A high-transparency, weather-resistant, flexible polyurethane acrylate resin for 3D printing
By introducing sterically hindered urea bonds and all-alicyclic raw materials into the polyurethane acrylate backbone, the problems of transparency and weather resistance of DLP printing resin were solved, achieving high light transmittance and long-term optical stability. It also has self-healing and recyclable functions, which is in line with the concept of green chemistry.
Patent Information
- Application Number
- CN202611147961.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-30
- Publication Date
- 2026-11-17
AI Technical Summary
The transparency of existing polyurethane acrylate photosensitive resins in DLP printing is limited by microphase separation caused by hard segment aggregation, and their weather resistance and anti-yellowing properties are insufficient, making it difficult to meet the requirements of high light transmittance and long-term optical stability.
By introducing sterically hindered urea bonds into the polyurethane acrylate backbone and using a fully alicyclic raw material system, combined with benzotriazole UV absorbers and hindered amine light stabilizers, the resin is endowed with repairable and recyclable functions through dynamic covalent properties, and light scattering is eliminated by utilizing the refractive index matching of the alicyclic hard and soft segments.
It achieves high light transmittance (over 90% transmittance of visible light at 550nm), excellent weather resistance (yellowing index ΔE≤1.5), self-healing and secondary reshaping capabilities, and meets the requirements of green chemistry.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photopolymer 3D printing materials technology, specifically relating to a high-transmittance, weather-resistant polyurethane acrylate flexible photosensitive resin suitable for digital light processing (DLP) printing and its preparation method. Background Technology
[0002] Digital Light Processing (DLP) 3D printing technology has broad application prospects in flexible electronics, optical devices, and biomedicine due to its high forming accuracy and speed. Polyurethane acrylate (PUA) photosensitive resin has become the main choice for DLP printing flexible materials due to its adjustable mechanical properties, fast curing speed, and good weather resistance. However, traditional polyether / polyester type polyurethane acrylate oligomers, due to the thermodynamic incompatibility of the soft and hard segments, easily form microphase separation structures inside the material after curing, with the size of the hard segment micro-regions often reaching hundreds of nanometers. The refractive index difference between these micro-regions and the soft segment matrix causes significant light scattering, resulting in whitening and translucency of the material, severely limiting its application in optical lenses, transparent medical models, and other fields. At the same time, aromatic isocyanate systems are prone to yellowing under light or heat, affecting the long-term optical stability and weather resistance of the products.
[0003] To address the aforementioned issues, existing research has attempted to introduce dynamic covalent bonds into polyurethane acrylate systems. Li Yinghao, Wang Xinling, and others synthesized functionalized polyurethane acrylates containing sterically hindered urea bonds. Studies showed that these sterically hindered urea bonds exhibit an endothermic effect at 46–56 °C, and the system possesses the characteristics of a dynamic covalent polymer, resulting in good repair performance of the cured photosensitive resin. Kong Siyu et al. designed and prepared a photosensitive polyurethane acrylate (PUTA) containing multiple sterically hindered urea bonds and crystalline soft segments. The photocured material exhibited high elasticity, good mechanical properties, self-healing properties, and shape memory properties. Other studies have synthesized novel polyurethane acrylate photosensitive resins by introducing unsaturated double bonds and thermally driven reversible urea bonds, using 4,4'-diaminodicyclohexylmethane (PACM) as a chain extender. Zeng Ze et al. synthesized a novel photocurable polyurethane acrylate using isophorone diamine (IPDA), isophorone diisocyanate (IPDI), and hydroxyethyl acrylate (HEA) as raw materials.
[0004] However, the aforementioned studies mainly focus on the dynamic covalent properties of urea bonds (self-healing, shape memory, recyclability, etc.), and have not yet systematically solved the problem of synergistic optimization of high light transmittance and weather resistance in urea-bonded polyurethane acrylates for DLP printing. In existing technologies, the transparency of urea-bonded polyurethane acrylate photosensitive resins is still limited by microphase separation caused by hard segment aggregation, and most studies still use isocyanates containing aromatic structures, resulting in insufficient weather resistance and anti-yellowing properties. Therefore, developing DLP printing resins that combine high light transmittance, excellent weather resistance, and flexibility remains a technical challenge in this field. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a high-transmittance and weather-resistant flexible polyurethane acrylate resin for 3D printing and its preparation method. By introducing sterically hindered urea bonds into the polyurethane acrylate main chain and combining it with a fully alicyclic raw material system, the problems of light transmittance and weather resistance are fundamentally solved. At the same time, the dynamic thermal response characteristics of the sterically hindered urea bonds endow the resin with repairable and recyclable functions.
[0006] To achieve the above objectives, the present invention adopts the following technical solution.
[0007] A high-transparency, weather-resistant, flexible polyurethane acrylate resin for 3D printing, comprising the following components by weight: 50-75 parts of polyurethane acrylate oligomer containing urea bonds; 20-45 parts of reactive diluent; Photoinitiator 0.5-5 parts; Additives: 0.1-3 parts.
[0008] The polyurethane acrylate oligomer containing urea bonds has acrylate double bonds at both ends of its molecular chain, and the main chain consists of polyether soft segments and hard segments containing sterically hindered urea bonds. The sterically hindered urea bonds exhibit reversible dissociation-recombination characteristics in a temperature range of 46~56℃, endowing the photosensitive resin with dynamic covalent polymer properties and repair performance.
[0009] The urea-containing polyurethane acrylate oligomer is prepared by the following method: S1: Dehydration of polyether polyol The polyether polyol is vacuum dehydrated at 100-120°C for 1-2 hours. The polyether polyol is polytetrahydrofuran ether diol or polypropylene glycol with a number average molecular weight of 1000-3000.
[0010] S2: Synthesis of isocyanate-terminated prepolymers The polyether polyol obtained in S1 was cooled to 50-60°C, and an alicyclic diisocyanate was added. The molar ratio of isocyanate groups to hydroxyl groups was controlled at 1.8-2.2, and the mixture was reacted at 75-85°C for 2-3 hours to obtain a prepolymer with terminal isocyanate groups. The preferred alicyclic diisocyanate is isophorone diisocyanate (IPDI). Studies have shown that polyurethane acrylates based on alicyclic diisocyanates exhibit better optical properties than systems based on aromatic diisocyanates, mainly due to the lower refractive index of the alicyclic hard segments. The lower refractive index of the alicyclic hard segments compared to aromatic hard segments effectively reduces light scattering and improves the light transmittance of the material.
[0011] S3: Introduction of steric urea-blocking bonds The isocyanate-terminated prepolymer obtained from S2 is cooled to 40-50°C, and a sterically hindered alicyclic diamine solution in acetone is slowly added dropwise. The molar ratio of amino groups to remaining isocyanate groups is controlled at 0.4-0.6. The reaction is rapidly stirred for 0.5-1 hour to introduce sterically hindered urea bonds into the chain segments. The sterically hindered alicyclic diamine is 4,4'-diaminodicyclohexylmethane (PACM) or isophorone diamine (IPDA). The steric hindrance effect of the sterically hindered urea bonds can effectively suppress excessive aggregation of hard segments, control the microphase separation scale to a range much smaller than the visible light wavelength (<50nm), thereby eliminating light scattering and achieving high light transmittance.
[0012] S4: Acrylic end-capped Add a capping agent, which is hydroxyethyl acrylate or hydroxypropyl acrylate, to the reaction system obtained in S3. The amount of the capping agent is 1.02 to 1.1 times the molar amount of the remaining isocyanate group. React at 60 to 70°C until the characteristic peak of the isocyanate group at 2270 cm⁻¹ in the infrared spectrum completely disappears.
[0013] S5: Solvent Removal The reaction system obtained in S4 was subjected to vacuum distillation to remove acetone, yielding a polyurethane acrylate oligomer containing sterically hindered urea bonds.
[0014] The active diluent is composed of a monofunctional diluent and a difunctional diluent, wherein the monofunctional diluent is 3-8 parts of hydroxyethyl acrylate and 8-15 parts of isobornyl acrylate, and the difunctional diluent is 5-15 parts of tricyclodecanedimethyl diacrylate and 3-8 parts of polypropylene glycol diacrylate.
[0015] The photoinitiator is an acylphosphine oxide photoinitiator, selected from one or two of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide or ethyl 2,4,6-trimethylbenzoylphosphonate, and is used in an amount of 1 to 3 parts to match a 385 to 405 nm DLP light source.
[0016] The additives include 0.1-0.5 parts of benzotriazole UV absorber, 0.1-0.5 parts of hindered amine light stabilizer, and 0.1-1 parts of silicone defoaming and leveling agent. The synergistic use of benzotriazole UV absorber and hindered amine light stabilizer can effectively improve the weather resistance of materials under long-term ultraviolet light exposure.
[0017] S6: Final Synthesis ① Mixing and dissolving The polyurethane acrylate oligomer containing sterically hindered urea bonds obtained in S5 was stirred and mixed with an active diluent at 30-40°C for 1-2 hours to form a homogeneous solution. ② Addition of initiators and auxiliaries Add photoinitiator and additives to the homogeneous solution obtained in step ①, and disperse by high-speed stirring at 1000~1500 rpm for 30 minutes under light-protected conditions to obtain a photosensitive resin mixture. ③ Filtration and Degassing After filtering the photosensitive resin mixture obtained in step ② through a glass fiber filter with a pore size of 1 μm, it was allowed to stand in the dark and then vacuum degassed for 24 hours to obtain a polyurethane acrylate photosensitive resin containing sterically hindered urea bonds. After the photosensitive resin is formed by DLP 3D printing, it is heat-treated at 80°C for 0.5 to 2 hours to trigger the dynamic thermal response of the sterically hindered urea bonds, thereby realizing the rearrangement of the network topology of the printed part. At the same time, the refractive index matching effect of the alicyclic hard segment and soft segment is used to eliminate light scattering, so that the transmittance of 550nm visible light is not less than 90%.
[0018] After being 3D printed using DLP, the photosensitive resin is heat-treated at 80°C for 0.5–2 hours to trigger the dynamic thermal response of the sterically hindered urea bonds, thereby achieving a rearrangement of the network topology of the printed part. Studies have shown that the photosensitive resin containing sterically hindered urea bonds exhibits excellent shape memory and secondary shaping capabilities.
[0019] Compared with the prior art, the present invention has the following beneficial effects: (1) High light transmittance. This invention introduces sterically hindered urea bonds into the polyurethane acrylate backbone, utilizing their weak hydrogen bonding to suppress excessive aggregation of hard segments and control the microphase separation scale to a range much smaller than the visible light wavelength (<50nm), effectively eliminating light scattering. Simultaneously, the use of alicyclic diisocyanate (IPDI), whose alicyclic hard segment refractive index is lower than that of aromatic hard segments, further reduces light scattering. The cured product achieves a visible light transmittance of over 90% at 550nm, meeting the application requirements of optical-grade transparent parts.
[0020] (2) Excellent weather resistance. This invention uses a fully alicyclic raw material system (alicyclic diisocyanate + alicyclic diamine), which completely avoids the formation of conjugated chromophores in aromatic isocyanate systems from a molecular structure perspective. Combined with the synergistic stabilization system of benzotriazole UV absorbers and hindered amine light stabilizers, the accelerated aging yellowing index ΔE ≤ 1.5, which is much lower than that of aromatic systems (ΔE > 8), resulting in excellent optical stability of the product during long-term outdoor use.
[0021] (3) Dynamic covalent properties endow the material with repair and recyclability. The sterically hindered urea bonds introduced in this invention exhibit reversible dissociation-recombination characteristics at 46~56℃, and the system possesses the characteristics of a dynamic covalent polymer. The cured photosensitive resin exhibits good repair performance, and the tensile strength of the repaired sample can be restored from 13.8MPa to 18.4MPa. After heat treatment at 80℃, the sterically hindered urea bonds undergo dynamic thermal response, enabling network topology rearrangement and endowing the material with self-repair and secondary shaping capabilities.
[0022] (4) Adjustable mechanical properties and good printability. By adjusting the oligomer molecular weight and diluent ratio, the tensile strength can be flexibly adjusted within the range of 8~13MPa, the elongation at break within the range of 150~300%, and the hardness within the range of Shore A60~90. The resin viscosity is moderate, which is well matched with the DLP process. It can be cured and molded quickly, and the printing accuracy is high, meeting the different needs of flexible devices and transparent models.
[0023] (5) Green and environmentally friendly. This invention adopts a fully alicyclic system, avoiding the toxicity problem of aromatic isocyanates. The dynamic reversible properties of the sterically hindered urea bonds make the material recyclable, which is in line with the concept of green chemistry and sustainable development. Detailed Implementation
[0024] The present invention will be further described in detail below with reference to specific embodiments, but the implementation of the present invention is not limited thereto. Example
[0025] S1: Dehydration of polyether polyol 100g of polytetrahydrofuran ether diol (PTMG) with a number average molecular weight of 2000 was placed in a three-necked flask and dehydrated under vacuum at 110°C for 1.5 hours.
[0026] S2: Synthesis of isocyanate-terminated prepolymers The PTMG obtained from S1 was cooled to 55°C, and isophorone diisocyanate (IPDI) was added. The molar ratio of NCO to OH was controlled to be 2.0, and the reaction was carried out at 80°C for 2.5 hours to obtain the terminal isocyanate prepolymer.
[0027] S3: Introduction of steric urea-blocking bonds The isocyanate-terminated prepolymer obtained from S2 was cooled to 45°C, and an acetone solution of 4,4'-diaminodicyclohexylmethane (PACM) was slowly added dropwise. The molar ratio of NH2 to the remaining NCO was controlled at 0.5, and the reaction was stirred rapidly for 0.75 hours to introduce sterically hindered urea bonds into the chain segment.
[0028] S4: Acrylic end-capped Hydroxyethyl acrylate (HEA) was added to the reaction system obtained in S3, with the amount being 1.05 times the remaining molar amount of NCO. The reaction was carried out at 65°C until the characteristic peak of NCO at 2270 cm⁻¹ in the infrared spectrum completely disappeared.
[0029] S5: Solvent Removal The reaction system obtained in S4 was subjected to vacuum distillation to remove acetone, yielding a polyurethane acrylate oligomer containing sterically hindered urea bonds.
[0030] S6: Mixed Dissolution Weigh 65 parts by weight of the oligomer obtained from S5, add reactive diluent (5 parts HEA, 12 parts IBOA, 10 parts TCDDA, and 6 parts PPGDA), and stir and mix at 35°C for 1.5 hours to form a homogeneous solution.
[0031] S7: Initiator and Additive Addition Add 2 parts of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 0.3 parts of benzotriazole ultraviolet absorber, 0.3 parts of hindered amine light stabilizer, and 0.5 parts of organosilicon defoaming and leveling agent to the homogeneous solution obtained in S6. Stir and disperse at high speed of 1200 rpm for 30 minutes under light-protected conditions to obtain a photosensitive resin mixture.
[0032] S8: Filtration and Degassing The photosensitive resin mixture obtained from S7 was filtered through a glass fiber filter with a pore size of 1μm, then allowed to stand in the dark and vacuum degassed for 24 hours to obtain a high-transparency, weather-resistant polyurethane acrylate flexible resin for 3D printing.
[0033] The photosensitive resin obtained in this embodiment was used for DLP 3D printing and then heat-treated at 80°C for 1 hour. Testing showed that the cured product had a 550nm visible light transmittance of 92%, a tensile strength of 10.5 MPa, an elongation at break of 220%, and a Shore A hardness of 75. The sterically hindered urea bonds exhibit an endothermic effect at 46-56°C, and the system possesses the characteristics of a dynamic covalent polymer. The tensile strength of the repaired sample recovered well. After accelerated aging (72 hours of UV irradiation), the yellowing index ΔE = 1.2. Example
[0034] S1: Dehydration of polyether polyol 100g of polypropylene glycol (PPG) with a number average molecular weight of 1000 was placed in a three-necked flask and dehydrated under vacuum at 100°C for 2 hours.
[0035] S2: Synthesis of isocyanate-terminated prepolymers The PPG obtained from S1 was cooled to 50°C, and isophorone diisocyanate (IPDI) was added. The molar ratio of NCO to OH was controlled at 1.8, and the mixture was reacted at 75°C for 3 hours to obtain the terminal isocyanate prepolymer.
[0036] S3: Introduction of steric urea-blocking bonds The isocyanate-terminated prepolymer obtained from S2 was cooled to 40°C, and an acetone solution of isophorone diamine (IPDA) was slowly added dropwise. The molar ratio of NH2 to the remaining NCO was controlled at 0.4, and the reaction was stirred rapidly for 1 hour to introduce sterically hindered urea bonds into the chain segment.
[0037] S4: Acrylic end-capped Hydroxypropyl acrylate (HPA) was added to the reaction system obtained in S3, with the amount being 1.02 times the remaining molar amount of NCO. The reaction was carried out at 60°C until the characteristic peak of NCO at 2270 cm⁻¹ in the infrared spectrum completely disappeared.
[0038] S5: Solvent Removal The reaction system obtained in S4 was subjected to vacuum distillation to remove acetone, yielding a polyurethane acrylate oligomer containing sterically hindered urea bonds.
[0039] S6: Mixed Dissolution Weigh 50 parts by weight of the oligomer obtained from S5, add reactive diluent (3 parts HEA, 8 parts IBOA, 5 parts TCDDA, and 4 parts PPGDA), and stir and mix at 30°C for 2 hours to form a homogeneous solution.
[0040] S7: Initiator and Additive Addition Add 1 part of ethyl 2,4,6-trimethylbenzoylphosphonate, 0.1 part of benzotriazole ultraviolet absorber, 0.1 part of hindered amine light stabilizer, and 0.1 part of organosilicon defoaming and leveling agent to the homogeneous solution obtained in S6. Stir and disperse at high speed of 1000 rpm for 30 minutes under light-protected conditions to obtain a photosensitive resin mixture.
[0041] S8: Filtration and Degassing The photosensitive resin mixture obtained from S7 was filtered through a glass fiber filter with a pore size of 1μm, then allowed to stand in the dark and vacuum degassed for 24 hours to obtain a high-transparency, weather-resistant polyurethane acrylate flexible resin for 3D printing.
[0042] The photosensitive resin obtained in this embodiment was used for DLP 3D printing and then heat-treated at 80°C for 0.5 hours. Testing showed that the cured product had a 550nm visible light transmittance of 90%, a tensile strength of 8.5 MPa, an elongation at break of 180%, and a Shore A hardness of 65. After accelerated aging, the yellowing index ΔE = 1.5. Example
[0043] S1: Dehydration of polyether polyol 100g of polytetrahydrofuran ether diol (PTMG) with a number average molecular weight of 3000 was placed in a three-necked flask and dehydrated under vacuum at 120°C for 1 hour.
[0044] S2: Synthesis of isocyanate-terminated prepolymers The PTMG obtained from S1 was cooled to 60°C, and isophorone diisocyanate (IPDI) was added. The molar ratio of NCO to OH was controlled at 2.2, and the mixture was reacted at 85°C for 2 hours to obtain the terminal isocyanate prepolymer.
[0045] S3: Introduction of steric urea-blocking bonds The isocyanate-terminated prepolymer obtained from S2 was cooled to 50°C, and an acetone solution of 4,4'-diaminodicyclohexylmethane (PACM) was slowly added dropwise. The molar ratio of NH2 to the remaining NCO was controlled at 0.6, and the reaction was stirred rapidly for 0.5 hours to introduce sterically hindered urea bonds into the chain segment.
[0046] S4: Acrylic end-capped Hydroxyethyl acrylate (HEA) was added to the reaction system obtained in S3, with the amount being 1.1 times the remaining molar amount of NCO. The reaction was carried out at 70°C until the characteristic peak of NCO at 2270 cm⁻¹ in the infrared spectrum completely disappeared.
[0047] S5: Solvent Removal The reaction system obtained in S4 was subjected to vacuum distillation to remove acetone, yielding a polyurethane acrylate oligomer containing sterically hindered urea bonds.
[0048] S6: Mixed Dissolution Weigh 75 parts by weight of the oligomer obtained from S5, add reactive diluent (8 parts HEA, 15 parts IBOA, 15 parts TCDDA, and 8 parts PPGDA), and stir and mix at 40°C for 1 hour to form a homogeneous solution.
[0049] S7: Initiator and Additive Addition Add 3 parts of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 0.5 parts of benzotriazole ultraviolet absorber, 0.5 parts of hindered amine light stabilizer, and 1 part of organosilicon defoaming and leveling agent to the homogeneous solution obtained in S6. Stir and disperse at high speed of 1500 rpm for 30 minutes under light-protected conditions to obtain a photosensitive resin mixture.
[0050] S8: Filtration and Degassing The photosensitive resin mixture obtained from S7 was filtered through a glass fiber filter with a pore size of 1μm, then allowed to stand in the dark and vacuum degassed for 24 hours to obtain a high-transparency, weather-resistant polyurethane acrylate flexible resin for 3D printing.
[0051] The photosensitive resin obtained in this embodiment was used for DLP 3D printing and then heat-treated at 80°C for 2 hours. Testing showed that the cured product had a 550nm visible light transmittance of 91%, a tensile strength of 12.5 MPa, an elongation at break of 280%, and a Shore A hardness of 88. After accelerated aging, the yellowing index ΔE = 1.0. Comparative Example 1 (Conventional polyurethane acrylate without sterically hindered urea bonds) A conventional polyurethane acrylate oligomer without sterically hindered urea bonds (prepared by direct reaction of PTMG and IPDI followed by HEA end-capping, without diamine chain extension) was used. The remaining components were the same as in Example 1 to prepare the photosensitive resin, which was then molded under the same DLP printing conditions. After curing, the product exhibited a 72% transmittance of visible light at 550 nm, was semi-transparent, had a tensile strength of 9.8 MPa, and an elongation at break of 195%. This indicates that the conventional polyurethane acrylate without sterically hindered urea bonds suffers from severe light scattering due to excessive aggregation of hard segments, resulting in significantly lower transmittance than in Example 1. Comparative Example 2 (Aromatic Diisocyanate System) 4,4'-diphenylmethane diisocyanate (MDI) was used to replace IPDI in Example 1, while the remaining components were the same as in Example 1. The photosensitive resin was then molded under the same DLP printing conditions. The cured product exhibited a 550nm visible light transmittance of 68%, and after accelerated aging (72 hours of UV irradiation), the yellowing index ΔE = 8.5, significantly higher than that of Example 1 (ΔE = 1.2). This indicates that the aromatic system has poor light transmittance and severely insufficient weather resistance. The above description of the disclosed embodiments is merely intended to enable those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A high-transparency, weather-resistant, flexible polyurethane acrylate resin for 3D printing, characterized in that, By weight, it includes the following components: 50-75 parts of urea-containing polyurethane acrylate oligomer; 20-45 parts of reactive diluent; 0.5-5 parts of photoinitiator; 0.1-3 parts of additives; The polyurethane acrylate oligomer containing urea bonds has acrylate double bonds at both ends of its molecular chain, and the main chain is composed of polyether soft segments and hard segments containing sterically hindered urea bonds. The sterically hindered urea bonds have reversible dissociation-recombination characteristics in the temperature range of 46~56℃, which endows the photosensitive resin with dynamic covalent polymer characteristics and repair performance. The above-mentioned polyurethane acrylate oligomers containing urea bonds are prepared by the following method: S1: Dehydration of polyether polyol ① Dehydrate the polyether polyol under vacuum at 100~120℃ for 1~2 hours; S2: Synthesis of isocyanate-terminated prepolymers ① Cool the polyether polyol obtained from S1 to 50~60℃, add alicyclic diisocyanate, control the molar ratio of isocyanate groups to hydroxyl groups to be 1.8~2.2, and react at 75~85℃ for 2~3 hours to obtain a terminal isocyanate group prepolymer; the refractive index of the alicyclic hard segment of the alicyclic diisocyanate is lower than that of the aromatic hard segment to reduce light scattering; S3: Introduction of steric urea-blocking bonds ① Cool the isocyanate-terminated prepolymer obtained from S2 to 40~50℃, slowly drop in an acetone solution of a sterically hindered alicyclic diamine, control the molar ratio of amino to remaining isocyanate groups to be 0.4~0.6, and stir rapidly for 0.5~1 hours to introduce sterically hindered urea bonds into the chain segment; S4: Acrylic end-capped ① Add hydroxyethyl acrylate or hydroxypropyl acrylate as a capping agent to the reaction system obtained in S3. The amount of hydroxyethyl acrylate or hydroxypropyl acrylate is 1.02 to 1.1 times the molar amount of the remaining isocyanate group. React at 60 to 70°C until the characteristic peak of the isocyanate group at 2270 cm⁻¹ in the infrared spectrum completely disappears. S5: Solvent Removal ①The reaction system obtained in S4 was subjected to vacuum distillation to remove acetone, and polyurethane acrylate oligomers containing sterically hindered urea bonds were obtained. The active diluent is composed of a monofunctional diluent and a difunctional diluent, wherein the monofunctional diluent is 3-8 parts of hydroxyethyl acrylate and 8-15 parts of isobornyl acrylate, and the difunctional diluent is 5-15 parts of tricyclodecanedimethyl diacrylate and 3-8 parts of polypropylene glycol diacrylate. S6: Final Synthesis ① Mixing and dissolving The polyurethane acrylate oligomer containing sterically hindered urea bonds obtained in S5 was stirred and mixed with an active diluent at 30-40°C for 1-2 hours to form a homogeneous solution. ② Addition of initiators and auxiliaries Add photoinitiator and additives to the homogeneous solution obtained in step ①, and disperse by high-speed stirring at 1000~1500 rpm for 30 minutes under light-protected conditions to obtain a photosensitive resin mixture. ③ Filtration and Degassing After filtering the photosensitive resin mixture obtained in step ② through a glass fiber filter with a pore size of 1μm, it was allowed to stand in the dark and vacuum degassed for 24 hours to obtain a polyurethane acrylate photosensitive resin containing sterically hindered urea bonds. This polyurethane acrylate photosensitive resin containing sterically hindered urea bonds is the desired high-transparency and weather-resistant 3D printing polyurethane acrylate flexible resin. After the photosensitive resin is formed by DLP 3D printing, it is heat-treated at 80°C for 0.5 to 2 hours to trigger the dynamic thermal response of the sterically hindered urea bonds, thereby realizing the rearrangement of the network topology of the printed part. At the same time, the refractive index matching effect of the alicyclic hard segment and soft segment is used to eliminate light scattering, so that the transmittance of 550nm visible light is not less than 90%.