An acrylic epoxy resin for white solder resist ink for PCBs and its preparation method
By grafting L-aspartic acid β-hydroxyoxime into the acrylic epoxy resin molecular chain, side chains containing hydroxyoxime and carboxyl groups are formed, solving the yellowing problem of white solder resist ink under long-term light and heat-oxidation conditions, improving color stability and light reflection performance, and making it suitable for LEDs and high-reflectivity PCBs.
Patent Information
- Application Number
- CN202611542004.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-04
- Publication Date
- 2026-11-17
AI Technical Summary
Existing white solder resist inks are prone to yellowing under long-term light and heat-oxygen conditions, affecting their color stability, especially in LED and high-reflectivity PCB applications.
L-aspartic acid β-hydroxyoxime is grafted onto the acrylic epoxy resin molecular chain, so that its side chain contains both hydroxyoxime group and carboxyl group. The hydroxyoxime group is enriched at the titanium dioxide pigment/resin interface, which increases the local effective concentration of carboxyl group near the interface and regulates the local interface environment to reduce the tendency of photooxidative yellowing.
It improves the color stability of white solder resist under long-term light and humid heat conditions, reduces yellowing, maintains whiteness and light reflection performance, and meets the application requirements of LED and high-reflectivity PCB.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of resin technology and relates to an acrylic epoxy resin for white solder resist ink for PCBs and its preparation method. Background Technology
[0002] PCB solder resist ink is mainly used to cover the surface of printed circuit board lines to protect the lines, prevent solder bridging, and improve the reliability of the circuit board. With the development of LED lighting, display devices, and high-reflectivity circuit boards, the application of white solder resist ink is gradually increasing. Compared with conventional solder resist ink, white solder resist ink, in addition to needing good adhesion, heat resistance, chemical resistance, and developability, also needs to have higher whiteness, hiding power, and light reflectivity.
[0003] Titanium dioxide, with its high refractive index and excellent light scattering properties, is a commonly used white pigment in white solder resist inks. To achieve good whiteness and hiding power, white solder resist inks typically require a high content of titanium dioxide. However, under prolonged exposure to light, heat, and oxygen, organic resin systems containing titanium dioxide are prone to photo-oxidative aging, causing changes in the resin structure and the formation of color-developing structures, leading to the gradual yellowing of the white solder resist film.
[0004] Yellowing of white solder resist not only affects its appearance but also leads to a decrease in whiteness and light reflectivity, especially in applications such as LEDs and high-reflectivity PCBs where high whiteness and color stability are required. Therefore, improving the yellowing resistance of acrylic epoxy resin used in white solder resist inks for PCBs, and ensuring that the resulting white solder resist maintains good color stability during long-term light exposure and use, is a technical problem that needs further resolution in this field. Summary of the Invention
[0005] The purpose of this invention is to provide an acrylic epoxy resin for white solder resist ink for PCBs and its preparation method, so as to improve the problem that existing white solder resist inks are prone to yellowing under long-term light exposure.
[0006] To achieve the above objectives, the present invention provides a method for preparing acrylic epoxy resin for white solder resist ink for PCBs, comprising the following steps:
[0007] S1. Epoxy resin and acrylic acid are subjected to ring-opening esterification reaction to obtain epoxy acrylate containing hydroxyl and olefin unsaturated groups;
[0008] S2. The epoxy acrylate obtained in step S1 is subjected to a half-esterification reaction with an acid anhydride, so that some of the hydroxyl groups in the epoxy acrylate are converted into carboxyl-containing side chains to obtain a carboxyl-containing acrylic epoxy resin.
[0009] S3. Activate some of the carboxyl groups in the acrylic epoxy resin containing carboxyl groups obtained in step S2 to obtain an acrylic epoxy resin containing activated carboxyl groups.
[0010] S4. Add L-aspartic acid β-hydroxyoxime acid to the reaction system obtained in step S3, so that the free amino group in L-aspartic acid β-hydroxyoxime acid undergoes an amidation reaction with the activated carboxyl group, and graft L-aspartic acid β-hydroxyoxime acid onto the side chain of the acrylic epoxy resin to obtain an acrylic epoxy resin for PCB white solder resist ink containing both hydroxyoxime acid group and carboxyl group in the side chain.
[0011] This invention grafts L-aspartic acid β-hydroxyoxime onto the molecular chain of a carboxyl-containing acrylic epoxy resin, thereby retaining both hydroxyoxime and carboxyl groups in the grafted side chain. The hydroxyoxime groups can generate strong interfacial interactions with the inorganic oxide sites on the surface of titanium dioxide pigments. When the acrylic epoxy resin is applied to a white solder resist ink containing titanium dioxide, the hydroxyoxime-containing side chains preferentially accumulate at the titanium dioxide pigment / resin interface.
[0012] Since the hydroxamic acid group and the carboxyl group are located in the same L-aspartic acid β-hydroxamic acid derived side chain, when the hydroxamic acid group generates a strong interfacial interaction at the titanium dioxide pigment / resin interface, the adjacent carboxyl group can be enriched in the local region of the interface, thereby increasing the local effective concentration of carboxyl groups near the interface. The carboxyl group can further participate in the regulation of the polar sites on the surface of titanium dioxide pigment and the adsorption state of interfacial water molecules, thereby changing the local interfacial environment of titanium dioxide pigment / resin and reducing the tendency of titanium dioxide to induce photo-oxidative yellowing of the resin.
[0013] Therefore, this invention does not utilize the effects of hydroxamic acid group or carboxyl group alone, but rather utilizes the interfacial positioning effect of hydroxamic acid group to create conditions for adjacent carboxyl groups to play their role near the titanium dioxide pigment / resin interface, so that the two groups form a synergy in terms of spatial position and action sequence.
[0014] Preferably, in step S1, the epoxy resin is a phenolic epoxy resin.
[0015] More preferably, the phenolic epoxy resin is o-cresol phenolic epoxy resin with an epoxy equivalent of 200-220 g / eq.
[0016] Preferably, in step S1, the epoxy resin and acrylic acid undergo a ring-opening esterification reaction at 95–105°C in the presence of a polymerization inhibitor and an esterification catalyst.
[0017] More preferably, the polymerization inhibitor is p-methoxyphenol, and the esterification catalyst is triphenylphosphine.
[0018] Preferably, in step S2, the acid anhydride is tetrahydrophthalic anhydride, and the temperature of the semi-esterification reaction is 90-105°C, so that the solid acid value of the resulting carboxyl-containing acrylic epoxy resin is 50-70 mgKOH / g.
[0019] Preferably, in step S3, carbodiimide and N-hydroxysuccinimide are used to activate some of the carboxyl groups in the carboxyl-containing acrylic epoxy resin.
[0020] More preferably, the carbodiimide is dicyclohexylcarbodiimide, and the activation reaction temperature in step S3 is 10–25°C.
[0021] Preferably, in step S4, the amount of L-aspartic acid β-hydroxyoxime added is 0.5 to 5 mol of the total initial number of epoxy groups in the epoxy resin used to prepare the acrylic epoxy resin.
[0022] More preferably, the amount of L-aspartic acid β-hydroxyoxime added is 1 to 3 mol of the total number of initial epoxy groups.
[0023] L-Aspartic acid β-hydroxyoxime is grafted into the acrylic epoxy resin molecular chain at a low ratio. This can form a titanium dioxide pigment / resin interface regulation effect while reducing changes to the original acrylic epoxy resin main structure, acid value and polarity. This is beneficial to balance the resin's photosensitive curing performance, alkali development performance and the basic performance of the resulting solder resist film.
[0024] Preferably, the amidation reaction temperature in step S4 is 20–35°C.
[0025] The present invention also provides an acrylic epoxy resin for white solder resist ink for PCBs prepared by the above preparation method, wherein the side chain of the acrylic epoxy resin contains both hydroxamic acid groups and carboxyl groups.
[0026] The beneficial effects of this invention are:
[0027] (1) The present invention grafts L-aspartic acid β-hydroxyoxime into the molecular chain of acrylic epoxy resin containing carboxyl groups, so that the same side chain has both hydroxyoxime group and carboxyl group; wherein, the hydroxyoxime group is beneficial to the side chain preferentially enriched at the titanium dioxide pigment / resin interface, thereby increasing the local effective concentration of adjacent carboxyl groups near the interface, so that they can further participate in the regulation of local interface state, thereby reducing the tendency of titanium dioxide to induce photo-oxidative yellowing of resin, and improving the color stability and yellowing resistance of white solder resist film under long-term light exposure conditions.
[0028] (2) By introducing a small amount of L-aspartic acid β-hydroxyoxime derivative side chain into the acrylic epoxy resin molecular chain, the present invention only performs local functionalization modification on the resin without significantly changing the main structure of the acrylic epoxy resin. Therefore, it is beneficial to maintain its photosensitive curing and developing process adaptability as a resin for PCB white solder resist ink, while avoiding significant changes in the basic application performance of the resin due to the introduction of functional groups.
[0029] (3) This invention utilizes the existing carboxyl groups of the carboxyl-containing acrylic epoxy resin as grafting sites, and introduces L-aspartic acid β-hydroxyoxime acid through carboxyl activation and amidation reaction. There is no need to rebuild the main skeleton of the acrylic epoxy resin. The preparation route has good compatibility with the existing preparation system of acrylic epoxy resin for white solder resist ink of PCB, which is easy to implement. Detailed Implementation
[0030] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with embodiments, is provided below.
[0031] The following descriptions explain some of the raw materials used in the examples, comparative examples, and preparation examples:
[0032] o-Cresol phenolic epoxy resin: sourced from DIC Corporation, model EPICLON N-680, with an epoxy equivalent of 200-220 g / eq; the batches used in this example and comparative example had an epoxy equivalent of 212.6 g / eq measured according to GB / T 4612-2008.
[0033] L-Aspartic acid β-hydroxyoxime: CAS No. 1955-68-6, purity not less than 98%;
[0034] Rutile titanium dioxide: sourced from Ishihara Sangyo Co., Ltd., model number TIPAQUE® R980;
[0035] Dispersant: DISPERBYK-110;
[0036] Defoamer: BYK-088;
[0037] Leveling agent: BYK-333;
[0038] Bisphenol A type epoxy resin: sourced from DIC Corporation, model EPICLON 850, epoxy equivalent of 184-194 g / eq, solid content not less than 99%;
[0039] Except for the raw materials explicitly stated above, all other raw materials not specifically mentioned are commercially available products and can be obtained through commercial channels.
[0040] Example 1
[0041] A method for preparing an acrylic epoxy resin for white solder resist ink on PCBs includes the following steps:
[0042] S1. Add 212.6 parts of o-cresol phenolic epoxy resin with an epoxy equivalent of 212.6 g / eq, 100 parts of diethylene glycol monoethyl ether acetate, and 0.10 parts of p-methoxyphenol to a reaction vessel equipped with a stirrer, thermometer, and condenser. Heat to 85°C under stirring to fully dissolve the o-cresol phenolic epoxy resin. Add 72 parts of acrylic acid and 0.8 parts of triphenylphosphine, and heat to 100°C for ring-opening esterification reaction. Stir continuously during the reaction and introduce a small amount of air to inhibit the polymerization of acrylic acid groups. React at 100°C for 5–7 h. The reaction endpoint is defined as the acid value decreasing to below 5 mg KOH / g based on solids, to obtain epoxy acrylate containing hydroxyl and olefinic unsaturated groups.
[0043] S2. While stirring, adjust the temperature of the reaction system to 95℃, add 52 parts of tetrahydrophthalic anhydride, and react at 95℃ for 3-4 h to allow the tetrahydrophthalic anhydride to undergo a semi-esterification reaction with some of the hydroxyl groups formed in step S1. The reaction endpoint is taken as the acid value reaches 56 mgKOH / g based on solids to obtain a carboxyl-containing acrylic epoxy resin.
[0044] S3. While stirring, cool the reaction system obtained in step S2 to 15°C, add 15 parts of N-methylpyrrolidone, then add 2.06 parts of dicyclohexylcarbodiimide and 1.15 parts of N-hydroxysuccinimide in sequence, react at 15°C for 1.5 h, then raise the temperature to 25°C and continue the reaction for 3 h, so that some of the carboxyl groups in the carboxyl-containing acrylic epoxy resin form activated esters; after the reaction is completed, filter to remove dicyclohexylurea, and obtain acrylic epoxy resin containing activated carboxyl groups.
[0045] S4. Add 1.48 parts of L-aspartic acid β-hydroxyoxime acid and 1.29 parts of N,N-diisopropylethylamine to 10 parts of N-methylpyrrolidone, mix well, and then slowly add to the reaction system obtained in step S3. Keep stirring and react at 25°C for 6 h to allow the free amino group in L-aspartic acid β-hydroxyoxime acid to undergo an amidation reaction with the activated carboxyl group, grafting L-aspartic acid β-hydroxyoxime acid into the acrylic epoxy resin molecular chain. After the reaction is completed, add diethylene glycol monoethyl ether acetate to adjust the solid content of the system to 70±1% to obtain acrylic epoxy resin for PCB white solder resist ink.
[0046] In this embodiment, the amount of L-aspartic acid β-hydroxyoxime added is 1 mol, based on the total number of initial epoxy groups in the o-cresol phenolic epoxy resin.
[0047] Example 2
[0048] A method for preparing an acrylic epoxy resin for white solder resist ink on PCBs includes the following steps:
[0049] S1. Add 212.6 parts of o-cresol phenolic epoxy resin with an epoxy equivalent of 212.6 g / eq, 100 parts of diethylene glycol monoethyl ether acetate, and 0.10 parts of p-methoxyphenol to a reaction vessel equipped with a stirrer, thermometer, and condenser. Heat to 85°C under stirring to fully dissolve the o-cresol phenolic epoxy resin. Add 72 parts of acrylic acid and 0.8 parts of triphenylphosphine, and heat to 100°C for ring-opening esterification reaction. Stir continuously during the reaction and introduce a small amount of air to inhibit the polymerization of acrylic acid groups. React at 100°C for 5–7 h. The reaction endpoint is defined as the acid value decreasing to below 5 mg KOH / g based on solids, to obtain epoxy acrylate containing hydroxyl and olefinic unsaturated groups.
[0050] S2. While stirring, adjust the temperature of the reaction system to 95℃, add 52 parts of tetrahydrophthalic anhydride, and react at 95℃ for 3-4 h to allow the tetrahydrophthalic anhydride to undergo a semi-esterification reaction with some of the hydroxyl groups formed in step S1. The reaction endpoint is taken as the acid value reaches 56 mgKOH / g based on solids to obtain a carboxyl-containing acrylic epoxy resin.
[0051] S3. While stirring, cool the reaction system obtained in step S2 to 15°C, add 15 parts of N-methylpyrrolidone, then add 4.13 parts of dicyclohexylcarbodiimide and 2.30 parts of N-hydroxysuccinimide in sequence, react at 15°C for 1.5 h, then raise the temperature to 25°C and continue the reaction for 3 h, so that some of the carboxyl groups in the carboxyl-containing acrylic epoxy resin form activated esters; after the reaction is completed, filter to remove dicyclohexylurea, and obtain acrylic epoxy resin containing activated carboxyl groups.
[0052] S4. Add 2.96 parts of L-aspartic acid β-hydroxyoxime acid and 2.58 parts of N,N-diisopropylethylamine to 10 parts of N-methylpyrrolidone, mix well, and then slowly add to the reaction system obtained in step S3. Keep stirring and react at 25°C for 6 h to allow the free amino group in L-aspartic acid β-hydroxyoxime acid to undergo an amidation reaction with the activated carboxyl group, grafting L-aspartic acid β-hydroxyoxime acid into the acrylic epoxy resin molecular chain. After the reaction is completed, add diethylene glycol monoethyl ether acetate to adjust the solid content of the system to 70±1% to obtain acrylic epoxy resin for PCB white solder resist ink.
[0053] In this embodiment, the amount of L-aspartic acid β-hydroxyoxime added is 2 mol, based on the total number of initial epoxy groups in the o-cresol phenolic epoxy resin.
[0054] Example 3
[0055] A method for preparing an acrylic epoxy resin for white solder resist ink on PCBs includes the following steps:
[0056] S1. Add 212.6 parts of o-cresol phenolic epoxy resin with an epoxy equivalent of 212.6 g / eq, 100 parts of diethylene glycol monoethyl ether acetate, and 0.10 parts of p-methoxyphenol to a reaction vessel equipped with a stirrer, thermometer, and condenser. Heat to 85°C under stirring to fully dissolve the o-cresol phenolic epoxy resin. Add 72 parts of acrylic acid and 0.8 parts of triphenylphosphine, and heat to 100°C for ring-opening esterification reaction. Stir continuously during the reaction and introduce a small amount of air to inhibit the polymerization of acrylic acid groups. React at 100°C for 5–7 h. The reaction endpoint is defined as the acid value decreasing to below 5 mg KOH / g based on solids, to obtain epoxy acrylate containing hydroxyl and olefinic unsaturated groups.
[0057] S2. While stirring, adjust the temperature of the reaction system to 95℃, add 52 parts of tetrahydrophthalic anhydride, and react at 95℃ for 3-4 h to allow the tetrahydrophthalic anhydride to undergo a semi-esterification reaction with some of the hydroxyl groups formed in step S1. The reaction endpoint is taken as the acid value reaches 56 mg KOH / g based on solids to obtain a carboxyl-containing acrylic epoxy resin.
[0058] S3. While stirring, cool the reaction system obtained in step S2 to 15°C, add 15 parts of N-methylpyrrolidone, then add 6.19 parts of dicyclohexylcarbodiimide and 3.45 parts of N-hydroxysuccinimide in sequence, react at 15°C for 1.5 h, then raise the temperature to 25°C and continue the reaction for 3 h, so that some of the carboxyl groups in the carboxyl-containing acrylic epoxy resin form activated esters; after the reaction is completed, filter to remove dicyclohexylurea, and obtain acrylic epoxy resin containing activated carboxyl groups.
[0059] S4. Add 4.44 parts of L-aspartic acid β-hydroxyoxime acid and 3.88 parts of N,N-diisopropylethylamine to 10 parts of N-methylpyrrolidone, mix well, and then slowly add to the reaction system obtained in step S3. Keep stirring and react at 25°C for 6 h to allow the free amino group in L-aspartic acid β-hydroxyoxime acid to undergo an amidation reaction with the activated carboxyl group, grafting L-aspartic acid β-hydroxyoxime acid into the acrylic epoxy resin molecular chain. After the reaction is completed, add diethylene glycol monoethyl ether acetate to adjust the solid content of the system to 70±1% to obtain acrylic epoxy resin for PCB white solder resist ink.
[0060] In this embodiment, the amount of L-aspartic acid β-hydroxyoxime added is 3 mol, based on the total number of initial epoxy groups in the o-cresol phenolic epoxy resin.
[0061] Comparative Example 1
[0062] A method for preparing an acrylic epoxy resin for white solder resist ink on PCBs includes the following steps:
[0063] The difference from Example 2 is that steps S3 and S4 are omitted.
[0064] Specifically, after the reaction in step S2 was completed, the reaction system was cooled to 25°C, 25 parts of N-methylpyrrolidone were added and stirred until homogeneous, and then diethylene glycol monoethyl ether acetate was added to adjust the solid content of the system to 70±1%, thus obtaining the acrylic epoxy resin of Comparative Example 1. The remaining steps and conditions were the same as in Example 2.
[0065] Comparative Example 2
[0066] A method for preparing an acrylic epoxy resin for white solder resist ink on PCBs includes the following steps:
[0067] The difference from Example 2 is that in step S4, L-aspartic acid β-hydroxyoxime acid is replaced with β-alanine.
[0068] Specifically, 2.96 parts of L-aspartic acid β-hydroxyoxime acid were replaced with 1.78 parts of β-alanine, and 2.58 parts of N,N-diisopropylethylamine were added to induce an amidation reaction between the amino group and the activated carboxyl group in β-alanine. This grafted β-alanine onto the acrylic epoxy resin molecular chain, resulting in an acrylic epoxy resin with only carboxyl functional side chains. The obtained resin was tested and found to have a solid acid value of 55–56 mgKOH / g. The remaining steps and conditions were the same as in Example 2.
[0069] Comparative Example 3
[0070] A method for preparing an acrylic epoxy resin for white solder resist ink on PCBs includes the following steps:
[0071] The difference from Example 2 is that in step S2, the amount of tetrahydrophthalic anhydride was adjusted from 52 parts to 55 parts, and the reaction was carried out at 95°C for 3-4 hours. The reaction endpoint was reached when the acid value reached 59 mgKOH / g based on solids, yielding a carboxyl-containing acrylic epoxy resin. In step S4, L-aspartic acid β-hydroxyxamic acid was replaced with glycine hydroxyxamic acid.
[0072] Specifically, 2.96 parts of L-aspartic β-hydroxyxamic acid were replaced with 1.80 parts of glycine hydroxamic acid, and 2.58 parts of N,N-diisopropylethylamine were added to induce an amidation reaction between the amino group and the activated carboxyl group in the glycine hydroxamic acid. This grafted glycine hydroxamic acid onto the acrylic epoxy resin molecular chain, yielding an acrylic epoxy resin containing hydroxamic acid functional grafted side chains. The resulting resin was tested and found to have a solid acid value of 56–57 mgKOH / g. The remaining steps and conditions were the same as in Example 2.
[0073] Comparative Example 4
[0074] A method for preparing an acrylic epoxy resin for white solder resist ink on PCBs includes the following steps:
[0075] The difference from Example 2 is as follows: In step S2, the amount of tetrahydrophthalic anhydride was adjusted from 52 parts to 55 parts, and the reaction was carried out at 95°C for 3-4 hours. The reaction endpoint was reached when the acid value reached 59 mgKOH / g based on solids, yielding a carboxyl-containing acrylic epoxy resin. In step S3, the amount of dicyclohexylcarbodiimide was adjusted to 8.25 parts, and the amount of N-hydroxysuccinimide was adjusted to 4.60 parts, so that some of the carboxyl groups in the carboxyl-containing acrylic epoxy resin underwent an activation reaction, and the amount of activated carboxyl groups was equivalent to 4 mol% of the total initial number of epoxy groups in the o-cresol phenolic epoxy resin. In step S4, L-aspartic acid β-hydroxyoxime acid was replaced with a composition of β-alanine and glycine hydroxyoxime acid.
[0076] Specifically, 2.96 parts of L-aspartic β-hydroxyxamic acid were replaced with 1.78 parts of β-alanine and 1.80 parts of glycine hydroxyxamic acid, and 5.17 parts of N,N-diisopropylethylamine were added. This caused the amino groups in β-alanine and glycine hydroxyxamic acid to undergo amidation reactions with activated carboxyl groups, respectively, grafting β-alanine and glycine hydroxyxamic acid onto the acrylic epoxy resin molecular chain. The resulting resin contained both carboxyl-containing grafted side chains and hydroxyxamic acid-containing grafted side chains, but the carboxyl and hydroxyxamic acid groups were located in different grafted side chains. The resulting resin was tested and found to have a solid acid value of 56–57 mgKOH / g. The remaining steps and conditions were the same as in Example 2.
[0077] Preparation Example
[0078] A white solder resist ink for PCBs comprises the following raw materials in parts by weight: 85 parts of an acrylic epoxy resin solution with a solid content of 70±1%, 55 parts of rutile titanium dioxide, 8 parts of bisphenol A epoxy resin, 10 parts of dipentaerythritol hexaacrylate, 10 parts of barium sulfate, 2.0 parts of 2,4,6-trimethylbenzoyl diphenylphosphine oxide, 0.8 parts of bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 0.3 parts of 2-ethyl-4-methylimidazole, 0.5 parts of dispersant (DISPERBYK-110), 0.2 parts of defoamer (BYK-088), 0.2 parts of leveling agent (BYK-333), and 22 parts of diethylene glycol monoethyl ether acetate.
[0079] A method for preparing a white solder resist ink for PCBs includes the following steps:
[0080] Y1. Add acrylic epoxy resin, dipentaerythritol hexaacrylate, part of diethylene glycol monoethyl ether acetate, dispersant and defoamer to a dispersion container and stir at 500-800 r / min for 10 min; then gradually add rutile titanium dioxide and barium sulfate, increase the speed to 1500-2000 r / min, and continue to disperse for 30 min.
[0081] Y2. The obtained mixture is ground by three roller mills to a fineness of no more than 10 μm. After the material temperature drops to below 35℃, bisphenol A epoxy resin, 2,4,6-trimethylbenzoyl diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2-ethyl-4-methylimidazole and leveling agent are added, along with the remaining diethylene glycol monoethyl ether acetate. The mixture is stirred at 500-800 r / min in the dark for 20 min to obtain white solder resist ink for PCB.
[0082] The acrylic epoxy resins prepared in Examples 1-3 and Comparative Examples 1-4 were used as the above-mentioned acrylic epoxy resins, while the other raw materials and preparation conditions remained unchanged, and the white solder resist inks for PCBs prepared in Examples 1-7 were obtained accordingly.
[0083] In this context, Preparation Examples 1 to 3 correspond to the acrylic epoxy resins obtained in Examples 1 to 3, and Preparation Examples 4 to 7 correspond to the acrylic epoxy resins obtained in Comparative Examples 1 to 4.
[0084] Test case
[0085] Test samples were prepared using the white solder resist inks for PCBs prepared in Examples 1-7, respectively. The specific methods are as follows: The white solder resist inks were coated onto the cleaned copper-clad laminate surface and pre-baked at 80°C for 20 min; ultraviolet exposure was performed using the same exposure equipment at an exposure dose of 500 mJ / cm²; subsequently, development was performed using a 1% sodium carbonate aqueous solution at 30°C, followed by washing and drying, and then curing at 150°C for 60 min to obtain the test samples. The dry film thickness of the solder resist was controlled to be 20 ± 2 μm.
[0086] The above test samples were subjected to the following performance tests:
[0087] Test 1: Light yellowing resistance test
[0088] Each test group used three parallel test samples. A spectrophotometer was used to measure the b* value of each sample before UV irradiation under D65 standard light source and 10° standard observer conditions; this value was recorded as b*0. Subsequently, the test samples were irradiated with a metal halide lamp for a cumulative UV irradiation dose of 50 J / cm². After irradiation, the b* value was measured again and recorded as b*1. The yellowing value was calculated using the following formula: Δb* = b*1 - b*0. The average value of the three parallel test samples was taken as the result for each group of tests.
[0089] The smaller the Δb* value, the lower the degree of yellowing of the solder resist film after ultraviolet irradiation, and the better its resistance to light yellowing.
[0090] Test 2: Resistance to light yellowing after damp heat treatment
[0091] Each test sample was placed in a constant temperature and humidity environment of 85℃ and 85% for 72 hours. After being removed, it was placed at room temperature for 2 hours to allow the test sample to return to a stable state.
[0092] Subsequently, using the same colorimetric conditions as in Test 1, the b* value of each test sample after damp heat treatment was measured and recorded as b*0. The test samples were then subjected to ultraviolet irradiation using a metal halide lamp, with a cumulative ultraviolet irradiation dose of 50 J / cm². After irradiation, the b* value was measured again and recorded as b*1. The yellowing value before and after ultraviolet irradiation following damp heat treatment was calculated using the following formula: Δb* = b*1 - b*0. The average value of three parallel test samples was taken as the result for each group of tests.
[0093] The smaller the Δb* value, the lower the degree of yellowing of the solder resist film after damp heat treatment and subsequent ultraviolet irradiation, indicating that it still has good yellowing resistance under the combined effects of damp heat and light.
[0094] The test results are shown in the table below:
[0095]
[0096] The test results show that the Δb* values of the white solder resist inks obtained in Preparation Examples 1-3 after UV irradiation at 50 J / cm² were 1.72, 1.49, and 1.58, respectively, which were significantly lower than the 2.62 of Preparation Example 4 without graft modification. This indicates that introducing L-aspartic acid β-hydroxyoxime-derived side chains into the acrylic epoxy resin molecular chain can effectively reduce the yellowing degree of the white solder resist film under UV irradiation conditions and improve its resistance to light yellowing.
[0097] Among them, Preparation Example 2 had the lowest Δb* at 1.49, indicating that when the amount of L-aspartic acid β-hydroxyoxime added was 2 mol% of the initial epoxy group, the resulting resin exhibited superior resistance to photoyellowing. Preparation Example 1 had a lower grafting amount, resulting in a relatively smaller number of functional side chains that could act on the titanium dioxide pigment / resin interface, thus its Δb* was higher than that of Preparation Example 2. When the grafting amount was further increased to 3 mol%, the Δb* of Preparation Example 3 was 1.58, and did not continue to decrease, indicating that the increase in functional side chains is not a simple linear relationship with resistance to yellowing; an appropriate amount of these side chains is more conducive to the interface regulation effect.
[0098] In Preparation Example 5, only a carboxyl-containing grafted side chain was introduced, and its Δb* was 2.47, only slightly lower than that of Preparation Example 4. In Preparation Example 6, only a hydroxamic acid-containing grafted side chain was introduced, and its Δb* was 2.25, showing a higher degree of improvement than Preparation Example 5, but still significantly higher than Preparation Examples 1-3. The above results indicate that adding a carboxyl group or introducing a hydroxamic acid group alone can affect the photochromic resistance of the white solder resist to some extent, but the effect is relatively limited.
[0099] In Preparation Example 7, the carboxyl and hydroxamic acid groups were located in different grafted side chains, and the Δb* decreased to 1.96, indicating that the simultaneous presence of both types of groups could further improve the photo-yellowing resistance; however, the degree of improvement was still weaker than in Preparation Example 2. This shows that simply having both hydroxamic acid and carboxyl groups present in the resin system does not achieve the same effect as the L-aspartic acid β-hydroxamic acid derived side chain. In contrast, when the hydroxamic acid and carboxyl groups are located in the same side chain, the localization effect of the hydroxamic acid group on the titanium dioxide pigment / resin interface is beneficial to increasing the local effective concentration of adjacent carboxyl groups near the interface, resulting in a more significant synergistic effect between the two, thereby further reducing titanium dioxide-induced photooxidative yellowing of the resin.
[0100] After treatment at 85℃ and 85%RH for 72 h, the Δb* values of all samples increased, indicating that the humid and hot environment exacerbates the yellowing of the white solder resist film under subsequent UV irradiation. Specifically, the Δb* value of Preparation Example 4 increased from 2.62 to 2.98, Preparation Examples 5 and 6 increased to 2.82 and 2.56 respectively, while Preparation Example 7 increased to 2.22. In contrast, Preparation Examples 1–3 remained at relatively low levels with values of 1.95, 1.69, and 1.82 respectively, with Preparation Example 2 showing the best performance.
[0101] The above results are consistent with the aforementioned titanium dioxide pigment / resin interface regulation mechanism, and indicate that the resin of the present invention can still maintain good resistance to photoyellowing under humid and hot conditions, thereby improving the color stability of the white solder resist film under the combined effects of humid heat and light. The present invention, by grafting L-aspartic acid β-hydroxyxamic acid into the acrylic epoxy resin molecular chain, simultaneously retains both hydroxamic acid and carboxyl groups in the same side chain, achieving superior resistance to photoyellowing compared to unmodified resin, single carboxyl side chain, single hydroxamic acid side chain, and when the two groups are located in different side chains. This indicates that the structure is not a simple superposition of the effects of the two types of functional groups, but rather has a significant synergistic effect.
[0102] In summary, this invention grafts L-aspartic acid β-hydroxyxamic acid onto the molecular chain of a carboxyl-containing acrylic epoxy resin, allowing the resulting resin side chain to retain both hydroxamic acid and carboxyl groups. Utilizing the localizing effect of the hydroxamic acid groups on the titanium dioxide pigment / resin interface, the effective local concentration of adjacent carboxyl groups near the titanium dioxide pigment / resin interface is increased, thereby regulating the local environment of the titanium dioxide pigment / resin interface. Test results show that the white solder resist ink for PCBs made with the resin of this invention exhibits low Δb* values under both UV irradiation and post-humid heat UV irradiation conditions, indicating its effective improvement in the photo-yellowing resistance of the white solder resist film. Furthermore, compared to comparative examples containing only carboxyl side chains, only hydroxamic acid side chains, and those with carboxyl and hydroxamic acid located on different side chains, the synergistic structure of hydroxamic acid and carboxyl groups in the same side chain of this invention exhibits better yellowing resistance, demonstrating that this structure has good interface regulation capabilities and application value.
[0103] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for preparing an acrylic epoxy resin for white solder resist ink on PCBs, characterized in that, Includes the following steps: S1. Epoxy resin and acrylic acid are subjected to ring-opening esterification reaction to obtain epoxy acrylate containing hydroxyl and olefin unsaturated groups; S2. The epoxy acrylate obtained in step S1 is subjected to a half-esterification reaction with an acid anhydride, so that some of the hydroxyl groups in the epoxy acrylate are converted into carboxyl-containing side chains to obtain a carboxyl-containing acrylic epoxy resin. S3. Activate some of the carboxyl groups in the acrylic epoxy resin containing carboxyl groups obtained in step S2 to obtain an acrylic epoxy resin containing activated carboxyl groups. S4. Add L-aspartic acid β-hydroxyoxime acid to the reaction system obtained in step S3, so that the amino group in L-aspartic acid β-hydroxyoxime acid undergoes an amidation reaction with the activated carboxyl group, and graft L-aspartic acid β-hydroxyoxime acid onto the side chain of the acrylic epoxy resin to obtain an acrylic epoxy resin for PCB white solder resist ink containing both hydroxyoxime acid group and carboxyl group in the side chain.
2. The method for preparing acrylic epoxy resin for PCB white solder resist ink according to claim 1, characterized in that, In step S1, the epoxy resin is a phenolic epoxy resin.
3. The method for preparing acrylic epoxy resin for PCB white solder resist ink according to claim 2, characterized in that, The phenolic epoxy resin is o-cresol phenolic epoxy resin with an epoxy equivalent of 200-220 g / eq.
4. The method for preparing acrylic epoxy resin for PCB white solder resist ink according to claim 1, characterized in that, In step S1, the epoxy resin and acrylic acid undergo a ring-opening esterification reaction at 95–105°C in the presence of a polymerization inhibitor and an esterification catalyst.
5. The method for preparing acrylic epoxy resin for PCB white solder resist ink according to claim 4, characterized in that, The polymerization inhibitor is p-methoxyphenol, and the esterification catalyst is triphenylphosphine.
6. The method for preparing acrylic epoxy resin for PCB white solder resist ink according to claim 1, characterized in that, In step S2, the acid anhydride is tetrahydrophthalic anhydride, and the temperature of the semi-esterification reaction is 90-105°C, so that the solid acid value of the resulting carboxyl-containing acrylic epoxy resin is 50-70 mgKOH / g.
7. The method for preparing acrylic epoxy resin for PCB white solder resist ink according to claim 1, characterized in that, In step S3, carbodiimide and N-hydroxysuccinimide are used to activate some of the carboxyl groups in the carboxyl-containing acrylic epoxy resin.
8. The method for preparing acrylic epoxy resin for PCB white solder resist ink according to claim 7, characterized in that, The carbodiimide is dicyclohexylcarbodiimide, and the activation reaction temperature in step S3 is 10–25 °C.
9. The method for preparing acrylic epoxy resin for PCB white solder resist ink according to claim 1, characterized in that, In step S4, the amount of L-aspartic acid β-hydroxyoxime added is 0.5 to 5 mol% of the total initial epoxy groups in the epoxy resin used to prepare the acrylic epoxy resin, and the temperature of the amidation reaction is 20 to 35°C.
10. An acrylic epoxy resin for white solder resist ink for PCBs, characterized in that, The acrylic epoxy resin is prepared by the preparation method according to any one of claims 1 to 9, and the side chain of the acrylic epoxy resin contains both hydroxamic acid group and carboxyl group.