A continuous glass fiber reinforced polyamide 6 composite material and its preparation method

By introducing carbon-carbon double bond side groups into the amino groups on the glass fiber surface through in-situ anionic ring-opening polymerization, the problem of insufficient interfacial bonding strength in the prior art is solved, and efficient load transfer and interfacial layer continuity of continuous glass fiber reinforced polyamide 6 composite material are achieved, significantly improving the tensile strength and impact toughness of the material.

CN123107068APending Publication Date: 2026-11-17QIANWAN INST OF CNITECH +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611321496.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing technology lacks a simple, one-step preparation method for continuous glass fiber reinforced polyamide 6 composite materials that does not require fiber pre-activation or post-treatment and can achieve covalent interfacial bonding between the resin matrix and reinforcing fibers through main chain functionalization. This results in limited interfacial bonding strength, difficulty in achieving efficient load transfer, and insufficient continuity of the interfacial layer.

Method used

In-situ anionic ring-opening polymerization is used to copolymerize functional comonomers containing carbon-carbon double bonds with caprolactam, so that carbon-carbon double bond side groups are directly suspended on the polyamide 6 main chain. During the polymerization process, they form covalent bonds with amino groups on the surface of continuous glass fibers, constructing an interface layer with covalent bonds as anchor nodes, and a continuous load transfer network with hydrogen bonds as synergistic effects.

Benefits of technology

It achieved an increase of ≥25% in tensile strength and ≥100% in impact toughness of composite materials, while simplifying the process, avoiding fiber pre-activation treatment, and improving the rigidity and impact resistance of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107068A_ABST
    Figure CN123107068A_ABST
Patent Text Reader

Abstract

This invention discloses a continuous glass fiber reinforced polyamide 6 composite material and its preparation method. The composite material is formed by in-situ anionic ring-opening polymerization of a mixture of caprolactam and caprolactam derivative monomers containing carbon-carbon double bonds to form a matrix. During polymerization, the derivative copolymerization causes the PA6 main chain to suspend double bond side groups, which are then covalently bonded in situ to the amino groups on the glass fiber surface, constructing a continuous load transfer network interface layer anchored by covalent bonds and synergistically supported by hydrogen bonds. Molding and interface construction are completed simultaneously. Preparation method: Under an inert atmosphere, caprolactam is melted and dehydrated. An alkaline catalyst, functional monomer, and isocyanate activator are added sequentially to obtain a reaction solution. A continuous glass fiber preform is poured in using RTM (Regenerative Thermal Injection), and polymerization is carried out at 150-180℃ while interface bonding occurs. Demolding is then performed. This invention achieves synergistic enhancement of tensile and impact properties in a one-step process, without the need for fiber preactivation or post-treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer materials technology, and in particular to a continuous glass fiber reinforced polyamide 6 composite material and its preparation method. Background Technology

[0002] Glass fiber reinforced polyamide 6 composites are widely used in automotive, aerospace, and other fields due to their lightweight and high strength properties. However, the interfacial bonding state between the glass fiber surface and the polyamide 6 matrix directly determines the overall mechanical properties of the composite. Conventional glass fiber reinforced polyamide 6 composites typically improve interfacial compatibility through physical blending or fiber surface coupling agent treatment. However, physical blending mainly relies on mechanical friction and weak hydrogen bonding between the fiber and resin, resulting in limited interfacial bonding strength and difficulty in achieving efficient load transfer. While coupling agent treatment can enhance interfacial interactions to some extent, it is mostly a monolayer physical or chemical modification of the fiber surface, leading to insufficient interfacial layer continuity. Furthermore, the introduction of coupling agents often requires pre-activation treatment of the fibers, increasing the process and cost. In terms of polymerization technology, traditional anionic ring-opening polymerization for polyamide 6 preparation typically uses caprolactam as the sole monomer. The resulting resin backbone has a saturated carbon chain structure, lacking active side groups for subsequent reactions or interfacial bonding. Therefore, it is impossible to simultaneously achieve chemical bonding with the reinforcing fibers during polymerization. A few studies have attempted to enhance the interface by grafting or blending active groups into the resin. However, these methods mostly require subsequent fiber surface activation treatment or multi-step reactions, resulting in lengthy process routes and complex parameter control. It is difficult to achieve effective synergy between resin matrix polymerization and interfacial bonding in situ in a single step. Regarding reinforcement forms, research on chopped fiber or nanofiller systems is relatively common, while in-situ interface construction schemes for continuous glass fiber reinforced systems are rarely reported. In particular, the technical route of directly introducing reactive double bond side groups onto the polyamide 6 molecular chain via main-chain copolymerization, and then forming covalent bonds with the amino groups on the continuous glass fiber surface to anchor the interface during polymerization, is still undisclosed.

[0003] Therefore, the existing technology lacks a continuous glass fiber reinforced polyamide 6 composite material and its preparation scheme that is simple to process, can be completed in one step, does not require fiber preactivation or post-treatment, and can achieve covalent interfacial bonding between the resin matrix and the reinforcing fiber through main chain functionalization. Summary of the Invention

[0004] To address the aforementioned shortcomings, this invention proposes a continuous glass fiber reinforced polyamide 6 composite material and its preparation method, which achieves synergistic enhancement of tensile strength and impact toughness. Simultaneously, matrix forming and interface construction are completed simultaneously in a one-step polymerization process, eliminating the need for fiber pre-activation or post-treatment.

[0005] This invention provides the following technical solution: a continuous glass fiber reinforced polyamide 6 composite material, comprising continuous glass fibers and a polyamide 6 matrix. The polyamide 6 matrix is ​​formed by in-situ anionic ring-opening polymerization of a monomer mixture containing caprolactam and a functional comonomer, wherein the functional comonomer is a caprolactam derivative containing a carbon-carbon double bond. During in-situ anionic ring-opening polymerization, the functional comonomer copolymerizes with caprolactam, causing carbon-carbon double bond side groups to be directly suspended on the polyamide 6 main chain. The carbon-carbon double bond side groups and the amino groups inherent on the surface of the continuous glass fiber undergo covalent bonding during in-situ polymerization, thereby constructing an interface layer in-situ between the continuous glass fiber and the polyamide 6 matrix. The interface layer forms a continuous load transfer network with covalent bonds as anchor nodes and hydrogen bonds as synergistic effects. Moreover, the molding of the composite material and the construction of this interface layer are completed simultaneously in the same process of in-situ anionic ring-opening polymerization.

[0006] As an improvement, the functional comonomer is α-allyl-ε-caprolactam, i.e., propylene caprolactam.

[0007] As an improvement, the mass of the functional comonomer is 1% to 10% of the mass of caprolactam.

[0008] As an improvement, continuous glass fiber is E-glass fiber, existing in the form of continuous fiber cloth or continuous fiber mat.

[0009] As an improvement, the covalent bond is a carbon-nitrogen covalent bond formed between the allyl carbon atom of the carbon-carbon double bond side group and the nitrogen atom of the amino group on the glass fiber surface.

[0010] As an improvement, the polyamide 6 matrix is ​​a continuous matrix phase formed by in-situ anionic ring-opening polymerization after being injected into a continuous glass fiber preform through a resin transfer molding process. This continuous matrix phase completely covers the continuous glass fiber and forms an integral structure with the interface layer.

[0011] As an improvement, the tensile strength of the composite material is increased by ≥25% compared to the same system without functional comonomers, and the impact toughness is increased by ≥100%.

[0012] A method for preparing a continuous glass fiber reinforced polyamide 6 composite material, for preparing any of the continuous glass fiber reinforced polyamide 6 composite materials as described above, includes the following steps: S1. Under an inert atmosphere, caprolactam is heated and melted, and then dehydrated under vacuum. S2. Add sodium caprolactam, an alkaline catalyst, to the melt obtained in step S1, then add a functional comonomer, and then add caprolactam-terminated hexamethylene diisocyanate, an isocyanate activator, to obtain a reaction solution. S3. The reaction liquid is injected into a closed mold with a continuous glass fiber preform laid on it through a resin transfer molding process; S4. Raise the mold temperature to 150℃~180℃ and react for 20-30 minutes to allow caprolactam and functional comonomer to undergo in-situ anionic ring-opening polymerization. At the same time, the carbon-carbon double bond side groups on the main chain of the polymerized polyamide 6 form covalent bonds with the amino groups on the surface of the continuous glass fiber. After cooling, demold to obtain the composite material.

[0013] As an improvement, sodium caprolactam is added in the form of a caprolactam solution containing 17 wt% sodium caprolactam, and the amount is 1.5 wt% of the total mass of caprolactam and functional comonomer in step S1, and the amount of activator is 2 wt% of the total mass.

[0014] As an improvement, the functional comonomer is α-allyl-ε-caprolactam, which is prepared by a method comprising the following steps: Under an inert atmosphere, caprolactam was dissolved in anhydrous tetrahydrofuran, cooled to -85°C to -70°C, and then n-butyllithium and trichlorosilane were added sequentially. The mixture was heated to -5°C to -10°C to react, and then cooled again to -85°C to -70°C before adding diisopropylaminolithium. After stirring, propylene bromide was added, and the mixture was heated to room temperature to continue the reaction. After the reaction was completed, the mixture was quenched, extracted, dried, and purified by column chromatography to obtain α-allyl-ε-caprolactam.

[0015] Compared with the prior art, the advantages of the present invention are as follows: In-situ anionic ring-opening polymerization is used to copolymerize functional comonomers containing carbon-carbon double bonds with caprolactam, directly introducing suspended carbon-carbon double bond side groups onto the polyamide 6 backbone. These double bond side groups covalently bond with the amino groups inherent on the continuous glass fiber surface during polymerization, thereby constructing a continuous load transfer network in-situ between the fiber and the matrix, anchored by covalent bonds and synergistically enhanced by hydrogen bonds. This interface layer enables the efficient transfer of external loads from the matrix to the fiber through chemical bonds, significantly inhibiting interface debonding and fiber pull-out. Simultaneously, the synergistic effect of hydrogen bonds endows the interface layer with appropriate energy dissipation capabilities, thus significantly improving both the rigidity and strength of the material and its impact toughness, achieving a synergistic reinforcement effect of at least 25% increase in tensile strength and at least 100% increase in impact toughness.

[0016] The matrix molding and interface layer construction of the composite material are completed simultaneously in the same in-situ anionic ring-opening polymerization process. The generation of resin matrix, fiber impregnation, interfacial covalent bonding and final product molding are integrated. The process is simple and controllable, and in-situ polymerization is completed in one step. There is no need to pre-activate the fiber or perform any interface post-treatment steps after the composite material is molded. The process has fewer steps, shorter cycle, and is easy to realize industrial production.

[0017] By enhancing the interface between glass fiber and polyamide 6 through in-situ copolymerization of α-allyl-ε-caprolactam and caprolactam, a technical route was achieved to directly suspend double bond side groups in polyamide 6 and covalently bond them with amino groups on the glass fiber surface via main chain copolymerization.

[0018] The resin transfer molding process allows the monomer mixture to be polymerized in situ in a continuous glass fiber preform. The resulting polyamide 6 continuous matrix phase completely encapsulates the fiber and forms an integral structure with it through covalent bonds. The product has few internal defects, controllable fiber volume fraction, and good dimensional stability, making it suitable for manufacturing complex continuous fiber reinforced thermoplastic composite structural parts.

[0019] The preparation method of the functional comonomer used has well-defined reaction conditions and is controllable. It can selectively introduce allyl groups into the caprolactam molecule, providing a new feasible monomer synthesis route for the molecular design of functionalized polyamide 6.

[0020] This technical solution provides a clear optimization range for key process parameters such as the amount of functional comonomer, polymerization temperature and time. The method has good repeatability, and the mechanical properties of the resulting composite material are stable between batches, which can meet the material reliability requirements of load-bearing structural components. Attached Figure Description

[0021] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments: Figure 1 The flow chart for the reaction of propylene bromide modifying caprolactam; Figure 2 This is a flowchart of the copolymerization reaction of propylene caprolactam and caprolactam. Figure 3 This is a schematic diagram of the interfacial interaction mechanism between modified copolymer nylon 6 and glass fiber; Figure 4 The 1H NMR spectrum of acrylamide; Figure 5 The infrared spectrum of acrylamide; Figure 6 This is the DSC spectrum of propylene caprolactam; Figure 7 A bar chart comparing the tensile strength of the composite material before and after modification; Figure 8 A bar chart comparing the impact strength of the composite material before and after modification; Figure 9 A bar chart comparing the interlaminar shear strength of the composite material before and after modification; Figure 10 Scanning electron microscope (SEM) comparison images of the 1%, 5%, and 10% modified composite materials and the comparative example. Detailed Implementation

[0022] Example 1 (Modified, Low Dose) like Figures 1 to 10 The preparation method of propylene caprolactam is as follows: Under nitrogen protection, 1 g of caprolactam is dissolved in 52 mL of ultra-dry tetrahydrofuran, cooled to -78 °C, and 5.3 mL of n-butyllithium in cyclohexane is added dropwise. After stirring evenly, 1.17 mL of trichlorosilane is added, and the mixture is heated to 0 °C and stirred for 30 minutes. The mixture is then cooled to -78 °C again, and 10.1 mL of diisopropylaminolithium solution is added dropwise. After stirring for 1 hour, 1.87 mL of propylene bromide is added, and the mixture is heated to room temperature and reacted under nitrogen protection for 8 hours. After the reaction is completed, the mixture is quenched with saturated ammonium chloride, extracted with ethyl acetate and water, and the organic phase is dried with anhydrous sodium sulfate. The mixture is purified by column chromatography using a mixed solvent of petroleum ether and ethyl acetate in a volume ratio of 4:1 to 3:1 as the eluent. The solvent is removed by rotary evaporation to obtain propylene caprolactam, i.e., α-allyl-ε-caprolactam. A method for preparing a continuous glass fiber reinforced polyamide 6 composite material, comprising taking 100 parts by mass of caprolactam and 1 part by mass of the above-mentioned propylene caprolactam, and drying them under vacuum; S1. Under nitrogen protection, take 20g of caprolactam and melt it at 130℃, then remove water by vacuum for 10 minutes. S2. Add 1.5wt% sodium caprolactam solution to the melt. The solution is a 17% mass fraction solution formed by dissolving sodium caprolactam in caprolactam. Add 270mg of the above-mentioned propylene caprolactam, and then add 2wt% caprolactam-terminated hexamethylene diisocyanate as an activator. Stir until homogeneous to obtain the reaction solution. S3. The reaction solution is injected into a closed mold pre-laid with continuous alkali-free glass fiber cloth through a resin transfer molding process, with the glass fiber volume fraction being 30%. S4. Raise the mold temperature to 150℃, keep it at that temperature for 30 minutes, and then demold after cooling to obtain a continuous glass fiber reinforced polyamide 6 composite material sheet.

[0023] Scanning electron microscopy revealed that the fiber surface of the modified composite material was densely coated with resin, significantly reducing fiber pull-out and exhibiting toughness failure characteristics at the interface; while the comparative cross-section showed a large number of exposed fibers and interface debonding voids.

[0024] A pure PA6 / continuous glass fiber composite material without acrylamide was prepared as a comparative example using the same process. The tensile strength of Example 1 was 240.3 MPa, an increase of 3.7% compared to the comparative example; the impact toughness was 128.3 kJ / m. 2 Compared with the control, it increased by 95.3%; the flexural strength and interlaminar shear strength increased by 15.9% and 17.4%, respectively.

[0025] Example 2 (Modified, Medium Dose) A method for preparing a continuous glass fiber reinforced polyamide 6 composite material, comprising taking 100 parts by mass of caprolactam and 5 parts by mass of the above-mentioned propylene caprolactam, and drying them under vacuum.

[0026] S1. Under nitrogen protection, take 20g of caprolactam and melt it at 130℃, then remove water by vacuum for 10 minutes. S2. Add 1.5wt% sodium caprolactam solution to the melt. This solution is a 17% mass fraction solution formed by dissolving sodium caprolactam in caprolactam. Add 1.35g of the above propylene caprolactam and then add 2wt% caprolactam-terminated hexamethylene diisocyanate as an activator. Stir until homogeneous to obtain the reaction solution. S3. The reaction solution is injected into a closed mold pre-laid with continuous alkali-free glass fiber cloth through a resin transfer molding process, with the glass fiber volume fraction being 30%. S4. Raise the mold temperature to 150℃, keep it at that temperature for 30 minutes, and then demold after cooling to obtain a continuous glass fiber reinforced polyamide 6 composite material sheet.

[0027] Scanning electron microscopy revealed that the fiber surface of the composite material cross-section was densely coated with resin, significantly reducing fiber pull-out and resulting in a tighter interfacial bond, exhibiting characteristics of ductile failure. Compared to Example 1, increasing the amount of acrylamide to 5% resulted in increased interfacial covalent bond anchoring density and a denser continuous load transfer network.

[0028] A pure PA6 / continuous glass fiber composite material without acrylamide was prepared as a comparative example using the same process. The tensile strength of Example 2 was 291.0 MPa, an increase of 26.0% compared to the comparative example; the impact toughness was 141.5 kJ / m. 2 Compared to the control example, the mechanical properties of Example 2 were improved by 115.3%; the flexural strength and interlaminar shear strength were improved by 33.4% and 32.4%, respectively. Compared with Example 1, the mechanical properties of Example 2 were improved more significantly, indicating that appropriately increasing the amount of acrylamide helps to further enhance the interfacial anchoring effect and the density of the continuous load transfer network.

[0029] Example 3 (Modified, High Dose) Take 100 parts by weight of caprolactam and 10 parts by weight of the above-mentioned propylene caprolactam, and dry them under vacuum.

[0030] S1. Under nitrogen protection, take 20g of caprolactam and melt it at 130℃, then remove water by vacuum for 10 minutes. S2. Add 1.5wt% sodium caprolactam solution to the melt. This solution is a 17% mass fraction solution formed by dissolving sodium caprolactam in caprolactam. Add 2.70g of the above propylene caprolactam and then add 2wt% caprolactam-terminated hexamethylene diisocyanate as an activator. Stir until homogeneous to obtain the reaction solution. S3. The reaction solution is injected into a closed mold pre-laid with continuous alkali-free glass fiber cloth through a resin transfer molding process, with the glass fiber volume fraction being 30%. S4. Raise the mold temperature to 150℃, keep it at that temperature for 30 minutes, and then demold after cooling to obtain a continuous glass fiber reinforced polyamide 6 composite material sheet.

[0031] Scanning electron microscopy revealed that the fiber surface of the composite material cross-section was densely coated with resin, further reducing fiber pull-out and demonstrating good interfacial bonding.

[0032] A pure PA6 / continuous glass fiber composite material without acrylamide was prepared as a comparative example using the same process. The tensile strength of Example 3 was 266 MPa, an increase of 14.9% compared to the comparative example; the impact toughness was 142.8 kJ / m. 2 Compared to the control, the strength increased by 117.3%; the flexural strength and interlaminar shear strength increased by 27.8% and 20.4%, respectively. Compared to Examples 1 and 2, when the amount of acrylamide was increased to 10%, the interfacial covalent bond anchoring density further increased, but the improvement in mechanical properties was more gradual compared to Example 2, indicating that a 5% dosage can achieve a better interfacial anchoring effect.

[0033] Comparative Example Take 100 parts by weight of caprolactam and dry them under vacuum.

[0034] S1. Under nitrogen protection, take 20g of caprolactam and melt it at 130℃, then remove water by vacuum for 10 minutes. S2. Add 1.5wt% sodium caprolactam solution to the melt. This solution is a 17% mass fraction solution formed by dissolving sodium caprolactam in caprolactam. Then add 2wt% caprolactam-terminated hexamethylene diisocyanate as an activator and stir until homogeneous to obtain the reaction solution. S3. The reaction solution is injected into a closed mold pre-laid with continuous alkali-free glass fiber cloth through a resin transfer molding process, with the glass fiber volume fraction being 30%. S4. Raise the mold temperature to 150℃, keep it at that temperature for 30 minutes, and then demold after cooling to obtain a continuous glass fiber reinforced polyamide 6 composite material sheet.

[0035] In this comparative example, no propylene caprolactam was added. The caprolactam was subjected to in-situ anionic ring-opening polymerization alone. The resulting polyamide 6 main chain had no unsaturated double bond side groups. During the polymerization process, the resin matrix was only bonded to the glass fiber surface through physical wetting and hydrogen bonding, and could not form a covalently anchored interface layer.

[0036] Scanning electron microscopy revealed that the cross-section of the comparative composite material showed a large number of exposed fibers and voids left after the fibers were pulled out. The fiber surface was smooth, the amount of resin attached was small, and the interface exhibited typical interfacial debonding and failure characteristics.

[0037] Mechanical properties were tested according to relevant standards such as ASTM D2344. The tensile strength of the comparative example was 231.3 MPa, and the impact toughness was 65.7 kJ / m. 2 The flexural strength was 286.3 MPa, and the interlaminar shear strength was 44.1 MPa. Compared with Examples 1, 2, and 3, all mechanical properties were significantly lower, indicating that without the introduction of acrylamide, there was a lack of effective covalent interfacial anchorage between the fiber and the matrix, resulting in low load transfer efficiency and limited mechanical properties of the composite material. This comparative example serves as a benchmark to evaluate the interfacial reinforcement effect of acrylamide in each example.

[0038] Example 2 uses 5% propylene caprolactam copolymer modification, where the double bond forms stable covalent and hydrogen bonds with the glass fiber amino group, resulting in the best interfacial anchoring effect and the most significant improvement in tensile strength and impact strength.

[0039] The above description only illustrates the preferred embodiments of the present invention and should not be construed as limiting the scope of the claims. The present invention is not limited to the above embodiments, and variations in its specific structure are permitted. All modifications made within the scope of the independent claims of this invention are also within the scope of protection of this invention.

Claims

1. A continuous glass fiber reinforced polyamide 6 composite material, comprising continuous glass fibers and a polyamide 6 matrix, characterized in that, The polyamide 6 matrix is ​​formed by in-situ anionic ring-opening polymerization of a monomer mixture containing caprolactam and a functional comonomer, wherein the functional comonomer is a caprolactam derivative containing a carbon-carbon double bond. During the in-situ anionic ring-opening polymerization process, the functional comonomer copolymerizes with caprolactam, causing carbon-carbon double bond side groups to be directly suspended on the polyamide 6 main chain. The carbon-carbon double bond side groups covalently bond with the amino groups inherent on the surface of the continuous glass fiber during in-situ polymerization, thereby constructing an interface layer in-situ between the continuous glass fiber and the polyamide 6 matrix. The interface layer forms a continuous load transfer network with covalent bonds as anchor nodes and hydrogen bonds as synergistic effects. Furthermore, the molding of the composite material and the construction of the interface layer are completed simultaneously in the same step of the in-situ anionic ring-opening polymerization.

2. A continuous glass fiber reinforced polyamide 6 composite material according to claim 1, characterized in that, The functional comonomer is α-allyl-ε-caprolactam, i.e., propylene caprolactam.

3. The continuous glass fiber reinforced polyamide 6 composite material according to claim 1, characterized in that, The mass of the functional comonomer is 1% to 10% of the mass of the caprolactam.

4. The continuous glass fiber reinforced polyamide 6 composite of claim 1, wherein, The continuous glass fiber is E-glass fiber, and exists in the form of continuous fiber cloth or continuous fiber mat.

5. The continuous glass fiber reinforced polyamide 6 composite material according to claim 1, wherein, The covalent bond is a carbon-nitrogen covalent bond formed between the allyl carbon atom of the carbon-carbon double bond side group and the nitrogen atom of the amino group on the glass fiber surface.

6. The continuous glass fiber reinforced polyamide 6 composite of claim 1, wherein, The polyamide 6 matrix is ​​a continuous matrix phase formed by in-situ anionic ring-opening polymerization after being injected into a continuous glass fiber preform through resin transfer molding. This continuous matrix phase completely covers the continuous glass fiber and forms an integral structure with the interface layer.

7. The continuous glass fiber reinforced polyamide 6 composite of claim 1, wherein, The tensile strength of the composite material is increased by ≥25% compared to the same system without the functional comonomer, and the impact toughness is increased by ≥100%.

8. A process for the preparation of a continuous glass fiber reinforced polyamide 6 composite for the preparation of a continuous glass fiber reinforced polyamide 6 composite according to any one of claims 1 to 7, characterized in that Includes the following steps: S1. Under an inert atmosphere, caprolactam is heated and melted, and then dehydrated under vacuum. S2. Add sodium caprolactam, an alkaline catalyst, to the melt obtained in step S1, then add a functional comonomer, and then add caprolactam-terminated hexamethylene diisocyanate, an isocyanate activator, to obtain a reaction solution. S3. The reaction liquid is injected into a closed mold on which a continuous glass fiber preform is laid through a resin transfer molding process; S4. Raise the mold temperature to 150℃~180℃ and react for 20-30 minutes to allow caprolactam and functional comonomer to undergo in-situ anionic ring-opening polymerization. At the same time, the carbon-carbon double bond side groups on the main chain of the polymerized polyamide 6 form covalent bonds with the amino groups on the surface of the continuous glass fiber. After cooling, demold to obtain the composite material.

9. The method for preparing a continuous glass fiber reinforced polyamide 6 composite material according to claim 8, characterized in that, The sodium caprolactam is added in the form of a caprolactam solution containing 17 wt% sodium caprolactam, and the amount used is 1.5 wt% of the total mass of caprolactam and functional comonomer in step S1. The amount of activator used is 2 wt% of the total mass.

10. The method for preparing a continuous glass fiber reinforced polyamide 6 composite material according to claim 8, characterized in that, The functional comonomer is α-allyl-ε-caprolactam, which is prepared by a method comprising the following steps: Under an inert atmosphere, caprolactam was dissolved in anhydrous tetrahydrofuran, cooled to -85°C to -70°C, and then n-butyllithium and trichlorosilane were added sequentially. The mixture was heated to -5°C to -10°C to react, and then cooled again to -85°C to -70°C before adding diisopropylaminolithium. After stirring, propylene bromide was added, and the mixture was heated to room temperature to continue the reaction. After the reaction was completed, the mixture was quenched, extracted, dried, and purified by column chromatography to obtain the α-allyl-ε-caprolactam.