Polyurethane foam composition, polyurethane foam, preparation method and recycling method, refrigeration equipment

Polyurethane foam was prepared by mixing modified lignin-based polyols with methyl 1,6-hexamethylene dicarboxylate and cyclic carbonate phenolic hydroxy alkylating agents. This method overcomes the shortcomings of non-isocyanate polyurethane foam in terms of bio-based content, thermal insulation performance, and mechanical properties, and achieves safe, economical, and recyclable polyurethane foam production.

CN123107076APending Publication Date: 2026-11-17TCL HOME APPLIANCES (HEFEI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611264964.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Non-isocyanate polyurethane foams cannot simultaneously meet the requirements of high bio-based content, thermal insulation, mechanical properties, and dimensional stability. Furthermore, traditional isocyanate-based polyurethanes pose safety hazards and are difficult to recycle.

Method used

Polyurethane foam compositions were prepared by modifying lignin-based polyols. A mixture of methyl 1,6-hexamethylene dicarboxylate, modified lignin-based polyols, cyclic carbonate phenolic hydroxyl alkylating agents, and polyether polyols was used for foaming and curing to form a polymer network with high crosslinking density.

Benefits of technology

With high bio-based content, polyurethane foam maintains excellent thermal insulation and mechanical properties, while reducing production costs and safety risks, and achieving recyclability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107076A_ABST
    Figure CN123107076A_ABST
Patent Text Reader

Abstract

This application discloses a polyurethane foam composition, polyurethane foam, preparation method and recycling method, and refrigeration equipment, relating to the field of polyurethane foam technology. The polyurethane foam composition includes methyl 1,6-hexamethylenedicarbamate and a mixture; the mixture contains a lignin-based polyol, which is mainly obtained by modifying lignin with polyether polyol and cyclic carbonate phenolic hydroxyl alkylating agents. The lignin-based polyol provided in this application can enhance the mechanical properties and thermal stability of polyurethane foam, thereby enabling polyurethane foam to maintain excellent thermal insulation and mechanical properties even with high bio-based content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of polyurethane foam technology, and in particular to polyurethane foam compositions, polyurethane foam, preparation methods and recycling methods, and refrigeration equipment. Background Technology

[0002] Non-isocyanate polyurethane (NIPU) foam is usually prepared by using cyclic carbonates and amine curing agents. This preparation method not only eliminates isocyanates, but also allows cyclic carbonates to be prepared using CO2 and epoxides, achieving carbon capture and curing.

[0003] However, NIPU foam cannot simultaneously meet the requirements for high bio-based content, thermal insulation, mechanical properties, and dimensional stability. Summary of the Invention

[0004] In view of this, this application provides a polyurethane foam composition, polyurethane foam, preparation method and recycling method, and refrigeration equipment.

[0005] The embodiments of this application are implemented as follows: a polyurethane foam composition comprising methyl 1,6-hexamethylenedicarbamate and a mixture thereof; the mixture comprising a lignin-based polyol, the lignin-based polyol being mainly obtained by modifying lignin with polyether polyol and cyclic carbonate phenolic hydroxyl alkylating agents.

[0006] Optionally, in some embodiments of this application, the lignin includes one or more of lignin sulfonate, organic solvent lignin, hydrolyzed lignin, and alkali lignin; the lignin sulfonate includes one or more of sodium lignin sulfonate and calcium lignin sulfonate; the organic solvent lignin includes one or more of birch organic solvent lignin, wheat straw alkali lignin, and pine sulfate lignin; the hydrolyzed lignin includes one or more of acid-hydrolyzed lignin and enzymatically hydrolyzed residue lignin; and the alkali lignin includes one or more of wheat straw soda ash lignin and sugarcane bagasse soda ash lignin. The functionality of the polyether polyol is 2 to 3, and the number-average molecular weight of the polyether polyol is 200 to 600 g / mol. Optionally, the polyether polyol includes one or more of polyethylene glycol, polypropylene glycol, polytetrahydrofuran ether glycol, and bio-based 1,3-propanediol polyether polyol; The cyclic carbonate phenolic hydroxy alkylating agent includes ethylene carbonate; The moisture content of the lignin is ≤0.1wt%, the moisture content of the polyether polyol is ≤0.05wt%, and the moisture content of the cyclic carbonate phenolic hydroxyalkylating agent is ≤0.05wt%. The mass ratio of the lignin to the polyether polyol is (3~5):(5~7); Based on a total mass of 100 parts by weight of the lignin and the polyether polyol, the mass of the cyclic carbonate phenolic hydroxy alkylating agent is 11.6 to 19.4 parts by weight.

[0007] Optionally, in some embodiments of this application, the methyl 1,6-hexamethylenedicarbamate is mainly obtained by reacting hexamethylenediamine and dimethyl carbonate; wherein the molar ratio of hexamethylenediamine to dimethyl carbonate is 1:(8.0~12.0). In the polyurethane foam composition, the molar ratio of the urethane ester of the methyl 1,6-hexamethylenedicarbamate to the hydroxyl group in the lignin-based polyol is (0.85~1.1):1.

[0008] Optionally, in some embodiments of this application, the mixture further comprises a first organic base catalyst; The first organic base catalyst comprises one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene; Based on a total mass of 100 parts by mass of the lignin and the polyether polyol, the first organic base catalyst comprises 2.5 to 4.2 parts by mass. The polyurethane foam composition further includes a foaming agent and a foam leveling agent; The foaming agent includes physical foaming agents, which include one or more of alkane-based physical foaming agents and fluoroolefin-based foaming agents. The alkane-based physical foaming agents include one or more of cyclopentane, isopentane, n-pentane, and cyclohexane. The fluoroolefin-based foaming agents include 1,3,3,3-tetrafluoropropylene foaming agent, 1-chloro-3,3,3-trifluoropropylene foaming agent, and 2,3,3,3-tetrafluoropropylene foaming agent. The foam stabilizer includes an organosilicone foam stabilizer, which includes one or more of the following: Mistide AK-8805, Mistide AK-8803, and Momentive L-580 silicone oil. Based on a total mass of 100 parts by weight of the lignin and the polyether polyol, the mass of methyl 1,6-hexamethylenedicarbamate is 29-44 parts by weight, the mass of the foaming agent is 10-12 parts by weight, and the mass of the foam leveling agent is 1.0-2.0 parts by weight.

[0009] Accordingly, this application also provides a polyurethane foam, which is obtained by foaming the polyurethane foam composition described above.

[0010] Optionally, in some embodiments of this application, the closed-cell rate of the polyurethane foam is ≥90%; The apparent core density of the polyurethane foam is ≤36 kg / m³. 3 ; The deformation compressive stress of the polyurethane foam is ≥130kPa; The low-temperature dimensional stability of the polyurethane foam is ≤1.0%; The dimensional stability of the polyurethane foam under humid heat is ≤1.5%; The initial thermal conductivity of the polyurethane foam is 0.0185 W / (m·K) to 0.0195 W / (m·K); The water absorption rate of the polyurethane foam is ≤4%.

[0011] Accordingly, this application also provides a method for preparing polyurethane foam, comprising the following steps: The invention provides methyl 1,6-hexamethylenedicarbamate and a mixture thereof; the mixture comprises a lignin-based polyol, which is mainly obtained by modifying lignin with polyether polyol and phenolic alkylating agent; The methyl 1,6-hexamethylenedicarbamate, the mixture, the foaming agent, and the blowing agent are mixed and then injected into a mold for curing and hot pressing to obtain polyurethane foam.

[0012] Optionally, in some embodiments of this application, the methyl 1,6-hexamethylenedicarbamate is provided, comprising: Hexamethylenediamine, dimethyl carbonate, and a second organic base catalyst are mixed to induce a carbamate reaction between the hexamethylenediamine and the dimethyl carbonate, yielding a reaction solution. The reaction solution was allowed to stand and filtered to obtain a reaction product and a reaction filtrate; the reaction filtrate included a second organic base catalyst, and the reaction product included methyl 1,6-hexamethylenedicarbamate. The reaction product was dried under vacuum to obtain methyl 1,6-hexamethylenedicarbamate. The reaction filtrate is mixed with the hexamethylenediamine and the dimethyl carbonate to obtain methyl 1,6-hexamethylenedicarbamate.

[0013] Optionally, in some embodiments of this application, The second organic base catalyst comprises one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene; The molar ratio of hexamethylenediamine to dimethyl carbonate is 1:(8.0~12.0). The molar ratio of hexamethylenediamine to the second organic base catalyst is 1:(0.05~0.15). The mixing conditions are as follows: under inert gas protection, the temperature is 80~100℃, the time is 10h~14h, and the stirring speed used for mixing is 200~400 rpm. The reaction solution was allowed to stand for 1 to 3 hours in an ice bath at a temperature of 0 to 4°C. The conditions for vacuum drying of the reaction product are: vacuum degree ≤ -0.095 MPa, temperature 35~45℃, and time 10~14h.

[0014] Optionally, in some embodiments of this application, the mixture is provided, comprising: Provides lignin; The lignin, polyether polyol, and cyclic carbonate phenolic hydroxyl alkylating agent are each independently vacuum dried; The first organic base catalyst, vacuum-dried lignin, the polyether polyol, and the cyclic carbonate phenolic hydroxyl alkylating agent are mixed to modify the lignin with the polyether polyol and the cyclic carbonate phenolic hydroxyl alkylating agent, thereby obtaining the mixture. The first organic base catalyst includes one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene; The mixing conditions are as follows: under inert gas protection, the temperature is 120~140℃, the time is 3~5h, and the stirring speed used for mixing is 300~500 rpm. During the independent vacuum drying process of the lignin, polyether polyol and cyclic carbonate phenolic hydroxy alkylating agent, the vacuum drying conditions are: vacuum degree ≤ -0.095 MPa, temperature 35~45℃, and time 10~14h. After vacuum drying, the moisture content of the lignin is ≤0.1wt%, the moisture content of the polyether polyol is ≤0.05wt%, and the moisture content of the cyclic carbonate phenolic hydroxy alkylating agent is ≤0.05wt%.

[0015] Optionally, in some embodiments of this application, the lignin comprises organic solvent lignin, and the provision of lignin includes: A mixed solution and an acid catalyst are added to the wood to induce a delignification reaction in the wood; wherein the mixed solution includes an organic solvent. After the reaction is complete, the product is filtered, precipitated, washed, and dried to obtain lignin, an organic solvent. The mixed solution comprises the organic solvent and water, wherein the organic solvent in the mixed solution has a mass percentage of 40 wt% to 60 wt%, and the organic solvent comprises one or more of acetone and ethanol; The acid catalyst includes sulfuric acid; The mass ratio of the wood to the volume ratio of the organic solvent is 1:(5.0~10.0); the mass ratio of the wood to the volume ratio of the acid catalyst is 1:(2.0~5.0). The conditions for the delignification reaction are: temperature 120~160℃, time 1~3h.

[0016] Optionally, in some embodiments of this application, the step of mixing the methyl 1,6-hexamethylenedicarbamate, the mixture, the foam stabilizer, and the foaming agent, then injecting the mixture into a mold, and subjecting it to curing and hot pressing to obtain polyurethane foam includes: The mixture and the methyl 1,6-hexamethylenedicarbamate were mixed and stirred at 1000 rpm to 2000 rpm for 3 min to 7 min to obtain the first mixed liquid. After adding foaming agent and foaming agent to the first mixture at a pressure of 0.3~0.5 MPa, stir at a speed of 1500rpm~2500rpm for 1~3min to obtain the second mixture. The second mixture is injected into the mold for initial and subsequent curing. After the post-curing process is completed, hot pressing is applied to the mold and the air is vented to obtain the polyurethane foam.

[0017] Optionally, in some embodiments of this application, based on a total mass of 100 parts by weight of the lignin and the polyether polyol, the mass of methyl 1,6-hexamethylenedicarbamate is 29-44 parts by weight, the mass of the foaming agent is 10-12 parts by weight, and the mass of the foam leveling agent is 1.0-2.0 parts by weight. The mass ratio of lignin to polyether polyol is (3~5):(5~7), and the molar ratio of the urethane ester of methyl 1,6-hexamethylene dicarboxylate to the hydroxyl groups in the lignin-based polyol is (0.85~1.1):1. The moisture content of the mixture is ≤0.05wt%, the moisture content of the methyl 1,6-hexamethylenedicarbamate is ≤0.05wt%, the moisture content of the foaming agent is ≤0.05wt%, and the moisture content of the foam stabilizer is ≤0.05wt%. The temperature of the mold is 130~150℃; The initial curing temperature is 130~150℃, and the initial curing time is 2~4h; The post-curing temperature is 150~170℃, and the post-curing time is 1~3h; During the process of applying hot pressure and venting the mold, the pressure of the hot pressure is 14-16 MPa, the temperature of the hot pressure is 150-170℃, the time of the hot pressure is 25-35 min, and the number of times the venting is performed is 3-7 times.

[0018] Accordingly, this application also provides a refrigeration device, which includes an insulation layer, wherein the insulation layer is made of the polyurethane foam described above, or polyurethane foam obtained by the preparation method of the polyurethane foam described above.

[0019] Accordingly, this application also provides a method for recycling polyurethane foam, comprising the following steps: Methanol is added to the polyurethane foam to be recycled to carry out a carbamate exchange reaction to obtain a depolymerization product; the depolymerization product contains methyl 1,6-hexamethylenedicarbamate and lignin-based polyol; wherein the polyurethane foam to be recycled includes the polyurethane foam described above, or the polyurethane foam obtained by the polyurethane foam preparation method described above. The depolymerization product was subjected to vacuum distillation to obtain a mixed product including the methyl 1,6-hexamethylenedicarbamate and the lignin-based polyol. After adding a third organic base catalyst, a foam leveler, and a foaming agent to the mixture, it is injected into a mold for curing and hot pressing to obtain polyurethane foam.

[0020] Optionally, in some embodiments of this application, the third organic base catalyst includes one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene; The average particle size of the polyurethane foam to be recycled is 100 mesh to 300 mesh. The solid-liquid ratio of the polyurethane foam to be recycled to the methanol is 1g:(10mL~20mL). The amount of the third organic base catalyst added is 2.2 wt% to 4 wt% of the mass of the mixed product. The conditions for the carbamate exchange reaction are: under closed conditions, the temperature is 130~150℃ and the time is 24h~36h; The conditions for vacuum distillation are as follows: pressure of 0.01–0.09 MPa, temperature of 60–180 °C, and time of 0.5–5 h.

[0021] The lignin-based polyol provided in this application is a multi-hydroxy crosslinking agent obtained by modifying lignin with polyether polyol and cyclic carbonate phenolic hydroxy alkylating agent. This multi-hydroxy crosslinking agent undergoes a urethane exchange reaction with methyl 1,6-hexamethylene dicarboxylate to construct a lignin-reinforced polymer crosslinking network. This not only improves the crosslinking density and rigidity of the polymer crosslinking network, but also enhances the mechanical properties and thermal stability of the prepared polyurethane foam. As a result, the polyurethane foam can still maintain excellent thermal insulation and mechanical properties even with high bio-based content. Attached Figure Description

[0022] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0023] Figure 1 This is a flowchart of the polyurethane foam preparation method provided in the embodiments of this application. Detailed Implementation

[0024] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application. Furthermore, it should be understood that the specific embodiments described herein are only for illustration and explanation of this application and are not intended to limit this application.

[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0026] In this application, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of the device in its actual use or operating state, specifically the drawing directions in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". The terms first, second, third, etc., are used merely as illustrative purposes and do not impose numerical requirements or establish a numerical order.

[0027] In this application, "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural.

[0028] In this application, "at least one" means one or more, and "more than one" means two or more. "One or more", "at least one of the following", or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0029] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.

[0030] Rigid polyurethane foam for refrigerators and freezers is the core insulation material for home appliance insulation systems, accounting for 20% to 30% of the production cost of refrigerators, with a global annual demand of over 8 million tons. Currently, almost 100% of the industry uses isocyanate-based polyurethane (PU) foam as insulation material, but the following problems exist: (1) Isocyanate is a highly toxic and allergenic substance, and its production depends on highly toxic phosgene. There are major safety hazards in the production process, and long-term exposure to workers can easily cause respiratory diseases and skin allergies; (2) Traditional isocyanate-based polyurethane is an irreversible thermosetting material that cannot be melted and reprocessed. Therefore, about 95% of waste polyurethane worldwide is ultimately disposed of through landfill or incineration. However, incineration releases highly toxic gases such as hydrogen cyanide; (3) Currently, lignin-based polyurethane all use the isocyanate route, and lignin modification generally depends on flammable, explosive, and highly toxic propylene oxide, which requires high-pressure reaction equipment. At the same time, lignin requires complex purification steps and is costly.

[0031] Based on this, non-isocyanate polyurethane (NIPU) foams that are not synthesized using isocyanate raw materials are usually prepared using cyclic carbonates and amine curing agents. This route not only eliminates isocyanates, but also allows cyclic carbonate raw materials to be prepared using CO2 and epoxides, achieving carbon capture and curing.

[0032] However, non-isocyanate polyurethane (NIPU) foam has the following problems: (1) Polyhydroxy polyurethane is generated by reacting cyclic carbonate with amine, but the structure of the reaction product is very different from that of traditional polyurethane, and it has poor compatibility with existing refrigerator production lines. Moreover, the cost of cyclic carbonate is 2 to 3 times that of isocyanate, making it difficult to apply on a large scale; (2) At present, the bio-based content of rigid polyurethane foam is generally less than 30%, and it cannot simultaneously meet the thermal insulation, mechanical and dimensional stability requirements of GB / T 26689-2024 "Rigid polyurethane foam for refrigerators and freezers", and it does not have recycling performance.

[0033] The technical solution of this application is as follows: In a first aspect, embodiments of this application provide a polyurethane foam composition comprising methyl 1,6-hexamethylenedicarbamate and a mixture, wherein the mixture comprises a lignin-based polyol, the lignin-based polyol being mainly obtained by modifying lignin with a polyether polyol and a cyclic carbonate phenolic hydroxyl alkylating agent.

[0034] In some embodiments, the lignin includes one or more of lignin sulfonate, organic solvent lignin, hydrolyzed lignin, and alkali lignin; the lignin sulfonate includes one or more of sodium lignin sulfonate and calcium lignin sulfonate; the organic solvent lignin includes one or more of birch organic solvent lignin, wheat straw alkali lignin, and pine sulfate lignin; the hydrolyzed lignin includes one or more of acid-hydrolyzed lignin and enzymatically hydrolyzed residue lignin; and the alkali lignin includes one or more of wheat straw soda ash lignin and sugarcane bagasse soda ash lignin.

[0035] It should be noted that organic solvent lignin refers to a type of lignin extracted from raw materials such as wood chips and timber using organic solvents (such as acetone and ethanol). Because birch organic solvent lignin has a high S / G ratio (the ratio of syringyl units to guaiacyl units), a low molecular weight, and a high phenolic hydroxyl content, it is beneficial for preparing lignin-based polyols with high hydroxyl values ​​and good processing fluidity. Therefore, preferably, the lignin includes birch organic solvent lignin.

[0036] It should also be noted that lignin modification refers to lignin undergoing a liquefaction-hydroxyalkylation reaction. Specifically, lignin undergoes a hydroxyalkylation reaction with a cyclic carbonate phenolic hydroxyl alkylating agent to convert the phenolic hydroxyl groups on the lignin into aliphatic hydroxyl groups, thereby improving the reactivity of lignin as a polyol. At the same time, a lignin liquefaction reaction is carried out using a polyether polyol.

[0037] Polyether polyols serve a dual function as both reaction solvents and providers of soft-segment structural units for lignin-based polyols. Therefore, the polyether polyols must be selected from those with low functionality, low molecular weight, and flexible polyether segments. In some embodiments, the functionality of the polyether polyol is 2-3, and the number-average molecular weight is 200-600 g / mol. It should be noted that as the molecular weight of the polyether polyol increases, the system viscosity rises sharply, which can affect bubble nucleation and growth during the foaming process, leading to a decrease in the cell uniformity of the polyurethane foam.

[0038] Optionally, the polyether polyol includes one or more of polyethylene glycol, polypropylene glycol, polytetrahydrofuran ether glycol, and bio-based 1,3-propanediol polyether polyol. Specifically, the number-average molecular weight of the polyethylene glycol is 300 g / mol, the number-average molecular weight of the polypropylene glycol is 200-600 g / mol, the number-average molecular weight of the polytetrahydrofuran ether glycol is 250-600 g / mol, and the number-average molecular weight of the bio-based 1,3-propanediol polyether polyol is 300-500 g / mol.

[0039] For example, when the polyether polyol includes polyethylene glycol with a number average molecular weight of 400 g / mol, the resulting NIPU rigid foam has improved toughness and its initial thermal conductivity is increased.

[0040] The cyclic carbonate phenolic hydroxyl alkylating agent may include one or more of ethylene carbonate (EC), propylene carbonate (PC), glycerol carbonate (GC), and vinyl ethylene carbonate (VEC). Considering that propylene carbonate (PC) has insufficient reactivity due to steric hindrance of the methyl group, glycerol carbonate (GC) is prone to intermolecular side reactions due to competition for reaction sites by its own hydroxyl groups, and vinyl ethylene carbonate (VEC) is prone to self-polymerization under alkaline conditions (such as TBD catalyst) due to high vinyl steric hindrance. Therefore, in some embodiments, the cyclic carbonate phenolic hydroxyl alkylating agent includes ethylene carbonate (CAS: 96-49-1).

[0041] In this embodiment, by using ethylene carbonate as the phenolic hydroxyl alkylating agent for lignin, 100% of the phenolic hydroxyl groups in lignin can be converted into highly reactive fatty alcohol hydroxyl groups, solving the problem of low reactivity of lignin before modification. It should be noted that the mixture in this embodiment refers to the reaction mixture after lignin modification, which is a reaction mixture without any purification treatment.

[0042] In some embodiments, the mixture further comprises a first organic base catalyst, the first organic base catalyst comprising one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene (MTBD).

[0043] In this embodiment, lignin is reacted with cyclic carbonate phenolic hydroxyalkylating agents and polyether polyols in a liquefaction-hydroxyalkylation reaction under the action of a first organic base catalyst to obtain a mixture, which includes lignin-based polyols and a first organic base catalyst.

[0044] Compared to the propylene oxide modification process for lignin, the lignin modification process provided in this embodiment not only avoids the use of flammable, explosive, and highly toxic raw materials and the need for high-pressure reaction equipment, but also, on the one hand, due to the selection of reaction raw materials, such as the use of cyclic carbonate phenolic hydroxyl alkylating agents (ethylene carbonate), 100% of the phenolic hydroxyl groups in lignin can be converted into highly active fatty alcohol hydroxyl groups. Using polyether polyols as the reaction medium, no additional reaction solvent is added, thus eliminating the need for solvent or byproduct recovery through other processes, and the resulting mixture does not require purification. On the other hand, the subsequent polymerization of lignin-based polyols with methyl 1,6-hexamethylenedicarbamate can be catalyzed using a first organic base catalyst, eliminating the need to separate and purify the first organic base catalyst and lignin-based polyols in the mixture. Therefore, the lignin modification process provided in this embodiment does not require complex purification steps, thereby reducing costs.

[0045] It should be noted that the lignin-based polyol provided in this embodiment is a liquid polyhydroxy crosslinking agent obtained by lignin modification. This polyhydroxy crosslinking agent not only improves the crosslinking density and rigidity of the polymer crosslinking network, but also enhances the mechanical properties and thermal stability of rigid polyurethane foam through the π-π stacking effect of its aromatic rings. This allows rigid polyurethane foam to maintain excellent thermal insulation and mechanical properties even with high bio-based content. Simultaneously, the aromatic structure of lignin can effectively reduce the radiative thermal conductivity of rigid polyurethane foam, which is one of the core factors for achieving low thermal conductivity and excellent mechanical properties in rigid polyurethane foam. It should also be noted that the polymer crosslinking network refers to the polymer crosslinking network formed by the polymerization of lignin-based polyol and methyl 1,6-hexamethylenedicarbamate.

[0046] In some embodiments, the hydroxyl value of the lignin-based polyol is 5.1 to 6.3 mmol / g, for example, it can be 5.1 mmol / g, 5.7 mmol / g, 6.3 mmol / g, or any value or range between two values.

[0047] The number-average molecular weight of the lignin-based polyol is 800~2500 g / mol, for example, it can be 800 g / mol, 900 g / mol, 1000 g / mol, 1100 g / mol, 1200 g / mol, 1500 g / mol, 2000 g / mol, 2500 g / mol, or any value or range between two such values. Within this range, the crosslinking point spacing of the lignin-based polyol is moderate, which can simultaneously ensure the compressive strength and toughness of the final polyurethane rigid foam.

[0048] In some embodiments, the viscosity of the lignin-based polyol at 25°C is 25~2100 Pa·s, and the viscosity of the lignin-based polyol at 160°C is 0.08~0.25 Pa·s.

[0049] In this embodiment, on the one hand, lignin is dispersed by using a reaction solvent (polyether polyol), and on the other hand, 100% of the phenolic hydroxyl groups in lignin are converted into highly active fatty alcohol hydroxyl groups by using ethylene carbonate, which breaks the hydrogen bond aggregation between lignin molecules and eliminates large unmodified lignin particles, thereby giving the obtained lignin-based polyol excellent high-temperature processing fluidity.

[0050] For example, when the polyether polyol includes polyethylene glycol with a number average molecular weight of 300 g / mol, the viscosity of the lignin-based polyol at 25°C is 29~1900 Pa·s, and the viscosity of the lignin-based polyol at 160°C is 0.08~0.23 Pa·s; when the polyether polyol includes polyethylene glycol with a number average molecular weight of 400 g / mol, the viscosity of the lignin-based polyol at 25°C is 35~2100 Pa·s, and the viscosity of the lignin-based polyol at 160°C is 0.09~0.25 Pa·s; when the polyether polyol includes polypropylene glycol with a number average molecular weight of 300 g / mol, the viscosity of the lignin-based polyol at 25°C is 25~1700 Pa·s, and the viscosity of the lignin-based polyol at 160°C is 0.08~0.20 Pa·s.

[0051] In some embodiments, the moisture content of the lignin is ≤0.1wt%, the moisture content of the polyether polyol is ≤0.05wt%, and the moisture content of the cyclic carbonate phenolic hydroxyalkylating agent is ≤0.05wt%.

[0052] In this embodiment, by controlling the moisture content of the three raw materials for lignin modification, not only can the deactivation of the first organic base catalyst due to hydrolysis be avoided, but also the urea side reaction caused by moisture can be prevented during the subsequent polymerization of lignin-based polyol and methyl 1,6-hexamethylenedicarbamate.

[0053] In some embodiments, the mass ratio of lignin to polyether polyol is (3~5):(5~7), for example, it can be 3:7, 4:6, 5:5 or any value or range between two ratios.

[0054] In this embodiment, when the total mass of the lignin and the polyether polyol is 100 parts by mass, the mass of lignin is 30 parts and the mass of polyether polyol is 70 parts, the hydroxyl value of the lignin-based polyol is 6.3 mmol / g; when the mass of lignin is 40 parts and the mass of polyether polyol is 60 parts, the hydroxyl value of the lignin-based polyol is 5.7 mmol / g; and when the mass of lignin is 50 parts and the mass of polyether polyol is 50 parts, the hydroxyl value of the lignin-based polyol is 5.1 mmol / g.

[0055] It should also be noted that, due to the tendency of propylene oxide to self-polymerize, the hydroxyl value of lignin-based polyols obtained by propylene oxide modification is not linearly related to the lignin content, and the batch-to-batch hydroxyl value fluctuates greatly. Therefore, compared to lignin-based polyols obtained by propylene oxide modification, the hydroxyl value of the lignin-based polyol provided in this embodiment is entirely determined by the mass ratio of lignin to polyether polyol. As the lignin quality increases, the hydroxyl value of the lignin-based polyol shows a linear decreasing trend, which conforms to the variation law of polyol hydroxyl value.

[0056] In some embodiments, based on 100 parts by mass of the total mass of the lignin and the polyether polyol, the cyclic carbonate phenolic hydroxy alkylating agent comprises 11.6 to 19.4 parts by mass, and the first organic base catalyst comprises 2.5 to 4.2 parts by mass.

[0057] It should be noted that the mass fraction of the cyclic carbonate phenolic hydroxyl alkylating agent is 11.6 to 19.4 parts, indicating that the mass fraction of the cyclic carbonate phenolic hydroxyl alkylating agent is 1.0 to 1.2 equivalents (relative to the total hydroxyl content of lignin); the mass fraction of the first organic base catalyst is 2.5 to 4.2 parts, indicating that the mass fraction of the first organic base catalyst is 0.1 to 0.2 equivalents (relative to the total hydroxyl content of lignin).

[0058] In some embodiments, the methyl 1,6-hexamethylenedicarbamate is mainly obtained by reacting hexamethylenediamine and dimethyl carbonate; wherein the molar ratio of the hexamethylenediamine and the dimethyl carbonate is 1:(8.0~12.0), for example, it can be 1:8.0, 1:9.0, 1:10.0, 1:11.0, 1:12.0 or any value or range between two ratios.

[0059] The structural formula of methyl 1,6-hexamethylene dicarboxylate (HMDC) is CH3OCO-NH-(CH2)6-NH-COOCH3; dimethyl carbonate is a green carbonate raw material, belonging to linear carbonates (chain carbonates).

[0060] In this embodiment, hexamethylenediamine and dimethyl carbonate undergo a carbamate reaction to obtain methyl 1,6-hexamethylenedicarbamate (HMDC). Since HMDC is a polycarbamate monomer, it can provide isocyanate groups (-NCO).

[0061] In some embodiments, in the polyurethane foam composition, the molar ratio of the urethane ester of methyl 1,6-hexamethylenedicarbamate to the hydroxyl groups in the lignin-based polyol is (0.85~1.1):1, for example, it can be 0.85:1, 0.9:1, 1.0:1, 1.1:1, or any value or range between two ratios. Within this range, the polyurethane foam can possess self-healing, recyclability, and good mechanical properties.

[0062] Preferably, the molar ratio of the urethane ester of the methyl 1,6-hexamethylene dicarbamate to the hydroxyl group in the lignin-based polyol is 0.95:1.

[0063] It is understandable that by using a solvent-free bulk polymerization process, namely the one-step curing and molding of methyl 1,6-hexamethylene dicarboxylate and lignin-based polyol through carbamate exchange reaction, a lignin-reinforced covalent adaptive network can be constructed. The resulting rigid polyurethane foam not only has dual chemical and mechanical recyclability, achieving green throughout its entire life cycle, but also takes into account high bio-based content and good thermal insulation, mechanical properties, and dimensional stability.

[0064] Specifically, the alkoxy group in the urethane bond (-NH-COO-) of methyl 1,6-hexamethylene dicarboxylate exchanges with the 100% converted hydroxyl group in the lignin-based polyol to form a new urethane bond, thereby forming a polymer crosslinking network. This polymer crosslinking network contains dynamic covalent bonds (urethane bonds), which can be further called a covalent adaptive network. This covalent adaptive network exhibits high strength and stability of thermosetting materials at room temperature, and can be recycled through the exchange of urethane bonds under heating and / or catalytic conditions.

[0065] Specifically, the final product is a non-isocyanate polyurethane rigid foam with an actual bio-based content of 19.7 wt%~35.6 wt%. Furthermore, due to the construction of a lignin-reinforced covalent adaptive network, this non-isocyanate polyurethane rigid foam is a cross-linked non-isocyanate polyurethane rigid foam, and its core performance fully complies with the refrigerator rigid foam standard of GB / T 26689-2024. Specifically, the initial thermal conductivity of this cross-linked non-isocyanate polyurethane rigid foam is 0.0185 W / (m·K)~0.0195 W / (m·K), the deformation compressive stress of this cross-linked non-isocyanate polyurethane rigid foam is ≥130 kPa, and the low-temperature dimensional stability of this cross-linked non-isocyanate polyurethane rigid foam is ≤1.0%.

[0066] It should also be noted that the actual bio-based content refers to the percentage of bio-based raw materials in the total raw material mass, calculated based on industrial raw material sources.

[0067] In some embodiments, the polyurethane foam composition further includes a foaming agent and a foam leveling agent.

[0068] In this embodiment, the foaming agent can be selected from physical foaming agents that meet environmental protection requirements. In some embodiments, the foaming agent includes physical foaming agents, which include one or more of alkane physical foaming agents and fluoroolefin foaming agents. The alkane physical foaming agents include one or more of cyclopentane, isopentane, n-pentane, and cyclohexane. The fluoroolefin foaming agents include 1,3,3,3-tetrafluoropropylene foaming agent, 1-chloro-3,3,3-trifluoropropylene foaming agent, and 2,3,3,3-tetrafluoropropylene foaming agent.

[0069] In this embodiment, the foam leveler can be selected from silicone foam levelers to adjust the cell structure. Therefore, in some embodiments, the foam leveler includes silicone foam levelers, which include one or more of the following: Mistide AK-8805, Mistide AK-8803, and Momentive L-580 silicone oil.

[0070] In some embodiments, based on a total mass of 100 parts by weight of the lignin and the polyether polyol, the mass of methyl 1,6-hexamethylenedicarbamate is 29-44 parts by weight, the mass of the foaming agent is 10-12 parts by weight, and the mass of the foam leveling agent is 1.0-2.0 parts by weight.

[0071] It should also be noted that the mass fraction of lignin used in the preparation of lignin-based polyols varies, and correspondingly, the mass fraction of methyl 1,6-hexamethylenedicarbamate varies as well. In one example, when the mass fraction of lignin is 30 parts and the mass fraction of the polyether polyol is 70 parts, the corresponding mass fraction of methyl 1,6-hexamethylenedicarbamate can be selected as 39 parts.

[0072] In another example, when the mass fraction of lignin is 40 parts and the mass fraction of polyether polyol is 60 parts, the mass fraction of methyl 1,6-hexamethylenedicarbamate is 37-44 parts. In another example, when the mass fraction of lignin is 50 parts and the mass fraction of polyether polyol is 50 parts, the mass fraction of methyl 1,6-hexamethylenedicarbamate is 29 parts.

[0073] Preferably, based on a total mass of 100 parts by mass of the lignin and the polyether polyol (of which 30 parts by mass of lignin and 70 parts by mass of polyether polyol), the methyl 1,6-hexamethylenedicarbamate is 39 parts by mass, cyclopentane is 11 parts by mass, and Mistex AK-8805 is 1.5 parts by mass.

[0074] Secondly, embodiments of this application provide a polyurethane foam, which is obtained by foaming the polyurethane foam composition described above.

[0075] Since this polyurethane foam adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought about by the technical solutions of the above embodiments, which will not be repeated here.

[0076] In some embodiments, The closed-cell rate of the polyurethane foam is ≥90%; The apparent core density of the polyurethane foam is ≤36 kg / m³. 3 ; The deformation compressive stress of the polyurethane foam is ≥130kPa; The low-temperature dimensional stability of the polyurethane foam is ≤1.0%; The dimensional stability of the polyurethane foam under humid heat is ≤1.5%; The initial thermal conductivity of the polyurethane foam is 0.0185 W / (m·K) to 0.0195 W / (m·K); The water absorption rate of the polyurethane foam is ≤4%.

[0077] Thirdly, embodiments of this application provide a method for preparing polyurethane foam; please refer to [link to relevant documentation]. Figure 1 This includes the following steps S10 to S30: Step S10, providing methyl 1,6-hexamethylenedicarbamate and a mixture; the mixture contains a lignin-based polyol, which is mainly obtained by modifying lignin with polyether polyol and phenolic alkylating agent; Step S20: After mixing the methyl 1,6-hexamethylenedicarbamate, the mixture, the foam stabilizer and the foaming agent, the mixture is injected into a mold, cured and hot-pressed to obtain polyurethane foam.

[0078] In some embodiments, providing the methyl 1,6-hexamethylenedicarbamate includes the following steps S11 to S13: Step S11: Mix hexamethylenediamine, dimethyl carbonate, and a second organic base catalyst to cause the hexamethylenediamine and dimethyl carbonate to undergo a carbamate reaction, thereby obtaining a reaction solution; Step S12: The reaction solution is allowed to stand and filtered to obtain a reaction product and a reaction filtrate; the reaction filtrate includes a second organic base catalyst, and the reaction product includes methyl 1,6-hexamethylenedicarbamate. Step S13: The reaction product is dried under vacuum to obtain methyl 1,6-hexamethylenedicarbamate. In step S14, the reaction filtrate is mixed with the hexamethylenediamine and the dimethyl carbonate to obtain methyl 1,6-hexamethylenedicarbamate.

[0079] The proportions of the hexamethylenediamine, the dimethyl carbonate, and the second organic base catalyst are as described above and will not be repeated here.

[0080] The second organic base catalyst includes one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene (MTBD).

[0081] The molar ratio of hexamethylenediamine to dimethyl carbonate is 1:(8.0~12.0), for example, it can be 1:8.0, 1:9.0, 1:10.0, 1:11.0, 1:12.0, or any value or range between two ratios. The molar ratio of hexamethylenediamine to the second organic base catalyst is 1:(0.05~0.15), for example, it can be 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, 1:0.10, 1:0.11, 1:0.12, 1:0.013, 1:0.14, 1:0.15, or any value or range between two ratios. Preferably, the molar ratio of hexamethylenediamine to dimethyl carbonate is 1:10.0, and the molar ratio of hexamethylenediamine to the second organic base catalyst is 1:0.10.

[0082] The mixing conditions are as follows: under inert gas protection, the temperature is 80~100℃, the time is 10h~14h, and the stirring speed is 200~400 rpm. Preferably, the mixing conditions are as follows: under argon gas with a purity of ≥99.99%, the temperature is 90℃, the time is 12h, and the stirring speed is 300 rpm.

[0083] The reaction solution is allowed to stand under the following conditions: at a temperature of 0-4°C in an ice bath for 1-3 hours. Preferably, the reaction solution is allowed to stand under the following conditions: at a temperature of 0°C in an ice bath for 2 hours.

[0084] The vacuum drying conditions for the reaction product are: vacuum degree ≤ -0.095 MPa, temperature 35~45℃, and time 10~14h. Preferably, the vacuum drying conditions for the reaction product are: vacuum degree -0.098 MPa, temperature 40℃, and time 12h.

[0085] In step S13, the yield of methyl 1,6-hexamethylenedicarbamate is 85%~90%, and the purity of methyl 1,6-hexamethylenedicarbamate is ≥98%.

[0086] In step S14, the yield of methyl 1,6-hexamethylenedicarbamate is 83%~87%, and the purity of methyl 1,6-hexamethylenedicarbamate is ≥97%. It should be noted that since the reaction filtrate includes dimethyl carbonate (excess dimethyl carbonate), an inactivated second organic base catalyst, and trace amounts of methanol as a byproduct, no purification treatment is required. New hexamethylenediamine can be added directly to initiate the next batch of reaction. This process can be repeated 5 times or less, maintaining a final yield of methyl 1,6-hexamethylenedicarbamate of 83~87% and a purity ≥97%. Furthermore, after a single cycle, the process environmental factor decreases from 5.0 to 3.3, and after more than 5 consecutive cycles, the environmental factor can be further reduced to below 2.0, achieving the green production level for bulk chemicals.

[0087] It should also be noted that the environmental factor is a core authoritative indicator of green chemistry. The environmental factor = total mass of all waste generated during the production process (mass of excess dimethyl carbonate + mass of by-product methanol + mass of undeactivated second organic base catalyst + mass of other waste) / mass of target product (mass of methyl 1,6-hexamethylenedicarbamate). The smaller the value of the environmental factor, the higher the resource utilization rate and the more environmentally friendly the process.

[0088] It is understood that in this embodiment, the solvent-free one-pot synthesis of methyl 1,6-hexamethylenedicarbamate using hexamethylenediamine and dimethyl carbonate is not only simple but also environmentally friendly. Specifically, on the one hand, compared to inorganic base catalysts, the catalyst used in this embodiment is a second organic base catalyst, which eliminates the need for water washing and desalting. Furthermore, the second organic base catalyst can be recycled with the reaction filtrate. Moreover, since the reaction filtrate is free of impurities, it does not require purification; new hexamethylenediamine and new dimethyl carbonate can be added directly for the reaction without the need for the second organic base catalyst, thus achieving the recycling of the reaction filtrate and significantly reducing environmental factors. On the other hand, since excess dimethyl carbonate serves as the reaction medium in the reaction system, and no additional solvent is required, the reaction solution including the target product only needs to be allowed to stand and vacuum dried to obtain methyl 1,6-hexamethylenedicarbamate. This eliminates the need for recrystallization purification of the target product and also eliminates the need to recover solvents or byproducts through distillation.

[0089] In some embodiments, the mixture is provided, comprising: Provides lignin; The lignin, polyether polyol, and cyclic carbonate phenolic hydroxyl alkylating agent are each independently vacuum dried; The first organic base catalyst, vacuum-dried lignin, the polyether polyol, and the cyclic carbonate phenolic hydroxyl alkylating agent are mixed to modify the lignin, thereby obtaining the mixture.

[0090] The types and proportions of the lignin, the polyether polyol, the cyclic carbonate phenolic hydroxyl alkylating agent, and the first organic base catalyst are as described above and will not be repeated here.

[0091] During the independent vacuum drying process of the lignin, polyether polyol and cyclic carbonate phenolic hydroxy alkylating agent, the vacuum drying conditions are: vacuum degree ≤ -0.095 MPa, temperature 35~45℃, and time 10~14h.

[0092] In this embodiment, after vacuum drying, the moisture content of the lignin is ≤0.1wt%, the moisture content of the polyether polyol is ≤0.05wt%, and the moisture content of the cyclic carbonate phenolic hydroxyalkylating agent is ≤0.05wt%.

[0093] The mixing conditions are as follows: under inert gas protection, the temperature is 120~140℃, the time is 3~5h, and the stirring speed is 300~500 rpm. Preferably, the mixing conditions are as follows: under inert gas protection, the temperature is 130℃, the time is 4h, and the stirring speed is 400 rpm.

[0094] In this embodiment, the inert gas can be argon or nitrogen. Inert gas protection not only prevents lignin oxidation, degradation, and discoloration at high temperatures but also isolates it from moisture in the air. It should also be noted that if the modification temperature exceeds 140°C, it will trigger the self-polymerization of cyclic carbonate phenolic hydroxyl alkylating agents (ethylene carbonate) and the thermal degradation of lignin, resulting in the final lignin-based polyol turning black, increasing the amount of reaction byproducts in the mixture, and decreasing the hydroxyl value of the lignin-based polyol in the mixture.

[0095] In some embodiments, the lignin comprises organic solvent lignin, and the provision of lignin includes: A mixed solution and an acid catalyst are added to the wood to induce a delignification reaction in the wood; wherein the mixed solution includes an organic solvent. After the reaction is complete, the product is filtered, precipitated, washed, and dried to obtain organic solvent lignin.

[0096] For example, the wood can be birch wood chips that have been debarked, pith removed, and cut into segments, the length of which is 2 to 5 cm.

[0097] The mixed solution comprises the organic solvent and water, wherein the organic solvent in the mixed solution has a mass percentage of 40 wt% to 60 wt%, and the organic solvent includes one or more of acetone and ethanol.

[0098] The acid catalyst includes sulfuric acid.

[0099] The mass ratio of the wood to the volume ratio of the organic solvent is 1:(5.0~10.0), for example, it can be 1:5.0, 1:6.0, 1:7.0, 1:8.0, 1:9.0, 1:10.0, or any value or range between two ratios. The mass ratio of the wood to the volume ratio of the acid catalyst is 1:(2.0~5.0).

[0100] In some embodiments, the conditions for the delignification reaction are: a temperature of 120~160℃ and a time of 1~3h.

[0101] In some embodiments, step S20 includes steps S21 to S24: Step S21: Mix the mixture with the methyl 1,6-hexamethylenedicarbamate and stir at 1000 rpm to 2000 rpm for 3 min to 7 min to obtain the first mixed liquid. Step S22: After adding foaming agent and foaming agent to the first mixture at a pressure of 0.3~0.5 MPa, stir at a speed of 1500 rpm~2500 rpm for 1~3 minutes to obtain the second mixture. Step S23: Inject the second mixture into the mold for initial curing and post-curing. Step S24: After the post-curing is completed, hot pressing is applied to the mold and the air is vented to obtain the polyurethane foam.

[0102] In steps S21 and S22, based on a total mass of 100 parts by mass of lignin and polyether polyol, the mass of methyl 1,6-hexamethylenedicarbamate is 29-44 parts, the mass of the foaming agent is 10-12 parts, and the mass of the foam leveling agent is 1.0-2.0 parts. The mass ratio of lignin to polyether polyol is (3-5):(5-7), and the molar ratio of the carbamate ester of methyl 1,6-hexamethylenedicarbamate to the hydroxyl groups in the lignin-based polyol is (0.85-1.1):1. The types of foaming agent and foam leveling agent are as described above and will not be repeated here.

[0103] In this embodiment, the dynamic regulation of the polymer crosslinking network is achieved by controlling the molar ratio of the urethane ester of the methyl 1,6-hexamethylenedicarbamate to the hydroxyl groups in the lignin-based polyol.

[0104] Specifically, when the molar ratio of the urethane ester of methyl 1,6-hexamethylene dicarboxylate to the hydroxyl groups in the lignin-based polyol is <1.0, the system retains an appropriate amount of free hydroxyl groups provided by the lignin-based polyol. Under the action of the first organic base catalyst, these hydroxyl groups can undergo a dynamic exchange reaction with the urethane bonds, forming a polymer crosslinking network with self-healing and recyclable properties (i.e., the original urethane bonds of methyl 1,6-hexamethylene dicarboxylate are reversibly broken, and the free hydroxyl groups retained in the reaction system will attack the active sites of the urethane ester to form new urethane bonds). (To allow for dynamic exchange); when the molar ratio of methyl 1,6-hexamethylene dicarboxylate to the hydroxyl groups in the lignin-based polyol is 0.95, it is the optimal molar ratio, at which point the dynamics (self-healing and recyclability) and mechanical properties of the polymer crosslinking network are optimally balanced; when the molar ratio of methyl 1,6-hexamethylene dicarboxylate to the hydroxyl groups in the lignin-based polyol is >1.1, the excess carboxylate will trigger side reactions such as biuret and urea carbamate, leading to a significant decrease in the thermal insulation and mechanical properties of the polyurethane foam.

[0105] Wherein, the moisture content of the mixture is ≤0.05wt%, the moisture content of the methyl 1,6-hexamethylenedicarbamate is ≤0.05wt%, the moisture content of the foaming agent is ≤0.05wt%, and the moisture content of the foam leveler is ≤0.05wt%.

[0106] In this embodiment, by controlling the moisture content of all raw materials to ≤0.05%, the generation of urea side reactions can be avoided, thereby preventing the increase in brittleness and decrease in thermal insulation performance of polyurethane foam caused by urea side reactions.

[0107] It is understandable that by controlling the molar ratio of the urethane ester of methyl 1,6-hexamethylene dicarboxylate to the hydroxyl groups in the lignin-based polyol, and by controlling the moisture content of all raw materials, the side reactions of urethane ester can be controlled to below 1%.

[0108] In step S23, the mold needs to be preheated to a temperature of 130-150℃; the initial curing temperature is 130-150℃, and the initial curing time is 2-4 hours; the post-curing temperature is 150-170℃, and the post-curing time is 1-3 hours. It should also be noted that during the initial or post-curing process, the temperature uniformity between the mold and the mold cavity should be ≤5℃ to ensure a consistent curing rate throughout the mold cavity, avoiding localized over-curing or under-curing, reducing internal stress, and thus improving cell uniformity and dimensional stability.

[0109] In step S24, during the process of applying hot pressure to the mold and venting, the pressure of applying hot pressure is 14-16 MPa, the temperature of applying hot pressure is 150-170°C, the time of applying hot pressure is 25-35 min, and the number of times venting is 3-7.

[0110] In this embodiment, by using a precise cell control process (controlling the foaming agent injection pressure, the stirring speed after foaming agent injection, the setting of the curing gradient temperature, and hot pressing and venting), not only can the average cell diameter of rigid polyurethane foam be controlled at 50~80μm, the cell uniformity be ≥90%, and the closed-cell rate be increased to 93% or above, but the initial thermal conductivity of rigid polyurethane foam is 0.0185W / (m·K)~0.0195W / (m·K), the deformation compressive stress is ≥130kPa, the low-temperature dimensional stability is ≤1.0%, and the humid heat dimensional stability is ≤1.5%, which fully meets the requirements of GB / T 26689-2024 standard. This is another core factor in achieving low thermal conductivity and excellent mechanical properties in rigid polyurethane foam.

[0111] Specifically, injecting the foaming agent under a pressure of 0.3~0.5 MPa ensures that the foaming agent is uniformly dispersed into micron-sized droplets in the second mixture, providing a basis for subsequent homogeneous nucleation. This is the core factor for achieving high closed-cell ratio in rigid polyurethane foam.

[0112] Specifically, the setting of the curing gradient temperature allows for initial curing (i.e., the first stage of curing) to bring the urethane exchange reaction between methyl 1,6-hexamethylenedicarbamate and lignin-based polyol to the gel point, initiating cross-linking of the reaction system. During this process, the cell growth and shaping are completed, preventing cell collapse and merging. Subsequent curing (i.e., the second stage of curing) ensures complete cross-linking, achieving a urethane bond conversion rate of ≥98%. This process eliminates internal curing stress, stabilizes the polymer cross-linking network, and prevents later shrinkage of rigid polyurethane foam products. It should also be noted that the methanol byproduct released during initial curing can be recovered and reused through a condensation system, with a methanol recovery rate of ≥95%.

[0113] Furthermore, by applying hot pressure to the mold, the cell structure can be compacted, defects on the surface of rigid polyurethane foam can be eliminated, and residual reactions can be fully promoted to further improve the closed-cell rate and dimensional stability of rigid polyurethane foam. Furthermore, the rigid polyurethane foam after hot pressing in the mold is subjected to repeated depressurization and venting 3 to 7 times to remove residual air bubbles and large pores in the system, avoid internal large pore defects, and improve the cell uniformity of rigid polyurethane foam.

[0114] Fourthly, embodiments of this application provide a refrigeration device, the refrigeration device including a heat insulation layer, the heat insulation layer being made of the polyurethane foam described above, or polyurethane foam obtained by the preparation method of the polyurethane foam described above.

[0115] Since this refrigeration equipment adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought about by the technical solutions of the above embodiments, which will not be repeated here. The refrigeration equipment can be various refrigeration and insulation equipment such as household refrigerators, cold chain refrigerators, freezers, and refrigerated trucks.

[0116] Fifthly, embodiments of this application provide a method for recycling polyurethane foam, comprising the following steps: Methanol is added to the polyurethane foam to be recycled to carry out a carbamate exchange reaction to obtain a depolymerization product; the depolymerization product contains methyl 1,6-hexamethylenedicarbamate and lignin-based polyol. The depolymerization product was subjected to vacuum distillation to obtain a mixed product including the methyl 1,6-hexamethylenedicarbamate and the lignin-based polyol. After adding a third organic base catalyst, a foam leveler, and a foaming agent to the mixture, it is injected into a mold for curing and hot pressing to obtain polyurethane foam.

[0117] The polyurethane foam to be recycled can be the polyurethane foam described above, or polyurethane foam obtained by the preparation method described above, whose polymer crosslinking network has self-healing and recyclable properties. In order to carry out the reverse exchange reaction of urethane bonds more effectively, the polyurethane foam to be recycled can be crushed to an average particle size of 100-300 mesh before carrying out the reverse exchange reaction of urethane bonds.

[0118] In some embodiments, the solid-liquid ratio of the polyurethane foam to be recycled to the methanol is 1 g:(10 mL~20 mL), for example, it can be 1:10 (g / mL), 1:15 (g / mL), 1:20 (g / mL) or any value or range between two ratios.

[0119] The conditions for the carbamate exchange reaction are: under closed conditions, at a temperature of 130~150℃, for a time of 24h~36h.

[0120] It should be noted that this carbamate exchange reaction is a reverse carbamate exchange reaction. Specifically, under heating conditions, the hydroxyl groups of excess methanol exchange with the alkoxy groups in the carbamate bonds (formed by the carbamate bonds of methyl 1,6-hexamethylenedicarbamate and the hydroxyl groups in the lignin-based polyol) in the polymer crosslinking network, thereby depolymerizing the three-dimensional polymer crosslinking network into initial monomers, which include methyl 1,6-hexamethylenedicarbamate and lignin-based polyols, thus completing the reverse exchange.

[0121] In some embodiments, the conditions for vacuum distillation are: pressure of 0.01–0.09 MPa, temperature of 60–180°C, and time of 0.5–5 h.

[0122] In some embodiments, the third organic base catalyst comprises one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene (MTBD).

[0123] The amount of the third organic base catalyst added is 2.2 wt% to 4 wt% of the mass of the mixed product, for example, it can be 2.2 wt%, 2.5 wt%, 3.0 wt%, 4.0 wt%, or any value or range between two values.

[0124] The types and proportions of the foaming agent and the foaming agent, as well as the process parameters for curing and hot pressing, are as described in the above embodiments and will not be repeated here.

[0125] It is understood that, due to the dynamic nature (self-healing and recyclable characteristics) of the polymer crosslinking network of the polyurethane foam provided above, the addition of excess methanol under heating conditions can cause a carbamate exchange reaction to obtain a depolymerization product containing methyl 1,6-hexamethylenedicarbamate and lignin-based polyol. After removing excess methanol from the depolymerization product by vacuum distillation, a mixed product of methyl 1,6-hexamethylenedicarbamate and lignin-based polyol can be obtained. This mixed product can then be used to regenerate rigid polyurethane foam, and the retention rate of the core properties of the regenerated rigid polyurethane foam can reach ≥85%.

[0126] Sixthly, embodiments of this application provide another method for recycling polyurethane foam, comprising: hot pressing and cooling the polyurethane foam to be recycled to obtain polyurethane foam.

[0127] The polyurethane foam to be recycled can be the polyurethane foam described above, or polyurethane foam obtained by the polyurethane foam preparation method described above, and the average particle size of the polyurethane foam to be recycled is 100 mesh to 300 mesh.

[0128] In some embodiments, the hot pressing conditions are: pressure of 14MPa~16MPa, temperature of 140~160℃, and time of 2h~6h.

[0129] The cooling can be natural cooling, and the cooling time is 24h~36h.

[0130] Because the polyurethane foam provided above has self-healing and recyclable polymer crosslinking network, it can be recycled through the exchange of urethane bonds under heating and / or catalytic conditions. Therefore, in addition to the chemical recycling method provided in the above embodiments, this embodiment also provides a mechanical recycling method. Under heating and pressure, the urethane bonds in the network undergo a rapid exchange reaction, causing the pulverized particles to re-fuse into a complete board. After cooling, the crosslinking structure is restored, and the performance retention rate is ≥70%. This process is simpler.

[0131] The present application will be specifically described below through specific embodiments. These embodiments are only some embodiments of the present application and are not intended to limit the present application. Unless otherwise specified, the raw materials used in the following embodiments are all commercially available products.

[0132] Example 1 Preparation of methyl 1,6-hexamethylenedicarbamate Hexamethylenediamine, dimethyl carbonate, and 1,5,7-triazabicyclo[4.4.0]dec-5-ene were mixed in a molar ratio of 1:10.0:0.10 and reacted under argon protection with a purity ≥99.99% at 90°C for 12 hours with a stirring speed of 300 rpm. After the reaction was complete, the product was allowed to stand at 0°C in an ice bath for 2 hours. After standing, the filtered product was dried under vacuum at 40°C with a vacuum degree of -0.098 MPa for 12 hours to obtain methyl 1,6-hexamethylenedicarbamate, which was a white crystalline powder with an average yield of 86%, a purity of 98%, and a melting point of 124°C.

[0133] Preparation of mixtures After removing the bark and pith from birch wood chips and cutting them into segments, 50 wt% acetone aqueous solution (the mass ratio of birch wood chips to the volume ratio of acetone aqueous solution was 1:8) and 1 wt% sulfuric acid (the mass ratio of birch wood chips to the volume ratio of sulfuric acid was 1:2) were added to carry out a delignification reaction. The delignification reaction temperature was 140℃, and after 2 hours of reaction, birch organic solvent lignin was obtained. The total hydroxyl groups of this organic solvent lignin were 5.0 mmol / g, the phenolic hydroxyl groups were 2.2 mmol / g, the number average molecular weight was 1500 g / mol, the polydispersity index was 2.2, the ash content was 0.5%, and the sugar residues were 2%.

[0134] Polyethylene glycol (molecular weight 300 g / mol) and ethylene carbonate were pre-dried at 40℃ and -0.098 MPa vacuum for 12 h to remove moisture to a content ≤0.05%; birch organic solvent lignin did not require any purification treatment and could be used directly, with the moisture content controlled to ≤0.1%.

[0135] Under nitrogen atmosphere and at 130°C, 40 parts of birch organic solvent lignin, 60 parts of polyethylene glycol (PEG300), 15.5 parts of ethylene carbonate, and 3.3 parts of 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD) were mixed at 400 rpm to modify lignin. After 4 hours, a mixture containing lignin-based polyol and 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD) was obtained. The hydroxyl value of the lignin-based polyol was determined to be 5.7 mmol / g according to GB / T 12008.3-2009 "Polyether Polyols Part 3: Determination of Hydroxyl Value". The viscosity of the lignin-based polyol was determined to be 210 Pa·s at 25°C and 0.12 Pa·s at 160°C according to GB / T 10247-2008 "Viscosity Measurement Methods". It should also be noted that the viscosity of the product (mixture) is being tested at this time. Since 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD) is a small molecule compound, the test result is the viscosity of the lignin-based polyol.

[0136] Preparation of polyurethane foam 100 parts of a mixture and 37 parts of methyl 1,6-hexamethylenedicarbamate were mixed, wherein the molar ratio of the carbamate ester of methyl 1,6-hexamethylenedicarbamate to the hydroxyl groups in the lignin-based polyol of the mixture was 0.9:1. After stirring at 1500 rpm for 5 minutes, a first mixture was obtained. 11 parts of cyclopentane foaming agent and 1.5 parts of AK-8805 silicone foam leveling agent were injected into the first mixture within 10 seconds at a pressure of 0.4 MPa. After stirring at 2000 rpm for 2 minutes, a second mixture was obtained. The second mixture was injected into a mold at 140°C and pre-cured at 160°C for 2 hours, followed by post-curing at 160°C for 2 hours. The mold was then hot-pressed at 160°C and 15 MPa for 30 minutes to form the polyurethane foam, with venting occurring 5 times during the hot-pressing process. The actual bio-based content of the polyurethane foam was 26.8 wt%.

[0137] Example 2 The only difference between this embodiment and Example 1 is that the mass ratio of lignin used in preparing the mixture is different, and the proportions of methyl 1,6-hexamethylenedicarbamate and foaming agent are adjusted accordingly.

[0138] Specifically, when preparing the mixture, the amount of birch organic solvent lignin is 30 parts, the amount of polyethylene glycol (PEG300) is 70 parts, the amount of ethylene carbonate is 11.6 parts (1.1 equivalents), and the amount of 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD) is 2.5 parts.

[0139] The hydroxyl value of the lignin-based polyol in the mixture was determined to be 6.3 mmol / g, and the viscosity of the lignin-based polyol was 29 Pa·s at 25°C and 0.08 Pa·s at 160°C.

[0140] When preparing polyurethane foam, the mixture consists of 100 parts, 39 parts of methyl 1,6-hexamethylene dicarboxylate (the molar ratio of the carbamate of methyl 1,6-hexamethylene dicarboxylate to the hydroxyl groups in the lignin-based polyol in the mixture is 0.9:1), and 12 parts of cyclopentane blowing agent.

[0141] Example 3 The only difference between this embodiment and Example 1 is that the mass ratio of lignin used in preparing the mixture is different, and the proportions of methyl 1,6-hexamethylenedicarbamate and foaming agent are adjusted accordingly.

[0142] Specifically, when preparing the mixture, the proportions of birch organic solvent lignin are 50 parts, the proportions of polyethylene glycol (PEG300) are 50 parts, the proportions of ethylene carbonate are 19.4 parts, and the proportions of 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD) are 4.2 parts.

[0143] The hydroxyl value of the lignin-based polyol in the mixture was determined to be 5.1 mmol / g, and the viscosity of the lignin-based polyol was 1900 Pa·s at 25°C and 0.23 Pa·s at 160°C.

[0144] When preparing polyurethane foam, the mixture consists of 100 parts, 29 parts of methyl 1,6-hexamethylene dicarboxylate (the molar ratio of the carbamate of methyl 1,6-hexamethylene dicarboxylate to the hydroxyl groups in the lignin-based polyol in the mixture is 0.9:1), and 10 parts of cyclopentane blowing agent.

[0145] Example 4 The only difference between this embodiment and Example 1 is the amount of methyl 1,6-hexamethylenedicarbamate.

[0146] Specifically, in this embodiment, the amount of methyl 1,6-hexamethylene dicarboxylate is 39 parts (the molar ratio of the carbamate of methyl 1,6-hexamethylene dicarboxylate to the hydroxyl group in the lignin-based polyol in the mixture is 0.95:1).

[0147] Example 5 The only difference between this embodiment and Example 1 is the amount of methyl 1,6-hexamethylenedicarbamate.

[0148] Specifically, in this embodiment, the amount of methyl 1,6-hexamethylene dicarboxylate is 41 parts (the molar ratio of the carbamate of methyl 1,6-hexamethylene dicarboxylate to the hydroxyl group in the lignin-based polyol in the mixture is 1.0:1).

[0149] Example 6 The only difference between this embodiment and Example 1 is the amount of methyl 1,6-hexamethylenedicarbamate.

[0150] Specifically, in this embodiment, the amount of methyl 1,6-hexamethylene dicarboxylate is 44 parts (the molar ratio of the carbamate of methyl 1,6-hexamethylene dicarboxylate to the hydroxyl group in the lignin-based polyol in the mixture is 1.1:1).

[0151] Comparative Example 1 100 parts of polyether polyol 4110, 12 parts of cyclopentane foaming agent, and 1.5 parts of AK-8805 organosilicon foaming agent were added to a reaction vessel and stirred at high speed for 60 seconds at 20°C and 2000 rpm until uniformly mixed to obtain the combined polyether.

[0152] The combined polyether obtained above was mixed with 130 parts of polyisocyanate PMDI at a high speed of 5000 rpm for 10 seconds, and then quickly injected into the refrigerator body mold. The mold temperature was controlled at 35°C for free foaming and curing. After curing for 12 hours, the mixture was demolded to obtain rigid polyurethane foam for refrigerators.

[0153] Comparative Example 2 The only difference between this embodiment and Example 5 is that the lignin-based polyol is obtained by using a propylene oxide modification process.

[0154] Specifically, in a closed high-pressure reactor, lignin, potassium hydroxide, and water are mixed at a mass ratio of 1:0.1:10 and reacted at 2.0 MPa pressure and 120°C for 1-2 hours. After filtration, hydrolyzed lignin is obtained. Ethylene glycol, propylene oxide, and potassium hydroxide (mass ratio of hydrolyzed lignin to ethylene glycol, propylene oxide, and potassium hydroxide is 20:10:50:2) are added to the hydrolyzed lignin. After mixing, the mixture is heated to 140°C and stirred continuously at 2000 rpm for 30 minutes. After filtration, crude lignin-based liquid polyol is obtained. The crude lignin-based liquid polyol is cooled to 1°C through a heat exchanger, filtered to obtain solid crystalline material, washed three times with ethylene glycol, and naturally heated to 20°C to obtain lignin-based liquid polyol.

[0155] 100 parts of lignin-based liquid polyol and 41 parts of methyl 1,6-hexamethylene dicarboxylate were mixed, wherein the molar ratio of the carbamate ester of methyl 1,6-hexamethylene dicarboxylate to the hydroxyl groups in the lignin-based liquid polyol was 0.9:1. After stirring at 1500 rpm for 5 minutes, a first mixture was obtained. 11 parts of cyclopentane foaming agent and 1.5 parts of AK-8805 silicone foam leveling agent were injected into the first mixture within 10 seconds at a pressure of 0.4 MPa. After stirring at 2000 rpm for 2 minutes, a second mixture was obtained. The second mixture was injected into a mold at 140°C and pre-cured at 160°C for 2 hours, followed by post-curing at 160°C for 2 hours. After post-curing, the mold was hot-pressed at 160°C and 15 MPa for 30 minutes to form the polyurethane foam. The venting was performed 5 times during the hot-pressing process.

[0156] Comparative Example 3 The only difference between this embodiment and Example 1 is that there is no mixture (the mixture contains lignin-based polyol and 1,5,7-triazabicyclo[4.4.0]dec-5-ene).

[0157] Specifically, 48 parts of methyl 1,6-hexamethylene dicarboxylate, 100 parts of polyethylene glycol (PEG300), and 5 parts of 1,5,7-triazabicyclo[4.4.0]dec-5-ene were mixed, wherein the molar ratio of the carbamate in methyl 1,6-hexamethylene dicarboxylate to the hydroxyl groups in polyethylene glycol was 0.9:1. The mixture was stirred at 1500 rpm for 5 minutes to obtain a first mixture. Then, 12 parts of cyclopentane foaming agent and 1.5 parts of AK-8805 silicone foaming agent were injected into the first mixture within 10 seconds at a pressure of 0.4 MPa. Finally, the mixture was stirred at 2000... After stirring at rpm for 2 minutes, a second mixture is obtained. The second mixture is injected into a mold at 140°C and pre-cured at 160°C for 2 hours, followed by post-curing at 160°C for 2 hours. After post-curing, the mold is hot-pressed at 160°C and 15MPa for 30 minutes to form the polyurethane foam. The venting is performed 5 times during the hot-pressing process.

[0158] Comparative Example 4 The only difference between this embodiment and Embodiment 1 is that the precise control process of cell size was not used when preparing the polyurethane foam.

[0159] Specifically, 100 parts of a mixture, 37 parts of methyl 1,6-hexamethylenedicarbamate, 11 parts of cyclopentane blowing agent, and 1.5 parts of AK-8805 silicone foaming agent were mixed together. The molar ratio of the carbamate ester of methyl 1,6-hexamethylenedicarbamate to the hydroxyl groups in the lignin-based polyol in the mixture was 0.9:1. The mixture was stirred at 1500 rpm for 5 minutes and then quickly injected into a refrigerator cabinet mold. The mold temperature was controlled at 140℃, and the mixture was cured for 12 hours before demolding to obtain polyurethane foam.

[0160] Comparative Example 5 The only difference between this embodiment and Example 1 is the reaction temperature during the preparation of the mixture.

[0161] Specifically, after removing the bark and pith from birch wood chips and cutting them into segments, 50 wt% acetone aqueous solution (the mass ratio of birch wood chips to the volume ratio of acetone aqueous solution is 1:8) and 1 wt% sulfuric acid (the mass ratio of birch wood chips to the volume ratio of sulfuric acid is 1:2) were added to carry out a delignification reaction. The delignification reaction temperature was 140℃, and after reacting for 2 hours, birch organic solvent lignin was obtained. The total hydroxyl groups of this organic solvent lignin were 5.0 mmol / g, the phenolic hydroxyl groups were 2.2 mmol / g, the number average molecular weight was 1500 g / mol, the polydispersity index was 2.2, the ash content was 0.5%, and the sugar residues were 2%.

[0162] Polyethylene glycol (molecular weight 300 g / mol) and ethylene carbonate were pre-dried at 40℃ and -0.098 MPa vacuum for 12 h to remove moisture to a content ≤0.05%; birch organic solvent lignin did not require any purification treatment and could be used directly, with the moisture content controlled to ≤0.1%.

[0163] Under nitrogen atmosphere and at 250°C, 40 parts of birch organic solvent lignin, 60 parts of polyethylene glycol (PEG300), 15.5 parts of ethylene carbonate, and 3.3 parts of 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD) were mixed at 400 rpm to modify lignin. After 4 hours, a mixture containing lignin-based polyol and 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD) was obtained. The hydroxyl value of the lignin-based polyol in the mixture was determined to be 4.1 mmol / g.

[0164] Performance tests were conducted on Examples 1-6 and Comparative Examples 1-5. The performance test results for each example and comparative example are shown in Tables 1 and 2. The performance test items included: initial thermal conductivity, 10% deformation compressive stress, low temperature / humid heat dimensional stability, apparent core density, closed-cell rate, water absorption rate, and high and low temperature cycling performance.

[0165] Initial thermal conductivity (λ0): According to GB / T 26689-2024, the thermal conductivity of polyurethane foam within 72 h of production (average temperature 10℃) is tested, and the unit is W / (m·K). 10% Deformation Compressive Stress: Tested according to GB / T 26689-2024, the compressive stress (minimum values ​​in the length, width, and height directions) of the specimen when it undergoes 10% deformation, in kPa, is used to reflect the structural stability of polyurethane foam. Dimensional stability: Tested according to GB / T 8811-2008, including low-temperature dimensional change rate (test conditions: temperature -30±2℃, time 24h) and damp-heat dimensional change rate (test conditions: temperature 70±2℃, relative humidity 95±5%, time 24h), in %. The unit is %, with Class I rigid foam requiring a low-temperature dimensional change rate ≤1.0% and a damp-heat dimensional change rate ≤1.5%. Apparent core density (ρ): Tested according to GB / T 6343-2009, unit is kg / m³ 3 Class I rigid polyurethane foam requires a strength of ≤36 kg / m³. 3 ; Closed-cell ratio (θ): Tested according to GB / T 10799-2008 "Determination of open-cell and closed-cell volume percentage of rigid foamed plastics", unit is %, Class I rigid polyurethane foam requires a closed-cell ratio ≥90%; Water absorption rate: Determined according to GB / T 8810-2005 by measuring the buoyancy of polyurethane foam after immersion in water for 50 mm and 96 hours, with the unit being % . High and low temperature cycling performance: Tested according to GB / T 26689-2024 6.9. The test cycle is: temperature (-30±2)℃, time 24h, equilibration 2h, temperature (55±2)℃, time 24h, equilibration 2h, air as heat transfer medium, the test is carried out for 3 cycles, and visual inspection is performed after taking it out.

[0166] Table 1. Performance test results of polyurethane foam in Examples 1-6

[0167] Table 2. Performance test results of polyurethane foams from Comparative Examples 1 to 5

[0168] As can be seen from Tables 1 and 2, As can be seen from Examples 2, 1 and 3, with the increase of lignin content, the compressive strength, dimensional stability and closed-cell rate of polyurethane foam increase linearly, while the initial thermal conductivity continues to decrease. This indicates that lignin plays a core role as a multifunctional crosslinking agent and aromatic reinforcing phase, and increasing the lignin content can simultaneously achieve performance improvement and increase the bio-based content.

[0169] As can be seen from Examples 1, 4, 5, and 6, as the molar ratio of urethane in methyl 1,6-hexamethylenedicarbamate to hydroxyl groups in cross-linked lignin-based polyol increases from 0.9 to 1.1, the performance of polyurethane foam first improves and then decreases, reaching global optimum (optimal example) at a molar ratio of 0.95. This indicates that a slight excess of hydroxyl groups (e.g., 5 wt% excess hydroxyl groups at a molar ratio of 0.95) can promote the urethane exchange reaction, forming a more uniform covalent adaptive network (CAN), while retaining the material's recyclability. The performance critical point is a molar ratio of 1.1; exceeding this value will trigger side reactions leading to a decrease in performance.

[0170] As can be seen from Comparative Examples 1-3, Comparative Example 1 uses the industry-standard "polyether polyol 4110 + polymeric MDI" formula, which is the benchmark formula currently used on a large scale in refrigerator factories. It is used to demonstrate that the performance of the NIPU rigid foam provided in this application has reached and partially exceeded that of traditional isocyanate-based rigid foam, demonstrating its feasibility for industrial substitution. Comparative Example 2 uses the traditional high-pressure hydroxyalkylation process of propylene oxide to prepare lignin-based polyols. Experimental results show that the propylene oxide-modified lignin-based polyols have uneven reactivity, resulting in large pores, low closed-cell rate, and poor dimensional stability in the rigid foam, with many indicators failing to meet standards. This indicates that the ethylene carbonate process without propylene oxide modification provided in this application has significant advantages. Comparative Example 3 did not add any lignin and only used PEG300 as the polyol component. The experimental results showed that the crosslinking density of the polyurethane foam was insufficient without lignin, the compressive strength was only 95 kPa, and the dimensional stability and closed-cell rate were seriously substandard. This shows the necessity of lignin as a crosslinking agent and reinforcing phase. When the polyurethane rigid foam formulation of methyl 1,6-hexamethylene dicarboxylate does not include the lignin-based polyol (i.e., liquid polyhydroxy crosslinking agent) provided in this application, it is impossible to prepare rigid foam with satisfactory performance.

[0171] As can be seen from the examples and Comparative Example 4, the examples achieved a stable thermal conductivity of lignin-based NIPU rigid foam between 0.0185 and 0.0195 W / (m·K) through precise control of the foam cells, thereby preparing rigid foam with satisfactory core thermal insulation performance.

[0172] As can be seen from the examples and Comparative Example 5, when the temperature exceeds 140°C during the preparation of lignin-based polyols (i.e., liquid polyhydroxy crosslinking agents), it will cause the self-polymerization of ethylene carbonate (EC) and the thermal degradation of lignin raw materials. The resulting lignin-based polyol will turn black. More importantly, the amount of by-products will increase, and the hydroxyl value of the lignin-based polyol will decrease (the hydroxyl value of the lignin-based polyol in Example 2 is 6.3 mmol / g, the hydroxyl value of the lignin-based polyol in Example 1 is 5.7 mmol / g, the hydroxyl value of the lignin-based polyol in Example 3 is 5.1 mmol / g, and the hydroxyl value of the lignin-based polyol in Comparative Example 5 is 4.1 mmol / g). Ultimately, the closed-cell rate, deformation compressive stress, dimensional stability and other properties of the polyurethane rigid foam in Comparative Example 5 will not meet the standards.

[0173] The technical solutions provided by the embodiments of this application have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A polyurethane foam composition, characterized in that, The polyurethane foam composition comprises methyl 1,6-hexamethylenedicarbamate and a mixture thereof; the mixture comprises a lignin-based polyol, which is mainly obtained by modifying lignin with polyether polyol and cyclic carbonate phenolic hydroxyl alkylating agent.

2. The polyurethane foam composition according to claim 1, characterized in that, The lignin includes one or more of lignin sulfonate, organic solvent lignin, hydrolyzed lignin, and alkali lignin; the lignin sulfonate includes one or more of sodium lignin sulfonate and calcium lignin sulfonate; the organic solvent lignin includes one or more of birch organic solvent lignin, wheat straw alkali lignin, and pine sulfate lignin; the hydrolyzed lignin includes one or more of acid hydrolyzed lignin and enzymatic hydrolysis residue lignin; and the alkali lignin includes one or more of wheat straw soda ash lignin and sugarcane bagasse soda ash lignin. The functionality of the polyether polyol is 2 to 3, and the number-average molecular weight of the polyether polyol is 200 to 600 g / mol. Optionally, the polyether polyol includes one or more of polyethylene glycol, polypropylene glycol, polytetrahydrofuran ether glycol, and bio-based 1,3-propanediol polyether polyol; The cyclic carbonate phenolic hydroxy alkylating agent includes ethylene carbonate; The moisture content of the lignin is ≤0.1wt%, the moisture content of the polyether polyol is ≤0.05wt%, and the moisture content of the cyclic carbonate phenolic hydroxyalkylating agent is ≤0.05wt%. The mass ratio of the lignin to the polyether polyol is (3~5):(5~7). Based on a total mass of 100 parts by weight of the lignin and the polyether polyol, the mass of the cyclic carbonate phenolic hydroxy alkylating agent is 11.6 to 19.4 parts by weight.

3. The polyurethane foam composition according to claim 1, characterized in that, The methyl 1,6-hexamethylenedicarbamate is mainly obtained by reacting hexamethylenediamine and dimethyl carbonate; wherein the molar ratio of hexamethylenediamine to dimethyl carbonate is 1:(8.0~12.0). In the polyurethane foam composition, the molar ratio of the urethane ester of the methyl 1,6-hexamethylenedicarbamate to the hydroxyl group in the lignin-based polyol is (0.85~1.1):

1.

4. The polyurethane foam composition according to claim 1, characterized in that, The mixture also contains a first organic base catalyst; The first organic base catalyst comprises one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene; Based on a total mass of 100 parts by mass of the lignin and the polyether polyol, the first organic base catalyst comprises 2.5 to 4.2 parts by mass. The polyurethane foam composition further includes a foaming agent and a foam leveling agent; The foaming agent includes physical foaming agents, which include one or more of alkane-based physical foaming agents and fluoroolefin-based foaming agents. The alkane-based physical foaming agents include one or more of cyclopentane, isopentane, n-pentane, and cyclohexane. The fluoroolefin-based foaming agents include 1,3,3,3-tetrafluoropropylene foaming agent, 1-chloro-3,3,3-trifluoropropylene foaming agent, and 2,3,3,3-tetrafluoropropylene foaming agent. The foam stabilizer includes an organosilicone foam stabilizer, which includes one or more of the following: Mistide AK-8805, Mistide AK-8803, and Momentive L-580 silicone oil. Based on a total mass of 100 parts by weight of the lignin and the polyether polyol, the mass of methyl 1,6-hexamethylenedicarbamate is 29-44 parts by weight, the mass of the foaming agent is 10-12 parts by weight, and the mass of the foam leveling agent is 1.0-2.0 parts by weight.

5. A polyurethane foam, characterized in that, The polyurethane foam is obtained by foaming the polyurethane foam composition according to any one of claims 1 to 4.

6. The polyurethane foam as described in claim 5, characterized in that, The closed-cell rate of the polyurethane foam is ≥90%; The apparent core density of the polyurethane foam is ≤36 kg / m³. 3 ; The deformation compressive stress of the polyurethane foam is ≥130kPa; The low-temperature dimensional stability of the polyurethane foam is ≤1.0%; The dimensional stability of the polyurethane foam under humid heat is ≤1.5%; The initial thermal conductivity of the polyurethane foam is 0.0185 W / (m·K) to 0.0195 W / (m·K); The water absorption rate of the polyurethane foam is ≤4%.

7. A method for preparing polyurethane foam, characterized in that, Includes the following steps: The invention provides methyl 1,6-hexamethylenedicarbamate and a mixture thereof; the mixture comprises a lignin-based polyol, which is mainly obtained by modifying lignin with polyether polyol and phenolic alkylating agent; The methyl 1,6-hexamethylenedicarbamate, the mixture, the foaming agent, and the blowing agent are mixed and then injected into a mold for curing and hot pressing to obtain polyurethane foam.

8. The method for preparing polyurethane foam as described in claim 7, characterized in that, The methyl 1,6-hexamethylenedicarbamate is provided, comprising: Hexamethylenediamine, dimethyl carbonate, and a second organic base catalyst are mixed to induce a carbamate reaction between the hexamethylenediamine and the dimethyl carbonate, yielding a reaction solution. The reaction solution was allowed to stand and filtered to obtain a reaction product and a reaction filtrate; the reaction filtrate included a second organic base catalyst, and the reaction product included methyl 1,6-hexamethylenedicarbamate. The reaction product was dried under vacuum to obtain methyl 1,6-hexamethylenedicarbamate. The reaction filtrate is mixed with the hexamethylenediamine and the dimethyl carbonate to obtain methyl 1,6-hexamethylenedicarbamate.

9. The method for preparing polyurethane foam as described in claim 8, characterized in that, The second organic base catalyst comprises one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene; The molar ratio of hexamethylenediamine to dimethyl carbonate is 1:(8.0~12.0). The molar ratio of hexamethylenediamine to the second organic base catalyst is 1:(0.05~0.15). The mixing conditions are as follows: under inert gas protection, the temperature is 80~100℃, the time is 10h~14h, and the stirring speed used for mixing is 200~400 rpm. The reaction solution was allowed to stand for 1 to 3 hours in an ice bath at a temperature of 0 to 4°C. The conditions for vacuum drying of the reaction product are: vacuum degree ≤ -0.095 MPa, temperature 35~45℃, and time 10~14h.

10. The method for preparing polyurethane foam according to claim 7, characterized in that, The mixture is provided, comprising: Provides lignin; The lignin, polyether polyol, and cyclic carbonate phenolic hydroxyl alkylating agent are each independently vacuum dried; The first organic base catalyst, vacuum-dried lignin, the polyether polyol, and the cyclic carbonate phenolic hydroxyl alkylating agent are mixed to modify the lignin with the polyether polyol and the cyclic carbonate phenolic hydroxyl alkylating agent, thereby obtaining the mixture. The first organic base catalyst includes one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene; The mixing conditions are as follows: under inert gas protection, the temperature is 120~140℃, the time is 3~5h, and the stirring speed used for mixing is 300~500 rpm. During the independent vacuum drying process of the lignin, polyether polyol and cyclic carbonate phenolic hydroxy alkylating agent, the vacuum drying conditions are: vacuum degree ≤ -0.095 MPa, temperature 35~45℃, and time 10~14h. After vacuum drying, the moisture content of the lignin is ≤0.1wt%, the moisture content of the polyether polyol is ≤0.05wt%, and the moisture content of the cyclic carbonate phenolic hydroxy alkylating agent is ≤0.05wt%.

11. The method for preparing polyurethane foam according to claim 10, characterized in that, The lignin includes organic solvent lignin, and the provision of lignin includes: A mixed solution and an acid catalyst are added to the wood to induce a delignification reaction in the wood; wherein the mixed solution includes an organic solvent. After the reaction is complete, the product is filtered, precipitated, washed, and dried to obtain lignin, an organic solvent. The mixed solution comprises the organic solvent and water, wherein the organic solvent in the mixed solution has a mass percentage of 40 wt% to 60 wt%, and the organic solvent comprises one or more of acetone and ethanol; The acid catalyst includes sulfuric acid; The mass ratio of the wood to the volume ratio of the organic solvent is 1:(5.0~10.0); the mass ratio of the wood to the volume ratio of the acid catalyst is 1:(2.0~5.0). The conditions for the delignification reaction are: temperature 120~160℃, time 1~3h.

12. The method for preparing polyurethane foam as described in claim 7, characterized in that, The process involves mixing the methyl 1,6-hexamethylenedicarbamate, the mixture, the foaming agent, and the blowing agent, then injecting the mixture into a mold for curing and hot pressing to obtain polyurethane foam, comprising: The mixture and the methyl 1,6-hexamethylenedicarbamate were mixed and stirred at 1000 rpm to 2000 rpm for 3 to 7 minutes to obtain the first mixed liquid. After adding foaming agent and foam leveling agent to the first mixture at a pressure of 0.3~0.5 MPa, stir at a speed of 1500 rpm~2500 rpm for 1~3 minutes to obtain the second mixture. The second mixture is injected into the mold for initial and subsequent curing. After the post-curing process is completed, hot pressing is applied to the mold and the air is vented to obtain the polyurethane foam.

13. The method for preparing polyurethane foam according to claim 12, characterized in that, Based on a total mass of 100 parts by weight of the lignin and the polyether polyol, the mass of methyl 1,6-hexamethylene dicarboxylate is 29-44 parts, the mass of the foaming agent is 10-12 parts, and the mass of the foam leveling agent is 1.0-2.0 parts. The mass ratio of lignin to polyether polyol is (3~5):(5~7), and the molar ratio of the urethane ester of methyl 1,6-hexamethylene dicarboxylate to the hydroxyl groups in the lignin-based polyol is (0.85~1.1):

1. The moisture content of the mixture is ≤0.05wt%, the moisture content of the methyl 1,6-hexamethylenedicarbamate is ≤0.05wt%, the moisture content of the foaming agent is ≤0.05wt%, and the moisture content of the foam stabilizer is ≤0.05wt%. The temperature of the mold is 130~150℃; The initial curing temperature is 130~150℃, and the initial curing time is 2~4h; The post-curing temperature is 150~170℃, and the post-curing time is 1~3h; During the process of applying hot pressure and venting the mold, the pressure of applying hot pressure is 14-16 MPa, the temperature of applying hot pressure is 150-170℃, the time of applying hot pressure is 25-35 min, and the number of times venting is 3-7.

14. A refrigeration device, characterized in that, The refrigeration equipment includes an insulation layer, which is made of polyurethane foam as described in claim 5 or 6, or polyurethane foam prepared by any one of the methods described in claims 7 to 13.

15. A method for recycling polyurethane foam, characterized in that, Includes the following steps: Methanol is added to the polyurethane foam to be recycled to carry out a carbamate exchange reaction and obtain depolymerization products. The depolymerization product comprises methyl 1,6-hexamethylenedicarbamate and lignin-based polyol; wherein the polyurethane foam to be recycled comprises the polyurethane foam described in claim 5 or 6 above, or the polyurethane foam obtained by the method for preparing polyurethane foam described in any one of claims 7 to 13 above. The depolymerization product was subjected to vacuum distillation to obtain a mixed product including the methyl 1,6-hexamethylenedicarbamate and the lignin-based polyol. After adding a third organic base catalyst, a foam leveler, and a foaming agent to the mixture, it is injected into a mold for curing and hot pressing to obtain polyurethane foam.

16. The method for recycling polyurethane foam as described in claim 15, characterized in that, The third organic base catalyst includes one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene; The average particle size of the polyurethane foam to be recycled is 100 mesh to 300 mesh. The solid-liquid ratio of the polyurethane foam to be recycled to the methanol is 1g:(10mL~20mL). The amount of the third organic base catalyst added is 2.2 wt% to 4 wt% of the mass of the mixed product. The conditions for the carbamate exchange reaction are: under closed conditions, the temperature is 130~150℃ and the time is 24h~36h; The conditions for vacuum distillation are as follows: pressure of 0.01–0.09 MPa, temperature of 60–180 °C, and time of 0.5–5 h.