A repair material for trenchless pipeline lining and its preparation method
By introducing a hybrid photocuring modification of rigid triazine rings, perfluorinated hydrophobic carbon chains, and flexible ether chains into epoxy resin, the problems of toughness, antifouling properties, and photocuring compatibility of epoxy resin-based CIPP materials have been solved, resulting in a high-strength, high-toughness, antifouling, and corrosion-resistant pipeline repair material suitable for long-term service of sewage pipelines.
Patent Information
- Application Number
- CN202611269045.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing epoxy resin-based CIPP repair materials are insufficient in terms of toughness, antifouling properties, and photocuring compatibility, making it difficult to meet the comprehensive performance requirements of sewage pipelines in complex service environments.
By employing a free radical-cationic hybrid photocuring system, epoxy resin is covalently grafted with a multifunctional hydroxylated acrylate compound containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain, which is synthesized in-house. This process constructs a repair material that is reinforced, toughened, antifouling, and corrosion-resistant, achieving a synergistic effect of multiple functions, including rigidity enhancement, flexibility and toughness enhancement, low surface energy antifouling, and dense corrosion resistance.
It improves the material's strength and toughness balance, enhances its impact resistance and anti-fouling performance for sewage pipes, improves its acid and alkali corrosion resistance, is compatible with rapid light curing construction, and extends the service life of the pipes.
Smart Images

Figure SMS_4 
Figure SMS_5 
Figure SMS_6
Abstract
Description
Technical Field
[0001] This invention relates to the field of in-situ curing trenchless repair technology for drainage pipelines, specifically to a repair material for trenchless pipeline linings and its preparation method. Background Technology
[0002] Cured-in-Place Pipe (CIPP) is one of the most widely used techniques in the field of trenchless repair of municipal drainage pipelines. This technique involves inserting a fiber-reinforced flexible tube impregnated with thermosetting or photosensitive resin into the old pipe to be repaired, either by inverting or pulling it in. The tube expands under air pressure, water pressure, or fluid pressure during the inversion process, causing it to fit tightly against the inner wall of the original pipe. Then, the resin is cured by heating, steam, or ultraviolet light, forming a new inner lining with sufficient structural strength inside the original pipe. This achieves structural reinforcement, leak prevention, and restoration of flow capacity.
[0003] In CIPP repair material systems, the resin matrix is the core component that determines the mechanical properties, durability, and construction adaptability of the liner pipe. Currently, commonly used resin systems in CIPP repair projects include unsaturated polyester resin and epoxy resin. Among them, epoxy resin is widely used as the structural matrix material for CIPP liner pipes due to its excellent mechanical strength, good dimensional stability, and adhesive properties. However, epoxy resin systems have the following shortcomings in CIPP pipeline repair applications: A balance between strength and toughness is difficult to achieve: Epoxy resin, after curing, has a high cross-linking density, resulting in high strength and modulus, but the cured product is brittle and has poor impact resistance. To meet the requirements of CIPP lining pipes during pipeline operation, which must withstand complex loads such as external earth pressure, traffic loads, and uneven foundation settlement, the repair material needs both sufficient stiffness to provide structural support and good toughness to resist impact and deformation. Traditional epoxy resin toughening methods (such as adding rubber elastomers, thermoplastic resins, or flexible segments) usually lead to a decrease in the material's mechanical strength and heat resistance while improving toughness, making it difficult to simultaneously meet the dual requirements of high strength and good toughness for CIPP lining pipes.
[0004] Insufficient antifouling and corrosion resistance: The internal environment of sewage pipes is complex, involving long-term contact with various corrosive media such as acids, alkalis, salts, and microbial metabolic products. Although epoxy resin has a certain degree of chemical stability, in the long-term service environment of sewage pipes, water molecules and corrosive media can still slowly penetrate through the free volume and microscopic defects of the resin matrix, leading to resin plasticization, interfacial hydrolysis, and adhesion failure, which in turn causes a decline in mechanical properties and debonding of the inner lining from the pipe wall. In addition, epoxy resin has a high surface energy, making it easy for grease, organic matter, and microorganisms contained in sewage to adhere and deposit on the inner wall of the pipe, increasing the pipe's transport resistance, reducing its flow capacity, and accelerating the occurrence of microbial induced corrosion (MIC).
[0005] UV-curing compatibility issues: UV-CIPP (ultraviolet light curing) technology has become an important development direction for CIPP technology due to its advantages such as fast curing speed, high construction efficiency, and low environmental impact. Traditional cationic UV-curing systems of epoxy resins have advantages such as low volume shrinkage, strong adhesion, and wear resistance, but also suffer from drawbacks such as slow curing speed, long curing time, limited types of reactive diluents, and difficulty in adjusting the properties of the cured product. Existing technologies achieve free radical UV curing by esterifying epoxy resins to prepare epoxy acrylate resins. While free radical UV-curing systems of epoxy resins offer advantages such as fast curing speed and easy performance adjustment, they also suffer from severe shrinkage, low precision, poor adhesion, and susceptibility to oxygen inhibition. Furthermore, the resulting products still have significant deficiencies in toughness and antifouling properties, making it difficult to meet the comprehensive performance requirements of repair materials for the complex service environment of sewage pipelines.
[0006] Based on this, the present invention develops an epoxy resin-based UV-CIPP (free radical-cationic hybrid photocuring system) pipe lining repair material that can simultaneously achieve multiple functions such as reinforcement, toughening, antifouling and corrosion resistance at the molecular level. This material has significant engineering value and practical significance for improving the construction quality of trenchless pipeline repair technology and the long-term service performance of repaired pipelines. Summary of the Invention
[0007] This invention provides a trenchless pipeline lining repair material and its preparation method. It involves the independent synthesis of a multifunctional hydroxylated acrylate compound containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain. This compound is then covalently grafted onto E-51 bisphenol A epoxy resin to construct a free radical-cationic hybrid photocuring system. This system simultaneously achieves multiple functions at the molecular structure level, including enhanced rigidity, increased flexibility and toughness, low surface energy antifouling, and dense corrosion resistance. It addresses the technical problems of traditional repair materials, such as decreased strength with increased toughness, easy adhesion of sewage and oil, easy penetration and hydrolysis by acid and alkali media, and poor photocuring quality. The resulting high-performance trenchless pipeline repair material combines high strength and toughness, hydrophobicity and antifouling properties, acid and alkali corrosion resistance, and compatibility with rapid UV curing, meeting the long-term service requirements of municipal sewage pipelines under complex operating conditions.
[0008] A trenchless pipeline lining repair material comprises the following raw materials in parts by weight: 65-75 parts of multifunctional grafted modified epoxy acrylate resin; 20-30 parts diluent; 2-4 parts free radical photoinitiator; 1-3 parts cationic photoinitiator; The multifunctional graft-modified epoxy acrylate resin is prepared by solution grafting modification of bisphenol A type epoxy resin with a multifunctional hydroxylated acrylate compound; wherein, the multifunctional hydroxylated acrylate compound is anchored on the main chain of the bisphenol A type epoxy resin molecule through a hydroxyl-epoxy ring-opening reaction. Preferably, the formulation of the multifunctional graft-modified epoxy acrylate resin is: 80-90 wt% bisphenol A type epoxy resin and 10-20 wt% multifunctional hydroxylated acrylate compound.
[0009] Preferably, the bisphenol A type epoxy resin is of type E-51 and has an epoxy value of 0.50-0.51 mol / 100g; Preferably, the epoxy value of the multifunctional graft-modified epoxy acrylate resin is 0.39-0.45 mol / 100g; Preferably, the grafting rate of the multifunctional hydroxylated acrylate compound in the multifunctional graft-modified epoxy acrylate resin is 9-19 wt%.
[0010] Preferably, the diluent is tripropylene glycol diacrylate; Preferably, the free radical photoinitiator is benzoin dimethyl ether; Preferably, the cationic photoinitiator is diphenyliodonium p-toluenesulfonate.
[0011] A method for preparing a trenchless pipeline lining repair material specifically involves: mixing benzoin dimethyl ether, diphenyliodonium p-toluenesulfonate, and tripropylene glycol diacrylate evenly, then adding the mixture to a multifunctional graft-modified epoxy acrylate resin, dispersing the mixture at a speed of 1000-1500 r / min for 20-40 min, operating entirely in the dark at 20-25℃, and then vacuum degassing after stirring to obtain the trenchless pipeline lining repair material.
[0012] Preferably, the preparation method of the multifunctional graft-modified epoxy acrylate resin is as follows: Add 80-90 parts by weight of bisphenol A type epoxy resin to anhydrous N,N-dimethylformamide, heat to 55-65℃ and stir to dissolve for 0.5-1.5 hours; Maintain a temperature of 55-65℃, add 0.9-1.5 parts by weight of triphenylphosphine catalyst and 0.05-0.15 parts by weight of MEHQ stabilizer, and stir to mix for 5-15 minutes; Dissolve 10-20 parts by weight of the multifunctional hydroxylated acrylate compound in anhydrous N,N-dimethylformamide, add it to the reaction system under mechanical stirring and nitrogen protection, and then heat to 85-95℃ and stir until the epoxy value of the system tends to stabilize. After the reaction was completed, the mixture was cooled to room temperature, and after post-treatment, it was vacuum dried to obtain a multifunctional graft-modified epoxy acrylate resin.
[0013] Preferably, the preparation method of the multifunctional hydroxylated acrylate compound is as follows: In anhydrous N,N-dimethylformamide solvent, with anhydrous potassium carbonate as an acid-binding agent, a stepwise nucleophilic substitution reaction is carried out between the three chlorine groups of 1 molar equivalent of cyanuric chloride and the hydroxyl groups of 3.01-3.09 molar equivalents of hydroxyethyl acrylate to generate 2,4,6-tris(2-acryloyloxyethoxy)-1,3,5-triazine. In anhydrous N,N-dimethylformamide solvent, using triethylamine as an acid-binding agent, a monosubstitution reaction is carried out between the primary amino group of 1 molar equivalent 1-amino-3,6,9-triox-11-undecanol and the iodine group of 0.95-0.99 molar equivalent 1,1,2,2-tetrahydroperfluorohexyliodine to generate a hydroxylated secondary amine intermediate containing a perfluorinated hydrophobic carbon chain and a flexible ether chain. In anhydrous N,N-dimethylformamide solvent, using triethylamine as a catalyst, a multifunctional hydroxylated acrylate compound is generated by the addition reaction of a 1 molar equivalent of the monoacryloyloxy group of 2,4,6-tris(2-acryloyloxyethoxy)-1,3,5-triazine with a 0.95-0.99 molar equivalent of the secondary amine group of a hydroxylated secondary amine intermediate containing a perfluorinated hydrophobic carbon chain and a flexible ether chain.
[0014] Application of a trenchless pipeline lining repair material in the field of in-situ curing trenchless repair of drainage pipelines; Preferably, the application method is as follows: At 20-30℃, alkali-free fiberglass cloth is immersed in the repair material for trenchless pipe lining. The temperature is then raised to 35-45℃ to ensure the repair material is fully impregnated into the fiberglass cloth. The resin content is controlled at 35-45 wt%. The impregnated fiber cloth is placed in a flat vulcanizing machine for rolling, and then subjected to vacuum degassing to prepare a glass fiber hose impregnated with resin. After the resin-impregnated fiberglass tubing is pulled to the predetermined position inside the pipe to be repaired, compressed air is used to pressurize and radially expand the tubing, ensuring a tight fit against the inner wall of the pipe. Then, light with a wavelength of 365nm and a light intensity of 35-50mW / cm² is introduced through the tubing wall. 2 The ultraviolet lamp is placed inside the tube, and the ultraviolet lamp is controlled to move at a constant speed of 0.3-0.4 m / min from one end to the other so that the tube gradually solidifies. A nitrogen purging device is set in front of the ultraviolet lamp to inhibit oxygen polymerization. After curing, the hose fits tightly against the inner wall of the pipe to be repaired, forming a hard pipe-in-pipe structure, which allows the underground pipe that has been damaged or lost its transport function to be repaired in situ.
[0015] Preferably, the areal density of the alkali-free glass fiber cloth is 500-650 g / m². 2 The thickness of a single layer is 0.50-0.65mm.
[0016] Preferably, the alkali-free glass fiber cloth is impregnated with silane coupling agent KH570 before being immersed in the repair material for trenchless pipe lining.
[0017] The core technical principle of this invention lies in the synergistic effect of multifunctional integrated design at the molecular level and free radical-cation hybrid photocuring: Enhancement mechanism: The rigid triazine ring is branched onto the epoxy resin backbone through a flexible ether link, introducing a rigid aromatic heterocyclic structure, which improves the modulus and strength of the resin crosslinking network. At the same time, the conjugated structure of the triazine ring enhances the heat resistance. Toughening mechanism: Flexible ether chains form deformable segments in the cross-linked network. Under the action of external force, the chain segments absorb impact energy through movement, thereby improving impact toughness. The chemical grafting method ensures that the toughening component is firmly bonded to the matrix interface. Antifouling and corrosion resistance mechanism: During the curing process, the perfluorinated hydrophobic carbon chain migrates and accumulates on the surface, forming a low surface energy hydrophobic layer (water contact angle >100°), which hinders the adhesion of water molecules and pollutants. At the same time, the high bond energy of the CF bond provides a chemical inert barrier. Hybrid photocuring mechanism: Free radical photoinitiators rapidly initiate the double bond polymerization of acrylates, achieving rapid surface curing; cationic photoinitiators initiate the ring-opening polymerization of epoxy groups, achieving deep and continuous curing and reducing volume shrinkage; Compared with the prior art, the present invention has the following beneficial technical effects: This invention utilizes molecular-level covalent grafting modification to integrate rigid triazine rings and flexible ether chains into the epoxy backbone. The rigid triazine skeleton ensures the tensile and flexural strength of the material, while the flexible polyether segments effectively absorb impact energy and improve the inherent brittleness of the resin. Test results show that the modified resin material exhibits significantly better mechanical properties than the comparative example, achieving a balanced modification goal of strength and toughness for the repair material. It can effectively resist bending deformation caused by external soil pressure, traffic dynamic loads, and uneven foundation settlement, while also resisting sudden impact loads from fluid impacts and installation work. The perfluorinated hydrophobic carbon chain anchored in the epoxy backbone can construct a low surface energy interface, significantly improving the hydrophobicity of the material surface and effectively inhibiting the adsorption and deposition of organic matter, biological proteins, inorganic salts and heavy oil stains in municipal sewage. After simulated sewage and oil pollution tests, the modified material of this invention has a high contact angle retention rate, no obvious dirt accumulation and graying phenomenon on the surface, and significantly improved anti-fouling durability, which can effectively alleviate the problems of pipe scaling, reduced flow capacity and microbial-induced corrosion. The integrated covalent grafting structure in the epoxy backbone eliminates interface defects and micropores in the blending modification. The dense cross-linked network can effectively block the penetration and diffusion of acid and alkali corrosive media. After 30 days of aging by soaking in acid and alkali solutions, the tensile strength change rate of the modified epoxy material is less than 10%. It can adapt to the complex service environment of alternating acid and alkali corrosion in sewage pipes and improve the service life of the inner lining pipe. The free radical-cationic hybrid photocuring system constructed in this invention has the dual advantages of fast curing speed and high initiation efficiency of free radical curing and small volume shrinkage and strong adhesion of cationic curing, and is suitable for UV-CIPP mobile progressive curing construction process. The trenchless pipe lining prepared using the repair material of this invention meets the technical requirements of T / CECS 559-2018 "Technical Specification for In-situ Curing Repair of Water Supply and Drainage Pipelines" and has promising engineering application prospects. Detailed Implementation Example 1:
[0018] The preparation of multifunctional hydroxylated acrylate compounds containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain includes the following process: (1) Preparation of 2,4,6-tris(2-acryloyloxyethoxy)-1,3,5-triazine: In anhydrous N,N-dimethylformamide solvent, using anhydrous potassium carbonate as an acid-binding agent, a stepwise nucleophilic substitution reaction is carried out between the three chlorine groups of 1 molar equivalent of cyanuric chloride and the hydroxyl groups of 3.06 molar equivalents of hydroxyethyl acrylate (containing 200-400 ppm MEHQ stabilizer) to generate 2,4,6-tris(2-acryloyloxyethoxy)-1,3,5-triazine, the chemical structural formula of which is: ; Preparation steps: Add 3.7 g of cyanuric chloride and 40 mL of anhydrous N,N-dimethylformamide to a four-necked flask, install a mechanical stirrer, a constant pressure dropping funnel, a thermometer and a nitrogen inlet tube, purge the air with nitrogen (≥20 min), stir at room temperature until completely dissolved, and cool the system to 5 °C (ice-water bath). Under mechanical stirring, nitrogen protection, and an ice-water bath (5℃), 50 mL of anhydrous N,N-dimethylformamide solution containing 2.4 g hydroxyethyl acrylate and 2.9 g anhydrous potassium carbonate was slowly added dropwise to a four-necked flask through a constant pressure dropping funnel. The addition was completed in 2 hours, and the reaction was stirred for another 2 hours at 5℃. TLC monitoring was performed (samples were taken every 30 minutes, developing solvent: ethyl acetate / petroleum ether = 1:3). Remove the ice-water bath and heat to 30°C. Slowly add 50 mL of anhydrous N,N-dimethylformamide solution containing 2.4 g of hydroxyethyl acrylate and 2.9 g of anhydrous potassium carbonate to the four-necked flask through a constant pressure dropping funnel. The addition is completed in 2 hours. Then, continue stirring the reaction at 30°C for 3 hours and monitor the reaction by TLC (samples are taken every 1 hour, developing solvent: ethyl acetate / petroleum ether = 1:3). The temperature was raised to 65℃ (oil bath), and 50 mL of anhydrous N,N-dimethylformamide solution containing 2.4 g hydroxyethyl acrylate and 2.9 g anhydrous potassium carbonate was slowly added dropwise to the four-necked flask through a constant pressure dropping funnel. The addition was completed in 2 h, and the reaction was continued to be stirred at 65℃ for 8 h (operated in the dark). TLC monitoring was performed (samples were taken every 2 h, developing solvent: ethyl acetate / petroleum ether = 1:3). After the reaction was completed, the mixture was cooled to room temperature, filtered to remove insoluble matter, and the filter cake was washed twice with 30 mL of anhydrous N,N-dimethylformamide. The filtrates were combined and concentrated by rotary evaporation to remove most of the N,N-dimethylformamide. Pour into 200 mL of ice water, stir for 15 min, extract three times with ethyl acetate, combine the organic phases, wash once with saturated sodium bicarbonate solution and twice with saturated brine, dry with anhydrous sodium sulfate for 4 h, filter to remove the desiccant, and remove the solvent from the filtrate by rotary evaporation. The crude product was purified by silica gel column chromatography with a gradient elution of ethyl acetate / petroleum ether = 1:4 → 1:2, monitored by TLC (developing solvent: ethyl acetate / petroleum ether = 1:2). The target fraction was collected, the solvent was removed by rotary evaporation, and the product was dried under vacuum to give 2,4,6-tris(2-acryloyloxyethoxy)-1,3,5-triazine, with a yield of 82.9%. 1 H NMR (DMSO-d6, 400MHz) δ: 4.34-4.44 (m, 12H), 5.87-5.90 (d, 6H), 6.07-6.12 (m, 3H).
[0019] (2) Preparation of a hydroxylated secondary amine intermediate containing a perfluorinated hydrophobic carbon chain and a flexible ether chain: In anhydrous N,N-dimethylformamide solvent, using triethylamine as an acid-binding agent, a monosubstitution reaction is carried out between the primary amino group of 1 molar equivalent of 1-amino-3,6,9-triox-11-undecanol and the iodine group of 0.96 molar equivalent of 1,1,2,2-tetrahydroperfluorohexyl iodine to generate a hydroxylated secondary amine intermediate containing a perfluorinated hydrophobic carbon chain and a flexible ether chain. Its chemical structural formula is as follows: ; Preparation steps: Add 3.9 g of 1-amino-3,6,9-triox-11-undecyl alcohol and 40 mL of anhydrous N,N-dimethylformamide to a four-necked flask, install a mechanical stirrer, a constant pressure dropping funnel, a thermometer and a nitrogen inlet tube, purge the air with nitrogen (≥15 min), and stir at room temperature until completely dissolved; Under mechanical stirring and nitrogen protection, 2.3 g of triethylamine was added to the four-necked flask at once, and the mixture was stirred at room temperature for 10 min. 60 mL of anhydrous N,N-dimethylformamide solution containing 7.2 g of 1,1,2,2-tetrahydroperfluorohexyl iodine was slowly added dropwise to a four-necked flask using a constant-pressure dropping funnel. The addition was completed over 2 hours, with the reaction system temperature maintained at 25 °C (room temperature) during the addition. After the addition was complete, the temperature was raised to 50 °C and the reaction was stirred for 10 hours. The reaction was monitored by TLC (samples were taken every 2 hours, with ethyl acetate / methanol as the developing solvent: 10:1). After the reaction was completed, the mixture was cooled to room temperature and slowly poured into 200 mL of ice water. The mixture was stirred for 15 min and extracted three times with ethyl acetate. The organic phases were combined and washed once with 0.5 mol / L dilute hydrochloric acid, once with saturated sodium bicarbonate solution, and twice with saturated brine. The mixture was dried over anhydrous sodium sulfate for 4 h, filtered to remove the desiccant, and the solvent was removed by rotary evaporation of the filtrate. The crude product was purified by silica gel column chromatography with a gradient elution of ethyl acetate / methanol from 15:1 to 8:1, monitored by TLC (eluent: ethyl acetate / methanol = 10:1). The target fraction was collected, the solvent was removed by rotary evaporation, and the product was dried under vacuum to obtain a hydroxylated secondary amine intermediate containing a perfluorinated hydrophobic carbon chain and a flexible ether chain, with a yield of 77.5%. 1 H NMR (DMSO-d6, 400MHz) δ: 2.64-2.66 (t, 2H), 2.90-2.93 (m, 2H), 2.99-3.02 (m, 2H), 3.46-3.48 (t, 2H), 3.55-3.62 (m, 12H), 4.26-4.29 (t, 1H), 5.71-5.76 (m, 1H).
[0020] (3) Preparation of a multifunctional hydroxylated acrylate compound containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain: In anhydrous N,N-dimethylformamide solvent, using triethylamine as a catalyst, a 1 molar equivalent of the monoacryloxy group of 2,4,6-tris(2-acryloyloxyethoxy)-1,3,5-triazine undergoes an addition reaction with a 0.97 molar equivalent of the secondary amine intermediate containing a perfluorinated hydrophobic carbon chain and a flexible ether chain to generate a multifunctional hydroxylated acrylate compound containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain. Its chemical structural formula is as follows: ; Add 4.2 g of 2,4,6-tris(2-acryloyloxyethoxy)-1,3,5-triazine and 50 mL of anhydrous N,N-dimethylformamide to a four-necked flask, install a mechanical stirrer, a constant pressure dropping funnel, a thermometer and a nitrogen inlet tube, purge the air with nitrogen (≥15 min), and stir at room temperature until completely dissolved; Under mechanical stirring and nitrogen protection, 50 mL of anhydrous N,N-dimethylformamide solution containing 4.3 g of a hydroxylated secondary amine intermediate with a perfluorinated hydrophobic carbon chain and a flexible ether chain and 0.2 g of triethylamine was slowly added dropwise to a four-necked flask through a constant-pressure dropping funnel. The addition was completed in 2 h, and the reaction system temperature was maintained at 25 °C (room temperature) during the addition. After the addition was completed, the temperature was raised to 40 °C and the reaction was stirred for 8 h (operated in the dark). TLC monitoring was performed (samples were taken every 2 h, developing solvent: ethyl acetate / methanol = 10:1). After the reaction was completed, the mixture was cooled to room temperature, and 5 mL of glacial acetic acid was added to quench the reaction. The mixture was stirred for 10 min, then slowly poured into 200 mL of ice water and stirred for 15 min. The mixture was extracted three times with ethyl acetate, and the organic phases were combined. The organic phases were washed twice with saturated brine, once with 0.5 mol / L dilute hydrochloric acid, once with saturated sodium bicarbonate solution, and once with saturated brine. The mixture was dried over anhydrous sodium sulfate for 4 h, filtered to remove the desiccant, and the solvent was removed by rotary evaporation of the filtrate. The crude product was purified by silica gel column chromatography with a gradient elution of ethyl acetate / methanol from 15:1 to 8:1, monitored by TLC (eluent: ethyl acetate / methanol = 10:1). The target fraction was collected, the solvent was removed by rotary evaporation, and the product was dried under vacuum to obtain a multifunctional hydroxylated acrylate compound containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain, with a yield of 71.8%. 1H NMR (DMSO-d6, 400MHz) δ: 2.71-2.74(t, 2H), 2.79-2.82(t, 2H), 2.96-2.98(t, 2H), 3.27-3.30(t, 2H), 3.35-3.3 9(t, 2H), 3.52-3.68(m, 14H), 4.06-4.30(m, 13H), 5.89-5.93(d, 4H), 6.05-6.12(m, 2H); The elemental analysis was performed using a Vario EL Ⅲ type elemental analyzer, and the results are as follows: Theoretical values: C 44.55%, H 5.02%, N 6.49%; Measured values: C 44.47%, H 4.86%, N 6.40%; HPLC-MS showed that the main peak [M+H]⁺ was 863.7 m / z, which is consistent with the theoretical molecular weight (862.70) of the multifunctional hydroxylated acrylate compound containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain. Example 2:
[0021] A multifunctional graft-modified epoxy acrylate resin I containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain was prepared. The formulation was: 90 wt% bisphenol A type epoxy resin and 10 wt% multifunctional hydroxylated acrylate compound containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain. Raw materials for preparation: Bisphenol A type epoxy resin (model E-51) with an epoxy value of 0.508 mol / 100g (actual value). Multifunctional hydroxylated acrylate compounds containing rigid triazine rings, perfluorinated hydrophobic carbon chains, and flexible ether chains; Triphenylphosphine catalyst; Anhydrous N,N-dimethylformamide solvent; MEHQ stabilizer; Preparation principle: Bisphenol A type epoxy resin is modified by solution grafting using a multifunctional hydroxylated acrylate compound. The hydroxyl functional groups of the multifunctional hydroxylated acrylate compound undergo a ring-opening reaction with the epoxy groups on the main chain of E-51 bisphenol A type epoxy resin to obtain multifunctional graft-modified epoxy acrylate resin I. Preparation steps: Add 90g of bisphenol A epoxy resin and 450mL of anhydrous N,N-dimethylformamide to a four-necked flask, install a mechanical stirrer, thermometer and nitrogen inlet tube, purge the air with nitrogen (≥20min), heat to 60℃ and stir to dissolve for 1h; Maintain 60℃, add 0.9g of triphenylphosphine catalyst and 50mg of MEHQ stabilizer, and stir to mix for 10min; 10g of multifunctional hydroxylated acrylate compound was dissolved in 50mL of anhydrous N,N-dimethylformamide and added to the reaction system under mechanical stirring and nitrogen protection. The temperature was then raised to 90℃ (oil bath) and the reaction was stirred. The epoxy value was measured every 1h (hydrochloric acid-acetone method). The reaction endpoint was reached when the epoxy value tended to stabilize. After the reaction was completed, the mixture was cooled to room temperature, and most of the solvent was removed by rotary evaporation under reduced pressure. The mixture was then subjected to Soxhlet extraction with n-hexane for 24 hours to remove the free multifunctional hydroxylated acrylate compounds that did not participate in the grafting reaction. The mixture was then dried under vacuum to obtain multifunctional graft-modified epoxy acrylate resin I. The epoxy value of the multifunctional grafted modified epoxy acrylate resin I, determined by the hydrochloric acid-acetone method, is 0.448 mol / 100g. Therefore, the actual grafting rate of the multifunctional grafted modified epoxy acrylate resin I (the percentage of the mass of the multifunctional hydroxylated acrylate compound grafted onto the main chain of the epoxy resin molecule to the total mass of the final grafted product) is 9.62 wt%. Example 3:
[0022] A multifunctional graft-modified epoxy acrylate resin II containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain was prepared. The formulation was: 85 wt% bisphenol A type epoxy resin and 15 wt% multifunctional hydroxylated acrylate compound containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain. The raw materials and preparation principle of multifunctional graft-modified epoxy acrylate resin II are the same as those of multifunctional graft-modified epoxy acrylate resin I: Preparation steps: Add 85g of bisphenol A epoxy resin and 420mL of anhydrous N,N-dimethylformamide to a four-necked flask, install a mechanical stirrer, thermometer and nitrogen inlet tube, purge the air with nitrogen (≥20min), heat to 60℃ and stir to dissolve for 1h; Maintain 60℃, add 1.2g of triphenylphosphine catalyst and 100mg of MEHQ stabilizer, and stir for 10min; 15g of multifunctional hydroxylated acrylate compound was dissolved in 75mL of anhydrous N,N-dimethylformamide and added to the reaction system under mechanical stirring and nitrogen protection. The temperature was then raised to 90℃ (oil bath) and the reaction was stirred. The epoxy value was measured every 1h (hydrochloric acid-acetone method). The reaction endpoint was reached when the epoxy value tended to stabilize. After the reaction was completed, the mixture was cooled to room temperature, the solvent was removed by rotary evaporation under reduced pressure, and the mixture was subjected to Soxhlet extraction with n-hexane for 24 h to remove the free multifunctional hydroxylated acrylate compounds that did not participate in the grafting reaction. The mixture was then dried under vacuum to obtain multifunctional grafted modified epoxy acrylate resin II. The epoxy value of the multifunctional grafted modified epoxy acrylate resin II, determined by the hydrochloric acid-acetone method, is 0.419 mol / 100g. Therefore, the actual grafting rate of the multifunctional grafted modified epoxy acrylate resin II (the percentage of the mass of the multifunctional hydroxylated acrylate compound grafted onto the main chain of the epoxy resin molecule to the total mass of the final grafted product) is 14.27 wt%. Example 4:
[0023] A multifunctional graft-modified epoxy acrylate resin III containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain was prepared. The formulation was: 80 wt% bisphenol A type epoxy resin and 20 wt% multifunctional hydroxylated acrylate compound containing a rigid triazine ring, a perfluorinated hydrophobic carbon chain, and a flexible ether chain. The raw materials and preparation principle of multifunctional graft-modified epoxy acrylate resin III are the same as those of multifunctional graft-modified epoxy acrylate resin I: Preparation steps: Add 80g of bisphenol A epoxy resin and 400mL of anhydrous N,N-dimethylformamide to a four-necked flask, install a mechanical stirrer, thermometer and nitrogen inlet tube, purge the air with nitrogen (≥20min), heat to 60℃ and stir to dissolve for 1h; Maintain 60℃, add 1.5g of triphenylphosphine catalyst and 150mg of MEHQ stabilizer, and stir for 10min; 20g of multifunctional hydroxylated acrylate compound was dissolved in 100mL of anhydrous N,N-dimethylformamide and added to the reaction system under mechanical stirring and nitrogen protection. The temperature was then raised to 90℃ (oil bath) and the reaction was stirred. The epoxy value was measured every 1h (hydrochloric acid-acetone method). The reaction endpoint was reached when the epoxy value tended to stabilize. After the reaction was completed, the mixture was cooled to room temperature, and most of the solvent was removed by rotary evaporation under reduced pressure. The mixture was then subjected to Soxhlet extraction with n-hexane for 24 hours to remove the free multifunctional hydroxylated acrylate compounds that did not participate in the grafting reaction. The mixture was then dried under vacuum to obtain multifunctional grafted modified epoxy acrylate resin III. The epoxy value of the multifunctional grafted modified epoxy acrylate resin III, determined by the hydrochloric acid-acetone method, is 0.390 mol / 100g. Therefore, the actual grafting rate of the multifunctional grafted modified epoxy acrylate resin III (the percentage of the mass of the multifunctional hydroxylated acrylate compound grafted onto the main chain of the epoxy resin molecule to the total mass of the final grafted product) is 18.91 wt%. Example 5:
[0024] A repair material I for trenchless pipeline lining is shown in Table 1.
[0025] Table 1. Formulation of Repair Material I for Trenchless Pipeline Liners Example 6:
[0026] Preparation of trenchless pipeline lining repair material I: According to the formula in Table 1, the formulated amounts of benzoin dimethyl ether, diphenyliodonium p-toluenesulfonate and tripropylene glycol diacrylate were mixed evenly and then added to the formulated amount of multifunctional graft-modified epoxy acrylate resin I. The mixture was dispersed at a speed of 1200 r / min for 30 min. The entire process was carried out under light-proof and room temperature (25℃) conditions. After stirring evenly, the mixture was degassed under vacuum to obtain trenchless pipeline lining repair material I. Example 7:
[0027] Repair material II for trenchless pipeline lining is prepared. The only difference between it and repair material I for trenchless pipeline lining is that multifunctional graft-modified epoxy acrylate resin II is used instead of multifunctional graft-modified epoxy acrylate resin I. Example 8:
[0028] Repair material III for trenchless pipeline lining is prepared. The only difference between it and repair material I for trenchless pipeline lining is that multifunctional graft-modified epoxy acrylate resin III is used instead of multifunctional graft-modified epoxy acrylate resin I. Comparative Example 1:
[0029] The epoxy resin material a is prepared, and its only difference from the trenchless pipeline lining repair material I is that the conventional epoxy acrylate resin is used instead of the multifunctional graft-modified epoxy acrylate resin I. The conventional method for preparing epoxy acrylate resin is as follows: E-51 bisphenol A type epoxy resin is solution grafted with hydroxyethyl acrylate. The hydroxyl functional groups of hydroxyethyl acrylate undergo a ring-opening reaction with the epoxy groups on the main chain of the E-51 bisphenol A type epoxy resin to obtain the conventional epoxy acrylate resin. Raw materials for preparation: Bisphenol A type epoxy resin (model E-51) with an epoxy value of 0.508 mol / 100g (actual value). Hydroxyethyl acrylate; Triphenylphosphine catalyst; Anhydrous N,N-dimethylformamide solvent; MEHQ stabilizer; Preparation steps: Add 90g of bisphenol A epoxy resin and 450mL of anhydrous N,N-dimethylformamide to a four-necked flask, install a mechanical stirrer, thermometer and nitrogen inlet tube, purge the air with nitrogen (≥20min), heat to 60℃ and stir to dissolve for 1h; Maintain 60℃, add 0.9g of triphenylphosphine catalyst and 50mg of MEHQ stabilizer, and stir to mix for 10min; Dissolve 5g of hydroxyethyl acrylate in 50mL of anhydrous N,N-dimethylformamide and add it to the reaction system under mechanical stirring and nitrogen protection. Then heat to 90℃ (oil bath) and stir to react. Take samples every 1h to measure the epoxy value (hydrochloric acid-acetone method). The reaction endpoint is reached when the epoxy value tends to stabilize. After the reaction was completed, the mixture was cooled to room temperature, and most of the solvent was removed by rotary evaporation under reduced pressure. The mixture was then subjected to Soxhlet extraction with ethanol for 24 hours to remove free hydroxyethyl acrylate that did not participate in the grafting reaction. The mixture was then dried under vacuum to obtain a conventional epoxy acrylate resin. The epoxy value of conventional epoxy acrylate resin was determined to be 0.445 mol / 100g using the hydrochloric acid-acetone method. Comparative Example 2:
[0030] The epoxy resin material b was prepared, and its formulation is shown in Table 2.
[0031] Table 2 Formulation of epoxy resin material b
[0032] The preparation method of epoxy resin material b is as follows: According to the formula in Table 2, the formulated amounts of benzoin dimethyl ether, diphenyliodonium p-toluenesulfonate, tripropylene glycol diacrylate, polyethylene glycol diacrylate, 2-(perfluorobutyl)ethyl acrylate and 1,3,5-triazine are mixed evenly and then added to the formulated amount of conventional epoxy acrylate resin. The mixture is dispersed at a speed of 1200 r / min for 30 min. The entire process is carried out under light-proof and room temperature (25℃) conditions. After stirring evenly, the mixture is degassed under vacuum to obtain epoxy resin material b. Performance testing:
[0033] The samples from Examples 6, 7, and 8, and Comparative Examples 1 and 2 were placed in a vacuum drying oven for 15 minutes to degas, then poured into polytetrafluoroethylene molds coated with a release agent. They were cured using ultraviolet light at a wavelength of 365 nm, achieving a curing strength of 40 mW / cm². 2 After curing at room temperature for 24 hours, the surface is sanded smooth and performance tests are conducted. I. Mechanical property testing: Mechanical property testing was conducted in accordance with GB / T 2567-2021 "Test Methods for Properties of Resin Castings". The tensile strength (tensile speed 10 mm / min), flexural strength (flexural speed 10 mm / min), and impact toughness (size 80 mm × 10 mm × 4 mm, unnotched, pendulum weight 5.5 J) of the specimen were recorded. II. Heat resistance test: According to GB / T 1634.2-2019 "Determination of load deflection temperature of plastics - Part 2: Plastics and hard rubber", an 80mm×10mm×4mm sample was placed on a support with a span of 64mm, a load of 1.80MPa was applied, and the temperature was increased at a rate of 120℃ / h. The initial temperature was 25℃, and the temperature at which the bending deflection of the sample reached 0.34mm was recorded as the heat deflection temperature. The results of the above performance tests are shown in Table 3 below.
[0034] Table 3 Performance Test Results of Repair Materials for Trenchless Pipe Liners
[0035] As shown in Table 3: This invention utilizes a self-developed multifunctional hydroxylated acrylate compound to perform solution grafting modification on E-51 bisphenol A type epoxy resin. The resulting trenchless pipeline lining repair material, compared with conventional epoxy acrylate resin (Comparative Example 1) and blended modified epoxy acrylate resin (Comparative Example 2), achieves a significant improvement in impact toughness. It also exhibits excellent tensile and flexural mechanical strength and heat resistance, demonstrating a balance of strength and toughness. This achieves the technical goal of high-strength and high-toughness modification for trenchless pipeline lining repair materials. The tensile and flexural mechanical strengths of the trenchless pipeline lining repair material prepared by this invention are significantly greater than the technical requirements of T / CECS 559-2018 "Technical Specification for In-situ Curing Repair Engineering of Water Supply and Drainage Pipelines" regarding the performance of in-situ curing (CIPP) special resin castings (tensile strength ≥80MPa, flexural strength ≥100MPa). The heat distortion temperature of the trenchless pipeline lining repair material prepared by this invention is significantly greater than the technical requirements of T / CECS559-2018 "Technical Specification for In-situ Curing Repair Engineering of Water Supply and Drainage Pipelines" regarding the performance of in-situ curing (CIPP) special resin castings (heat distortion temperature ≥85℃). III. Hydrophobic and antifouling performance test: (1) The water contact angle of the sample was tested by the droplet method using a contact angle measuring instrument. The sample was placed stably on the stage of the contact angle measuring instrument, and 4 μL of pure water was dropped onto the sample surface using a micro syringe (the test environment temperature was controlled at 25℃ and the relative humidity was maintained at 50%). After the droplet state stabilized (about 30s), the static water contact angle of the sample surface was measured by the tangent method. (2) Wastewater and oil stains were used to simulate pipeline pollutants. The samples were evenly coated on the sample surface and left to stand at room temperature for 12 hours to fully absorb and adsorb the pollutants. Then, the samples were rinsed with pure water at room temperature under low pressure for 30 seconds and the surface moisture was dried. The surface dirt residue, graying, and oil residue were observed. The water contact angle after contamination was tested according to the method in (1), and the contact angle retention rate after contamination was calculated. The specific method is as follows: Water contact angle retention rate (%) = (Contact angle of contaminated water / Initial water contact angle) × 100%; Simulated wastewater formulation: formulated by mass fraction, COD simulated pollutants (glucose 0.2wt%), inorganic salt impurities (sodium chloride 0.3wt%, magnesium sulfate 0.1wt%), detergent (sodium dodecylbenzenesulfonate 0.05wt%), simulated biological pollutants (bovine serum albumin 0.1wt%), with the remainder being deionized water, simulating a municipal domestic wastewater system. Simulated oil stain formula: It is a mixture of 80wt% engine oil and 20wt% diesel oil to simulate the heavy oil stains from industrial and domestic use that have accumulated in pipelines over a long period of time. The results of the above performance tests are shown in Table 4 below.
[0036] Table 4 Performance Test Results of Repair Materials for Trenchless Pipe Liners (Part 2)
[0037] (3) The sample in Example 8 was immersed in deionized water at room temperature (25°C), and the water contact angle was tested after immersion for 7 days, 15 days and 30 days according to the method in (1); The results of the above performance tests are shown in Table 5 below.
[0038] Table 5 Performance Test Results of Repair Materials for Trenchless Pipe Liners (Part 3)
[0039] As shown in Tables 4 and 5, this invention uses multifunctional hydroxylated acrylate compounds to chemically graft and modify epoxy resin, anchoring perfluorinated hydrophobic carbon chains into the epoxy backbone molecular skeleton. The trenchless pipeline lining repair material prepared in this way has excellent surface hydrophobicity, resistance to sewage / oil adhesion, and long-term antifouling stability. Its comprehensive hydrophobic and antifouling performance is significantly better than that of conventional epoxy acrylate resin (Comparative Example 1) and blended modification system (Comparative Example 2), providing a new material solution for the long-term reliable service of trenchless underground pipeline repair in harsh media environments such as sewage and oil. IV. Resistance to Corrosion and Media Tests: (1) Acid corrosion resistance: The sample was immersed in 5wt% H2SO4 solution (simulated acidic wastewater) for 30 days, then taken out, rinsed with pure water at room temperature and dried. Tensile test was carried out according to GB / T 2567-2021 "Test Method for Performance of Resin Castings" standard. The tensile speed was 10 mm / min. The tensile strength of the sample was recorded. The change rate of tensile strength of the sample after immersion in 5wt% H2SO4 solution for 30 days was calculated. The specific calculation method is as follows: Tensile strength change rate (%) = (Initial longitudinal tensile strength - Tensile strength after immersion in 5wt% H2SO4 solution for 30 days) / Initial longitudinal tensile strength × 100%; (2) Alkali corrosion resistance: The sample was immersed in 5wt% NaOH solution (simulated alkaline wastewater) for 30 days, then rinsed with pure water at room temperature and dried. Tensile test was performed according to GB / T 2567-2021 "Test Method for Performance of Resin Castings" standard. The tensile speed was 10 mm / min. The tensile strength of the sample was recorded. The change rate of tensile strength of the sample after immersion in 5wt% NaOH solution for 30 days was calculated. The specific calculation method is as follows: Tensile strength change rate (%) = (Initial longitudinal tensile strength - Tensile strength after immersion in 5wt% NaOH solution for 30 days) / Initial longitudinal tensile strength × 100%; The results of the above performance tests are shown in Table 6 below.
[0040] Table 6 Performance Test Results of Repair Materials for Trenchless Pipe Liners (Part 4)
[0041] As shown in Table 6, this invention uses multifunctional hydroxylated acrylate compounds to chemically graft and modify epoxy resin, anchoring perfluorinated hydrophobic carbon chains into the epoxy backbone molecular skeleton, thus constructing a stable and dense hydrophobic protective barrier on the material surface. After being immersed in 5wt% H2SO4 and 5wt% NaOH solutions for 30 days, the tensile strength change rate is less than 10%. It exhibits long-term service reliability and durability in harsh corrosive media environments such as strong acids and strong alkalis, and can provide technical support for the application of trenchless repair engineering of underground pipelines in complex chemical media environments. Example 9:
[0042] Application experiment of repair materials for trenchless pipeline lining: At room temperature, alkali-free glass fiber cloth (area density 600 g / m²) 2 The single-layer thickness is 0.60mm. Before use, it is impregnated with silane coupling agent KH570 and then immersed in the trenchless pipe lining repair material. The material is heated to 40℃ to fully impregnate the fiberglass cloth. The resin content is controlled at 40wt%. The impregnated fiber cloth is placed in a flat vulcanizing machine for rolling, and then subjected to vacuum degassing to prepare a glass fiber hose impregnated with resin. After the resin-impregnated fiberglass tubing is pulled to the predetermined position inside the pipe to be repaired, compressed air is used to pressurize and radially expand the tubing, ensuring a tight fit against the inner wall of the pipe. Then, light with a wavelength of 365nm and a light intensity of 40mW / cm² is introduced through the tubing wall. 2 The ultraviolet lamp is placed inside the tube, and the ultraviolet lamp is controlled to move at a constant speed of 0.3 m / min from one end to the other so that the tube gradually solidifies. A nitrogen purging device is set in front of the ultraviolet lamp to inhibit oxygen polymerization. After curing, the hose fits tightly against the inner wall of the pipe to be repaired, forming a hard pipe-in-pipe structure, which allows the underground pipe that has been damaged or lost its transport function to be repaired in situ. Among them, when the repair materials for trenchless pipeline lining pipes are repair materials I, II and III respectively, trenchless pipeline lining pipes I, II and III are obtained in sequence. According to T / CECS 559-2018 "Technical Specification for In-situ Curing Repair of Water Supply and Drainage Pipelines", the performance of the trenchless pipeline lining was tested, and the test results are shown in Table 7 below.
[0043] Table 7 Performance test results of trenchless pipeline lining
[0044] As shown in Table 7, the trenchless pipe liner prepared by the present invention meets the technical requirements specified in T / CECS 559-2018 "Technical Specification for In-situ Curing Repair of Water Supply and Drainage Pipelines".
Claims
1. A repair material for trenchless pipeline lining, characterized in that, The ingredients include the following parts by weight: 65-75 parts of multifunctional grafted modified epoxy acrylate resin; 20-30 parts diluent; 2-4 parts free radical photoinitiator; 1-3 parts cationic photoinitiator; The multifunctional graft-modified epoxy acrylate resin is prepared by solution grafting modification of bisphenol A type epoxy resin with a multifunctional hydroxylated acrylate compound; wherein, the multifunctional hydroxylated acrylate compound is anchored on the main chain of the bisphenol A type epoxy resin molecule through a hydroxyl-epoxy ring-opening reaction. The chemical structural formula of the multifunctional hydroxylated acrylate compound is as follows: 。 2. The repair material for trenchless pipeline lining according to claim 1, characterized in that, The formulation of the multifunctional graft-modified epoxy acrylate resin is: 80-90wt% bisphenol A type epoxy resin and 10-20wt% multifunctional hydroxylated acrylate compound.
3. The repair material for trenchless pipeline lining according to claim 2, characterized in that, The bisphenol A type epoxy resin is of type E-51 and has an epoxy value of 0.50-0.51 mol / 100g; The epoxy value of the multifunctional grafted modified epoxy acrylate resin is 0.39-0.45 mol / 100g; The grafting rate of the multifunctional hydroxylated acrylate compound in the multifunctional graft-modified epoxy acrylate resin is 9-19 wt%.
4. The repair material for trenchless pipeline lining according to claim 1, characterized in that, The diluent is tripropylene glycol diacrylate; The free radical photoinitiator is benzoin dimethyl ether; The cationic photoinitiator is diphenyliodonium p-toluenesulfonate.
5. A method for preparing a repair material for trenchless pipeline linings according to any one of claims 1-4, characterized in that, Specifically, benzoin dimethyl ether, diphenyliodonium p-toluenesulfonate, and tripropylene glycol diacrylate are mixed evenly and then added to a multifunctional graft-modified epoxy acrylate resin. The mixture is dispersed at a speed of 1000-1500 r / min for 20-40 min, and the entire process is carried out under conditions of avoiding light and 20-25℃. After stirring evenly, the mixture is degassed under vacuum to obtain a trenchless pipeline lining repair material.
6. The method for preparing a repair material for trenchless pipeline lining according to claim 5, characterized in that, The preparation method of the multifunctional graft-modified epoxy acrylate resin is as follows: Add 80-90 parts by weight of bisphenol A type epoxy resin to anhydrous N,N-dimethylformamide, heat to 55-65℃ and stir to dissolve for 0.5-1.5 hours; Maintain a temperature of 55-65℃, add 0.9-1.5 parts by weight of triphenylphosphine catalyst and 0.05-0.15 parts by weight of MEHQ stabilizer, and stir to mix for 5-15 minutes; Dissolve 10-20 parts by weight of the multifunctional hydroxylated acrylate compound in anhydrous N,N-dimethylformamide, add it to the reaction system under mechanical stirring and nitrogen protection, and then heat to 85-95℃ and stir until the epoxy value of the system tends to stabilize. After the reaction was completed, the mixture was cooled to room temperature, and after post-treatment, it was vacuum dried to obtain a multifunctional graft-modified epoxy acrylate resin.
7. The method for preparing a repair material for trenchless pipeline lining according to claim 6, characterized in that, The preparation method of the multifunctional hydroxylated acrylate compound is as follows: In anhydrous N,N-dimethylformamide solvent, with anhydrous potassium carbonate as an acid-binding agent, a stepwise nucleophilic substitution reaction is carried out between the three chlorine groups of 1 molar equivalent of cyanuric chloride and the hydroxyl groups of 3.01-3.09 molar equivalents of hydroxyethyl acrylate to generate 2,4,6-tris(2-acryloyloxyethoxy)-1,3,5-triazine. In anhydrous N,N-dimethylformamide solvent, using triethylamine as an acid-binding agent, a monosubstitution reaction is carried out between the primary amino group of 1 molar equivalent 1-amino-3,6,9-triox-11-undecanol and the iodine group of 0.95-0.99 molar equivalent 1,1,2,2-tetrahydroperfluorohexyliodine to generate a hydroxylated secondary amine intermediate containing a perfluorinated hydrophobic carbon chain and a flexible ether chain. In anhydrous N,N-dimethylformamide solvent, using triethylamine as a catalyst, a multifunctional hydroxylated acrylate compound is generated by the addition reaction of a 1 molar equivalent of the monoacryloyloxy group of 2,4,6-tris(2-acryloyloxyethoxy)-1,3,5-triazine with a 0.95-0.99 molar equivalent of the secondary amine group of a hydroxylated secondary amine intermediate containing a perfluorinated hydrophobic carbon chain and a flexible ether chain.
8. The application of a repair material for trenchless pipeline linings according to any one of claims 1-4, characterized in that, The application method of the repair material in the field of in-situ curing trenchless repair of drainage pipes is as follows: At 20-30℃, alkali-free fiberglass cloth is immersed in the repair material for trenchless pipe lining. The temperature is then raised to 35-45℃ to ensure the repair material is fully impregnated into the fiberglass cloth. The resin content is controlled at 35-45 wt%. The impregnated fiber cloth is placed in a flat vulcanizing machine for rolling, and then subjected to vacuum degassing to prepare a glass fiber hose impregnated with resin. After the resin-impregnated fiberglass tubing is pulled to the predetermined position inside the pipe to be repaired, compressed air is used to pressurize and radially expand the tubing, ensuring a tight fit against the inner wall of the pipe. Then, light with a wavelength of 365nm and a light intensity of 35-50mW / cm² is introduced through the tubing wall. 2 The ultraviolet lamp is placed inside the tube, and the ultraviolet lamp is controlled to move at a constant speed of 0.3-0.4 m / min from one end to the other so that the tube gradually solidifies. A nitrogen purging device is set in front of the ultraviolet lamp to inhibit oxygen polymerization. After curing, the hose fits tightly against the inner wall of the pipe to be repaired, forming a hard pipe-in-pipe structure, which allows the underground pipe that has been damaged or lost its transport function to be repaired in situ.
9. The application of the trenchless pipeline lining repair material according to claim 8, characterized in that, The areal density of the alkali-free glass fiber cloth is 500-650 g / m². 2 The thickness of a single layer is 0.50-0.65mm.
10. The application of the repair material for trenchless pipeline lining according to claim 9, characterized in that, Before being immersed in the repair material for trenchless pipe lining, the alkali-free glass fiber cloth is impregnated with silane coupling agent KH570.