A core-shell structured high-temperature resistant guanidine-based strong base resin and its preparation method
By combining a silica core with a guanidine-based strong base resin shell through a core-shell structure design, the problem of easy degradation of traditional resins at high temperatures is solved, thereby improving high-temperature resistance and simplifying the preparation process. This makes it suitable for high-temperature water treatment and catalytic reactions.
Patent Information
- Application Number
- CN202510636359.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing ion exchange resins are prone to degradation under high temperature conditions, have insufficient mechanical strength and heat resistance, and have complex preparation processes and high costs.
A core-shell structure design is adopted, with silica as the core and guanidine-based strong base resin as the shell. The high-temperature resistant guanidine-based strong base resin with core-shell structure is prepared by sol-gel method and seed emulsion polymerization method. Combining the heat resistance of silica and the basicity of guanidine, the preparation process is simplified and the cost is reduced.
It improves the high-temperature resistance and mechanical strength of the resin, simplifies the preparation process, reduces production costs, and is suitable for water treatment and catalytic reactions under high-temperature conditions.
Abstract
Description
Technical Field
[0001] This invention relates to an ion exchange resin material and its preparation method, specifically to a core-shell structured, high-temperature resistant guanidine-based strong base resin and its preparation method. This resin has a core-shell structure and is suitable for applications such as water treatment and catalysis under high-temperature conditions. Background Technology
[0002] Ion exchange resins are high-molecular-weight polymers containing active groups that enable ion exchange in solution, and are widely used in water treatment, chemical, and pharmaceutical fields. Traditional ion exchange resins are typically copolymerized from monomers such as styrene and divinylbenzene, offering advantages such as low cost and ease of preparation. However, traditional ion exchange resins are prone to degradation under high-temperature conditions, leading to a decrease in ion exchange capacity and mechanical strength, thus affecting their service life and application performance.
[0003] In certain specific applications, such as high-temperature industrial wastewater treatment and high-temperature catalytic reactions, ion exchange resins require excellent high-temperature resistance. To improve the high-temperature resistance of ion exchange resins, researchers have developed various modification methods. One common modification method is to introduce inorganic materials, such as silica (SiO2) and alumina (Al2O3), into the resin to form composite materials. Inorganic materials possess good heat resistance and mechanical strength, which can effectively improve the high-temperature resistance of the resin. By combining inorganic materials with organic resins, the advantages of both can be combined, improving the overall performance of the material. Another modification method is to introduce high-temperature resistant functional groups onto the resin surface. The guanidine group is a functional group with good heat resistance and basicity; introducing it into ion exchange resins can improve their stability under high-temperature alkaline conditions. Through functionalization modification, specific chemical properties can be endowed to the resin, improving its selectivity and reactivity.
[0004] However, existing high-temperature resistant ion exchange resins still have some problems. For example, uneven dispersion of inorganic fillers and poor bonding with organic resins result in low mechanical strength of the composite materials; the preparation processes of some functionalized resins are complex and costly. Therefore, developing a guanidine-based strong base resin with a simple preparation method, low cost, and good high-temperature resistance remains a research hotspot in this field.
[0005] This invention addresses the shortcomings of existing technologies by providing a core-shell structured high-temperature resistant guanidine-based strong base resin and its preparation method. The resin uses silica as its core and guanidine-based strong base resin as its shell, utilizing the synergistic effect of the heat resistance of silica and the basicity of guanidine to improve the resin's high-temperature resistance. Furthermore, this invention employs a simple preparation method, reducing production costs and demonstrating promising application prospects. This core-shell structure design aims to optimize material performance, balancing heat resistance and ion exchange capacity, while simplifying the preparation process and reducing production costs. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a guanidine-based strong base resin with a simple preparation method, low cost, and good high-temperature resistance, as well as its preparation method. To achieve the above objective, this invention adopts the following technical solution: A core-shell structured high-temperature resistant guanidine-based strong base resin, characterized in that the material is a core-shell structured composite, wherein the core is silicon dioxide (SiO2) and the outer shell is a guanidine-based strong base resin.
[0007] A method for preparing a core-shell structured high-temperature resistant guanidine-based strong base resin, characterized by comprising the following steps: a) A silicon source, solvent and catalyst are mixed to prepare a silicon dioxide (SiO2) core via the sol-gel method, followed by aging, washing and drying. b) Add the silica (SiO2) core obtained in step a) to the hydrophobic modifier solution, and react for 1-2 hours at 25-35℃ with ultrasonic power of 150-250W under ultrasonic assistance. Centrifuge, wash, and dry to obtain the hydrophobic modified silica (SiO2) core. c) The initiator, functional monomer, crosslinking agent and hydrophobic modified silica (SiO2) core obtained in step b) are mixed and reacted at 60-80℃ for 8-16 hours under nitrogen or argon protection using seed emulsion polymerization. The core is then coated with a resin shell to obtain a core-shell structured silica composite microsphere. d) Mix the core-shell structured silica composite microspheres obtained in step c) with a chloromethylating agent, add a phase transfer catalyst, react at 30-45℃ for 4-8 h, filter, and obtain a chloromethylated resin composite. e) The prepared chloromethylated resin complex is added to N,N-dimethylformamide (DMF) for swelling, guanidine salt is added, and sodium hydroxide or potassium hydroxide is added as an alkaline catalyst. The reaction is carried out at 50-70℃ for 6-12 hours, filtered, washed, and dried to obtain a high-temperature resistant guanidine-based strong base resin.
[0008] 3. The method for preparing the core-shell structure high-temperature resistant guanidine strong base resin is characterized in that the silicon source in step a) is tetraethyl orthosilicate (TEOS), tetraethoxysilane or methyl orthosilicate, the solvent is ethanol, isopropanol or deionized water, and the catalyst is ammonia, hydrochloric acid or sodium hydroxide.
[0009] 4. The method for preparing the core-shell structure high-temperature resistant guanidine strong base resin, characterized in that the hydrophobic modifier solution in step b) is a silane coupling agent isopropanol solution with a mass fraction of 0.1wt% to 5wt%.
[0010] 5. The method for preparing the core-shell structure high-temperature resistant guanidine strong base resin, characterized in that the initiator in step c) is azobisisobutyronitrile (AIBN), potassium persulfate (KPS) or ammonium persulfate, the functional monomer is styrene, butyl acrylate, methyl methacrylate or (meth)acrylamide, and the crosslinking agent is divinylbenzene (DVB) or ethylene glycol dimethacrylate.
[0011] 6. The method for preparing the core-shell structure high-temperature guanidine strong base resin, characterized in that the mass ratio of the initiator, functional monomer, crosslinking agent and hydrophobically modified silica (SiO2) core in step c) is 0.1-1:10-50:0.5-5:1-10.
[0012] 7. The method for preparing the core-shell structure high-temperature resistant guanidine strong base resin, characterized in that the chloromethylating agent in step d) is chloromethyl ether and the phase transfer catalyst is tetrabutylammonium bromide.
[0013] 8. The method for preparing the core-shell structure high-temperature resistant guanidine-based strong base resin, characterized in that the guanidine salt in step e) is guanidine hydrochloride or guanidine carbonate.
[0014] 9. The method for preparing the core-shell structure high-temperature resistant guanidine-based strong base resin, characterized in that, in step e), the mass ratio of guanidine salt to chloromethylated resin composite is 1:1 to 5:1, and the molar ratio of alkaline catalyst to guanidine salt is 1:1 to 3:1. Example
[0015] 50 mL of anhydrous ethanol (solvent), 2 mL of ammonia (catalyst, 28% concentration), and 10 mL of tetraethyl orthosilicate (TEOS, silicon source) were mixed. The mixture was stirred at room temperature for 2 h to induce a sol-gel reaction. After aging for 12 h, the mixture was washed and rinsed three times with deionized water, and then dried at 60 °C for 4 h to obtain the SiO2 core.
[0016] The obtained SiO2 cores were dispersed in 100 mL of 0.5 wt% silane coupling agent (e.g., isopropanol solution). The mixture was ultrasonically treated at 30 °C for 1.5 h at an ultrasonic power of 200 W. After centrifugation, washing, and drying at 60 °C, hydrophobically modified SiO2 cores were obtained.
[0017] c) Mix 0.2 g of azobisisobutyronitrile (AIBN), 20 g of styrene, 1 g of divinylbenzene (DVB), and 2 g of hydrophobically modified SiO2 core. Under nitrogen protection, add 100 mL of deionized water and react at 70 °C for 12 h. Filter, wash, and dry at 60 °C to obtain core-shell structured SiO2 composite microspheres.
[0018] d) Core-shell structured SiO2 composite microspheres were mixed with chloromethyl ether, and tetrabutylammonium bromide catalyst was added. The mixture was stirred at 35°C for 6 h. After filtration and washing with ethanol, the chloromethylated resin composite was obtained.
[0019] e) The chloromethylated resin complex was added to N,N-dimethylformamide (DMF) for swelling. Guanidine hydrochloride (guanidine salt) and sodium hydroxide (alkaline catalyst) were added. The mass ratio of guanidine salt to chloromethylated resin complex was 2:1, and the molar ratio of alkaline catalyst to guanidine salt was 2:1. The reaction was carried out at 60°C for 8 hours. After filtration, washing, and drying at 60°C, a high-temperature resistant guanidine-based strong base resin was obtained. Example
[0020] a) Mix 100 mL isopropanol (solvent), 1 mL hydrochloric acid (catalyst, 36% concentration), and 5 mL tetraethoxysilane (TEOS, silicon source). The remaining steps are the same as in Case 1.
[0021] b) Use 2 wt% silane coupling agent (e.g., isopropanol solution), and follow the same steps as in Case 1.
[0022] c) Mix 0.5 g potassium persulfate (KPS), 30 g methyl methacrylate, 2 g divinylbenzene (DVB), and 5 g hydrophobically modified SiO2 core. The remaining steps are the same as in Case 1.
[0023] d) Use guanidine carbonate (guanidine salt), with a mass ratio of guanidine salt to chloromethylated resin complex of 3:1 and a molar ratio of alkaline catalyst to guanidine salt of 1.5:1. The remaining steps are the same as in Case 1. Example
[0024] Mix 75 mL of deionized water (solvent), 0.5 mL of sodium hydroxide (catalyst, 1 mol / L concentration), and 7 mL of methyl orthosilicate (silicon source). The remaining steps are the same as in Case 1.
[0025] Use 1 wt% silane coupling agent (e.g., isopropanol solution). The remaining steps are the same as in Case 1.
[0026] Mix 1.0 g ammonium persulfate (initiator), 15 g butyl acrylate (functional monomer), 0.5 g ethylene glycol dimethacrylate (crosslinking agent), and 10 g hydrophobically modified SiO2 core. The remaining steps are the same as in Case 1.
[0027] Performance comparisons are shown in Table 1:
[0028] Guanidinization reaction group conversion rate (%) 61.45 64.99 54.86 Strong base exchange capacity (mmol / g) 2.09 2.32 1.84 Loss rate of strong alkali exchange capacity (%) after 24 hours in a constant temperature water bath at 97℃ 5.78 7.36 9.65
Claims
1. A core-shell structured high-temperature resistant guanidine-based strong base resin, characterized in that, The material is a core-shell composite, with the core being silicon dioxide (SiO2) and the shell being a guanidine-based strong base resin.
2. A method for preparing a core-shell structured high-temperature resistant guanidine-based strong base resin, characterized in that, Includes the following steps: a) A silicon source, solvent and catalyst are mixed to prepare a silicon dioxide (SiO2) core via the sol-gel method, followed by aging, washing and drying. b) Add the silica (SiO2) core obtained in step a) to the hydrophobic modifier solution, and react for 1-2 hours at 25-35℃ with ultrasonic power of 150-250W under ultrasonic assistance. Centrifuge, wash, and dry to obtain the hydrophobic modified silica (SiO2) core. c) The initiator, functional monomer, crosslinking agent and hydrophobic modified silica (SiO2) core obtained in step b) are mixed and reacted at 60-80℃ for 8-16 hours under nitrogen or argon protection using seed emulsion polymerization. The core is then coated with a resin shell to obtain a core-shell structured silica composite microsphere. d) Mix the core-shell structured silica composite microspheres obtained in step c) with a chloromethylating agent, add a phase transfer catalyst, react at 30-45℃ for 4-8 h, filter, and obtain a chloromethylated resin composite. e) The prepared chloromethylated resin complex is added to N,N-dimethylformamide (DMF) for swelling, guanidine salt is added, and sodium hydroxide or potassium hydroxide is added as an alkaline catalyst. The reaction is carried out at 50-70℃ for 6-12 hours, filtered, washed, and dried to obtain a high-temperature resistant guanidine-based strong base resin.
3. The method for preparing the core-shell structured high-temperature resistant guanidine-based strong base resin according to claim 2, characterized in that, The silicon source mentioned in step a) is tetraethyl orthosilicate (TEOS), tetraethoxysilane or methyl orthosilicate, the solvent is ethanol, isopropanol or deionized water, and the catalyst is ammonia, hydrochloric acid or sodium hydroxide.
4. The method for preparing the core-shell structured high-temperature resistant guanidine-based strong base resin according to claim 2, characterized in that, The hydrophobic modifier solution mentioned in step b) is a silane coupling agent isopropanol solution with a mass fraction of 0.1wt% to 5wt%.
5. The method for preparing the core-shell structured high-temperature resistant guanidine-based strong base resin according to claim 2, characterized in that, The initiator mentioned in step c) is azobisisobutyronitrile (AIBN), potassium persulfate (KPS) or ammonium persulfate, the functional monomer is styrene, butyl acrylate, methyl methacrylate or (meth)acrylamide, and the crosslinking agent is divinylbenzene (DVB) or ethylene glycol dimethacrylate.
6. The method for preparing the core-shell structured high-temperature resistant guanidine-based strong base resin according to claim 2, characterized in that, The mass ratio of the initiator, functional monomer, crosslinking agent and hydrophobically modified silica (SiO2) core mentioned in step c) is 0.1-1:10-50:0.5-5:1-10.
7. The method for preparing the core-shell structured high-temperature resistant guanidine-based strong base resin according to claim 2, characterized in that, The chloromethylating agent mentioned in step d) is chloromethyl ether, and the phase transfer catalyst is tetrabutylammonium bromide.
8. The method for preparing the core-shell structured high-temperature resistant guanidine-based strong base resin according to claim 2, characterized in that, The guanidine salt mentioned in step e) is guanidine hydrochloride or guanidine carbonate.
9. The method for preparing the core-shell structured high-temperature resistant guanidine-based strong base resin according to claim 2, characterized in that, In step e), the mass ratio of guanidine salt to chloromethylated resin complex is 1:1 to 5:1, and the molar ratio of alkaline catalyst to guanidine salt is 1:1 to 3:1.