A biodegradable polyolefin material, its preparation method, and its application
By introducing degradable groups into the polyolefin molecular chain through free radical copolymerization, the structure of the polyolefin molecular chain is changed, solving the problem of the difficulty in degrading polyolefins and achieving efficient degradation and wide application.
Patent Information
- Application Number
- CN202611507353.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polyolefin materials are difficult to degrade, leading to environmental pollution. Current technologies mainly involve adding degradable agents to non-degradable polyolefins to form blends, without altering the molecular structure.
Polyolefins, organic aldehydes, and vinyl organic esters are copolymerized by free radical initiators using liquid-phase bulk polymerization, solution polymerization, or emulsion polymerization to introduce biodegradable groups and alter the molecular chain structure of polyolefins.
The prepared biodegradable polyolefin material can degrade by 45-56% under natural conditions and completely degrade within 3 years. It can degrade by 70-85% in marine environments and has excellent viscoelasticity, electrical properties and thermal stability, making it suitable for multiple industries.
Abstract
Description
Technical Field
[0001] This invention relates to the field of organic polymer materials technology, and in particular to a biodegradable polyolefin material, its preparation method, and its application. Background Technology
[0002] The biggest drawback of organic polymer materials, including various plastics, rubbers, fibers, coatings, adhesives, and low-value olefin oligomers, is environmental pollution. Therefore, the recycling and reuse of organic polymer materials is an urgent problem to be solved. Organic polymer materials include various polyethylene, polypropylene, and polystyrene. Polyethylene includes LDPE, HDPE, LLDPE, ULDPE, POE, PBE, EVA, EMMA, EAA, and low-value olefin oligomers. The main molecular chains of these organic polymer materials are formed by carbon-carbon chains, which are very stable and difficult to break down. Even though EVA, EMMA, and EAA are polar polymers, the polar groups are only side groups, and the main chain is still composed of carbon-carbon chains, making them difficult to break down.
[0003] Although patent (CN202511732537.1) discloses a bio-based biodegradable polyolefin alloy material and its preparation method, it only involves adding flame-retardant groups grafted from a bio-based flame-retardant biodegradable polyester to a non-degradable polyolefin base material to form a blend with the non-degradable polyolefin. Patent (CN202311053573.6) discloses a biodegradable polyolefin functional masterbatch, which essentially involves adding 3-5 parts of photosensitizer to a non-degradable polyolefin base material. The biodegradable polyolefin masterbatch disclosed in the patent (CN201110362396.0) includes 40-80 parts of sodium sulfate; 20-60 parts of starch; 12-18 parts of low-density polyethylene and linear low-density polyethylene; 4-8 parts of ethylene-vinyl acetate copolymer; 1-2 parts of coupling agent; 0.5-3 parts of photosensitizer; and 2-8 parts of processing aid. The production method is to first add sodium sulfate and starch to a high-speed mixer, stir and heat to 100°C, exhaust the air, then add the coupling agent and continue stirring for 8-12 minutes, and finally add low-density polyethylene and linear low-density polyethylene, ethylene-vinyl acetate copolymer, photosensitizer and processing aid, stir for 6 minutes, and discharge for later use; (2) Granulation: the prepared material is granulated by extruding through a co-rotating twin-screw extruder with a length-to-diameter ratio of 40 to obtain the finished product. The biodegradable polyethylene masterbatch disclosed in patent (CN202511517918.8) comprises: 100 parts LLDPE, 1.5-5 parts antioxidant, 0.5-3 parts acid scavenger, 25-35 parts starch, 0.4-1.0 parts photosensitizer, 10-20 parts aging resistant modifier, 2-4 parts starch plasticizer, and 8-15 parts modified filler; the aging resistant modifier is prepared by liquid-phase bulk blending of maleic anhydride-grafted polyolefin and amine-terminated polyamide in a mass ratio of 10:3-4. In both of the above schemes, the biodegradable polyolefin is a blend of non-biodegradable polyolefin and additives.
[0004] Therefore, existing polyolefins have not achieved their biodegradability by altering their molecular structure. Summary of the Invention
[0005] The purpose of this invention is to provide a biodegradable polyolefin material, its preparation method, and its application. By introducing biodegradable groups into the chain structure of non-biodegradable polyolefins, the molecular chain structure of non-biodegradable polyolefins is changed, thereby achieving biodegradability of polyolefins.
[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a method for preparing a biodegradable polyolefin material, comprising the following steps: Biodegradable polyolefin materials are obtained by mixing polyolefins, organic aldehydes, vinyl organic esters and free radical initiators using liquid-phase bulk polymerization, solution polymerization or emulsion polymerization.
[0007] Preferably, the mass ratio of the polyolefin, organic aldehyde, vinyl organic ester and initiator is 100:(0.05~30):(0.2~75):(0.01~5).
[0008] Preferably, the polyolefin includes polyethylene, polypropylene, polystyrene, EVA, EMMA, EAA, ABS, HIPS, EPR, EPDM, NBR, HNBR, SBS, SIS, SEBS, SEIS, SIBR, ESBR, SSBR, IIR, IR, NR, CR or any of the above-mentioned recycled polyolefin materials, or low-value olefin oligomers, or bio-based non-degradable polyolefins, or non-metallic materials from waste fans.
[0009] Preferably, the organic aldehyde has 1 to 10 carbon atoms; the organic aldehyde includes one or more of formaldehyde, trioxymethylene, benzaldehyde, butyraldehyde, acetaldehyde and propionaldehyde.
[0010] Preferably, the vinyl organic ester has 2 to 20 carbon atoms; the vinyl organic ester includes one or more of vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate, vinyl hexanoate, vinyl octanoate, vinyl undecenoate, methyl acrylate, methyl methacrylate, acrylic acid, butyl acrylate, hexyl methacrylate, fluorobutyl methacrylate, and hexyl acrylate.
[0011] Preferably, the free radical initiator includes one or more of azo initiators and organic peroxide initiators.
[0012] Preferably, when liquid-phase bulk polymerization is used, the temperature of the free radical copolymerization reaction is 50~280℃, the pressure is 0.2~5 MPa, and the reaction time is 0.5~45h; When solution polymerization is used, the process further includes adding a first solvent in the mixing step. The free radical copolymerization reaction is carried out at a temperature of 50–280°C, a pressure of 0.2–5 MPa, and a reaction time of 0.5–45 h. The mass ratio of the polyolefin to the first solvent is 100:(0.1–1500), and the first solvent comprises C5-C... 20 Inert organic solvents or C5-C 20 Halogenated organic solvents; When emulsion polymerization is used, the process further includes adding an emulsifier and a second solvent in the mixing step; the free radical copolymerization reaction is carried out at a temperature of 50~180℃, a pressure of 0.2~5 MPa, and a reaction time of 0.5~45 h; the mass ratio of the polyolefin, emulsifier, and second solvent is 100:(0.05~1):(50~1500), and the second solvent includes water and C5-C... 20 Inert organic solvents or C5-C 20 Halogenated organic solvents.
[0013] Preferably, the mixing of polyolefin, organic aldehyde, vinyl organic ester and free radical initiator includes: adding 80-95% by mass of organic aldehyde, 80-95% by mass of vinyl organic ester and all of the polyolefin from the raw material storage tank into the polymerization reactor; adding the remaining 5-20% by mass of organic aldehyde and 5-20% by mass of vinyl organic ester and all of the free radical initiator from the raw material storage tank into the free radical initiator material preparation tank, and then adding the free radical initiator material preparation tank into the polymerization reactor to carry out free radical copolymerization reaction.
[0014] This invention provides a biodegradable polyolefin material prepared by the preparation method described above, wherein the molecular weight of the biodegradable polyolefin material is 0.1~100×10⁻⁶. 4 g / mol, density 0.860~1.166 g / cm³ 3 .
[0015] This invention provides applications of the biodegradable polyolefin materials described in the above technical solutions in aerospace, power batteries, ship cables, nuclear reactors, automobiles, construction, communications, clothing, electronics, drones, agriculture, or daily use.
[0016] This invention provides a method for preparing biodegradable polyolefin materials. Polyolefins, organic aldehydes, and vinyl organic esters undergo free radical copolymerization reactions under the action of a free radical initiator via liquid-phase bulk polymerization, solution polymerization, or emulsion polymerization. This yields polyolefin copolymers with oxygen-containing or substituted oxygen-ether groups in their molecular chain structure, altering the polyolefin molecular chain structure and introducing biodegradable groups to obtain biodegradable polyolefin materials. Specifically, the free radical initiator generates free radicals, which initiate the generation of carbon free radicals in the polyolefin and polymerize it. The carbon free radicals also initiate the generation of carbon free radicals in the vinyl organic ester and polymerize it. Furthermore, the carbon free radicals initiate the generation of CO2 in the organic aldehyde. Oxygen free radicals polymerize, CO Oxygen free radicals initiate the production of carbon free radicals in vinyl organic esters, leading to polymerization, or initiate the production of carbon free radicals in polyolefins, leading to polymerization. This reaction is repeated cyclically to obtain polyolefin copolymers with oxygen-containing ether groups or substituted oxygen-ether groups in their molecular chain structure. Because the insertion of oxygen-ether bonds into the polyolefin molecular backbone elongates the surrounding C-C bonds, and because the electronegativity of oxygen atoms is much stronger than that of carbon atoms, neighboring carbon atoms become positively charged, enhancing the reactivity of carbon atoms and facilitating chain breakage, thus making the polyolefin more easily degraded. Therefore, the polyolefin material prepared by this invention readily undergoes degradation reactions under natural conditions, degrading by 45-56% in a natural environment after 3 years and by 70-85% in a marine environment after 1.5 years. This solves the problems of white pollution caused by the recalcitrant degradation of polyolefins and the challenges of recycling waste polyolefins.
[0017] The molecular weight of the biodegradable polyolefin material described in this invention is 0.1~100×10⁻⁶. 4 g / mol, density 0.860~1.166 g / cm³ 3 It possesses constant viscoelasticity, electrical properties, good adhesion, thermal stability, high elongation, and low stress; it also exhibits excellent dielectric properties, ease of molding and processing, and good compatibility; it can be used in aerospace, power batteries, ship cables, nuclear reactors, the automotive industry, the construction industry, the communications industry, the clothing industry, the electronics industry, fitness equipment, low-altitude economy, humanoid robots, drones, the military industry, agriculture, and daily use, etc.
[0018] The preparation method of the biodegradable polyolefin new material of the present invention is simple, mild, low-cost, requires little equipment, consumes little energy, and is green and environmentally friendly. Detailed Implementation
[0019] In this invention, unless otherwise specified, the raw materials or reagents required for preparation are all commercially available products well known to those skilled in the art.
[0020] This invention provides a method for preparing a biodegradable polyolefin material, comprising the following steps: Biodegradable polyolefin materials are obtained by mixing polyolefins, organic aldehydes, vinyl organic esters and free radical initiators using liquid-phase bulk polymerization, solution polymerization or emulsion polymerization.
[0021] In this invention, the mass ratio of the polyolefin, organic aldehyde, vinyl organic ester and initiator is preferably 100:(0.05~30):(0.2~75):(0.01~5), more preferably 100:(0.1~25):(1~50):(0.01~4).
[0022] In this invention, the polyolefin preferably includes polyethylene, polypropylene (PP), polystyrene (PS), EVA, EMMA, EAA, ABS, HIPS, PVC, EPR, EPDM, BR, NBR, HNBR, SBS, SIS, SEBS, SEIS, SIBR, ESBR, SSBR, IIR, IR, NR, CR or any of the above-mentioned recycled polyolefin materials, or low-value olefin oligomers, or bio-based non-degradable polyolefins, or non-metallic materials from waste fans.
[0023] In this invention, the polyethylene preferably includes LDPE, HDPE, MDPE, LLDPE, ULDPE, E / S copolymer, or POE; the polypropylene preferably includes iPP, aPP, sPP, PBE, impact polypropylene, EPR, EPDM, or propylene-butene copolymer, or the above-mentioned recycled polypropylene; this invention does not have a special limitation on the acquisition of the recycled polyolefin, and recycled polyolefin obtained by sorting, washing, and drying in a manner known in the art is acceptable; the low-value olefin oligomers preferably include C5 mixed olefins, C6 mixed olefins, C8 mixed olefins, ethylene oligomer mixtures, ethylene oligomer mixtures, propylene oligomer mixtures, or propylene oligomer mixtures; the bio-based non-degradable polyolefin is preferably a non-degradable polyolefin produced based on biomass resources. This invention does not have a special limitation on the source of the above-mentioned polyolefins, and commercially available products known in the art are acceptable.
[0024] In this invention, the organic aldehyde preferably has 1 to 10 carbon atoms; the organic aldehyde preferably includes one or more of formaldehyde, trioxymethylene, benzaldehyde, butyraldehyde, acetaldehyde, and propionaldehyde; when the organic aldehyde is two or more of the above, this invention does not have a special limitation on the ratio of different types of organic aldehydes, and any ratio is acceptable. The organic aldehyde is transformed into an oxyether group or a substituted oxyether group during free radical copolymerization.
[0025] In this invention, the vinyl organic ester preferably has 2 to 20 carbon atoms; the vinyl organic ester includes one or more of vinyl acetate (VAc), vinyl propionate, vinyl butyrate, vinyl valerate, vinyl hexanoate, vinyl octanoate, vinyl undecenoate, methyl acrylate, methyl methacrylate, acrylic acid, butyl acrylate, butyl trifluoromethacrylate, hexyl methacrylate, 2,2,3,3,4,4,4-heptafluorobutyl methacrylate, and hexyl acrylate. When the vinyl organic ester is two or more of the above, this invention does not have a special limitation on the ratio of different types of vinyl organic esters, and any ratio is acceptable.
[0026] In this invention, the free radical initiator preferably includes one or more of azo initiators and organic peroxide initiators. When the free radical initiator is two or more of the above, this invention does not have a special limitation on the ratio of different types of free radical initiators, and any ratio is acceptable.
[0027] In this invention, the azo initiator is preferably azobisisobutyronitrile (AIBN) and / or azobisisoheptanenitrile; the organic peroxide initiator is preferably one or more of benzoyl peroxide, dodecyl peroxide, diisopropyl peroxide, dicyclohexyl peroxide, cumene hydroperoxide, potassium persulfate-ferrous salt, benzoyl peroxide-dimethylaniline, cumene hydroperoxide, tert-butyl hydroperoxide, diisopropylbenzene peroxide, and ditert-butyl peroxide.
[0028] In this invention, when liquid-phase bulk polymerization is used, no solvent is added, and the raw materials are heated to a liquid-phase bulk state for free radical copolymerization; the temperature of the free radical copolymerization reaction is preferably 50~280℃, more preferably 100~220℃, the pressure is preferably 0.2~5 MPa, and the reaction time is preferably 0.5~45h.
[0029] In this invention, when solution polymerization is used, a first solvent is added in the mixing step. The temperature of the free radical copolymerization reaction is 50~280℃, more preferably 120~220℃, the pressure is 0.2~5 MPa, more preferably 1.0~2.0 MPa, and the reaction time is preferably 0.5~45h, more preferably 25~35h. The mass ratio of the polyolefin to the first solvent is preferably 100:(0.1~1500), more preferably 100:(1~1200), and even more preferably 100:(50~1000).
[0030] In this invention, the first solvent preferably comprises C5-C. 20An inert organic solvent or a halogenated organic solvent; more preferably, one or more of hexane, heptane, decane, dodecane, toluene, benzene, decahydronaphthalene, dioxane, propanol, butanol, octanol, hexafluoropropanol, 4,4,5,5,6,6,7,7,7-nonafluoro-1-heptanol, 1,1,1,-trifluorooctanol, perfluorotert-butanol, and trifluoroacetic acid.
[0031] In this invention, when emulsion polymerization is used, an emulsifier and a second solvent are added in the mixing step; the temperature of the free radical copolymerization reaction is preferably 50~180℃, more preferably 80~135℃, the pressure is preferably 0.2~5 MPa, more preferably 1.6~3 MPa, and the reaction time is preferably 0.5~45h, more preferably 18~25h; the emulsifier preferably includes one or more of anionic, cationic, amphoteric and nonionic types, more preferably sodium dodecyl sulfate, sorbitan fatty acid ester (Span) or polyvinyl alcohol; the mass ratio of the polyolefin, emulsifier and second solvent is preferably 100:(0.05~1):(50~1500), more preferably 100:(0.1~0.8):(100~1200), and even more preferably 100:(0.2~0.5):(300~500).
[0032] In this invention, the second solvent preferably includes water and C5-C. 20 Inert organic solvents or C5-C 20 The halogenated organic solvent is more preferably one or more of hexane, heptane, decane, dodecane, toluene, benzene, decahydronaphthalene, dioxane, propanol, butanol, octanol, hexafluoropropanol, 4,4,5,5,6,6,7,7,7-4,4,5,5,6,6,7,7,7-nonafluoro-1-heptanol, 1,1,1,-trifluorooctanol, perfluorotert-butanol, and trifluoroacetic acid.
[0033] In this invention, the mixing of polyolefin, organic aldehyde, vinyl organic ester and free radical initiator preferably includes: adding 80-95% by mass of organic aldehyde and 80-95% by mass of vinyl organic ester and all of the polyolefin from the raw material storage tank into the polymerization reactor; adding the remaining 5-20% by mass of organic aldehyde and 5-20% by mass of vinyl organic ester and all of the free radical initiator from the raw material storage tank into the free radical initiator material preparation tank, and then adding the free radical initiator material preparation tank into the polymerization reactor to carry out free radical copolymerization reaction.
[0034] This invention involves directly adding 80-95% of the total organic aldehyde and vinyl organic ester feedstock from the raw material storage tank into the polymerization reactor to contact the polyolefin. This enhances the mixing effect of the reactants polyolefin with the organic aldehyde and vinyl organic ester, which is beneficial for producing polyolefin copolymers with oxygen-containing or substituted oxygen-ether groups in the molecular chain structure. The remaining 5-20% of the total organic aldehyde and vinyl organic ester feedstock, along with the entire amount of free radical initiator, are added from the raw material storage tank to the free radical initiator material preparation tank, and then from the free radical initiator material preparation tank to the polymerization reactor. This further enhances the mixing effect of the reactants polyolefin with the organic aldehyde and vinyl organic ester with the free radical initiator, while maintaining thorough stirring at a relatively low temperature (0℃-40℃).
[0035] In this invention, the method for preparing the biodegradable polyolefin material more preferably includes the following steps: (1) Raw material storage and preparation: All raw materials are stored at room temperature; raw material storage tanks include: polyolefins are stored in polyolefin storage tanks (heated to 50~260℃ to make polyolefins into liquid bulk state or solution state); organic aldehydes are stored in organic aldehyde storage tanks, vinyl organic esters are stored in vinyl organic ester storage tanks, free radical initiators are stored in free radical initiator storage tanks, and solvents are stored in solvent storage tanks. (2) Preparation of free radical initiator materials: Take 5-20% by mass of organic aldehyde, 5-20% by mass of vinyl organic acid ester and all the free radical initiator from the raw material storage tank and add them to the free radical initiator material preparation tank to obtain free radical initiator materials for later use; the preparation temperature of the free radical initiator material preparation tank is preferably 0-40℃, more preferably 20-30℃, the operating pressure is preferably 0.1-2 MPa, more preferably 0.2-0.5 MPa, and the reaction time is preferably 0.1-3h, more preferably 1-2h; (3) Free radical copolymerization reaction: Take out all the feed amount of polyolefin, solvent, organic aldehyde accounting for 80-95% of the total feed amount and vinyl organic ester accounting for 80-95% of the total feed amount from the raw material storage tank and add them to the polymerization reactor; take out the prepared free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor; seal the polymerization reactor, and stir at 5-200 rpm to carry out the free radical copolymerization reaction to obtain the biodegradable polyolefin product; (4) Deviation: The polymer product is fed into a devolatilizer; the devolatilization temperature is preferably 50~280℃, more preferably 150~180℃, and the average residence time is preferably 10~300 min, more preferably 20~60 min; (5) Extrusion granulation: The devolatilized polyolefin product is fed into the feed inlet of a screw extruder. The screw extruder is divided into at least 2-3 sections between the feed inlet and the outlet. The operating temperature of each section is different or the same. The operating temperature of each section is preferably 150-350 ℃, more preferably 180-300 ℃, and the extrusion time is preferably 3-30 min, more preferably 3.5-10 min. Starting from the feed inlet, at least 1-2 sections are equipped with exhaust ports for vacuuming to further remove volatiles from the melt material until the volatiles are <0.1%. The material is then cooled with cold water, granulated, and dried to obtain biodegradable polyolefin material.
[0036] In this invention, in step (1), the volume of the raw material storage tank is preferably 0.5~200000L, more preferably 0.5~5000L, and even more preferably 5~500L, and it is made of stainless steel or glass.
[0037] In this invention, the volume of the free radical initiator material preparation tank is preferably 0.5~50000L, more preferably 0.5~5000L, and even more preferably 0.5~500L, and is made of stainless steel or glass. In this invention, the polymerization reactor is preferably a single-reactor reactor or multiple reactors in series, a reactor-tube reactor in series, a reactor-to-tower reactor in series, or a screw extruder, and is operated intermittently or continuously; the volume of the polymerization reactor is preferably 0.1~200000L, more preferably 0.5~5000L, and even more preferably 5L-500L, and is made of stainless steel or glass.
[0038] In this invention, the devolatilizer used for devolatilization is preferably a static thin-film devolatilizer, or a vertical or horizontal dynamic devolatilizer; the volume of the devolatilizer is preferably 0.1~100000L, more preferably 0.1~300L, and even more preferably 2~10L, and is made of stainless steel or glass; this invention removes volatile components such as solvents and unreacted monomers through devolatilization.
[0039] In the extrusion granulation step of the present invention, it is preferable to add an additive at the front end of the screw extruder. The additive preferably includes an anti-aging agent, and the mass ratio of the additive to the biodegradable polyolefin material is preferably (1~3):(100~10000).
[0040] This invention provides a biodegradable polyolefin material prepared by the preparation method described above, wherein the molecular weight of the biodegradable polyolefin material is 0.1~100×10⁻⁶. 4 g / mol, density 0.860~1.166 g / cm³ 3 .
[0041] This invention provides applications of the biodegradable polyolefin materials described in the above technical solutions in aerospace, power batteries, ship cables, nuclear reactors, automobiles, construction, communications, clothing, electronics, drones, agriculture, or daily use.
[0042] Specifically, the biodegradable polyolefin material described in this invention can be applied to power batteries, ship cables, optical data storage, AI think tanks, AI devices, quantum communication, quantum computing, superconducting devices, home appliances, aircraft interior parts, automobiles, sports and fitness equipment, humanoid robots, drones, optical discs, lenses, prisms, carrier plates, thin films, cover plates for solar cells, building materials, focusing plates, or glass fibers; or used in medical pre-filled syringes and medical testing consumables; it has excellent chemical stability and can be used in blood storage, test tubes, and high-temperature resistant medical goggles; or used in the preparation of thin films and substrates.
[0043] The specific embodiments of the present invention are described in detail below, but it should be understood that the scope of protection of the present invention is not limited to the specific embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0044] Unless otherwise specified, the experimental methods described in the various embodiments of this invention are conventional methods; unless otherwise specified, the raw materials used are all commercially available products, and the proportions are all by mass percentage.
[0045] In a specific embodiment, the raw material storage tank has a volume of 5L and is made of stainless steel.
[0046] The free radical initiator material preparation container has a volume of 0.5L and is made of stainless steel. The polymerization reactor is a single-reactor reactor, and the operation mode is batch; the volume of the polymerization reactor is 5L, and it is made of stainless steel. The devolatilizer used is a static thin-film devolatilizer; the volume of the devolatilizer is preferably 5L and it is made of glass.
[0047] Example 1
[0048] The raw materials, trioxymethylene, vinyl acetate, solvent 4,4,5,5,6,6,7,7,7-nonafluoro-1-heptanol, and initiator AIBN were stored in raw material storage tanks at room temperature; polyolefin POE was stored in a polyolefin storage tank at 130°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, prepared by using 0.05 g of initiator AIBN, 2.5 g of trioxymethylene, and 2.45 g of vinyl acetate at a preparation temperature of 20°C, an operating pressure of 0.2 MPa, and a preparation time of 0.5 h. Take 60g of polyolefin (POE) from the polyolefin storage tank, and take 12.0g of trioxymethylene, 15g of vinyl acetate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 60rpm, heat to 150℃, and stir until homogeneous. Take 5g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain the temperature at 150℃, the stirring speed at 60rpm, and the pressure at 1.0MPa in the polymerization reactor, and carry out the copolymerization reaction for 25h to obtain the polymer product. The polymerization product from the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 170°C for 30 minutes. Then, the biodegradable polyolefin was added to a twin-screw extruder at a temperature of 180°C in both the first and second sections for 3 minutes. After cooling with cold water, the product was pelletized and dried to obtain 67.2 grams of biodegradable polyolefin (POE).
[0049] The biodegradable polyolefin prepared in this embodiment has a weight-average molecular weight of 15.5 × 10⁻⁶. 4 g / mol, density 0.890 g / cm³ 3 The biodegradable polyolefin molecular chain contains 3.2% oxygen ether groups and 7.8% VAc (vinyl acetate) by mass. 13 The 12C NMR analysis results show that the presence of COC bonds in the polymer structure at chemical shifts δ=70.6 and 74.9 ppm indicates that the COC bonds are derived from free radical polymerization of aldehydes; the presence of ester bonds in the polymer structure at δ=71.5 and 170.2 ppm indicates that the polymer structure contains ester bonds, derived from free radical polymerization of vinyl acetate.
[0050] Example 2
[0051] The raw materials benzaldehyde, butyl acrylate, and initiator dicumyl peroxide were stored separately in raw material storage tanks at room temperature; the polyolefin LDPE was stored in a polyolefin storage tank at 150°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared using 0.06 g of initiator dicumyl peroxide, 1.8 g of benzaldehyde, and 2.4 g of butyl acrylate at a preparation temperature of 40°C, an operating pressure of 0.3 MPa, and a preparation time of 1 hour. 65 g of polyolefin LDPE was taken from the polyolefin storage tank, and 17.2 g of benzaldehyde and 17.5 g of butyl acrylate were taken from the raw material storage tank and added to the polymerization reactor. The mixture was stirred at 80 rpm and heated to 160°C until homogeneous. 4.26 g of free radical initiator material was taken from the free radical initiator material preparation tank and added to the polymerization reactor. The polymerization reactor was maintained at 160°C, stirred at 80 rpm, and pressure of 2.0 MPa for 35 h to obtain the polymerization product. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 180°C for 35 minutes. Then, the biodegradable polyolefin was added to a twin-screw extruder with a first-stage temperature of 190°C and a second-stage temperature of 185°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 73.9 grams of biodegradable polyolefin LDPE.
[0052] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 17.3 × 10⁻⁶. 4 g / mol, density 0.929 g / cm³ 3 The biodegradable polyolefin molecular chain contains 3.7% oxygen ether groups and 8.3% butyl acrylate by mass. 13 The 10⁻⁶ C NMR analysis results show that the presence of a signal at a chemical shift of δ=70.7 ppm indicates that the polymer structure contains COC bonds, which are derived from the free radical polymerization of aldehydes; the presence of signals at δ=74.3 and 170.2 ppm indicates that the polymer structure contains ester bonds, which are derived from the free radical polymerization of butyl acrylate.
[0053] Example 3
[0054] The raw materials, trioxymethylene, hexyl methacrylate, hexafluoropropanol, and di-tert-butyl peroxide initiator were stored in separate raw material storage tanks at room temperature; the polyolefin LLDPE was stored in a polyolefin storage tank at 150°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, and was prepared using 0.05 g of di-tert-butyl peroxide initiator, 2.1 g of trioxymethylene, and 3.0 g of hexyl methacrylate, at a preparation temperature of 40°C, an operating pressure of 0.3 MPa, and a preparation time of 1 h. 70 g of LLDPE polyolefin was taken from the polyolefin storage tank, and 18.4 g of paraformaldehyde, 21.8 g of hexyl methacrylate, and 8 g of solvent were taken from the raw material storage tank and added to the polymerization reactor. The mixture was stirred at 90 rpm and heated to 150°C until homogeneous. 5.15 g of free radical initiator material was taken from the free radical initiator material preparation tank and added to the polymerization reactor. The polymerization reactor was maintained at 150°C, stirred at 90 rpm, and at a pressure of 2.0 MPa for 40 h to obtain the polymerization product. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 170°C for 20 minutes. Then, the biodegradable polyolefin was added to a twin-screw extruder with a first-stage temperature of 190°C and a second-stage temperature of 185°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 79.7 grams of biodegradable polyolefin LLDPE.
[0055] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 18.1 × 10⁻⁶.4 g / mol, density 0.934 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.1% oxygen ether groups and 9.0% hexyl methacrylate. 13 The 10⁻⁶ C NMR analysis results show that the presence of a signal at a chemical shift of δ=70.6 ppm indicates that the polymer structure contains COC bonds, which are derived from free radical polymerization of alkyl aldehydes; the presence of signals at δ=73.1 and 173.0 ppm indicates that the polymer structure contains ester bonds, which are derived from free radical polymerization of hexyl acrylate.
[0056] Example 4
[0057] Formaldehyde, vinyl propionate, and initiator di-tert-butyl peroxide were stored separately in raw material storage tanks at room temperature; polyolefin SSBR was stored in a polyolefin storage tank at 150°C with stirring; free radical initiator material was stored in a free radical initiator material preparation tank, prepared with 0.05 g of initiator di-tert-butyl peroxide, 2.0 g of formaldehyde, and 2.25 g of vinyl propionate at a preparation temperature of 25°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. 85 grams of polyolefin SBR were taken from the polyolefin storage tank, and 20.9 grams of formaldehyde and 22.7 grams of vinyl propionate were taken from the raw material storage tank and added to the polymerization reactor. The mixture was stirred at 90 rpm and heated to 150°C until homogeneous. 4.3 grams of free radical initiator material were taken from the free radical initiator material preparation tank and added to the polymerization reactor. The polymerization reactor was maintained at 150°C, stirred at 90 rpm, and at a pressure of 2.0 MPa for 30 hours to obtain the polymerization product. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 160°C for 40 minutes. Then, the biodegradable polyolefin was added to a twin-screw extruder with a first-stage temperature of 190°C and a second-stage temperature of 185°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 97.0 grams of biodegradable polyolefin SBR.
[0058] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 15.7 × 10⁻⁶. 4 g / mol, density 0.912 g / cm³ 3 The biodegradable polyolefin molecular chain contains 3.9% oxygen ether groups and 8.7% vinyl propionate. 13C10 NMR analysis results show signals at chemical shifts δ=70.7 and 74.8 ppm, indicating the presence of COC bonds in the polymer structure, which originate from free radical polymerization of aldehydes; signals at δ=131.3-131.9 ppm belong to butadiene 1,4 structural units; δ=114.2 ppm belongs to butadiene 1,2 structural units; signals at δ=45.2-46.2 ppm, 141.7, and 126-128.8 ppm belong to styrene structural units; signals at δ=74.5 and 170.3 ppm indicate the presence of ester bonds in the polymer structure, which originate from free radical polymerization of vinyl propionate.
[0059] Example 5
[0060] The raw materials, butyraldehyde, vinyl butyrate, solvent decane, and initiator di-tert-butyl peroxide, were stored separately in raw material storage tanks at room temperature; the polyolefin BR was stored in a polyolefin storage tank at 130°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, and was prepared using 0.05 g of initiator di-tert-butyl peroxide, 2.6 g of butyraldehyde, and 2.95 g of vinyl butyrate at a preparation temperature of 25°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. 100 g of polyolefin BR was taken from the polyolefin storage tank, and 23.4 g of formaldehyde, 22.0 g of vinyl butyrate, and 8 g of solvent were taken from the raw material storage tank and added to the polymerization reactor. The mixture was stirred at 120 rpm and heated to 130°C until homogeneous. 5.6 g of free radical initiator material was taken from the free radical initiator material preparation tank and added to the polymerization reactor. The polymerization reactor was maintained at 130°C, stirred at 120 rpm, and pressure of 1.5 MPa for 28 hours to obtain the polymerization product. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 150°C for 20 minutes. Then, the biodegradable polyolefin BR was added to a twin-screw extruder with a first-stage temperature of 170°C and a second-stage temperature of 165°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 113.7 grams of biodegradable polyolefin BR.
[0061] The biodegradable polyolefin prepared in this embodiment has a weight-average molecular weight of 17.5 × 10⁻⁶. 4 g / mol, density 0.894 g / cm³ 3 The biodegradable polyolefin molecular chain contains 3.7% oxygen ether groups and 9.1% vinyl butyrate by mass. 13The 12C NMR analysis results show signals at chemical shifts δ=70.1 and 87.1 ppm, indicating the presence of COC bonds in the polymer structure. These COC bonds originate from the free radical polymerization of the butyraldehyde aldehyde. Signals at δ=128.8-135.3 ppm are attributed to double bonds in the butadiene backbone. Signals at δ=73.3 and 173.2 ppm indicate the presence of ester bonds in the polymer structure. These ester bonds originate from the free radical polymerization of vinyl butyrate.
[0062] Example 6
[0063] The raw materials, trioxymethylene, vinyl hexanoate, heptane solvent, and di-tert-butyl peroxide initiator were stored separately in raw material storage tanks at room temperature in 1L stainless steel tanks; polyolefin EPR was stored in a polyolefin storage tank at 135℃ with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05g of di-tert-butyl peroxide initiator, 2.6g of trioxymethylene, and 3.1g of vinyl hexanoate, at a preparation temperature of 25℃, an operating pressure of 0.5MPa, and a preparation time of 1h. 150 g of polyolefin EPR was taken from the polyolefin storage tank, and 23.5 g of trioxymethylene, 24.6 g of vinyl hexanoate, and 8 g of solvent were taken from the raw material storage tank and added to the polymerization reactor. The mixture was stirred at 90 rpm and heated to 135°C until homogeneous. 5.75 g of free radical initiator material was taken from the free radical initiator material preparation tank and added to the polymerization reactor. The polymerization reactor was maintained at a temperature of 135°C, stirred at 90 rpm, and a pressure of 1.8 MPa for 28 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 150°C for 30 minutes. Then, the biodegradable polyolefin EPR was added to a twin-screw extruder with a first-stage temperature of 170°C and a second-stage temperature of 165°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 171.6 grams of biodegradable polyolefin EPR.
[0064] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 21.5 × 10⁻⁶. 4 g / mol, density 0.920 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.6% oxygen ether groups and 9.3% vinyl hexanoate by mass. 13 The 10⁻⁶ C NMR analysis results show that the presence of signals at chemical shifts δ=70.6 and 74.9 ppm indicates that the polymer structure contains COC bonds, which are derived from the free radical polymerization of the alkyl aldehyde trioxymethylene; the presence of signals at δ=72.3 and 170.6 ppm indicates that the polymer structure contains ester bonds, which are derived from the free radical polymerization of vinyl acetate.
[0065] Example 7
[0066] The raw materials benzaldehyde, vinyl valerate, and initiator di-tert-butyl peroxide were stored in separate raw material storage tanks at room temperature; the polyolefin PP was stored in a polyolefin storage tank at 195°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05 g of initiator di-tert-butyl peroxide, 3.0 g of benzaldehyde, and 3 g of vinyl valerate at a preparation temperature of 25°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 200g of polyolefin (PP) from the polyolefin storage tank, and take 23.0g of benzaldehyde and 25g of vinyl valerate from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 195℃, and mix thoroughly. Take 6.05g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain the temperature at 195℃, stir at 30 rpm, and maintain the pressure at 2.0MPa in the polymerization reactor for 15 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 180°C for 30 minutes. Then, the biodegradable polyolefin (PP) was added to a twin-screw extruder with the first section temperature at 180°C and the second section temperature at 175°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 229.5 grams of biodegradable polyolefin (PP).
[0067] The biodegradable polyolefin prepared in this embodiment has a weight-average molecular weight of 22.3 × 10⁻⁶. 4 g / mol, density 0.894 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.7% oxygen ether groups and 8.7% vinyl valerate. 13 The 10⁻⁶ C NMR analysis results show that the presence of a signal at chemical shift δ=70.6 indicates that the polymer structure contains COC bonds, which are derived from the free radical polymerization of the hydroxyl aldehyde benzaldehyde; the presence of signals at δ=68.9 and 170.2 ppm indicates that the polymer structure contains ester bonds, which are derived from the free radical polymerization of vinyl valerate.
[0068] Example 8
[0069] The raw materials, trioxymethylene, 10-undecenoic acid vinyl ester, solvent perfluorotert-butanol, and initiator di-tert-butyl peroxide were stored in separate raw material storage tanks at room temperature. The polyolefin HIPS was stored in a polyolefin storage tank at 195°C with stirring. The free radical initiator material was stored in a free radical initiator material preparation tank and was prepared using 0.05 g of initiator di-tert-butyl peroxide, 3.1 g of trioxymethylene, and 3.6 g of 10-undecenoic acid vinyl ester at a preparation temperature of 35°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 200g of HIPS polyolefin from the polyolefin storage tank, and take 20g of paraformaldehyde, 18g of vinyl undecylenate, and 8g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 90 rpm, heat to 195℃, and stir until homogeneous. Take 6.75g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain the temperature at 195℃, stir at 90 rpm, and maintain the pressure at 1.6MPa in the polymerization reactor for 18 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 180°C for 35 minutes. Then, the biodegradable polyolefin HIPS was added to a twin-screw extruder with the first section temperature at 180°C and the second section temperature at 175°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 227.3 grams of biodegradable polyolefin HIPS.
[0070] The biodegradable polyolefin prepared in this embodiment has a weight-average molecular weight of 20.6 × 10⁻⁶. 4 g / mol, density 0.994 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.3% by mass of oxygen ether groups and 8.6% by mass of vinyl undecenoate. 13 C10 NMR analysis results show signals at chemical shifts δ=70.3 and 74.6 ppm, indicating the presence of COC bonds in the polymer structure, which originate from free radical polymerization of aldehydes; signals at δ=45.2-46.2 ppm, 141.8, and 126-128.8 ppm belong to styrene structural units; signals at δ=74.2 and 170.6 ppm indicate the presence of ester bonds in the polymer structure, which originate from free radical polymerization of vinyl undecenoate.
[0071] Example 9
[0072] The raw materials, trioxymethylene, vinyl octanoate, deionized water, and di-tert-butyl peroxide initiator were stored separately in raw material storage tanks at room temperature in 1 L glass tanks; the polyolefin NBR was stored in a polyolefin storage tank at 175°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05 g of di-tert-butyl peroxide initiator, 2.8 g of trioxymethylene, and 3.55 g of vinyl octanoate, at a preparation temperature of 35°C, an operating pressure of 0.5 MPa, and a preparation time of 1 h. Take 120g of NBR polyolefin from the polyolefin storage tank, and take 20g of paraformaldehyde, 19g of vinyl octanoate, 350g of solvent, and 0.5g of Span emulsifier from the raw material storage tank. Add them to the polymerization reactor, stir at 90 rpm, heat to 135℃, and mix thoroughly. Take 6.4g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain the temperature at 135℃, stir at 90 rpm, and maintain the pressure at 1.6MPa in the polymerization reactor for 18 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 175°C for 30 minutes. Then, the biodegradable polyolefin NBR was added to a twin-screw extruder with the first section temperature at 180°C and the second section temperature at 175°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 136.8 grams of biodegradable polyolefin NBR.
[0073] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 23.3 × 10⁻⁶. 4 g / mol, density 0.906 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.0% by mass of oxygen ether groups and 8.7% by mass of vinyl octanoate. 13 The 10⁻⁶ C NMR analysis results show signals at chemical shifts δ=70.7 and 74.9 ppm, indicating the presence of COC bonds in the polymer structure. These COC bonds originate from the free radical polymerization of the alkyl aldehyde paraformaldehyde. The signal at δ=130.3 ppm belongs to the butadiene 1,4 structural unit; the signal at δ=112.6 ppm belongs to the butadiene 1,2 structural unit; and the signal at δ=119.6 ppm belongs to the nitrile group of the acrylonitrile structural unit. Signals at δ=71.9 and 170.9 ppm indicate the presence of ester bonds in the polymer structure. These ester bonds originate from the free radical polymerization of vinyl octanoate.
[0074] Example 10
[0075] The raw materials, trioxymethylene, vinyl acetate, toluene solvent, and di-tert-butyl peroxide initiator were stored separately in raw material storage tanks at room temperature; the polyolefin NR was stored in a polyolefin storage tank at 155°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, and was prepared by using 0.05 g of di-tert-butyl peroxide initiator, 2.6 g of trioxymethylene, and 1.25 g of vinyl acetate at a preparation temperature of 35°C, an operating pressure of 0.5 MPa, and a preparation time of 1 h. Take 120g of polyolefin NR from the polyolefin storage tank, and take 20g of paraformaldehyde, 18g of vinyl acetate, and 1000g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 90 rpm, heat to 155℃, and mix thoroughly. Take 3.9g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain the temperature at 155℃, stir at 90 rpm, and maintain the pressure at 1.6MPa in the polymerization reactor for 18 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 155°C for 30 minutes. Then, the biodegradable polyolefin NR was added to a twin-screw extruder with a first-stage temperature of 180°C and a second-stage temperature of 175°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 137.5 grams of biodegradable polyolefin NR.
[0076] The biodegradable polyolefin prepared in this embodiment has a weight-average molecular weight of 25.6 × 10⁻⁶. 4 g / mol, density 0.908 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.8% oxygen ether groups and 8.9% VAc by mass. 13 The 124-135 ppm C NMR analysis results show signals at chemical shifts δ=70.5 and 74.9 ppm, indicating the presence of COC bonds in the polymer structure. These COC bonds originate from the free radical polymerization of aldehydes. Signals at δ=124-135 ppm are attributed to double bonds in the NR main chain. The signal at δ=110.6 ppm is attributed to double bonds in the NR side chain. Signals at δ=71.9 and 170.5 ppm indicate the presence of ester bonds in the polymer structure. These ester bonds originate from the free radical polymerization of vinyl acetate.
[0077] Example 11
[0078] The raw materials, trioxymethylene, vinyl acetate, toluene solvent, and di-tert-butyl peroxide initiator were stored in separate raw material storage tanks at room temperature; the polyolefin SBS was stored in a polyolefin storage tank at 165°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, and was prepared using 0.05 g of di-tert-butyl peroxide initiator, 2.5 g of trioxymethylene, and 3.5 g of vinyl acetate at a preparation temperature of 20°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 120g of polyolefin SBS from the polyolefin storage tank, and take 20g of trioxymethylene, 30g of vinyl acetate, and 10g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 40 rpm, heat to 165℃, and stir until homogeneous. Take 6.05g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain the temperature at 165℃, stir at 40 rpm, and maintain the pressure at 1.6MPa in the polymerization reactor for 18 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 165°C for 30 minutes. Then, the biodegradable polyolefin SBS was added to a twin-screw extruder at a temperature of 170°C in both the first and second sections for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 138.9 grams of biodegradable polyolefin SBS.
[0079] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 15.6 × 10⁻⁶. 4 g / mol, density 0.971 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.3% oxygen ether groups and 9.1% VAc groups by mass. 13 The 12C NMR analysis results show that the presence of signals at chemical shifts δ=70.7 and 74.8 ppm indicates the presence of COC bonds in the polymer structure, which originate from the free radical polymerization of aldehydes; the signals at δ=131.3-131.9 ppm belong to butadiene structural units; the signals at δ=45.2-46.2 ppm, 141.7, and 126-128.8 ppm belong to styrene structural units; and the presence of signals at δ=74.5 and 170.3 ppm indicates the presence of ester bonds in the polymer structure, which originate from the free radical polymerization of vinyl acetate.
[0080] Example 12
[0081] The raw materials, trioxymethylene, vinyl acetate, toluene solvent, and di-tert-butyl peroxide initiator were stored separately in raw material storage tanks at room temperature; the polyolefin PBE was stored in a polyolefin storage tank at 185°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, and was prepared by using 0.05 g of di-tert-butyl peroxide initiator, 3 g of trioxymethylene, and 2.5 g of vinyl acetate at a preparation temperature of 20°C, an operating pressure of 0.5 MPa, and a preparation time of 1 h. Take 120g of polyolefin (PBE) from the polyolefin storage tank, and take 20g of paraformaldehyde, 21g of vinyl acetate, and 15g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 50 rpm, heat to 185°C, and mix thoroughly. Take 5.55g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain the temperature at 185°C, stir at 50 rpm, and maintain the pressure at 1.6 MPa in the polymerization reactor for 18 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 180°C for 30 minutes. Then, the biodegradable polyolefin PBE was added to a twin-screw extruder with the first and second sections of the screw extruder at 170°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 137.7 grams of biodegradable polyolefin PBE.
[0082] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 15.6 × 10⁻⁶. 4 g / mol, density 0.911 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.3% oxygen ether groups and 9.4% VAc groups by mass. 13 The 10⁻⁶ C NMR analysis results show that the presence of signals at chemical shifts δ=70.7 and 74.9 ppm indicates that the polymer structure contains COC bonds, which are derived from free radical polymerization of aldehydes; the presence of signals at δ=71.3 and 170.2 ppm indicates that the polymer structure contains ester bonds, which are derived from free radical polymerization of vinyl acetate.
[0083] Example 13
[0084] The raw materials, trioxymethylene, vinyl acetate, toluene solvent, and di-tert-butyl peroxide initiator were stored in separate raw material storage tanks at room temperature; the polyolefin EVA was stored in a polyolefin storage tank at 155°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05 g of di-tert-butyl peroxide initiator, 3 g of trioxymethylene, and 3 g of vinyl acetate, at a preparation temperature of 30°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 120g of polyolefin EVA from the polyolefin storage tank, and take 20g of paraformaldehyde, 18g of vinyl acetate, and 8g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 70 rpm, heat to 155℃, and stir until homogeneous. Take 6.05g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain the temperature at 155℃, stir at 70 rpm, and maintain the pressure at 1.6MPa in the polymerization reactor for 18 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 160°C for 30 minutes. Then, biodegradable polyolefin EVA was added to a twin-screw extruder at a temperature of 150°C in both the first and second sections for 3.5 minutes. The extrusion was then cooled with cold water, pelletized, and dried to obtain 135.6 grams of biodegradable polyolefin EVA.
[0085] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 19.6 × 10⁻⁶. 4 g / mol, density 0.904 g / cm³ 3 The mass content of oxygen ether groups in the biodegradable polyolefin molecular chain is 11.5%. 13 C10 NMR analysis results show signals at chemical shifts δ=70.6 and 74.9 ppm, indicating the presence of COC bonds in the polymer structure. These COC bonds originate from the free radical polymerization of the aldehyde trioxymethylene. Signals at δ=74.5 and 170.2 ppm originate from the VA group of EVA. Signals at δ=71.5 and 170.3 ppm originate from the VA group adjacent to the CO group in the VA-CO-VA repeating unit. Signals at δ=74.9 and 74.9 ppm originate from the carbon atom signal of the CO group in the VA-CO-VA repeating unit. Signals at δ=46.9, 65.4, and 173.3 ppm indicate the presence of ester bonds in the polymer structure. These ester bonds originate from the free radical polymerization of vinyl acetate.
[0086] Example 14
[0087] The raw materials, trioxymethylene, butyl acrylate, toluene solvent, and di-tert-butyl peroxide initiator were stored separately in raw material storage tanks at room temperature; the polyolefin PBE was stored in a polyolefin storage tank at 185°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05 g of di-tert-butyl peroxide initiator, 3 g of trioxymethylene, and 3.5 g of butyl acrylate, at a preparation temperature of 30°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 120g of polyolefin (PBE) from the polyolefin storage tank, and take 20g of paraformaldehyde, 20g of butyl acrylate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 60 rpm, and heat to 195℃ until homogeneous. Take 6.55g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain the temperature at 195℃, stir at 60 rpm, and maintain the pressure at 1.6MPa in the polymerization reactor for 18 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 190°C for 30 minutes. Then, the biodegradable polyolefin PBE was added to a twin-screw extruder with the first and second sections of the screw extruder at 170°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 133.7 grams of biodegradable polyolefin PBE.
[0088] The biodegradable polyolefin prepared in this embodiment has a weight-average molecular weight of 16.0 × 10⁻⁶. 4 g / mol, density 0.906 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.5% oxygen ether groups and 7.2% butyl acrylate by mass. 13 The 12C NMR analysis results show that the presence of signals at chemical shifts δ=70.6 and 74.5 ppm indicates that the polymer structure contains COC bonds, which are derived from the free radical polymerization of the alkyl aldehyde paraformaldehyde; the presence of signals at δ=46.8, 65.3 and 173.1 ppm indicates that the polymer structure contains ester bonds, which are derived from the free radical polymerization of butyl acrylate.
[0089] Example 15
[0090] The raw materials, trioxymethylene, butyl acrylate, toluene solvent, and di-tert-butyl peroxide initiator were stored separately in raw material storage tanks at room temperature; the polyolefin POE was stored in a polyolefin storage tank at 165°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05 g of di-tert-butyl peroxide initiator, 2.6 g of trioxymethylene, and 3.5 g of butyl acrylate, at a preparation temperature of 25°C, an operating pressure of 0.5 MPa, and a preparation time of 1 h. Take 120g of polyolefin (POE) from the polyolefin storage tank, and take 20g of paraformaldehyde, 20g of butyl acrylate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 90 rpm, and heat to 175℃ until homogeneous. Take 6.15g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 90 rpm, temperature at 175℃, and pressure at 1.6MPa in the polymerization reactor for copolymerization reaction for 18 hours. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 170°C for 30 minutes. Then, the biodegradable polyolefin POE was added to a twin-screw extruder at a temperature of 170°C in both the first and second sections for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 132.5 grams of biodegradable polyolefin POE.
[0091] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 18.4 × 10⁻⁶.4 g / mol, density 0.890 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.7% oxygen ether groups and 5.7% butyl acrylate by mass. 13 The 10⁻⁶ C NMR analysis results show that the presence of signals at chemical shifts δ=70.6 and 74.5 ppm indicates that the polymer structure contains COC bonds, which are derived from the free radical polymerization of the alkyl aldehyde paraformaldehyde; signals at δ=46.7, 65.4 and 173.3 ppm indicate that the polymer structure contains ester bonds, which are derived from the free radical polymerization of butyl acrylate.
[0092] Example 16
[0093] The raw materials, trioxymethylene, butyl trifluoromethacrylate, toluene solvent, and di-tert-butyl peroxide initiator were stored separately in raw material storage tanks at room temperature; the polyolefin HDPE was stored in a polyolefin storage tank at 215°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05 g of di-tert-butyl peroxide initiator, 2 g of trioxymethylene, and 3.5 g of butyl trifluoromethacrylate, at a preparation temperature of 35°C, an operating pressure of 0.5 MPa, and a preparation time of 1 h. Take 120g of HDPE polyolefin from the polyolefin storage tank, and take 20g of paraformaldehyde, 23.8g of butyl trifluoromethacrylate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 220℃, and mix thoroughly. Take 5.55g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 30 rpm, temperature at 220℃, and pressure at 1.6MPa in the polymerization reactor for copolymerization reaction for 18h. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 190°C for 30 minutes. Then, the biodegradable polyolefin HDPE was added to a twin-screw extruder with the first section temperature at 190°C and the second section temperature at 185°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 132.9 grams of biodegradable polyolefin HDPE.
[0094] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 18.9 × 10⁻⁶. 4 g / mol, density 0.956 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.5% oxygen ether groups and 6.1% butyl trifluoromethacrylate. 13CNMR analysis results show signals at chemical shifts δ=70.6 and 74.7 ppm, indicating the presence of COC bonds in the polymer structure. These COC bonds originate from the free radical polymerization of the alkyl aldehyde paraformaldehyde. Signals at δ=46.1, 119.3, and 173.0 ppm indicate the presence of ester bonds in the polymer structure. These ester bonds originate from the free radical polymerization of butyl trifluoromethacrylate.
[0095] Example 17
[0096] The raw materials, trioxymethylene, butyl acrylate, toluene solvent, and di-tert-butyl peroxide initiator were stored separately in raw material storage tanks at room temperature; the recycled LDPE material was stored in a polyolefin storage tank at 215°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05 g of di-tert-butyl peroxide initiator, 3 g of trioxymethylene, and 3.5 g of butyl acrylate, at a preparation temperature of 35°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 120g of recycled LDPE from the polyolefin storage tank, and take 20g of paraformaldehyde, 18g of butyl acrylate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 200℃, and mix thoroughly. Take 6.55g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 30 rpm, temperature at 200℃, and pressure at 1.6MPa in the polymerization reactor for copolymerization reaction for 18h. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 190°C for 30 minutes. Then, biodegradable polyolefin LDPE was added to a twin-screw extruder with the first section temperature at 190°C and the second section temperature at 185°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 135.1 grams of biodegradable polyolefin LDPE.
[0097] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 13.7 × 10⁻⁶. 4 g / mol, density 0.923 g / cm³ 3 The biodegradable polyolefin molecular chain contains 5.0% oxygen ether groups and 7.3% butyl acrylate by mass. 13 The 10⁻⁶ C NMR analysis results show that the presence of signals at chemical shifts δ=70.7 and 74.4 ppm indicates that the polymer structure contains COC bonds, which are derived from the free radical polymerization of the alkyl aldehyde paraformaldehyde; signals at δ=46.5, 65.3, and 173.1 ppm indicate that the polymer structure contains ester bonds, which are derived from the free radical polymerization of butyl acrylate.
[0098] Example 18
[0099] The raw materials, trioxymethylene, vinyl acetate, toluene solvent, and di-tert-butyl peroxide initiator were stored separately in raw material storage tanks at room temperature; the recycled POE was stored in a polyolefin storage tank at 185°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05 g of di-tert-butyl peroxide initiator, 3 g of trioxymethylene, and 3.5 g of vinyl acetate at a preparation temperature of 35°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 120g of recycled polyolefin (POE) from the polyolefin storage tank, and take 20g of paraformaldehyde, 18g of vinyl acetate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 180°C, and mix thoroughly. Take 6.55g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 30 rpm, temperature at 180°C, and pressure at 1.6MPa in the polymerization reactor for copolymerization reaction for 18 hours. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 190°C for 30 minutes. Then, the biodegradable polyolefin POE was added to a twin-screw extruder with a first-stage temperature of 180°C and a second-stage temperature of 175°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 135.7 grams of biodegradable polyolefin POE.
[0100] The biodegradable polyolefin prepared in this embodiment has a weight-average molecular weight of 15.3 × 10⁻⁶. 4 g / mol, density 0.883 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.5% oxygen ether groups and 8.2% vinyl acetate by mass. 13 The 10⁻⁶ C NMR analysis results show that the presence of signals at chemical shifts δ=70.7 and 74.3 ppm indicates that the polymer structure contains COC bonds, which are derived from the free radical polymerization of the alkyl aldehyde paraformaldehyde; the presence of signals at δ=71.3 and 170.4 ppm indicates that the polymer structure contains ester bonds, which are derived from the free radical polymerization of butyl acrylate.
[0101] Example 19
[0102] The raw materials, trioxymethylene, hexyl methacrylate, toluene solvent, and di-tert-butyl peroxide initiator were stored in separate raw material storage tanks at room temperature; the recovered EVA was stored in a recovered material storage tank at 190°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05 g of di-tert-butyl peroxide initiator, 3 g of trioxymethylene, and 3.5 g of hexyl methacrylate, at a preparation temperature of 20°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 130g of recycled polyolefin EVA from the recycled material storage tank, and take 20g of paraformaldehyde, 18g of hexyl methacrylate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 180℃, and mix thoroughly. Take 6.55g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 30 rpm, temperature at 180℃, and pressure at 1.6MPa in the polymerization reactor for 18 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 190°C for 30 minutes. Then, biodegradable polyolefin EVA was added to a twin-screw extruder with the first section temperature set at 180°C and the second section temperature at 175°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 143.9 grams of biodegradable polyolefin EVA.
[0103] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 15.8 × 10⁻⁶. 4 g / mol, density 0.903 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.7% oxygen ether groups and 5.8% hexyl methacrylate groups by mass. 13 C10 NMR analysis results show signals at chemical shifts δ=70.8 and 74.8 ppm, indicating the presence of COC bonds in the polymer structure. These COC bonds originate from the free radical polymerization of the aldehyde trioxymethylene. Signals at δ=74.3 and 170.3 ppm originate from the VA group of EVA. Signals at δ=71.5 and 170.3 ppm originate from the VA group adjacent to the CO group in the VA-CO-VA chain segment. Signals at δ=74.8 and 74.8 ppm originate from the carbon atom signal of the CO group in the VA-CO-VA chain segment. Signals at δ=46.8, 65.3, and 173.2 ppm indicate the presence of ester bonds in the polymer structure. These ester bonds originate from the free radical polymerization of hexyl methacrylate.
[0104] Example 20
[0105] The raw materials, trioxymethylene, vinyl acetate, and initiator di-tert-butyl peroxide, were stored separately in raw material storage tanks at room temperature; the recycled PP was stored in a polyolefin storage tank at 200°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05 g of initiator di-tert-butyl peroxide, 3 g of trioxymethylene, and 4.1 g of vinyl acetate at a preparation temperature of 25°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 130g of recycled polyolefin (PP) from the polyolefin storage tank, and take 20g of paraformaldehyde and 18g of vinyl acetate from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 200℃, and mix thoroughly. Take 7.15g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 30 rpm, temperature at 200℃, and pressure at 1.6MPa in the polymerization reactor for 18 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 190°C for 30 minutes. Then, the biodegradable polyolefin (PP) was added to a twin-screw extruder at a temperature of 185°C in both the first and second sections for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 149.6 grams of biodegradable polyolefin (PP).
[0106] The biodegradable polyolefin prepared in this embodiment has a weight-average molecular weight of 19.0 × 10⁻⁶. 4 g / mol, density 0.901 g / cm³ 3 The biodegradable polyolefin molecular chain contains 4.9% oxygen ether groups and 9.1% vinyl acetate by mass. 13 The 10⁻⁶ C NMR analysis results show that the presence of signals at chemical shifts δ=70.6 and 74.9 ppm indicates that the polymer structure contains COC bonds, which are derived from the free radical polymerization of the alkyl aldehyde paraformaldehyde; the presence of signals at δ=71.4 and 170.3 ppm indicates that the polymer structure contains ester bonds, which are derived from the free radical polymerization of butyl acrylate.
[0107] Example 21
[0108] The raw materials, trioxymethylene, vinyl acetate, toluene solvent, and di-tert-butyl peroxide initiator were stored separately in raw material storage tanks at room temperature; the recycled PVC was stored in a polyolefin storage tank at 210°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by mixing 0.05 g of di-tert-butyl peroxide initiator, 3 g of trioxymethylene, and 3 g of acrylic acid at a preparation temperature of 30°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 150g of recycled PVC polyolefin from the polyolefin storage tank, and take 20g of paraformaldehyde, 18g of vinyl acetate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 200℃, and mix thoroughly. Take 6.05g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 30 rpm, temperature at 200℃, and pressure at 1.6MPa in the polymerization reactor for 18 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 190°C for 30 minutes. Then, the biodegradable polyolefin PVC was added to a twin-screw extruder with a first-stage temperature of 185°C and a second-stage temperature of 185°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 170.7 grams of biodegradable polyolefin PVC.
[0109] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 7.5 × 10⁻⁶. 4 g / mol, density 0.981 g / cm³ 3 The biodegradable polyolefin molecular chain contains 5.6% by mass of oxygen ether groups, 7.3% by mass of vinyl acetate, and 2.6% by mass of acrylic acid. 13 The 12C NMR analysis results show that the presence of signals at chemical shifts δ=70.7 and 74.7 ppm indicates that the polymer structure contains COC bonds, which originate from the free radical polymerization of aldehydes; the signals at δ=62.5-63.2 ppm belong to the vinyl chloride structural unit; and the presence of signals at δ=71.5 and 170.2 ppm indicates that the polymer structure contains ester bonds, which originate from the free radical polymerization of vinyl acetate.
[0110] Example 22
[0111] The raw materials, trioxymethylene, acrylic acid, toluene solvent, and di-tert-butyl peroxide initiator were stored in separate raw material storage tanks at room temperature; the recycled PS was stored in a polyolefin storage tank at 190°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by mixing 0.05 g of di-tert-butyl peroxide initiator, 3 g of trioxymethylene, and 3 g of acrylic acid at a preparation temperature of 30°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. 155g of recycled polyolefin (PS) was taken from the polyolefin storage tank. 20g of paraformaldehyde, 18g of acrylic acid, and 5g of solvent were taken from the raw material storage tank and added to the polymerization reactor. The mixture was stirred at 30 rpm and heated to 200°C until homogeneous. 6.05g of free radical initiator material was taken from the free radical initiator material preparation tank and added to the polymerization reactor. The polymerization reactor was maintained at 30 rpm, 200°C, and 1.6 MPa for 18 hours for copolymerization. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 190°C for 30 minutes. Then, the biodegradable polyolefin PS was added to a twin-screw extruder with a first-stage temperature of 185°C and a second-stage temperature of 185°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 173.4 grams of biodegradable polyolefin PS.
[0112] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 8.3 × 10⁻⁶. 4 g / mol, density 1.091 g / cm³ 3 The biodegradable polyolefin molecular chain contains 5.2% oxygen ether groups and 6.4% acrylic acid by mass. 13 C10 NMR analysis results show signals at chemical shifts δ=70.3 and 74.6 ppm, indicating the presence of COC bonds in the polymer structure, which originate from free radical polymerization of aldehydes; signals at δ=45.2-46.2 ppm, 141.8, and 126-128.8 ppm belong to styrene structural units; signals at δ=73.5 and 173.7 ppm indicate the presence of ester bonds in the polymer structure, which originate from free radical polymerization of acrylic acid.
[0113] Example 23
[0114] The raw materials, trioxymethylene, methyl methacrylate, toluene, and di-tert-butyl peroxide initiator were stored separately in raw material storage tanks at room temperature; ethylene oligomer (polyethylene wax, CAS No. 9002-88-4) with a molecular weight of 3000 was stored in a polyolefin storage tank at 60°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, prepared by using 0.05 g of di-tert-butyl peroxide initiator, 4 g of trioxymethylene, and 2.5 g of methyl methacrylate, at a preparation temperature of 35°C, an operating pressure of 0.5 MPa, and a preparation time of 1 h. Take 125g of ethylene oligomer from the polyolefin storage tank, and take 20g of paraformaldehyde, 18g of methyl methacrylate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 90℃, and mix thoroughly. Take 6.55g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 30 rpm, temperature at 90℃, and pressure at 2.1MPa in the polymerization reactor for copolymerization reaction for 18h. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 190°C for 30 minutes. Then, the biodegradable polyolefin was added to a twin-screw extruder with a first-stage temperature of 185°C and a second-stage temperature of 185°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 134.7 grams of biodegradable polyolefin.
[0115] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 8.4 × 10⁻⁶. 4 g / mol, density 0.897 g / cm³ 3 The biodegradable polyolefin molecular chain contains 5.8% oxygen ether groups and 6.2% methyl methacrylate groups by mass. 13The 10⁻⁶ C NMR analysis results show that the presence of signals at chemical shifts δ=70.7 and 74.9 ppm indicates that the polymer structure contains COC bonds, which are derived from free radical polymerization of aldehydes; the presence of signals at δ=71.9 and 170.3 ppm indicates that the polymer structure contains ester bonds, which are derived from free radical polymerization of methyl methacrylate.
[0116] Example 24
[0117] The raw materials, trioxymethylene, vinyl acetate, toluene solvent, and di-tert-butyl peroxide initiator were stored separately in raw material storage tanks at room temperature; the C8 mixed olefin raw material (refining by-product, domestic refining and chemical company) was stored in a polyolefin storage tank at 60°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05 g of di-tert-butyl peroxide initiator, 3 g of trioxymethylene, and 1.95 g of vinyl acetate, at a preparation temperature of 35°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 100g of C8 mixed olefin from the polyolefin storage tank, and take 20g of paraformaldehyde, 18g of vinyl acetate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 70℃, and stir until homogeneous. Take 5.0g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 30 rpm, temperature at 70℃, and pressure at 2.1MPa in the polymerization reactor for copolymerization reaction for 18h. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 190°C for 30 minutes. Then, the biodegradable polyolefin was added to a twin-screw extruder at a temperature of 185°C in both the first and second sections for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 109.1 grams of biodegradable polyolefin.
[0118] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 10.8 × 10⁻⁶. 4 g / mol, density 0.896 g / cm³ 3 The biodegradable polyolefin molecular chain contains 5.2% oxygen ether groups and 6.1% vinyl acetate by mass. 13 The 10⁻⁶ C NMR analysis results show that the presence of signals at chemical shifts δ=70.3 and 74.8 ppm indicates that the polymer structure contains COC bonds, which are derived from the free radical polymerization of the alkyl aldehyde paraformaldehyde; the presence of signals at δ=71.6 and 170.2 ppm indicates that the polymer structure contains ester bonds, which are derived from the free radical polymerization of butyl acrylate.
[0119] Example 25
[0120] The raw materials, trioxymethylene, vinyl acetate, trifluoroacetic acid solvent, and AIBN initiator were stored separately in raw material storage tanks at room temperature; C5 mixed olefins (refining by-products from domestic refining companies) were stored in polyolefin storage tanks at 50°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, prepared using 0.05 g of initiator AIBN, 3 g of trioxymethylene, and 3.5 g of vinyl acetate at a preparation temperature of 35°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 100g of C5 mixed olefin from the polyolefin storage tank, and take 20g of paraformaldehyde, 18g of vinyl acetate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 60℃, and stir until homogeneous. Take 6.55g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 30 rpm, temperature at 60℃, and pressure at 2.1MPa in the polymerization reactor for copolymerization reaction for 20h. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 150°C for 30 minutes. Then, the biodegradable polyolefin was added to a twin-screw extruder with a first-stage temperature of 185°C and a second-stage temperature of 185°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 87.8 grams of biodegradable polyolefin.
[0121] The biodegradable polyolefin prepared in this embodiment has a weight-average molecular weight of 19.0 × 10⁻⁶. 4 g / mol, density 0.892 g / cm³ 3 The biodegradable polyolefin molecular chain contains 6.4% oxygen ether groups and 7.6% vinyl acetate by mass. 13 The 10⁻⁶ C NMR analysis results show that the presence of signals at chemical shifts δ=70.3 and 74.5 ppm indicates that the polymer structure contains COC bonds, which are derived from the free radical polymerization of the alkyl aldehyde paraformaldehyde; the presence of signals at δ=71.2 and 170.4 ppm indicates that the polymer structure contains ester bonds, which are derived from the free radical polymerization of butyl acrylate.
[0122] Example 26
[0123] The raw materials, trioxymethylene, vinyl acetate, hexafluoropropanol, and initiator AIBN, were stored in separate raw material storage tanks at room temperature. C6 mixed olefins (refining by-products from domestic refining companies) were stored in polyolefin storage tanks at 50°C with stirring. The free radical initiator material was stored in a free radical initiator material preparation tank, prepared using 0.05 g of initiator AIBN, 3 g of trioxymethylene, and 3.5 g of vinyl acetate at a preparation temperature of 35°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 100g of C6 mixed olefins from the polyolefin storage tank, and take 20g of paraformaldehyde, 18g of vinyl acetate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 60℃, and stir until homogeneous. Take 6.55g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 30 rpm, temperature at 60℃, and pressure at 2.1MPa in the polymerization reactor for copolymerization reaction for 18h. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 150°C for 30 minutes. Then, the biodegradable polyolefin was added to a twin-screw extruder with a first-stage temperature of 185°C and a second-stage temperature of 185°C for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 89.2 grams of biodegradable polyolefin.
[0124] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 18.8 × 10⁻⁶. 4 g / mol, density 0.891 g / cm³ 3 The biodegradable polyolefin molecular chain contains 7.1% oxygen ether groups and 8.3% vinyl acetate by mass. 13 The 10⁻⁶ C NMR analysis results show that the presence of signals at chemical shifts δ=70.7 and 74.1 ppm indicates that the polymer structure contains COC bonds, which are derived from the free radical polymerization of the alkyl aldehyde trioxymethylene; the presence of signals at δ=71.2 and 170.0 ppm indicates that the polymer structure contains ester bonds, which are derived from the free radical polymerization of butyl acrylate.
[0125] Example 27
[0126] The raw materials, trioxymethylene, vinyl acetate, toluene, and di-tert-butyl peroxide, were stored separately in raw material storage tanks at room temperature; the recycled POE was stored in a polyolefin storage tank at 150°C with stirring; the free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared by using 0.05 g of di-tert-butyl peroxide initiator, 3 g of trioxymethylene, and 3.5 g of vinyl acetate, at a preparation temperature of 25°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 100g of recycled POE from the polyolefin storage tank, and take 20g of paraformaldehyde, 18g of vinyl acetate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 160℃, and mix thoroughly. Take 6.55g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 30 rpm, temperature at 160℃, and pressure at 0.5MPa in the polymerization reactor for copolymerization reaction for 21h. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 160°C for 30 minutes. Then, the biodegradable polyolefin was added to a twin-screw extruder at a temperature of 165°C in both the first and second sections for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 115.7 grams of biodegradable polyolefin.
[0127] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 12.5 × 10⁻⁶. 4 g / mol, density 0.882 g / cm³ 3 The biodegradable polyolefin molecular chain contains 6.3% oxygen ether groups and 7.1% vinyl acetate by mass. 13 The 10⁻⁶ C NMR analysis results show that the presence of signals at chemical shifts δ=70.3 and 74.7 ppm indicates that the polymer structure contains COC bonds, which are derived from the free radical polymerization of the alkyl aldehyde paraformaldehyde; the presence of signals at δ=71.6 and 170.2 ppm indicates that the polymer structure contains ester bonds, which are derived from the free radical polymerization of butyl acrylate.
[0128] Example 28
[0129] The raw materials, trioxymethylene, vinyl acetate, toluene, and di-tert-butyl peroxide, were stored in separate raw material storage tanks at room temperature. The recycled EVA was stored in a polyolefin storage tank at 175°C with stirring. The free radical initiator material was stored in a free radical initiator material preparation tank, which was prepared using 0.05 g of di-tert-butyl peroxide initiator, 3 g of trioxymethylene, and 3.5 g of vinyl acetate at a preparation temperature of 35°C, an operating pressure of 0.5 MPa, and a preparation time of 1 hour. Take 100g of recycled EVA from the polyolefin storage tank, and take 20g of paraformaldehyde, 18g of vinyl acetate, and 5g of solvent from the raw material storage tank. Add them to the polymerization reactor, stir at 30 rpm, heat to 180℃, and mix thoroughly. Take 6.55g of free radical initiator material from the free radical initiator material preparation tank and add it to the polymerization reactor. Maintain stirring at 30 rpm, temperature at 180℃, and pressure at 0.5MPa in the polymerization reactor for copolymerization reaction for 25h. The polymerization product in the polymerization reactor was transferred to a devolatilizer for devolatilization at a temperature of 165°C for 30 minutes. Then, the biodegradable polyolefin was added to a twin-screw extruder at a temperature of 175°C in both the first and second sections for 3.5 minutes. After cooling with cold water, the product was pelletized and dried to obtain 119.6 grams of biodegradable polyolefin.
[0130] The weight-average molecular weight of the biodegradable polyolefin prepared in this embodiment is 17.3 × 10⁻⁶. 4 g / mol, density 0.891 g / cm³3 The biodegradable polyolefin molecular chain contains 8.3% oxygen ether groups and 8.7% vinyl acetate by mass. 13 The 10⁻⁶ C NMR analysis results show that the presence of signals at chemical shifts δ=70.7 and 74.9 ppm indicates that the polymer structure contains COC bonds, which are derived from free radical polymerization of aldehydes; the presence of signals at δ=71.4 and 170.6 ppm indicates that the polymer structure contains ester bonds, which are derived from free radical polymerization of vinyl acetate.
[0131] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a biodegradable polyolefin material, characterized in that, Includes the following steps: Biodegradable polyolefin materials are obtained by mixing polyolefins, organic aldehydes, vinyl organic esters and free radical initiators using liquid-phase bulk polymerization, solution polymerization or emulsion polymerization.
2. The preparation method according to claim 1, characterized in that, The mass ratio of the polyolefin, organic aldehyde, vinyl organic ester and initiator is 100:(0.05~30):(0.2~75):(0.01~5).
3. The preparation method according to claim 1 or 2, characterized in that, The polyolefins include polyethylene, polypropylene, polystyrene, EVA, EMMA, EAA, ABS, HIPS, PVC, EPR, EPDM, NBR, HNBR, SBS, SIS, SEBS, SEIS, SIBR, ESBR, SSBR, IIR, IR, NR, CR, or any of the above-mentioned recycled polyolefins, or low-value olefin oligomers, or bio-based non-degradable polyolefins, or non-metallic materials from waste fans.
4. The preparation method according to claim 1 or 2, characterized in that, The organic aldehyde has 1 to 10 carbon atoms; the organic aldehyde includes one or more of formaldehyde, trioxymethylene, benzaldehyde, butyraldehyde, acetaldehyde and propionaldehyde.
5. The preparation method according to claim 1 or 2, characterized in that, The vinyl organic ester has 2 to 20 carbon atoms; the vinyl organic ester includes one or more of vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate, vinyl hexanoate, vinyl octanoate, vinyl undecenoate, methyl acrylate, methyl methacrylate, acrylic acid, butyl acrylate, hexyl methacrylate, fluorobutyl methacrylate, and hexyl acrylate.
6. The preparation method according to claim 1 or 2, characterized in that, The free radical initiator includes one or more of azo initiators and organic peroxide initiators.
7. The preparation method according to claim 1 or 2, characterized in that, When liquid-phase bulk polymerization is used, the temperature of the free radical copolymerization reaction is 50~280℃, the pressure is 0.2~5 MPa, and the reaction time is 0.5~45h; When solution polymerization is used, the process further includes adding a first solvent in the mixing step. The free radical copolymerization reaction is carried out at a temperature of 50–280°C, a pressure of 0.2–5 MPa, and a reaction time of 0.5–45 h. The mass ratio of the polyolefin to the first solvent is 100:(0.1–1500), and the first solvent comprises C5-C... 20 Inert organic solvents or C5-C 20 Halogenated organic solvents; When emulsion polymerization is used, the process further includes adding an emulsifier and a second solvent in the mixing step; the free radical copolymerization reaction is carried out at a temperature of 50~180℃, a pressure of 0.2~5 MPa, and a reaction time of 0.5~45 h; the mass ratio of the polyolefin, emulsifier, and second solvent is 100:(0.05~1):(50~1500); the second solvent includes water and C5-C... 20 Inert organic solvents or C5-C 20 Halogenated organic solvents.
8. The preparation method according to claim 1 or 2, characterized in that, The mixing of polyolefin, organic aldehyde, vinyl organic acid ester and free radical initiator includes: adding 80-95% by mass of organic aldehyde, 80-95% by mass of vinyl organic acid ester and all of the polyolefin from the raw material storage tank into the polymerization reactor; adding the remaining 5-20% by mass of organic aldehyde and 5-20% by mass of vinyl organic acid ester and all of the free radical initiator from the raw material storage tank into the free radical initiator material preparation tank, and then adding the free radical initiator material preparation tank into the polymerization reactor to carry out free radical copolymerization reaction.
9. The biodegradable polyolefin material prepared by the preparation method according to any one of claims 1 to 8, characterized in that, The molecular weight of the biodegradable polyolefin material is 0.1~100×10⁻⁶. 4 g / mol, density 0.860~1.166 g / cm³ 3 .
10. The application of the biodegradable polyolefin material of claim 9 in aerospace, power batteries, ship cables, nuclear reactors, automobiles, construction, communications, clothing, electronics, drones, agriculture, or daily use.
Citation Information
Patent Citations
Degradable polyolefin masterbatch and production method thereof
CN102504347A
Degradable polyolefin functional master batch and preparation method thereof
CN119119632A
Bio-based degradable polyolefin alloy material and preparation method thereof
CN121226885A
Degradable polyethylene master batch, preparation method and degradable linear low-density polyethylene
CN121343268A