 4 h to carry out a free radical polymerization reaction. After the reaction was completed, the product was precipitated in a mixed solvent of dichloromethane and n-hexane, dried, and poly(4-trifluoromethylstyrene-r-poly(glycidyl methacrylate)) (abbreviated as P4T-r-PGMA), i.e., random copolymer B1, was obtained.

[0167] The 1H NMR spectrum of the prepared P4T-r-PGMA (random copolymer B1) product (characterized using deuterated tetrahydrofuran as solvent) is as follows: Figure 2 As shown in the spectrum, the h peak representing the benzene ring in 4-trifluoromethylstyrene and the g peak representing glycidyl methacrylate both appear in the spectrum, indicating that a random copolymer of P4T-r-PGMA has been obtained, with the following structure:

[0168]

[0169] The random copolymer B1 was found to have a weight-average molecular weight of 43.4 kg / mol, a number-average molecular weight of 28 kg / mol, and a degree of polymerization q:p (molar ratio) of 151:14.

[0170] Example: Preparation of B2-B5 random copolymer B2-B5

[0171] The monomer type, initiator type, and reaction solvent type are the same as in Example B1. The differences and results are shown in the table below.

[0172]

[0173] Example: Preparation of homopolymer C1

[0174] 2g of glycidyl methacrylate monomer and 20mg of azobisisobutyronitrile (AIBN) were added to a reaction tube as initiators. Under a protective nitrogen atmosphere, 12mL of tetrahydrofuran was used as the reaction solvent. The reactants and tetrahydrofuran solvent were refluxed at 65°C for 4 hours to carry out free radical polymerization. After the reaction, the product was precipitated in a mixed solvent of dichloromethane and n-hexane, dried, and polyglycidyl methacrylate (PGMA), i.e., homopolymer C1, was obtained.

[0175] The 1H NMR spectrum of the prepared PGMA (homopolymer C1) product (characterized using deuterated tetrahydrofuran as solvent) is as follows: Figure 3 As shown in the figure, the characteristic peak I, representing polyglycidyl methacrylate, appears in the spectrum, indicating that a PGMA homopolymer has been obtained, with the following structure:

[0176]

[0177] The homopolymer C1 was tested and found to have a weight-average molecular weight of 26 kg / mol and a number-average molecular weight of 17.2 kg / mol.

[0178] Example: Preparation of C2-C3 homopolymer

[0179] The initiator type and reaction solvent type are the same as in Example C1. The differences and results are shown in the table below.

[0180]

[0181] Application Example A1

[0182] A guided self-assembly graphical method (process flow as follows) Figure 4 The process includes the following steps:

[0183] (1) Cleaning silicon wafers: Take a 4-inch silicon wafer and cut it into 1cm*1cm square pieces with a glass cutter. Collect the pieces in a glass petri dish and spread them out. Add 30mL of 30wt% hydrogen peroxide aqueous solution and then slowly add 70mL of concentrated sulfuric acid. After the concentrated sulfuric acid is added, place the dish on a hot plate while maintaining a slight boil. Cover the petri dish and heat at 95℃ for 0.5h to react. After the reaction is complete, pour the cleaning solution into a special acid and alkali waste liquid tank. Then, ultrasonically clean the wafer for 10min with 100mL of ultrapure water, 100mL of acetone and 100mL of ethanol in sequence. After cleaning, dry the silicon wafer with high-pressure nitrogen and then clean it with O2 plasma for 20min.

[0184] (2) Create a finishing layer:

[0185] Weigh 50 mg of PMS-r-PGMA from Example A1 into a round-bottom flask, and add 5 mL of propylene glycol methyl ether acetate (PGMEA) solvent to the flask. Stir until completely dissolved. Filter the solution through a 0.23 μm PTFE filter to prepare a 1% (w / w) PMS-r-PGMA solution. Spin-coat the PMS-r-PGMA solution onto a silicon wafer surface, first at 500 rpm for 5 s, then at 2000 rpm for 60 s, to obtain a 40 nm thick PMS-GMA film. Then, heat the film at 60°C for 5 min under N2 atmosphere until the solvent evaporates completely, and then anneal at 190°C for 3 h to allow the epoxy portion of glycidyl methacrylate to crosslink and cure, providing the surface required for modification and thus obtaining the modified layer.

[0186] (3) Spin-coated block copolymer: Weigh 50 mg of poly(p-hydroxystyrene-b-poly(1H,1H-perfluorobutyl methacrylate)) (layered block copolymer, abbreviated as P4HS-b-PHFBMA, with the structure as follows) A mixture of cyclohexanone (j:k = 21:31, molecular weight 10.8 kg / mol) was placed in a round-bottom flask. 5 mL of cyclohexanone solvent was added to the flask and stirred until completely dissolved. The solution was filtered through a 0.23 μm PTFE filter to prepare a 1% (w / w) P4HS-b-PHFBMA solution. The P4HS-b-PHFBMA solution was spin-coated onto the modified layer surface at 500 rpm for 5 s and then at 2000 rpm for 60 s to obtain a 30 nm thick poly(p-hydroxystyrene-b-poly(1H,1H-perfluorobutyl methacrylate)).

[0187] (4) Thermal annealing: Place the silicon wafer obtained in step (3) in an N2 environment, heat it at 40°C for 3 minutes on a hot plate until the solvent evaporates, and then heat it at 120°C for 10 minutes to perform self-assembly.

[0188] Typically, during phase separation, the spatial orientation of block copolymers depends primarily on the surface energy differences between the individual blocks of the copolymer, the substrate surface, and the air interface. When these surface energy differences are significant, vertical orientation becomes difficult to achieve. Since the two blocks of the block copolymer used in this method have significantly different surface energies, parallel orientation would result without a modified substrate layer. Therefore, this invention modifies the substrate surface beforehand using the random copolymer PMS-r-PGMA, ensuring the modified surface energy is suitable for the two blocks of the copolymer, ultimately achieving vertically oriented lines.

[0189] The assembly size and morphology of the layered phase of the block polymer on the modified silicon wafer in Application Example A1 above were analyzed using scanning electron microscopy, such as... Figure 5 As shown. When the silicon wafer used is flat and has no additional patterns, the flowchart is as follows. Figure 4 As shown in Figure A, the obtained morphology is as follows: Figure 5 As shown in Figure A, the block polymers are arranged perpendicular to the silicon wafer, forming a fingerprint-like structure. From... Figure 5 The scale in A shows that the width of the 6 sets of repeating lines is 98 nm, meaning the period of the block copolymer material is 16.3 nm. This results in lines approximately 8 nm wide, indicating that the invention can ultimately achieve sub-10 nm vertically oriented lines, reaching sub-10 nm resolution. If a certain period of line trenches is pre-fabricated on the silicon wafer using photolithography-etching, the flowchart is as follows... Figure 4 As shown in B, the obtained morphology is as follows: Figure 5 As shown in Figure B, it can be seen that by using a silicon wafer with periodic trenches, the block copolymers can achieve long-range ordered alignment both perpendicular to the silicon wafer and along the direction of the trench lines. In other words, the block copolymers can ultimately be oriented, demonstrating their potential for use in semiconductor lithography.

[0190] Application Examples A2-A5

[0191] Similar to application example A1, the difference is that the copolymer used to prepare the modified layer is changed from random copolymer A1 to one of random copolymers A2-A5.

[0192] The assembly size and morphology of the layered phase of the block polymer on the modified silicon wafer in Application Example A2 above were analyzed using scanning electron microscopy, such as... Figure 6 As shown, the block polymers are arranged perpendicular to the silicon wafer, forming a fingerprint-like structure.

[0193] Furthermore, if other conditions remain unchanged, and only the random copolymer is adjusted to one of A3-A5, similar conclusions can be reached. Therefore, keeping other conditions constant and only changing the ratio of the two components in the random copolymer yields essentially the same results. Therefore, in subsequent application examples, only one representative example will be given to illustrate the application effect of a certain type of random copolymer, rather than showing all the results for this type of random copolymer.

[0194] Application Example B1

[0195] Similar to application example A1, the difference is that the copolymer used to prepare the modified layer is changed from random copolymer A1 to random copolymer B1.

[0196] The assembly size and morphology of the layered phase of the block polymer on the modified silicon wafer in Application Example B1 above were analyzed using scanning electron microscopy, such as... Figure 7 As shown, when the random copolymer and block copolymer used are mismatched, their orientation control ability changes, and they cannot achieve a good vertical orientation effect.

[0197] Application example C1

[0198] Similar to application example A1, the difference is that the copolymer used to prepare the modified layer is changed from random copolymer A1 to homopolymer C1.

[0199] The assembly size and morphology of the layered phase of the block polymer on the modified silicon wafer in Application Example C1 were analyzed using scanning electron microscopy. Figure 8 As shown, it can be seen that when a homopolymer is prepared using only a single component, it does not have the ability to control orientation.

[0200] Similarly, using only homopolymers C2 or C3 to prepare the modification layer does not provide the ability to control orientation.

[0201] Application Example A11

[0202] A guided self-assembly graphical method differs from application example A1 in that the annealing temperature is replaced with 100℃ and the annealing time is replaced with 20min.

[0203] The assembly size and morphology of the layered phase of the block polymer on the modified silicon wafer in Application Example A11 above were analyzed using scanning electron microscopy, such as... Figure 9 As shown, the block polymers are arranged perpendicular to the silicon wafer.

[0204] Application Example A12

[0205] A guided self-assembly graphical method differs from application example A1 in that the annealing temperature is replaced with 80℃ and the annealing time is replaced with 30min.

[0206] The assembly size and morphology of the layered phase of the block polymer on the modified silicon wafer in Application Example A12 above were analyzed using scanning electron microscopy, such as... Figure 10 As shown, the block polymers are arranged perpendicular to the silicon wafer.

[0207] Comparative Application Example 1

[0208] A guided self-assembly graphical method (process flow as follows) Figure 11 The process includes the following steps:

[0209] (1) Cleaning silicon wafers: Take a 4-inch silicon wafer and cut it into 1cm*1cm square pieces with a glass cutter. Collect the pieces in a glass petri dish and spread them out. Add 30mL of 30wt% hydrogen peroxide aqueous solution and then slowly add 70mL of concentrated sulfuric acid. After the concentrated sulfuric acid is added, place the dish on a hot plate while maintaining a slight boil. Cover the petri dish and heat at 95℃ for 0.5h to react. After the reaction is complete, pour the cleaning solution into a special acid and alkali waste liquid tank. Then, ultrasonically clean the wafer for 10min with 100mL of ultrapure water, 100mL of acetone and 100mL of ethanol in sequence. After cleaning, dry the silicon wafer with high-pressure nitrogen and then clean it with O2 plasma for 20min.

[0210] (2) Spin-coated block copolymer: Weigh 50 mg of P4HS-b-PHFBMA (structure is...) A cyclohexanone solvent (j:k = 21:31, molecular weight 10.8 kg / mol) was added to a round-bottom flask. 5 mL of cyclohexanone solvent was added to the flask and stirred until completely dissolved. The solution was filtered through a PTFE filter with a pore size of 0.23 μm to prepare a 1% (w / w) P4HS-b-PHFBMA solution. The P4HS-b-PHFBMA solution was spin-coated at 500 rpm for 5 s and then at 2000 rpm for 60 s to obtain a 30 nm thick P4HS-b-PHFBMA layer.

[0211] (3) Thermal annealing: Place the silicon wafer obtained in step (2) in an N2 environment, heat it at 40°C for 3 minutes on a hot plate until the solvent evaporates, and then heat it at 120°C for 10 minutes to perform self-assembly.

[0212] The self-assembled silicon wafer was fractured in liquid nitrogen, and the interface morphology of the block copolymer was observed using a scanning electron microscope. Figure 12 A and Figure 12As shown in B, the SEM images of the phase separation morphology of the block copolymer material on the silicon substrate in Comparative Application Example 1 are a planar image and a 45° cross-section image, respectively. It can be seen that when observing the surface from top to bottom, the arrangement of lines cannot be observed. However, when observing the cross-section of the film, only lines arranged parallel to the substrate can be observed. This indicates that when no modification layer is made in Comparative Application Example 1, only parallel orientation can be obtained, and vertically oriented lines cannot be obtained.

[0213] Comparative Application Example 2

[0214] A guided self-assembly graphical method includes the following steps:

[0215] (1) Cleaning silicon wafers: Take a 4-inch silicon wafer and cut it into 1cm*1cm square pieces with a glass cutter. Collect the pieces in a glass petri dish and spread them out. Add 30mL of 30wt% hydrogen peroxide aqueous solution and then slowly add 70mL of concentrated sulfuric acid. After the concentrated sulfuric acid is added, place the dish on a hot plate while maintaining a slight boil. Cover the petri dish and heat at 95℃ for 0.5h to react. After the reaction is complete, pour the cleaning solution into a special acid and alkali waste liquid tank. Then, ultrasonically clean the wafer for 10min with 100mL of ultrapure water, 100mL of acetone and 100mL of ethanol in sequence. After cleaning, dry the silicon wafer with high-pressure nitrogen and then clean it with O2 plasma for 20min.

[0216] (2) Spin-coated block copolymer: Weigh 50 mg of P4HS-b-PHFBMA (structure is...) A cyclohexanone solvent (j:k = 21:31, molecular weight 10.8 kg / mol) was added to a round-bottom flask. 5 mL of cyclohexanone solvent was added to the flask and stirred until completely dissolved. The solution was filtered through a PTFE filter with a pore size of 0.23 μm to prepare a 1% (w / w) P4HS-b-PHFBMA solution. The P4HS-b-PHFBMA solution was spin-coated at 500 rpm for 5 s and then at 2000 rpm for 60 s to obtain a 30 nm thick P4HS-b-PHFBMA layer.

[0217] (3) Solvent annealing: The silicon wafer obtained in step (2) is placed in a closed chloroform solvent atmosphere and annealed for 2 hours. During the solvent annealing, the silicon wafer does not come into direct contact with the solvent, but only the film swells in the vapor and further generates orientation microphase separation.

[0218] The interface morphology of the block copolymer was observed using a scanning electron microscope, such as... Figure 13 As shown, when observing the surface from above, the vertical arrangement of the lines can also be observed.

[0219] Comparative Application Example 3

[0220] A guided self-assembly graphical method includes the following steps:

[0221] (1) Cleaning silicon wafers: Take a 4-inch silicon wafer and cut it into 1cm*1cm square pieces with a glass cutter. Collect the pieces in a glass petri dish and spread them out. Add 30mL of 30wt% hydrogen peroxide aqueous solution and then slowly add 70mL of concentrated sulfuric acid. After the concentrated sulfuric acid is added, place the dish on a hot plate while maintaining a slight boil. Cover the petri dish and heat at 95℃ for 0.5h to react. After the reaction is complete, pour the cleaning solution into a special acid and alkali waste liquid tank. Then, ultrasonically clean the wafer for 10min with 100mL of ultrapure water, 100mL of acetone and 100mL of ethanol in sequence. After cleaning, dry the silicon wafer with high-pressure nitrogen and then clean it with O2 plasma for 20min.

[0222] (2) Spin-coated block copolymer: Weigh 50 mg of P2VP-b-PHFBMA (structure is...) A 1% P2VP-b-PHFBMA solution (s:t = 15:36, molecular weight 7.5 kg / mol) was prepared by adding 5 mL of toluene solvent to a round-bottom flask and stirring until completely dissolved. The solution was then filtered through a 0.23 μm PTFE filter to prepare a 1% P2VP-b-PHFBMA solution. The P2VP-b-PHFBMA solution was spin-coated at 500 rpm for 5 s and then at 2000 rpm for 60 s to obtain a 60 nm thick P2VP-b-PHFBMA film.

[0223] (3) Solvent annealing: The silicon wafer obtained in step (2) is placed in a closed chloroform solvent atmosphere and annealed for 2 hours. During the solvent annealing, the silicon wafer does not come into direct contact with the solvent, but only the film swells in the vapor and further generates orientation microphase separation.

[0224] The interface morphology of the block copolymer was observed using a scanning electron microscope, such as... Figure 14 As shown, when observing the surface from above, the vertical arrangement of the lines can also be observed.

[0225] Comparative application examples 1, 2, and 3 show that without a modification layer, thermal annealing cannot produce vertical orientation in the material; only solvent annealing can achieve vertical orientation. However, solvent annealing is not suitable for semiconductor manufacturing (in actual industrial production, the solvent annealing method is incompatible with existing semiconductor manufacturing technologies), thus limiting the application scope of block copolymers.

[0226] All documents mentioned in this invention are incorporated herein by reference as if each document were individually incorporated by reference. Furthermore, it should be understood that after reading the foregoing teachings of this invention, those skilled in the art can make various alterations or modifications to this invention, and these equivalent forms also fall within the scope defined by the appended claims.

Claims

1. A random copolymer characterized in that, The random copolymer is prepared by polymerization of a first monomer and a second monomer; The first monomer has the structure shown in Formula I: R1 is selected from the following group: H, halogen, C1-C6 alkyl, halo-C1-C6 alkyl; X1 is selected from the following group: none, O, C1-C6 alkylene, halo-C1-C6 alkylene; R2is selected from the group consisting of: Ci-C6-alkyl, C2-C6-alkenyl, C2-C6-alkynyl, halogenated Ci-C6-alkyl; X2 is selected from the following group: O, C1-C6 alkylene groups; The second monomer is selected from the following group: the structure shown in Formula II and the structure shown in Formula III; R3 is selected from the following group: H, halogens, C1-C6 alkyl, and halo-C1-C6 alkyl; Each R4 is independently selected from the following group: halogen, halogenated C1-C20 alkyl, -CR5R6-OH, OH; m is selected from the following groups: 1, 2, 3, 4, 5; R5 is selected from the following group: halogens, halogenated C1-C6 alkyl groups; R6 is selected from the following group: halogens, halogenated C1-C6 alkyl groups; R7 is selected from the following group: halogens, halogenated C1-C20 alkyl groups.

2. The random copolymer of claim 1, wherein The structure shown in Equation II is the same as the structure shown in Equation IV. R3 is defined as in claim 1; R4 is selected from the following group: halogens, halogenated C1-C20 alkyl groups, -CR5R6-OH; R5 is selected from the following group: halogens, halogenated C1-C6 alkyl groups; R6 is selected from the following group: halogens, halogenated C1-C6 alkyl groups.

3. The random copolymer as described in claim 2, characterized in that, R4 is -CR5R6-OH; R5 is selected from the following group: halogens, halogenated C1-C6 alkyl groups; R6 is selected from the following group: halogens, halogenated C1-C6 alkyl groups.

4. The random copolymer of claim 1, wherein The first monomer is selected from the following group: and / or The second monomer is selected from the following group:

5. The random copolymer of claim 1, wherein In the random copolymer, the molar ratio of the second fragment obtained by polymerization of the second monomer to the first fragment obtained by polymerization of the first monomer is 1-300:1-100.

6. The random copolymer of claim 1, wherein The weight-average molecular weight of the random copolymer is 10-200 kg / mol.

7. A silicon wafer modified with a modification layer, characterized in that, It comprises: a silicon wafer and a modification layer located on the surface of the silicon wafer; The modified layer is prepared by crosslinking and curing the random copolymer according to claim 1.

8. A silicon wafer containing a self-assembled pattern of vertically oriented block copolymer, characterized in that, In order of importance: 1) A silicon wafer modified with the modification layer of claim 7; and 2) Vertically oriented block copolymer self-assembly pattern located on the surface of the modified layer.

9. The silicon wafer containing a self-assembled pattern of vertically aligned block copolymer of claim 8, wherein, The block copolymer is an F-containing block copolymer.

10. The silicon wafer containing a self-assembled pattern of vertically aligned block copolymer of claim 8, wherein the block copolymer is a diblock copolymer. The resolution of the block copolymer self-assembled pattern is ≤10nm.

Citation Information

Patent Citations

  • Small-size block polymer material rapidly assembled at low quenching temperature as well as preparation and application of small-size block polymer material

    CN107245133A

  • Ultrahigh-resolution fluorine-containing oxygen-containing block copolymer and preparation method and application thereof