A polymer based on benzobisisothiadiazole units and its preparation method
By designing a blend of DA-type polymer materials based on benzobisisothiadiazole units and acceptor materials, the problem of low photoelectric conversion efficiency in all-polymer solar cells was solved, and a high-efficiency photoelectric conversion performance improvement was achieved.
Patent Information
- Application Number
- CN202611497049.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-17
AI Technical Summary
The photoelectric conversion efficiency of existing all-polymer solar cells still needs to be improved. Traditional materials have a low absorption coefficient in the near-infrared region, which limits the further improvement of photoelectric conversion efficiency, and excitons are prone to recombination quenching.
A DA-type polymer material based on benzobisisothiadiazole units was designed and synthesized, and blended with polymer acceptor materials to fabricate photovoltaic devices. The excellent optical absorption properties and good energy level matching of this polymer were utilized to promote charge dissociation.
The photoelectric conversion performance of the all-polymer solar cell was improved, with high charge dissociation efficiency. The photovoltaic device exhibited excellent photoelectric performance, with a photoelectric conversion efficiency of 13.61%.
Smart Images

Figure CN123107045A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer preparation technology, specifically to a polymer based on benzobisisothiadiazole units and its preparation method. Background Technology
[0002] Energy plays a vital role in human survival and development. Since the First Industrial Revolution, traditional fossil fuels such as coal, oil, and natural gas have become increasingly important in production and daily life. However, fossil fuel reserves are limited, and human energy demand increases year by year with economic development. Furthermore, the acidic gases and particulate matter released during fossil fuel use harm the human environment. Therefore, there is an urgent need to develop sustainable and environmentally friendly new energy sources to gradually reduce dependence on fossil fuels. Solar energy is environmentally friendly and has no geographical limitations. Solar cells, as a clean and pollution-free energy conversion technology, have abundant raw materials and a wide range of potential applications, playing a crucial role in addressing the energy crisis and environmental pollution. Organic solar cells, using organic materials as their core component, have attracted widespread attention due to their low cost, light weight, and environmental friendliness. All-polymer solar cells, as an important branch, have become a research hotspot in the photovoltaic field.
[0003] Polymer solar cells have undergone long-term development, with device structures evolving from early Schottky and bilayer DA heterojunction types to D / A bulk heterojunction types. Both forward and reverse configurations are commonly used, improving exciton separation, charge transport, and collection performance. The active layer of all-polymer solar cells consists of polymer donors and polymer acceptors, offering advantages over fullerene and non-fullerene small molecule acceptor systems, including thinness, flexibility, and stability. Researchers have developed various polymer donor materials with wide and narrow band gaps, as well as multiple polymer acceptor materials. Among these, benzothiadiazole units possess good conjugated planes and strong electron affinity; polymer donor materials based on these units are widely used in all-polymer solar cells. Furthermore, polymers can be constructed using isothiadiazole fused ring units to enhance the performance of organic solar cells.
[0004] The photoelectric conversion efficiency of existing all-polymer solar cells still needs improvement. Traditional polymer materials have low absorption coefficients in the near-infrared region, limiting further improvements in photoelectric conversion efficiency. Existing material systems cannot fully utilize near-infrared sunlight, and exciton recombination quenching is prone to occur, restricting further improvements in the photoelectric performance of devices. Therefore, it is necessary to design polymer materials with higher absorption coefficients in the near-infrared region to overcome the performance bottleneck of all-polymer solar cells.
[0005] In conclusion, a new technical solution is urgently needed to address the problems existing in the current technology. Summary of the Invention
[0006] Based on this, the present invention provides a polymer based on a benzobisisothiadiazole unit and its preparation method. The present invention designs and synthesizes a benzobisisothiadiazole acceptor unit structure and constructs a polymer based on the benzobisisothiadiazole unit. This polymer is a DA-type polymer material and a polymer donor material. Furthermore, a photovoltaic device is prepared by blending the polymer based on the benzobisisothiadiazole unit and the acceptor material. The polymer based on the benzobisisothiadiazole unit prepared by the present invention possesses excellent optical absorption properties and can form good spectral complementary absorption with the polymer acceptor PA5. Simultaneously, the energy level matching between the polymer and the polymer acceptor PA5 is good, which can effectively promote charge dissociation. The photovoltaic device prepared based on this polymer exhibits excellent photoelectric performance and high charge dissociation efficiency, effectively improving the overall photoelectric conversion performance of the all-polymer solar cell.
[0007] One object of the present invention is to provide a polymer based on a benzobisisothiadiazole unit, said polymer having the following structure: ; in, The n is a positive integer from 1 to 10000; R1, R2, R3, and R4 are independently selected from alkyl, alkyl derivatives, aryl, aryl derivatives, and hydrogen atoms; All hydrogen atoms on the alkyl derivative were not substituted. or One or more hydrogen atoms at any position on an alkyl derivative are substituted by one or more of a halogen, mercapto, carbonyl, hydroxyl, amino, carboxyl, cyano, nitro, aryl, olefinic, alkyneic, or ester group. The aryl derivative is selected from groups containing one or more aromatic ring structures, wherein all hydrogen atoms on the aromatic ring are unsubstituted. or One or more hydrogen atoms at any position on one or more aromatic rings are substituted by one or more oxygen atoms, mercapto, halogen, hydroxyl, amino, carboxyl, cyano, nitro, aryl, olefinic, alkyneic, or ester groups. X is independently selected from one of S and NH.
[0008] Furthermore, R1, R2, R3, and R4 are independently selected from C1-C30 alkyl groups with straight or branched structures, and C1-C30 alkyl derivatives with straight or branched structures.
[0009] Furthermore, the polymer based on the benzobisisothiadiazole unit has the following structure: ; in, The n is a positive integer from 1 to 10000.
[0010] Another object of the present invention is to provide a method for preparing the polymer based on the benzobisisothiadiazole unit, comprising the following steps: S1. 1,5-Dichloro-2,4-dinitrobenzene and sodium sulfide nonahydrate were mixed, heated and reacted, and purified to obtain compound 2 (4,6-diaminobenzene-1,3-dimercapto). S2. Under low temperature conditions, tert-butyl nitrite was added to compound 2, the mixture was stirred and reacted, and after purification, compound 3 (benzo[1,2-d:5,4-d']bis([1,2,3]thiadiazole)) was obtained. S3. Compound 3 and bromosubstituted alkylthiophene were blended, and palladium catalyst, phosphine ligand precursor, aliphatic carboxylic acid, and inorganic base reagent were added. The mixture was heated under an inert atmosphere and purified to obtain compound 4 (4,8-bis(4-(2-butyloctyl)thiophen-2-yl)benzo[1,2-d:5,4-d']bis([1,2,3]thiadiazole)). S4. Under light-protected conditions, N-bromosuccinimide (NBS) was added to compound 4, and the mixture was stirred and reacted. After purification, the polymer monomer M1 (4,8-bis(5-bromo-4-(2-butyloctyl)thiophene-2-yl)benzo[1,2-d:5,4-d']bis([1,2,3]thiadiazole)) was obtained. S5. Polymer monomer M1 and (4,8-bis(5-(2-ethylhexyll)thiophen-2-yl)benzo[1,2-b:4,5-b']dithiophen-2,6-diyl)bis(trimethyltin) (BDT-Sn) were blended, and palladium catalyst and phosphine ligand were added. The mixture was heated under an inert atmosphere and purified to obtain a polymer based on benzobisisothiadiazole units.
[0011] Starting material 1,5-dichloro-2,4-dinitrobenzene was subjected to nitro reduction and mercapto substitution with sodium sulfide to yield compound 2. Compound 2 was then subjected to diazotization and cyclization with tert-butyl nitrite to yield the important intermediate compound 3. Compound 3 was coupled with a bromosubstituted alkylthiophene via a CH-activated coupling reaction to yield compound 4. Compound 4 was then subjected to bromination to yield the polymer monomer M1 in high yield. Finally, the polymer monomer M1 was coupled with the bistin monomer BDT-Sn via Stille coupling polymerization to obtain PiBBTSS-H. PiBBTSS-H exhibits good solvent processing properties and is well soluble in halogen solvents such as chloroform (CF) and chlorobenzene (CB), as well as non-halogen solvents such as toluene and o-xylene.
[0012] Further, in step S1, the mass ratio of 1,5-dichloro-2,4-dinitrobenzene to sodium sulfide nonahydrate is 1:(20-40).
[0013] Furthermore, in step S1, the temperature of the heating reaction is 100-110℃; the reaction time is 12-36 h.
[0014] Further, in step S2, the mass ratio of compound 2 to tert-butyl nitrite is 1:(3-6).
[0015] Furthermore, in step S2, the low temperature condition is -10 to 30°C; preferably, an ice bath condition.
[0016] Further, in step S3, the mass ratio of compound 3 to bromosubstituted alkylthiophene is 1:(3-6).
[0017] Furthermore, in step S3, the temperature of the heating reaction is 110-130℃; the reaction time is 12-48 h.
[0018] Further, in step S3, the bromine-substituted alkylthiophene is preferably 2-bromo-4-(2-butyloctyl)thiophene; the palladium catalyst is preferably palladium acetate; the phosphine ligand precursor is preferably di-tert-butylmethylphosphonium fluoroborate; the aliphatic carboxylic acid is preferably tert-valerate; and the inorganic base reagent is preferably potassium carbonate.
[0019] Further, in step S4, the molar ratio of compound 4 to NBS is 1:(2-3).
[0020] Further, in step S5, the mass ratio of the polymeric monomer M1 to BDT-Sn is 1:(0.9-1.1).
[0021] Further, in step S5, the palladium catalyst is preferably tris(dibenzylacetone)palladium (Pd2(dba)3); the phosphine ligand is preferably tris(o-methylphenyl)phosphine (P(o-tol)3).
[0022] Furthermore, in step S5, the temperature of the heating reaction is 80-180℃; the reaction time is 24-96 h.
[0023] The present invention has the following beneficial effects: This invention provides a polymer based on a benzobisisothiadiazole unit and its preparation method. The invention designs and synthesizes a benzobisisothiadiazole acceptor unit structure and constructs a polymer based on the benzobisisothiadiazole unit. This polymer is a DA-type polymer material and a polymer donor material. Furthermore, a photovoltaic device is fabricated by blending the polymer based on the benzobisisothiadiazole unit with the acceptor material.
[0024] Test results show that the polymer based on the benzobisisothiadiazole unit of this invention has a maximum absorption peak of 701 nm in solution and an absorption cutoff edge of 798 nm in thin film, exhibiting a good optical band gap of 1.55 eV, which can form complementary absorption with the polymer acceptor PA5. Ultraviolet photoelectron spectroscopy (UPS) tests show that the polymer based on the benzobisisothiadiazole unit of this invention has matched energy levels with the polymer acceptor PA5, which is beneficial for achieving effective charge dissociation. Under optimized conditions, the photovoltaic device prepared from this polymer and polymer acceptor PA5 exhibits excellent photoelectric performance (PCE = 13.61%). J SC =23.73 mA cm -2 , V OC =0.894V, FF=0.642). Charge generation test results show that the photovoltaic device has a charge dissociation efficiency of 94.3%. Attached Figure Description
[0025] Figure 1 A synthetic route diagram for polymer PiBBTSS-H is shown.
[0026] Figure 2 The results of compound 3 in CDCl3 are shown. 1 ¹H NMR (δ 5.30 for CH₂Cl₂, δ 1.55 for H₂O).
[0027] Figure 3 The mass spectrum (APCI mode) of compound 3 is shown.
[0028] Figure 4 The results of compound 4 in CDCl3 are shown. 1 HNMR.
[0029] Figure 5 The results of compound 4 in CDCl3 are shown. 13 C10 NMR spectrum.
[0030] Figure 6 The mass spectrum (APCI mode) of compound 4 is shown.
[0031] Figure 7 The figure shows the measured values of monomer M1 in CDCl3. 1 HNMR spectrum.
[0032] Figure 8 The figure shows the measured values of monomer M1 in CDCl3. 13 CNMR spectrum.
[0033] Figure 9The mass spectrum (APCI mode) of polymeric monomer M1 is shown.
[0034] Figure 10 The high-temperature GPC spectrum of polymer PiBBTSS-H in trichlorobenzene is shown.
[0035] Figure 11 Normalized CF solution absorption spectra and thin film absorption spectra of PiBBTSS-H and its receptor PA5 are shown. in, Figure 11 (a) shows the normalized CF solution absorption spectrum of PiBBTSS-H with receptor PA5; Figure 11 (b) shows the normalized thin-film absorption spectra of PiBBTSS-H and the receptor PA5.
[0036] Figure 12 The UPS test diagram of polymer PiBBTSS-H is shown.
[0037] Figure 13 The current density-voltage (JV) curves and external quantum efficiency (EQE) of the polymer PiBBTSS-H for photovoltaic devices are shown. in, Figure 13 (a) shows the current density-voltage (JV) curves of the polymer PiBBTSS-H for photovoltaic devices; Figure 13 (b) shows the external quantum efficiency (EQE) of the polymer PiBBTSS-H for photovoltaic devices.
[0038] Figure 14 This demonstrates a device based on PEDTQ:PA5. J ph -V eff Characteristic curves. Detailed Implementation
[0039] To more clearly illustrate the technical solution of the present invention, the following embodiments are provided. Unless otherwise stated, the raw materials, reactions, and post-processing methods appearing in the embodiments are all commercially available raw materials and technical methods well known to those skilled in the art.
[0040] The terms "preferred," "more preferably," and "more suitable" used in this invention refer to embodiments of the invention that provide certain beneficial effects under certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. Furthermore, the description of one or more preferred embodiments does not imply that other embodiments are unavailable, nor is it intended to exclude other embodiments from the scope of this invention.
[0041] It should be understood that, except in any operational instance or otherwise indicated, the amounts or all figures representing ingredients used, for example, in the specification and claims, should be understood to be modified by the term "about" in all cases. Therefore, unless otherwise stated, the numerical parameters set forth in the following specification and appended claims are approximate values varying according to the desired performance to be obtained according to the invention.
[0042] The present invention uses the following raw materials: 200-300 mesh silica gel for column chromatography: purchased from Qingdao Ocean Chemical Company.
[0043] Example A polymer based on benzobisisothiadiazole units (PiBBTSS-H) has the following structure: .
[0044] The method for preparing the polymer based on benzobisisothiadiazole units includes the following steps: S1. Add 1,5-dichloro-2,4-dinitrobenzene (Compound 1, 11.85 g) and sodium sulfide nonahydrate (360 g) to a 1 L single-necked round-bottom flask, and add 800 mL of deionized water. Reflux the reaction under air for 24 h. After the reaction is complete, filter the reaction solution through a Buchner funnel to obtain the filtrate. Add ice to the filtrate and neutralize it with glacial acetic acid to pH 7. During neutralization, a large amount of hydrogen sulfide gas and a large amount of yellow solid are produced, accompanied by exothermic reaction. After neutralization is complete, filter to obtain the solid, which is the crude product of Compound 2. Compound 2 is unstable and does not require purification; it is directly added to the next reaction step. S2. Compound 2 (8.6 g) was added to a 250 mL single-necked round-bottom flask, and 100 mL of acetonitrile was added. The mixture was stirred and tert-butyl nitrite (4 equivalents) was added dropwise under ice bath conditions. The reaction was carried out in air at room temperature with stirring for 2 h. After the reaction was complete, 400 mL of methanol was added to the reaction solution, and the mixture was filtered to obtain a solid crude product. The crude product was subjected to silica gel column chromatography using petroleum ether:dichloromethane (1:1) as eluent to obtain a white solid compound 3 (8.34 g, yield 86%). S3. Compound 3 (1.94 g), 2-bromo-4-(2-butyloctyl)thiophene (9.93 g), palladium acetate (200 mg), di-tert-butylmethylphosphonium fluoroborate (450 mg), tert-valerate (910 mg), potassium carbonate (3.7 g), and dry toluene (50 mL) were added to a 150 mL pressure-resistant bottle. The reaction system was purged with argon gas for 15 min, then sealed and reacted at 120 °C for 24 h. After the reaction solution cooled to room temperature, the solvent was removed by rotary evaporation under reduced pressure. The crude product was purified by silica gel column chromatography using petroleum ether:dichloromethane (3:1) as eluent to obtain a red solid compound 4 (2.08 g, 30% yield). S4. Compound 4 (695 mg) and 30 mL of chloroform were added to a 50 mL round-bottom flask. Under light protection, NBS (392 mg) was added in three batches to the reaction solution. The reaction was stirred at room temperature for 2 h. After the reaction was completed, water was added to the reaction flask to quench the reaction. The organic phase was collected and the organic solvent was removed by rotary evaporation under reduced pressure. The crude product M1 was subjected to silica gel column chromatography with petroleum ether:dichloromethane (3:1) as eluent to obtain red solid polymer monomer M1 (758 mg, yield 89%). S5. Add monomer M1 (170.6 mg), BDT-Sn (180.9 mg), catalyst Pd2(dba)3 (6 mg), and phosphine ligand P(o-tol)3 (9 mg) to a 48 mL pressure-resistant bottle. Add 8 mL of dry chlorobenzene to the reaction bottle under an argon atmosphere. Stir the reaction mixture at 110 °C for 48 h. After cooling to room temperature, add the reaction mixture dropwise to methanol (500 mL). Collect the flocculent precipitate and extract with methanol, n-hexane, dichloromethane, chloroform, and chlorobenzene using a Soxhlet extractor. Concentrate and precipitate the collected chlorobenzene phase in methanol. Collect the PiBBTSS-H polymer and dry under vacuum for 24 h to obtain the product (yield 88%). M n =38.3 kDa, M w =116.3 kDa).
[0045] Figure 1 A synthetic route diagram for polymer PiBBTSS-H is shown.
[0046] Figure 2 The results of compound 3 in CDCl3 are shown. 1 ¹H NMR (δ 5.30 for CH₂Cl₂, δ 1.55 for H₂O). (From...) Figure 2 It can be seen that, 1 H NMR (500 MHz, CDCl3) δ 9.89 (s, 1H), 8.72 (s, 1H). MS (m / z): [M]+ calcd. For C6H2N4S2, 194.2300; found, 194.9792.
[0047] Figure 3 The mass spectrum (APCI mode) of compound 3 is shown.
[0048] Figure 4 The results of compound 4 in CDCl3 are shown. 1 HNMR. (By) Figure 4 It can be seen that, 1 H NMR (600 MHz, CDCl3)δ 8.88 (d, J = 1.2 Hz, 1H), 7.42 – 7.36 (m, 2H), 7.16 (s, 1H), 2.72 (d, J =6.8 Hz, 2H), 2.67 (d, J = 6.8 Hz, 2H), 1.73 (d, J = 35.0 Hz, 2H), 1.32 – 1.23 (m, 32H), 0.95 – 0.83 (m, 12H).
[0049] Figure 5 The results of compound 4 in CDCl3 are shown. 13 C NMR spectrum. (From...) Figure 5 It can be seen that, 13 C NMR (151 MHz, CDCl3) δ 154.97, 143.91, 143.22, 141.28, 140.85, 137.30, 133.78, 129.59,129.51, 123.44, 39.03, 39.00, 34.99, 34.97, 33.42, 33.37, 33.10, 33.04,31.94, 29.76, 29.73, 28.97, 28.90, 26.71, 26.64, 23.12, 23.10, 22.71, 14.20,14.14, 14.13. MS (m / z): [M] + calcd. For C 38 H 54 N4S4, 695.1180; found, 695.3304.
[0050] Figure 6 The mass spectrum (APCI mode) of compound 4 is shown.
[0051] Figure 7 The figure shows the measured values of monomer M1 in CDCl3.1 HNMR spectrum. (From) Figure 7 It can be seen that, 1 H NMR (600 MHz, CDCl3) δ 8.84 (s, 1H), 7.24 (s, 1H), 2.66 (d, J = 7.2 Hz, 2H), 2.61 (d, J =7.1 Hz, 2H), 1.86 – 1.71 (m, 2H), 1.33 – 1.23 (m, 32H), 0.97 – 0.81 (m, 12H).
[0052] Figure 8 The figure shows the measured values of monomer M1 in CDCl3. 13 CNMR spectrum. (From...) Figure 8 It can be seen that, 13 C NMR (151MHz, CDCl3) δ 154.49, 143.35, 142.79, 141.28, 140.36, 137.09, 133.70, 129.22,124.69, 120.54, 113.88, 113.09, 38.66, 38.57, 34.34, 34.27, 33.48, 33.39,33.19, 33.08, 31.93, 29.74, 28.89, 28.80, 26.62, 26.55, 23.11, 22.71, 22.70,14.19, 14.17, 14.15, 14.12. MS (m / z): [M] + calcd. For C 38 H 52 Br2N4S4, 852.9100; found, 853.1497.
[0053] Figure 9 The mass spectrum (APCI mode) of polymeric monomer M1 is shown.
[0054] Figure 10 The high-temperature GPC spectrum of polymer PiBBTSS-H in trichlorobenzene is shown.
[0055] Test Example 1 The optical properties of PiBBTSS-H were tested.
[0056] Test method: The solution absorption spectra and thin film absorption spectra of polymer donor PiBBTSS-H and polymer acceptor PA5 were measured.
[0057] Polymer acceptor PA5: Synthesized according to previously reported literature, it has the following chemical structure: .
[0058] Test results are as follows Figure 11 As shown.
[0059] Figure 11 Normalized CF solution absorption spectra and thin film absorption spectra of PiBBTSS-H and its receptor PA5 are shown. in, Figure 11 (a) shows the normalized CF solution absorption spectrum of PiBBTSS-H with receptor PA5; Figure 11 (b) shows the normalized thin-film absorption spectra of PiBBTSS-H and the receptor PA5.
[0060] The test results above show that the maximum absorption peak of PiBBTSS-H in solution is 701 nm, and the absorption cutoff edge is close to 800 nm. Compared with the absorption in solution, the thin film absorption has a maximum absorption peak of 643 nm, and the absorption cutoff edge is close to 800 nm. The corresponding optical band gap (E) is 798nm. g opt The absorption rate is 1.55 eV. Furthermore, the solution absorption of the polymer acceptor PA5 exhibits two shoulder peaks at 715 nm and 772 nm, while the corresponding thin film shows only a single maximum absorption peak at 807 nm, possibly due to J-aggregation of PA5 from solution to film. The absorption cutoff edge of PA5 (…) The wavelength is 906 nm, and the corresponding optical band gap is (E g opt The value is 1.37 eV. For example... Figure 11 As shown in (b), PiBBTSS-H and PA5 have complementary spectral characteristics, which can capture photons and convert them into photocurrents to the greatest extent possible.
[0061] Test Example 2 The electronic energy level characteristics of PiBBTSS-H were tested.
[0062] Test method: The ionization potential (IP) of polymer PiBBTSS-H and polymer acceptor PA5 was measured using ultraviolet photoelectron spectroscopy (UPS).
[0063] Test results are as follows Figure 12 As shown in Table 1.
[0064] Figure 12 The UPS test diagram of polymer PiBBTSS-H is shown.
[0065] Table 1 Optical and electronic energy level characteristics of polymer PiBBTSS-H The test results above show that the ionization potential of the polymer PiBBTSS-H is 5.24 eV, which is close to that of common donor polymers such as PBDB-T. This ensures that holes can be effectively transferred from the acceptor PA5 to the donor PiBBTSS-H, resulting in efficient charge dissociation.
[0066] Test Example 3 The photovoltaic performance of PiBBTSS-H was tested.
[0067] Test method: A photovoltaic device with the structure ITO / PEDOT:PSS / PiBBTSS-H:PA5 / PNDIT-F3N / Ag was prepared using PiBBTSS-H and PA5 as polymer donor and polymer acceptor, respectively, and chloroform as processing solvent, to verify the photovoltaic performance of polymer PiBBTSS-H.
[0068] Test results are as follows Figure 13 As shown in Table 2.
[0069] Figure 13 The current density-voltage (JV) curves and external quantum efficiency (EQE) of the polymer PiBBTSS-H for photovoltaic devices are shown. in, Figure 13 (a) shows the current density-voltage (JV) curves of the polymer PiBBTSS-H for photovoltaic devices; Figure 13 (b) shows the external quantum efficiency (EQE) of the polymer PiBBTSS-H for photovoltaic devices.
[0070] Table 2 Photovoltaic parameters of photovoltaic devices The test results above show that the device based on PiBBTSS-H:PA5... V OC The parameter is 0.894 V. J SC It is 23.73 mA·cm -2 The FF was 0.642, corresponding to a photoelectric conversion efficiency (PCE) of 13.61%. Furthermore, the external quantum efficiency (EQE) curve of the PiBBTSS-H:PA5 all-polymer solar cell device was tested. Figure 13As shown in (b), the device exhibits a spectral response in the 300-900 nm range, but the EQE response value is less than 75% across the entire spectral range, and the current value obtained by integrating the EQE is 23.07 mA cm⁻¹. -2 , and through JV The tested current error is less than 3%.
[0071] Test Example 4 Photocurrent of PiBBTSS-H based photovoltaic devices ( J ph - Effective voltage ( V eff The characteristic curves were tested.
[0072] Test results are as follows Figure 14 As shown.
[0073] Figure 14 This demonstrates a device based on PEDTQ:PA5. J ph -V eff Characteristic curves.
[0074] The test results above show that the ratio of the current density under no bias to the saturation current when all carriers in the device are swept out under bias can measure the charge dissociation efficiency of the device. Figure 14 As shown, the charge dissociation efficiency of the PEDTQ:PA5 device ( P(E,T) The efficiency of 94.3% indicates that there is a suitable energy level difference between the donor and acceptor, which enables the device to have high charge dissociation efficiency.
[0075] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.
[0076] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A polymer based on benzobisisothiadiazole units, characterized in that, The polymer based on benzobisisothiadiazole units has the following structure: ; in, The n is a positive integer from 1 to 10000; R1, R2, R3, and R4 are independently selected from alkyl, alkyl derivatives, aryl, aryl derivatives, and hydrogen atoms; All hydrogen atoms on the alkyl derivative were not substituted. or One or more hydrogen atoms at any position on an alkyl derivative are substituted by one or more of a halogen, mercapto, carbonyl, hydroxyl, amino, carboxyl, cyano, nitro, aryl, olefinic, alkyneic, or ester group. The aryl derivative is selected from groups containing one or more aromatic ring structures, wherein all hydrogen atoms on the aromatic ring are unsubstituted. or One or more hydrogen atoms at any position on one or more aromatic rings are substituted by one or more oxygen atoms, mercapto, halogen, hydroxyl, amino, carboxyl, cyano, nitro, aryl, olefinic, alkyneic, or ester groups. X is independently selected from one of S and NH.
2. The polymer based on benzobisisothiadiazole units according to claim 1, characterized in that, R1, R2, R3, and R4 are independently selected from C1-C30 alkyl groups with straight or branched structures, and C1-C30 alkyl derivatives with straight or branched structures.
3. The polymer based on benzobisisothiadiazole units according to claim 1, characterized in that, The polymer based on benzobisisothiadiazole units has the following structure: ; in, The n is a positive integer from 1 to 10000.
4. The method for preparing the polymer based on benzobisisothiadiazole units according to any one of claims 1-3, characterized in that, Includes the following steps: S1. 1,5-Dichloro-2,4-dinitrobenzene and sodium sulfide nonahydrate were mixed, heated and reacted, and purified to obtain compound 2. S2. Under low temperature conditions, tert-butyl nitrite was added to compound 2, the mixture was stirred and reacted, and after purification, compound 3 was obtained. S3. Compound 3 and bromosubstituted alkylthiophene were blended, and palladium catalyst, phosphine ligand precursor, fatty carboxylic acid and inorganic base reagent were added. The mixture was heated under an inert atmosphere and purified to obtain compound 4. S4. Under light-protected conditions, N-bromosuccinimide was added to compound 4, the mixture was stirred and reacted, and the resulting polymer monomer M1 was obtained after purification. S5. The polymer monomers M1 and BDT-Sn are blended, and palladium catalyst and phosphine ligand are added. The mixture is heated under an inert atmosphere and purified to obtain a polymer based on benzobisisothiadiazole units.
5. The method for preparing the polymer based on benzobisisothiadiazole units according to claim 4, characterized in that, In step S1, the mass ratio of 1,5-dichloro-2,4-dinitrobenzene to sodium sulfide nonahydrate is 1:(20-40).
6. The method for preparing the polymer based on benzobisisothiadiazole units according to claim 4, characterized in that, In step S2, the mass ratio of compound 2 to tert-butyl nitrite is 1:(3-6).
7. The method for preparing the polymer based on benzobisisothiadiazole units according to claim 4, characterized in that, In step S2, the low temperature condition is -10 to -10°C.
8. The method for preparing the polymer based on benzobisisothiadiazole units according to claim 4, characterized in that, In step S3, the mass ratio of compound 3 to bromosubstituted alkylthiophene is 1:(4-6).
9. The method for preparing the polymer based on benzobisisothiadiazole units according to claim 4, characterized in that, In step S4, the mass ratio of compound 4 to NBS is 1:(0.1-1).
10. The method for preparing the polymer based on benzobisisothiadiazole units according to claim 4, characterized in that, In step S5, the mass ratio of the polymeric monomer M1 to BDT-Sn is 1:(1-1.5).