Triarylamine conjugated polymers, materials, devices and electronic equipment
By designing triarylamine conjugated polymers and utilizing the synergistic effect of fluorene derivatives and triphenylamine side groups, an electrochromic effect with rapid color change and high optical contrast under low voltage was achieved, solving the problems of slow color change speed and insufficient transparency of existing materials.
Patent Information
- Application Number
- CN202510623490.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing electrochromic materials cannot achieve a rapid transition from a transparent neutral state to a dark tinted state, and the color-changing speed is slow, which cannot meet the high requirements of dynamic display effects.
By using a triarylamine conjugated polymer and a fluorene derivative as a rigid conjugated backbone, combined with the precise control of triphenylamine side groups, the distribution of side groups with different electron-donating capabilities can be controlled to achieve the coexistence of multiple valence states, reduce the driving voltage, and improve the color-changing speed.
It achieves low-voltage driving, uniform film formation, and color state transmittance of less than 5%, and has high optical contrast and fast color change response characteristics, thus improving the overall performance of electrochromic devices.
Smart Images

Figure CN123107044A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of display technology, and in particular to a triarylamine conjugated polymer, material, device, and electronic device. Background Technology
[0002] Electrochromic technology is a functional technology that achieves reversible color changes by modulating the electronic structure or optical properties of materials using an electric field. Its core advantages include low power consumption, millisecond-level fast response, and low manufacturing cost. It is widely recognized as a passive display technology with significant commercial potential in fields such as electronic tags, electronic paper, and low-refresh-rate displays.
[0003] In the early stages, inorganic electrochromic materials, such as tungsten oxide, nickel oxide, and vanadium oxide, were extensively studied. However, inorganic electrochromic materials and devices suffer from significant technical bottlenecks, such as limited color options, slow response speeds, and difficulties in large-area coating processes. In recent decades, research on conductive polymer electrochromic materials and corresponding devices has flourished, including polymer electrochromic materials such as polythiophene, polypyrrole, and polyaniline. These materials have attracted widespread attention due to their rich and tunable colors, low driving voltages, and ability to be prepared in large areas using solution methods. However, the highly conjugated molecular structure of these materials results in noticeable color residue under visible light, an inability to transition from a transparent neutral state to a dark-colored state, and slow color-changing response speeds, thus limiting the effectiveness of dynamic displays. Summary of the Invention
[0004] In view of this, this application provides a triarylamine conjugated polymer, material, device and electronic device that can solve the problems of being unable to achieve the transition from a transparent neutral state to a dark colored state and the slow color change speed.
[0005] Some embodiments of this application provide a triarylamine conjugated polymer. The application is described below from multiple aspects, and the embodiments and beneficial effects of these aspects can be referred to each other.
[0006] In a first aspect, embodiments of this application provide a triarylamine conjugated polymer, characterized in that the triarylamine conjugated polymer comprises units with the general structural formula (1):
[0007]
[0008] In equation (1), 0 < n < 50, and n is a natural number, a + b + c + d = 1, (a + b) / (c + d) = 1:1, and 0 < a ≤ 0.15, 0 < c ≤ 0.2;
[0009] Unit A is a derivative of fluorene;
[0010] Each B group is independently selected from hydrogen, fluorine, methyl, trifluoromethyl, oxymethyl, phenyl, 2,4,6-trimethylphenyl, 4-methylphenyl, 4-methoxyphenyl, alkyl C x H 2x+1 x is a natural number from 1 to 10, oxygen-substituted alkyl chain OC x H 2x+1 x is a natural number from 1 to 10, and is an oligoether group. m is a natural number from 1 to 4;
[0011] The C group can be hydrogen, fluorine, methyl, trifluoromethyl, oxymethyl, phenyl, 2,4,6-trimethylphenyl, 4-methylphenyl, 4-methoxyphenyl, or alkyl C. x H 2x+1 x is a natural number from 1 to 10, and the alkyl chain is oxygen-substituted (OC). x H 2x+1 x is a natural number from 1 to 10, and the OC is an oxygen-substituted alkenyl chain. x H 2x-1 x is a natural number from 1 to 10, or an oligoether group. m is a natural number from 1 to 4;
[0012] The D group is selected from hydrogen, fluorine, methyl, trifluoromethyl, oxymethyl, phenyl, 2,4,6-trimethylphenyl, 4-methylphenyl, 4-methoxyphenyl, alkyl C x H 2x+1 x is a natural number from 1 to 10, oxygen-substituted alkyl chain OC x H 2x+1 x is a natural number from 1 to 10, or an oligoether group. m is a natural number from 1 to 4, wherein the B group and the D group are not both alkyl groups.
[0013] The triarylamine conjugated polymer of this application utilizes fluorene derivatives as a rigid conjugated backbone to enhance charge transport capabilities. By precisely controlling the proportion of triphenylamine side groups, the distribution of side groups with different electron-donating abilities is controlled, thereby affecting the overall electron cloud density and redox properties of the molecule. Furthermore, the synergistic effect of the electron-donating effect of fluorene derivatives and triphenylamine allows the colored state to be formed at a lower voltage, reducing the driving voltage. Moreover, the different electron-donating abilities of the triphenylamine side groups cause differentiated oxidation of triphenylamine units with different side groups at the same voltage (some units preferentially lose electrons). This multi-valence coexistence phenomenon allows the polymer material to achieve a high colored state at low voltage, significantly reducing transmittance to less than 5%.
[0014] As an embodiment of the first aspect of this application, the value of a in formula (1) is 0.05 < a ≤ 0.12. This value range can satisfy the formation of the structure of general formula 1, and the polymer is more uniform after film formation, and the color change is obvious and fast.
[0015] As an embodiment of the first aspect of this application, the values of a, b, c and d in formula (1) are combined in the following ways: a is 0.05, b is 0.45, c is 0.05 and d is 0.45.
[0016] The value of a is 0.08, the value of b is 0.42, the value of c is 0.05, and the value of d is 0.45; or,
[0017] The values of a are 0.12, b is 0.38, c is 0.05, and d is 0.45. Combinations of these substances can yield triphenylamine exhibiting different valence states under the same voltage, and produce conjugated polymer electrochromic materials with low voltage drive, uniform film formation, and a colored state transmittance of <5%. This allows for the fabrication of electrochromic devices with high optical contrast and fast color-changing speed.
[0018] As an embodiment of the first aspect of this application, the fluorene derivative comprises a unit with the general structural formula (2):
[0019]
[0020] In formula (2), E is selected from methyl, oxymethyl, phenyl, 4-methoxyphenyl, 4-methylphenyl, alkyl C x H 2x+1 x is a natural number from 1 to 8, oxygen-substituted alkyl chain OC x H 2x+1 x is a natural number from 1 to 8, or an oligoether group. m is a natural number from 1 to 4. These substituents can modulate the HOMO (highest occupied molecular orbital) and LUMO (lowest unoccupied molecular orbital) energy levels of the entire molecule, thereby affecting the charge transport properties of the material. Appropriate energy level matching is beneficial for carrier injection and transport in devices, improving the electrical performance of the devices.
[0021] As an embodiment of the first aspect of this application, the fluorene derivative comprises a unit with the structural formula (3):
[0022]
[0023] In formula (3), E1 is selected from H, methyl, oxymethyl, phenyl, 4-methoxyphenyl, 4-methylphenyl, alkyl C x H 2x+1x is a natural number from 1 to 8, oxygen-substituted alkyl chain OC x H 2x+1 x is a natural number from 1 to 8, or an oligoether group. m is a natural number from 1 to 4;
[0024] F is selected from H, oxymethyl, oxygen-substituted alkyl chain, and OC. x H 2x+1 x is a natural number from 1 to 8, an ethyl ester substituent, or an oligoether group. m is a natural number from 1 to 4. These substituents can modulate the energy levels of the highest occupied molecular orbitals and the lowest unoccupied molecular orbitals of the entire molecule, thereby affecting the charge transport properties of the material. Appropriate energy level matching is beneficial for the injection and transport of charge carriers in the device, thus improving the electrical performance of the device.
[0025] As an embodiment of the first aspect of this application, the conjugated polymer is selected from the structures shown in the following structural formulas (N-2) or (N-3):
[0026]
[0027]
[0028] As an embodiment of the first aspect of this application, the molecular weight of the conjugated polymer is between 10,000 g / mol and 30,000 g / mol.
[0029] Secondly, this application also discloses an electrochromic material, the raw materials of which include the triarylamine conjugated polymer explained in the first aspect of the embodiments above.
[0030] Thirdly, this application also provides an organic electrochromic device, including the electrochromic material explained in the second aspect of the embodiments above.
[0031] Fourthly, this application also provides an electronic device including the organic electrochromic device explained in the third aspect of the embodiments described above. Attached Figure Description
[0032] Figure 1 The nuclear magnetic resonance spectrum of the structure of the conjugated polymer N-2 in this application embodiment;
[0033] Figure 2 The nuclear magnetic resonance spectrum of the structure of the conjugated polymer N-3 in this application embodiment is shown. Detailed Implementation
[0034] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings.
[0035] To facilitate understanding of the technical solutions of the embodiments of this application, the technical problems to be solved by the embodiments of this application will be explained first.
[0036] Triarylamines are a class of compounds containing three aromatic groups attached to a nitrogen atom, typically exhibiting excellent electron-donating properties. Due to their unique chemical structure and physical properties, these compounds have wide applications in various fields. For example, triarylamines possess electrochemical stability and high carrier transport capabilities, and are therefore commonly used as electrochromic chromophores.
[0037] Fluorene is a polycyclic aromatic hydrocarbon composed of three fused benzene rings. Two of the benzene rings are connected by a five-membered ring (bridging ring) sharing two adjacent carbon atoms. The molecular formula of fluorene is C6H2O. 13 H 10 Furthermore, its structure is highly symmetrical, with a rigid bridge ring at the center and benzene rings at both ends, exhibiting a unique rigid conjugate structure. This structure endows it with highly stable mechanical properties and excellent photoelectric properties.
[0038] Fluorene derivatives are products formed by replacing hydrogen atoms in the fluorene molecule with other functional groups. By introducing different functional groups, fluorene derivatives can significantly alter the physical and chemical properties and applications of fluorene itself. For example, the substituents in fluorene derivatives can regulate electron distribution; when the substituent is an electron-withdrawing group, it can enhance the stability of the conjugated system, while when the substituent is an electron-donating group, such as a methoxy group, it may improve fluorescence performance.
[0039] In some embodiments, the electrochromic materials obtained by combining triphenylamine and fluorene are limited by energy level mismatch, single-site oxidation mechanism, and inefficient charge (ion transport), resulting in insufficient high voltage requirements and optical performance. A driving voltage exceeding 3V is required to achieve a low transmittance. Furthermore, the achieved transmittance is still greater than 10%, and there are still problems with color gradation and dynamic display, which cannot meet the current high requirements for displays.
[0040] To address the aforementioned technical problems, this application provides a triarylamine conjugated polymer. By combining triarylamines with fluorene derivatives, the electron-donating properties of the triphenylamine side groups are adjusted, and the proportion of triphenylamines with different electron-donating properties is controlled in the molecular structure, thereby inducing triphenylamines in different valence states under the same voltage. This design enables the resulting conjugated polymer electrochromic material to possess excellent properties such as low-voltage driving, uniform film formation, and colored state transmittance of less than 5%. Simultaneously, it allows for the fabrication of electrochromic devices with high optical contrast and rapid color-changing response characteristics.
[0041] The triarylamine conjugated polymers of this application will be described below with reference to specific embodiments.
[0042] The triarylamine conjugated polymer of this application embodiment has a unit with the general structural formula (1):
[0043]
[0044] In equation (1), n is a natural number.
[0045] a + b + c + d = 1, (a + b) / (c + d) = 1:1, that is, a + b = 0.5, c + d = 0.5. And 0 < a ≤ 0.15, 0 < c ≤ 0.2.
[0046] Unit A is a fluorene derivative, which serves as the core backbone, providing a rigid conjugated backbone and enhancing charge transport capabilities. Substituents in the fluorene derivative can regulate electron distribution; for example, electron-withdrawing groups, ethers, and oxygen-substituted groups enhance the stability of the conjugated system, while electron-donating groups such as alkanes can improve fluorescence performance.
[0047] Each B group is independently selected from hydrogen, fluorine, methyl, trifluoromethyl, oxymethyl, phenyl, 2,4,6-trimethylphenyl, 4-methylphenyl, 4-methoxyphenyl, alkyl C x H 2x+1 x is a natural number from 1 to 10, oxygen-substituted alkyl chain OC x H 2x+1 x is a natural number from 1 to 10, and is an oligoether group. m is a natural number from 1 to 4.
[0048] The C group can be hydrogen, fluorine, methyl, trifluoromethyl, oxymethyl, phenyl, 2,4,6-trimethylphenyl, 4-methylphenyl, 4-methoxyphenyl, or alkyl C. x H 2x+1 x is a natural number from 1 to 10, and the alkyl chain is oxygen-substituted (OC). x H 2x+1 x is a natural number from 1 to 10, and the OC is an oxygen-substituted alkenyl chain. x H 2x-1 x is a natural number from 1 to 10, or an oligoether group. m is a natural number from 1 to 4.
[0049] The D group is selected from hydrogen, fluorine, methyl, trifluoromethyl, oxymethyl, phenyl, 2,4,6-trimethylphenyl, 4-methylphenyl, 4-methoxyphenyl, alkyl C x H 2x+1 x is a natural number from 1 to 10, oxygen-substituted alkyl chain OC x H 2x+1 x is a natural number from 1 to 10, or an oligoether group. m is a natural number from 1 to 4.
[0050] In Formula 1, the B group and the D group cannot both be alkyl groups. If the B group and the D group are both alkanes, different electron-loss properties cannot be achieved. For example, when selecting substituents, it is necessary to note that when the B group is alkyl, the D group cannot be alkyl, and when the D group is alkyl, the B group cannot be alkyl, in order to avoid not being able to achieve different electron-loss properties.
[0051] According to the embodiments of this application, the triarylamine conjugated polymer uses fluorene derivatives as a rigid conjugated backbone to enhance charge transport capability. By precisely controlling the proportion of triphenylamine side groups, the distribution of side groups with different electron-donating capabilities is controlled, thereby affecting the overall electron cloud density and redox properties of the molecule. Furthermore, the synergistic effect of the electron-donating effect of fluorene derivatives and triphenylamine lowers the highest occupied molecular orbital (HOMO) energy level of the conjugated polymer, allowing the colored state to be formed at a lower voltage, thus reducing the driving voltage. Furthermore, since the electron cloud of the polymer backbone is more likely to lose electrons after diffusion and ionization, the electron-donating ability of the triphenylamine side groups is designed to be different. The groups of the triphenylamine side groups at different positions have opposite effects on the electron cloud of the triphenylamine itself, thus ensuring that triphenylamine can exhibit different valence states under a certain low voltage. When these triphenylamines with different valence states coexist, the triarylamine conjugated polymer material as a whole will exhibit a low-transmittance state. That is, this multi-valence coexistence phenomenon allows the polymer material to reach a high coloring state under low voltage, and the transmittance is significantly reduced, reaching less than 5%.
[0052] In one embodiment of this application, the value of 'a' in Formula 1 is 0.05 < a ≤ 0.12. This range of values can satisfy the formation of the structure of Formula 1, and the polymer is more uniform after film formation, with obvious color changes and a fast color change speed.
[0053] In some embodiments of this application, the values of a, b, c, and d in the general formula (Formula 1) can be in the following combinations: First combination: a can be 0.05, b can be 0.45, c can be 0.05, and d can be 0.45. Second combination: a can be 0.08, b can be 0.42, c can be 0.05, and d can be 0.45. Third combination: a can be 0.12, b can be 0.38, c can be 0.05, and d can be 0.45. These combinations of substances can yield triphenylamine exhibiting different valence states under the same voltage, and conjugated polymer electrochromic materials with low voltage drive, uniform film formation, and color transmittance <5%, enabling the fabrication of electrochromic devices with high optical contrast and fast color-changing speed.
[0054] In some embodiments, the fluorene derivative comprises a unit with the general structural formula (2):
[0055]
[0056] In the general formula (Formula 2), E is selected from methyl, oxymethyl, phenyl, 4-methoxyphenyl, 4-methylphenyl, alkyl CxH2x+1, where x is a natural number from 1 to 8, oxygen-substituted alkyl chain OCxH2x+1, where x is a natural number from 1 to 8, or oligoether groups. m is a natural number from 1 to 4. When E is an aryl group such as methyl, methoxy, or phenyl, it increases the steric hindrance between molecules, making the molecules more ordered in solution or thin film states, reducing close packing between molecules, thereby improving the solubility and film-forming properties of the material, which is beneficial for preparing high-quality device thin films. Especially in organic electroluminescent devices, good film-forming properties can ensure the uniformity and stability of the device structure. In addition, these substituents can modulate the HOMO (highest occupied molecular orbital) and LUMO (lowest unoccupied molecular orbital) energy levels of the entire molecule, thus affecting the charge transport performance of the material. Appropriate energy level matching is beneficial for the injection and transport of charge carriers in the device, improving the electrical performance of the device.
[0057] In some embodiments, E in general formula (Formula 2) is selected from phenyl groups substituted with E1 and F groups. In this case, the fluorene derivative comprises a unit with the structural formula (Formula 3):
[0058]
[0059] In the general formula (Formula 3), E1 is H, methyl, oxymethyl, phenyl, 4-methoxyphenyl, 4-methylphenyl, alkyl C x H 2x+1 x is a natural number from 1 to 8, oxygen-substituted alkyl chain OC x H 2x+1 x is a natural number from 1 to 8, or an oligoether group. m is a natural number from 1 to 4. When E1 is an aromatic substituent such as 4-methoxyphenyl or 4-methylphenyl, these groups can enhance the conjugation effect of the molecule, increase the electron density of the molecule, and thus affect its optical properties and reactivity. The HOMO (highest occupied molecular orbital) and LUMO (lowest unoccupied molecular orbital) energy levels of the entire molecule can be tuned, thereby affecting the charge transport performance of the material. Appropriate energy level matching is beneficial for carrier injection and transport in devices, improving the electrical performance of the devices.
[0060] F represents H, oxymethyl, or an oxygen-substituted alkyl chain. OC x H 2x+1 x is a natural number from 1 to 8, an ethyl ester substituent, or an oligoether group. m is a natural number from 1 to 4.
[0061] In some embodiments of this application, the conjugated polymer is selected from the group consisting of the following structural formulas (N-2) or (N-3):
[0062]
[0063]
[0064] In some optional embodiments, the molecular weight of the conjugated polymer is 10,000 g / mol to 30,000 g / mol. This range is more conducive to purification and separation, and also to uniform film formation, which is beneficial to improving the overall optical performance of the device.
[0065] The triarylamine conjugated polymer of this application achieves corresponding technical effects by combining triarylamines with fluorene derivatives. On the one hand, by finely controlling the electron-donating properties of the triphenylamine side groups, the proportion of triphenylamines with different electron-losing capabilities in the polymer can be adjusted, thereby enabling the manifestation of triphenylamines in different valence states under the same applied voltage. This allows for effective color change of the electrochromic material under low driving voltage. Furthermore, such color change is not only fast but also has high optical contrast, with a color transmittance of less than 5%, improving the overall performance and response efficiency of the device. On the other hand, fluorene derivatives can enhance the overall rigidity and thermal stability of the material, helping to improve the film-forming properties and smoothness of the electrochromic material, thereby improving the optical quality of the material.
[0066] Furthermore, in some embodiments, a triarylamine conjugated polymer containing the embodiments of this application is used as the electrochromic material, which makes the electrochromic material have low voltage drive, uniform film formation and color state transmittance <5%. The light-emitting device made of the electrochromic material has high luminous efficiency, high optical contrast, fast color change speed and more stable performance, making it better suited for application in the field of electroluminescence, for example, in electronic devices or electronic equipment that require light-emitting devices.
[0067] In the embodiments of this application, the electronic device can be any product or component with display function, such as a mobile phone, tablet computer, television, monitor, laptop computer, camera, navigator, in-vehicle display, smartwatch, smart bracelet, etc.
[0068] According to some embodiments of the present invention, this application also provides a method for preparing a triarylamine conjugated polymer, the specific synthetic route of which (reaction formula 1) is as follows:
[0069]
[0070] Specifically, the Suzuki-Miyaura polymerization reaction steps are as follows:
[0071] S10, add b equivalents of triarylamine monomer (I) containing B group and borate ester, c equivalents of triarylamine monomer (II) containing C group and bromine, a equivalent of borate ester fluorene derivative monomer (III) and d equivalents of triarylamine monomer (IV) containing D group and bromine to a pressure-resistant bottle, add an appropriate amount of toluene to dissolve, and form a monomer mixture.
[0072] S20, under an inert atmosphere, a palladium catalyst and an alkaline compound are added to a monomer mixture, and a coupling polymerization reaction is carried out at 80-100℃ for 20-30 hours to obtain a reaction solution.
[0073] In some embodiments of this application, after blowing under a nitrogen atmosphere for 30 minutes, 5% equivalent of PdP ( t Add Bu)3 catalyst and 3 equivalents of TMSOK base to the flask, and continue to purge with nitrogen for 10 minutes. After sealing, heat to 90°C and react for 24 hours.
[0074] S30 is used to purify the reaction solution.
[0075] After the S20 reaction is complete, the reaction solution is poured into a methanol solution, filtered, and the filter cake is collected. The polymer is then extracted using Soxhlet extraction. The purification solution is prepared in the following order: methanol, n-hexane, acetone, and chloroform.
[0076] S40, collect the purified solution, and obtain conjugated polymers of triarylamine and fluorene and their derivatives by solvent extraction.
[0077] In one embodiment of this application, the solvent is evaporated using a rotary evaporator, and the chloroform solution collected in step S30 is dried in a vacuum oven to obtain product N1 in reaction formula 1.
[0078] The preparation method is simple and can produce the electrochromic material mentioned above, which has low voltage drive, uniform film formation and color transmittance of <5%.
[0079] The following detailed description, in conjunction with specific embodiments, illustrates the triarylamine conjugated polymer, preparation method, and performance of devices prepared from electrochromic materials according to the embodiments of this application.
[0080] Comparative Example
[0081] The synthetic route for polymer N-1 is as follows:
[0082]
[0083] The specific preparation process is as follows:
[0084] In a round-bottom flask, 1-butyl-4-aminobenzene (1-1, 1.2 g, 8.04 mmol) and 1-bromo-4-iodobenzene (1-2, 6.32 g, 22.35 mmol) were added and dissolved in toluene. Nitrogen gas was then applied for 30 minutes. Cuprous iodide (0.1 g, 0.5 mmol), o-phenanthroline (0.16 g, 1 mmol), and potassium carbonate (2.11 g, 15.24 mmol) were added, and nitrogen gas was applied for another 10 minutes. The flask was then sealed and heated to reflux. The reaction was monitored by thin-layer chromatography. After the reaction was complete, the reaction mixture was washed with deionized water and separated. The organic phase was dried over anhydrous sodium sulfate, concentrated, and eluented with petroleum ether. Column chromatography was used to obtain 1-3 (3.2 g, 73.59% yield).
[0085] Add 1-3 (2 g, 4.36 mmol) and 1-4 (2.8 g, 4.36 mmol) to a pressure-resistant flask, dissolve in 15 mL of toluene, and purge with nitrogen for 30 minutes. Weigh out PdP(tBu)3 catalyst (0.06 g, 0.18 mmol) and TMSOK (1.42 g, 11.0 mmol), and continue purging with nitrogen for 10 minutes. After sealing, heat to 90 °C and react for 24 hours. After the reaction is complete, pour the reaction solution into a methanol solution, filter and collect the filter cake, then extract the polymer using Soxhlet extraction. The purification order of the solutions is methanol, n-hexane, acetone, and chloroform. Finally, collect the chloroform solution, evaporate the solvent using a rotary evaporator, and dry in a vacuum oven overnight to obtain polymer N-1.
[0086] Example 1
[0087] Synthesis of polymer N-2:
[0088]
[0089] The specific synthesis route is as follows:
[0090]
[0091]
[0092] The specific preparation process is as follows:
[0093] Compounds 2-3 correspond to compounds 1-3 in the comparative examples. For specific synthesis methods, please refer to the synthesis process of comparative examples 1-3.
[0094] Other synthesis processes are as follows:
[0095] Add 2-3 (2 g, 4.36 mmol), pinacol borate (3.56 g, 14 mmol), and PdCl2(PPh3)2 (0.16 g, 0.23 mmol) to a round-bottom flask, dissolve in N,N-dimethylformamide, purge with nitrogen for 30 minutes, and seal. React at 120 °C, monitoring the reaction using thin-layer chromatography. After the reaction is complete, wash the reaction mixture with deionized water and separate the layers. Dry the organic phase with anhydrous sodium sulfate, concentrate, and elute with petroleum ether / ethyl acetate (6:1) by column chromatography to obtain 2-4 (1.8 g, 74% yield).
[0096] Add 2-6 (5.7 g, 76.9 mmol) and sodium hydroxide (2.9 g, 73.4 mmol) to a round-bottom flask, dissolve in tetrahydrofuran, place in an ice bath, and add p-toluenesulfonyl chloride (10.0 g, 52.5 mmol) dropwise. After addition, react at room temperature for 5 hours, quench the reaction with deionized water, and separate the layers. Dry the organic phase with anhydrous sodium sulfate, concentrate, and elute with petroleum ether by column chromatography to obtain 2-7 (12.0 g, 93.64% yield).
[0097] In a round-bottom flask, 2-10 (4.0 g, 10.4 mmol) was dissolved in dichloromethane. The mixture was kept in an ice bath, and boron tribromide (20.87 g, 83.3 mmol) was added dropwise. After the addition was complete, the reaction was allowed to proceed at room temperature for 2 hours. The reaction was then quenched with deionized water, and the mixture was separated. The organic phase was dried over anhydrous sodium sulfate, concentrated, and separated by column chromatography using petroleum ether / ethyl acetate (5:1) as the eluent to obtain 2-11 (3.4 g, 91.7% yield).
[0098] In a round-bottom flask, 2-11 (3 g, 8.4 mmol) was dissolved in tetrahydrofuran, and nitrogen gas was applied for 30 minutes. Sodium hydride (0.8 g, 33.7 mmol) was added, followed by dropwise addition of 2-7 (2.3 g, 10.1 mmol) after 10 minutes. The reaction was allowed to proceed at room temperature. The reaction was monitored using thin-layer chromatography. After the reaction was complete, the reaction mixture was washed with deionized water and separated. The organic phase was dried over anhydrous sodium sulfate, concentrated, and eluted with petroleum ether / ethyl acetate (8:1) to obtain 2-12 (4.0 g, 8.5 mmol) by column chromatography.
[0099] Add 2-12 (2 g, 4.36 mmol), pinacol borate (3.56 g, 14 mmol), and PdCl2(PPh3)2 (0.16 g, 0.23 mmol) to a round-bottom flask, dissolve in N,N-dimethylformamide, purge with nitrogen for 30 minutes, and seal. React at 120 °C, monitoring the reaction using thin-layer chromatography. After the reaction is complete, wash the reaction solution with deionized water and separate the layers. Dry the organic phase with anhydrous sodium sulfate, concentrate, and elute with petroleum ether / ethyl acetate (6:1) by column chromatography to obtain 2-13.
[0100] In a round-bottom flask, 2-14 (1.2 g, 8.04 mmol) and 2-2 (6.32 g, 22.35 mmol) were added and dissolved in toluene. Nitrogen gas was then applied for 30 minutes. Cuprous iodide (0.1 g, 0.5 mmol), o-phenanthroline (0.16 g, 1 mmol), and potassium carbonate (2.11 g, 15.24 mmol) were added, and nitrogen gas was applied for another 10 minutes. The flask was then sealed and heated to reflux. The reaction was monitored by thin-layer chromatography. After the reaction was complete, the reaction mixture was washed with deionized water and separated. The organic phase was dried over anhydrous sodium sulfate, concentrated, and eluted with petroleum ether to obtain 2-15 by column chromatography.
[0101] Using 2-4, 2-15, 2-13, and 1-3 as raw materials, dissolve them in 15 mL of toluene, and purge with nitrogen for 30 minutes. Weigh out PdP(tBu)3 catalyst (0.06 g, 0.18 mmol) and TMSOK (1.42 g, 11.0 mmol), and continue purging with nitrogen for 10 minutes. After sealing, heat to 90 °C and react for 24 hours. After the reaction is complete, pour the reaction solution into a methanol solution, filter and collect the filter cake, then extract the polymer using Soxhlet extraction. The purified solution is in the order of methanol, n-hexane, acetone, and chloroform. Finally, collect the chloroform solution, evaporate the solvent using a rotary evaporator, and dry in a vacuum oven overnight to obtain N-2.
[0102] The nuclear magnetic resonance (NMR) spectrum of N-3 can be found in the reference section. Figure 1 .
[0103] Example 3
[0104] Synthesis of polymer N-3:
[0105]
[0106] The synthesis process of polymer N-3 is as follows:
[0107]
[0108] The synthesis process of polymer N-3 is as follows:
[0109] In a round-bottom flask, 3-1 (1.2 g, 8.04 mmol) and 3-2 (6.32 g, 22.35 mmol) were added and dissolved in toluene. Nitrogen gas was then applied for 30 minutes. Cuprous iodide (0.1 g, 0.5 mmol), o-phenanthroline (0.16 g, 1 mmol), and potassium carbonate (2.11 g, 15.24 mmol) were added, and nitrogen gas was applied for another 10 minutes. The flask was then sealed and heated to reflux. The reaction was monitored using thin-layer chromatography. After the reaction was complete, the reaction mixture was washed with deionized water and separated. The organic phase was dried over anhydrous sodium sulfate, concentrated, and eluented with petroleum ether by column chromatography to obtain 3-3.
[0110] Add 3-3 (2 g, 4.36 mmol), pinacol borate (3.56 g, 14 mmol), and PdCl2(PPh3)2 (0.16 g, 0.23 mmol) to a round-bottom flask, dissolve in N,N-dimethylformamide, purge with nitrogen for 30 minutes, and seal. React at 120 °C, monitoring the reaction using thin-layer chromatography. After the reaction is complete, wash the reaction solution with deionized water and separate the layers. Dry the organic phase with anhydrous sodium sulfate, concentrate, and elute with petroleum ether / ethyl acetate (6:1) by column chromatography to obtain 3-4.
[0111] Using 3-4, 2-15, 3-5, and 3-6 as raw materials, dissolve them in 15 mL of toluene, and purge with nitrogen for 30 minutes. Weigh out PdP(tBu)3 catalyst (0.06 g, 0.18 mmol) and TMSOK (1.42 g, 11.0 mmol), and continue purging with nitrogen for 10 minutes. After sealing, heat to 90 °C and react for 24 hours. After the reaction is complete, pour the reaction solution into a methanol solution, filter and collect the filter cake, then extract the polymer using Soxhlet extraction. The purified solution is in the order of methanol, n-hexane, acetone, and chloroform. Finally, collect the chloroform solution, evaporate the solvent using a rotary evaporator, and dry in a vacuum oven overnight to obtain polymer N-3.
[0112] The nuclear magnetic resonance (NMR) spectrum of N-3 can be found in the reference section. Figure 2 .
[0113] Example 4
[0114] Compared with Example 3, the synthesis of N-3 in Example 4 differs in the feed ratio, while the other synthesis steps are the same as in Example 3. Specifically, in Example 4, the feed ratio is: 3-4, 2-15, 3-5, and 3-6 are fed in a molar ratio of 0.42:0.05:0.08:0.45. The other steps are the same as the polymerization steps of N-3 in Example 3, to obtain N-3.
[0115] Example 5
[0116] Compared with Example 3, the synthesis of N-3 in Example 5 differs in the feed ratio, while the other synthesis steps are the same as in Example 3. Specifically, in Example 5, the feed ratio is: 3-4, 2-15, 3-5, and 3-6 are fed in a molar ratio of 0.38:0.05:0.12:0.45. The other steps are the same as the polymerization steps of N-3 in Example 3, to obtain N-3.
[0117] The products obtained from the comparative examples and Examples 1-4 of this application were used to prepare electrochromic devices, and the electrochromic performance of the devices was investigated. The specific preparation process is as follows:
[0118] The product N-1 obtained in the comparative example above, as well as the products N-2, N-3, N-4 and N-5 obtained in Examples 1-4, were each prepared into chloroform solutions of 30 mg / mL for later use.
[0119] Transparent indium tin oxide (ITO) conductive glass was cut into 3cm*3cm pieces. Different areas of transparent ITO conductive glass were soaked in a mixed solvent of ammonia and hydrogen peroxide. The glass was then soaked in toluene, acetone, deionized water and isopropanol in sequence and sonicated for 15 minutes each. After removal, the ITO glass was dried with dry nitrogen gas and set aside for use.
[0120] The prepared chloroform solution was spin-coated onto corresponding ITO glass plates, and then bonded to another ITO glass plate with 3M tape. A propylene carbonate electrolyte solution containing 0.1 mol / L tetrabutylammonium hexafluorophosphate and 0.01 mol / L ethyl amethyst hexafluorophosphate was then poured into the cavity between the glass plates. The electrolyte solution was sealed with UV-curable adhesive to obtain electrochromic devices M-1, M-2, M-3, M-4, and M-5, respectively. A voltage was applied to the electrochromic devices, and their color change, driving voltage, and electrochromic response time were tested. Specific results are shown in Table 1 below.
[0121] Table 1 Comparison of detection results between the comparative example and the embodiment.
[0122]
[0123] As shown in Table 1, M-1, serving as a comparative example, exhibits a color change from transparent to dark blue; a driving voltage of 3.5V; and a response time of 34 seconds for coloring and 21 seconds for fading. In contrast, the driving voltages of embodiments M-2 to M-5 in this application are all 2.5V, significantly lower than the 3.5V of M-1. This indicates that the electrochromic materials of this application can operate with lower energy consumption, which is more beneficial for energy saving and extending equipment lifespan. Furthermore, M-2 has a response time of 23 seconds for coloring and 16 seconds for fading; M-3 has a response time of 29 seconds for coloring and 15 seconds for fading, demonstrating even faster response times.
[0124] Although this application has been illustrated and described with reference to certain preferred embodiments thereof, those skilled in the art should understand that various changes in form and detail may be made thereto without departing from the spirit and scope of this application.
Claims
1. A triarylamine conjugated polymer, characterized in that, The triarylamine conjugated polymer comprises units with the general structural formula (1): In equation (1), 0 < n < 50, and n is a natural number, a + b + c + d = 1, (a + b) / (c + d) = 1:1, and 0 < a ≤ 0.15, 0 < c ≤ 0.2; The A unit is a derivative of fluorene; Each of the B groups is independently selected from hydrogen, fluorine, methyl, trifluoromethyl, oxymethyl, phenyl, 2,4,6-trimethylphenyl, 4-methylphenyl, 4-methoxyphenyl, alkyl C x H 2x+1 x is a natural number from 1 to 10, oxygen-substituted alkyl chain OC x H 2x+1 x is a natural number from 1 to 10, and is an oligoether group. m is a natural number from 1 to 4; The C group is hydrogen, fluorine, methyl, trifluoromethyl, oxymethyl, phenyl, 2,4,6-trimethylphenyl, 4-methylphenyl, 4-methoxyphenyl, or alkyl C. x H 2x+1 x is a natural number from 1 to 10, and the alkyl chain is oxygen-substituted (OC). x H 2x+1 x is a natural number from 1 to 10, and the OC is an oxygen-substituted alkenyl chain. x H 2x-1 x is a natural number from 1 to 10, or an oligoether group. m is a natural number from 1 to 4; The D group is selected from hydrogen, fluorine, methyl, trifluoromethyl, oxymethyl, phenyl, 2,4,6-trimethylphenyl, 4-methylphenyl, 4-methoxyphenyl, alkyl C x H 2x+1 x is a natural number from 1 to 10, oxygen-substituted alkyl chain OC x H 2x+1 x is a natural number from 1 to 10, or an oligoether group. m is a natural number from 1 to 4, wherein the B group and the D group are not both alkyl groups.
2. The triarylamine conjugated polymer according to claim 1, characterized in that, The value of a in the formula (1) is 0.05 < a ≤ 0.
12.
3. The triarylamine conjugated polymer according to claim 1 or 2, characterized in that, The values of a, b, c, and d in equation (1) are the following combinations: The value of a is 0.05, the value of b is 0.45, the value of c is 0.05, and the value of d is 0.
45. The value of 'a' is 0.08, the value of 'b' is 0.42, the value of 'c' is 0.05, and the value of 'd' is 0.45; or, The value of 'a' is 0.12, the value of 'b' is 0.38, the value of 'c' is 0.05, and the value of 'd' is 0.
45.
4. The triarylamine conjugated polymer according to claim 3, characterized in that, The fluorene derivative comprises a unit with the general structural formula (2): In formula (2), E is selected from methyl, oxymethyl, phenyl, 4-methoxyphenyl, 4-methylphenyl, alkyl C x H 2x+1 x is a natural number from 1 to 8, oxygen-substituted alkyl chain OC x H 2x+1 x is a natural number from 1 to 8, or an oligoether group. m is a natural number from 1 to 4.
5. The triarylamine conjugated polymer according to claim 4, characterized in that, The fluorene derivative comprises a unit with the structural formula (3): In formula (3), E1 is selected from H, methyl, oxymethyl, phenyl, 4-methoxyphenyl, 4-methylphenyl, alkyl C x H 2x+1 x is a natural number from 1 to 8, oxygen-substituted alkyl chain OC x H 2x+1 x is a natural number from 1 to 8, or an oligoether group. m is a natural number from 1 to 4; F is selected from H, oxymethyl, oxygen-substituted alkyl chain, and OC. x H 2x+1 x is a natural number from 1 to 8, an ethyl ester substituent, or an oligoether group. m is a natural number from 1 to 4.
6. The triarylamine conjugated polymer according to claim 1, characterized in that, The The conjugated polymer is selected from the structures shown in (N-2) or (N-3):
7. The triarylamine conjugated polymer according to claim 1, characterized in that, The molecular weight of the conjugated polymer is between 10,000 g / mol and 30,000 g / mol.
8. An electrochromic material, characterized in that, Its raw materials include the triarylamine conjugated polymer as described in any one of claims 1-7.
9. An organic electrochromic device, characterized in that, Including the electrochromic material as described in claim 8.
10. An electronic device, characterized in that, Including the organic electrochromic device as described in claim 9.