Solvent-free polysiloxane compositions and methods for preparing polysiloxane compounds

By employing specific structural design and end-capping treatment of solvent-free polysiloxane compositions, the problems of insufficient stability and hardness in existing low-refractive-index film-forming compositions have been solved, enabling the application of solvent-free polysiloxane compositions with high pencil hardness and low refractive index.

CN123107086APending Publication Date: 2026-11-17SAKATA INX
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610606816.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-05-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing low-refractive-index film-forming compositions cannot simultaneously achieve both long-term stability and high pencil hardness, and contain solvents, failing to meet the environmental requirements for solvent-free formulations.

Method used

A solvent-free polysiloxane composition containing polysiloxane compounds with specific structural units is used. The stability of the silanol groups is ensured by end-capping treatment, and the molar ratio and weight-average molecular weight are controlled. Combined with a suitable preparation method, a cured film with high pencil hardness and low refractive index is formed.

Benefits of technology

This study achieves the time-stability of solvent-free polysiloxane compositions and the low refractive index and high pencil hardness of cured films, meeting environmental protection and performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107086A_ABST
    Figure CN123107086A_ABST
Patent Text Reader

Abstract

This invention provides a solvent-free polysiloxane composition exhibiting excellent long-term stability, low refractive index of the cured film, and excellent pencil hardness. A solvent-free polysiloxane composition comprising a polysiloxane compound and satisfying conditions 1 and 2 below, wherein the polysiloxane compound has at least a structural unit derived from formula (1) and at least one terminal silanol group is capped with a trimethylsilyl group. In formula (1), A 1 A represents a monovalent organic group with a double bond that exhibits free radical polymerization. 2 R indicates alkyl or siloxy groups. 1 Indicates alkyl group, multiple R 1 They can be the same or different, and a is 0 or 1; Condition 1: The refractive index of the cured covering film is 1.48 or less; Condition 2: In the above polysiloxane compound, when the molar ratio of the structural units derived from the above formula (1) relative to all structural units is set to M1, M1 is 40 to 100.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] [Cross-reference to related applications]

[0002] This application claims priority to Japanese Patent Application No. 2025-082017, filed with the Japan Patent Office on May 15, 2025, and all contents disclosed therein are incorporated herein by reference. Technical Field

[0003] This invention relates to solvent-free polysiloxane compositions and methods for preparing polysiloxane compounds. Background Technology

[0004] Various lens materials, planarization films, and other coating materials are used in solid-state imaging devices such as charge-coupled devices (CCD), complementary metal-oxide-semiconductor (CMOS) image sensors, substrates for displays, and various anti-reflection films.

[0005] In addition to optical properties such as transparency and appropriate refractive index, such coating materials also require many other properties, including heat resistance and low-temperature processability. Furthermore, depending on the application, alkali solubility is also a requirement. For these requirements, resin compositions containing polysiloxane compounds are known to be suitable.

[0006] For example, Patent Document 1 discloses a composition for forming a low refractive index film, characterized by containing a mixture of raw materials comprising two or more specific silane compounds, which is formed by hydrolyzing the mixture. Silicone resin obtained by condensation.

[0007] Existing technical documents

[0008] Patent documents

[0009] Patent Document 1: Japanese Patent Application Publication No. 2012-203059 Summary of the Invention

[0010] The problem the invention aims to solve

[0011] However, the low refractive index film-forming composition described in Patent Document 1 cannot simultaneously achieve both long-term stability and high pencil hardness.

[0012] In addition, the low refractive index film forming composition described in Patent Document 1 contains a solvent.

[0013] In recent years, there has been a demand for solvent-free low-refractive-index film-forming compositions due to environmental concerns, and there is room for further improvement.

[0014] Therefore, the object of the present invention is to provide a solvent-free polysiloxane composition that has excellent stability over time, low refractive index of the cured film (cured coating), and excellent pencil hardness.

[0015] means for solving problems

[0016] The present invention is a solvent-free polysiloxane composition comprising a polysiloxane compound and satisfying conditions 1 and 2 below, wherein the polysiloxane compound has at least a structural unit derived from the following formula (1) and at least one terminal silanol group is capped with a trimethylsilyl group.

[0017]

[0018] In equation (1), A 1 A represents a monovalent organic group with a double bond that exhibits free radical polymerization. 2 R indicates alkyl or siloxy groups. 1 Indicates alkyl group, multiple R 1 They can be the same or different, and 'a' can be 0 or 1. [Condition 1] The refractive index of the cured film is below 1.48; [Condition 2] In the above polysiloxane compounds, when the molar ratio of the structural units derived from the above formula (1) relative to all structural units is set to M1, M1 is 40 to 100.

[0019] In the solvent-free polysiloxane composition of the present invention, it is preferable that the molar ratio M1 of the structural units derived from the above formula (1) of the above polysiloxane compound is 60 or more.

[0020] In addition, the above-mentioned polysiloxane composition preferably contains at least one structural unit derived from the group consisting of the following formulas (2) and (3), and satisfies the following condition 3.

[0021]

[0022] In equation (2), B 1 B indicates alkyl group. 2 R represents the silicon-oxygen group. 2 Indicates alkyl group, multiple R 2 They can be the same or different, and b is 0 or 1;

[0023] In equation (3), C 1 Indicates alkyl, C 2 R represents the silicon-oxygen group. 3 Indicates alkyl; two carbon atoms 1They can be the same or different, multiple Rs 3 They can be the same or different, and c can be 0 or 1; [Condition 3] For the above polysiloxane compounds, when the molar ratio of structural units derived from the above formula (2) relative to all structural units is set to M2 and the molar ratio of structural units derived from the above formula (3) is set to M3, M2 is 0 to 40 and M3 is 0 to 40.

[0024] Furthermore, the weight-average molecular weight of the aforementioned polysiloxane compound is preferably 800 to 10,000.

[0025] In addition, the present invention is also a method for preparing a polysiloxane compound, which sequentially includes the following steps 1, 2 and 3, and satisfies the following condition 4.

[0026] (Process 1)

[0027] The process of reacting a silane compound containing at least one of the following formula (1) to prepare a polysiloxane compound with a terminal silanol group,

[0028] In equation (1), A 1 A represents a monovalent organic group with a double bond that exhibits free radical polymerization. 2 R indicates alkyl or siloxy groups. 1 Indicates alkyl group, multiple R 1 They can be the same or different, and 'a' can be 0 or 1. (Process 2) The process of removing the solvent after adding the diluent; (Process 3) The process involves dissolving the aforementioned polysiloxane compound with terminal silanol groups in an organic solvent and then adding a protective agent with trimethylsilyl groups to obtain a polysiloxane compound with at least one terminal silanol group capped. [Condition 4] In the above polysiloxane compounds, when the molar ratio of structural units derived from the above formula (1) relative to all structural units is set to M1, M1 is 40 to 100.

[0029] Furthermore, step 1 is preferably included in the above step of further reacting at least one silane compound selected from the group consisting of the following formulas (2) to (3) to prepare a polysiloxane compound with a silanol group at the end, and condition 5 is satisfied.

[0030]

[0031] In equation (2), B 1 B indicates alkyl group.2 R represents the silicon-oxygen group. 2 Indicates alkyl group, multiple R 2 They can be the same or different, and b is 0 or 1;

[0032] In equation (3), C 1 Indicates alkyl, C 2 R represents the silicon-oxygen group. 3 Indicates alkyl; two carbon atoms 1 They can be the same or different, multiple Rs 3 They can be the same or different, and c can be 0 or 1; [Condition 5] In the above-mentioned polysiloxane compound, M1 is 60 or more. When the molar ratio of structural units derived from the above formula (2) relative to all structural units is set to M2 and the molar ratio of structural units derived from the above formula (3) is set to M3, M2 is 0 to 40 and M3 is 0 to 40.

[0033] Invention Effects

[0034] Based on the present invention, a solvent-free polysiloxane composition with excellent stability over time, low refractive index of cured film and excellent pencil hardness can be provided. Detailed Implementation

[0035] The solvent-free polysiloxane composition of the present invention comprises a polysiloxane compound and satisfies conditions 1 and 2 below, wherein the polysiloxane compound has at least a structural unit derived from the following formula (1) and at least one terminal silanol group is capped with a trimethylsilyl group.

[0036]

[0037] In equation (1), A 1 A represents a monovalent organic group with a double bond that exhibits free radical polymerization. 2 R indicates alkyl or siloxy groups. 1 Indicates alkyl group, multiple R 1 They can be the same or different, and 'a' can be 0 or 1. [Condition 1] The refractive index of the cured film is below 1.48; [Condition 2] In the above polysiloxane compounds, when the molar ratio of the structural units derived from the above formula (1) relative to all structural units is set to M1, M1 is 40 to 100.

[0038] The above-mentioned polysiloxane composition comprises at least one polysiloxane compound whose terminal silanol group is capped with a trimethylsilyl group, thereby suppressing the condensation reaction between polysiloxane compounds via the silanol group, and exhibiting excellent stability over time even in solvent-free forms.

[0039] Furthermore, by setting the molar ratio of silane compounds with monovalent organic groups containing free radical polymerizable double bonds to 40 or more, a strong cross-linked structure can be formed during curing, resulting in a cured film with low refractive index and excellent pencil hardness.

[0040] (Polysiloxane compounds)

[0041] The solvent-free polysiloxane composition of the present invention comprises a polysiloxane compound.

[0042] First, let’s explain equation (1).

[0043]

[0044] In equation (1), A 1 A represents a monovalent organic group with a double bond that exhibits free radical polymerization. 2 R indicates alkyl or siloxy groups. 1 Indicates alkyl group, multiple R 1 They can be the same or different, and 'a' can be 0 or 1. In the above formula (1), A 1 Preferably, it has a monovalent organic group having a vinyl, allyl, or (meth)acryloyl group.

[0045] In the above general formula (1), A 2 Preferably, it is an alkyl group having 1 to 10 carbon atoms.

[0046] Such alkyl groups are methyl, ethyl, propyl, isopropyl, tert-butyl, n-butyl, or sec-butyl.

[0047] In the above general formula (1), R 1 Preferably, it is an alkyl group having 1 to 10 carbon atoms.

[0048] Such alkyl groups are methyl, ethyl, propyl, isopropyl, tert-butyl, n-butyl, or sec-butyl.

[0049] In the above general formula (1), a is preferably 0.

[0050] Examples of the general formula (1) above include: vinyltrimethoxysilane, vinyltriethoxysilane, methylvinyldimethoxysilane, methylvinyldiethoxysilane and other vinyl silane compounds; 3-(meth)acryloyloxypropylmethyldimethoxysilane, 3-(meth)acryloyloxypropyltrimethoxysilane, 3-(meth)acryloyloxypropylethyldiethoxysilane, 3-(meth)acryloyloxypropyltriethoxysilane and other 3-(meth)acryloyloxypropyltriethoxysilane compounds; allyltrimethoxysilane, allyltriethoxysilane and other allyl silane compounds.

[0051] The aforementioned polysiloxane compound preferably further contains structural units derived from at least one of the groups consisting of (2) and (3) below.

[0052] Next, we will explain (2).

[0053]

[0054] In equation (2), B 1 B indicates alkyl group. 2 R represents the silicon-oxygen group. 2 Indicates alkyl group, multiple R 2 They can be the same or different, and b is 0 or 1; In equation (2) above, B 1 Preferably, it is an alkyl group having 1 to 10 carbon atoms.

[0055] Such alkyl groups are methyl, ethyl, propyl, isopropyl, tert-butyl, n-butyl, or sec-butyl.

[0056] In equation (2) above, B 2 It is a silicon-oxygen group.

[0057] In equation (2) above, R 2 Preferably, it is an alkyl group having 1 to 10 carbon atoms.

[0058] Such alkyl groups are methyl, ethyl, propyl, isopropyl, tert-butyl, n-butyl, or sec-butyl.

[0059] In equation (2) above, b is preferably 0.

[0060] Examples of the above formula (2) include: methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltriisopropoxysilane, methyltri-n-butoxysilane, methyltri-tert-butoxysilane, methyltri-sec-butoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, butyltrimethoxysilane, pentyltrimethoxysilane, hexyltrimethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, etc.

[0061] Next, we will explain (3).

[0062]

[0063] In equation (3), C 1 Indicates alkyl, C 2 R represents the silicon-oxygen group. 3 Indicates alkyl; two carbon atoms 1 They can be the same or different, multiple Rs 3 They can be the same or different, and c can be 0 or 1; In the above formula (3), C 1 Preferably, it is an alkyl group having 1 to 10 carbon atoms.

[0064] Such alkyl groups are methyl, ethyl, propyl, isopropyl, tert-butyl, n-butyl, or sec-butyl.

[0065] In the above formula (3), C 2 It is a siloxy group.

[0066] In equation (3) above, R 3 Preferably, it is an alkyl group having 1 to 10 carbon atoms.

[0067] Such alkyl groups are methyl, ethyl, propyl, isopropyl, tert-butyl, n-butyl, or sec-butyl.

[0068] In the above formula (3), c is preferably 0.

[0069] Examples of the above formula (3) include dimethyldimethoxysilane and dimethyldiethoxysilane.

[0070] In the above polysiloxane compounds, when the molar ratio of the structural units derived from the above formula (1) relative to all structural units is set to M1, M1 is 40 to 100.

[0071] From the viewpoint of imparting a suitable pencil hardness to the cured film, the above-mentioned M1 is preferably 50 or more, more preferably 60 or more, even more preferably 70 or more, and particularly preferably 80 or more.

[0072] In addition, when the above polysiloxane compound contains a structural unit derived from at least one of the groups consisting of formulas (2) and (3) above, the above M1 is less than 100.

[0073] For the above-mentioned polysiloxane compound, from the viewpoint of appropriately reducing the refractive index of the cured film, when the molar ratio of the structural units derived from the above formula (2) relative to all structural units is set to M2, M2 is preferably 0 to 40, more preferably 0 to 20.

[0074] For the above-mentioned polysiloxane compound, when the molar ratio of the structural units derived from the above formula (3) relative to all structural units is set to M3, M3 is preferably 0 to 40, more preferably 0 to 20.

[0075] In addition, when the above polysiloxane compound contains a structural unit derived from at least one of the groups consisting of formulas (2) and (3) above, either M2 or M3 is greater than 0.

[0076] Furthermore, the molar ratio of the structural units derived from formulas (1) to (3) above can be calculated from the molar ratio of each silane compound used in the synthesis of the above polysiloxane compound. Alternatively, it can be obtained by utilizing... 29 Si-NMR and 1 The above-mentioned siloxane compounds were obtained by measuring H-NMR.

[0077] In the above polysiloxane compounds, at least one terminal silanol group is capped with a trimethylsilyl group.

[0078] From the perspective of providing suitable stability over time, hexamethyldisilazane is preferred for end-capping.

[0079] The weight-average molecular weight (Mw) of the aforementioned polysiloxane compound is preferably 800 to 10,000. If the weight-average molecular weight (Mw) is less than 800, the film-forming and curable properties of the solvent-free polysiloxane composition may decrease. If the weight-average molecular weight (Mw) exceeds 10,000, there is a tendency for the viscosity to increase.

[0080] The weight-average molecular weight (Mw) of the above-mentioned polysiloxane compound is more preferably 1200-2500, and even more preferably 1500-2200.

[0081] Furthermore, the aforementioned weight-average molecular weight (Mw) can be measured as follows: the aforementioned polysiloxane compound is dissolved to prepare a solution of 0.02 parts by mass, which is then filtered (GL Sciences Inc., GL chromatographic disk, aqueous 25A, pore size 0.2 μm) and measured using an Alliance (Waters Corporation, Japan), which consists of a size exclusion chromatograph and a refractive index detector, under the following conditions.

[0082] Columns: pLgel mixed D (manufactured by Agilent Technologies) × 2 connected in series

[0083] Detector: Alliance (manufactured by Waters Corporation, Japan)

[0084] Eluent: Tetrahydrofuran (THF)

[0085] Flow rate: 1.0 ml / min

[0086] Injection volume: 100 μl

[0087] (Preparation methods for polysiloxane compounds)

[0088] The method for preparing the polysiloxane compound of the present invention comprises the following steps 1, 2 and 3 in sequence, and satisfies the following condition 4.

[0089] (Process 1)

[0090] The process of reacting a silane compound containing at least one of the following formula (1) to prepare a polysiloxane compound with a terminal silanol group,

[0091] In equation (1), A 1 A represents a monovalent organic group with a double bond that exhibits free radical polymerization. 2 R indicates alkyl or siloxy groups. 1 Indicates alkyl group, multiple R 1 They can be the same or different, and 'a' can be 0 or 1. (Process 2) The process of removing the solvent after adding the diluent; (Process 3) The process involves dissolving the aforementioned polysiloxane compound with terminal silanol groups in an organic solvent and then adding a protective agent with trimethylsilyl groups to obtain a polysiloxane compound with at least one terminal silanol group capped. [Condition 4] In the above polysiloxane compounds, when the molar ratio of the structural units derived from the above formula (1) relative to all structural units is set to M1, M1 is 40 to 100.

[0092] By using the preparation method of the polysiloxane compound of the present invention, the amount of protective reagents (such as hexamethyldisilazane, trimethylsilane chloride, trimethylsilyl acetate, N-(trimethylsilyl)diethylamine, N-trimethylsilylacetamide, and N-(trimethylsilyl)dimethylamine) can be reduced, and solvent-free polysiloxane compounds with excellent time stability and excellent pencil hardness of cured films can be prepared economically and stably.

[0093] Step 1 above is a step of reacting a silane compound containing at least the following formula (1) to prepare a polysiloxane compound with a silanol group at the end.

[0094] Furthermore, in step 1 above, it is preferable to further react at least one silane compound selected from the group consisting of the following formulas (2) to (3).

[0095]

[0096] In equation (2), B 1 B indicates alkyl group. 2 R represents the silicon-oxygen group. 2 Indicates alkyl group, multiple R 2 They can be the same or different, and b is 0 or 1;

[0097] In equation (3), C 1 Indicates alkyl, C 2 R represents the silicon-oxygen group. 3 Indicates alkyl; two carbon atoms 1 They can be the same or different, multiple Rs 3 They can be the same or different, and c can be 0 or 1; For formulas (1) to (3) above, formulas (1) to (3) described in the above polysiloxane compounds can be used.

[0098] In the above-mentioned process 1, from the viewpoint of balancing the stability over time and the pencil hardness of the cured film, it is preferable that the M1 of the above-mentioned polysiloxane compound is 60 or more. When the molar ratio of the structural units derived from the above-mentioned formula (2) relative to all structural units is set to M2 and the molar ratio of the structural units derived from the above-mentioned formula (3) is set to M3, it is preferable that M2 is 0 to 40 and M3 is 0 to 40.

[0099] In step 1 above, for example, a method can be used to add a polymerization catalyst to a solution obtained by dissolving the above formulas (1) to (3) in an organic solvent in a suitable container and to carry out the reaction while refluxing.

[0100] The preferred organic solvents are: lower alcohols such as ethanol, n-propanol, and isopropanol; ketones such as acetone and methyl ethyl ketone; and esters such as ethyl acetate and n-propyl acetate.

[0101] More preferably, lower alcohols are preferred, and from the viewpoint of being able to maintain an appropriate reaction temperature and be easily evaporated, ethanol or isopropanol are even more preferred.

[0102] For example, acid catalysts such as acetic acid, hydrochloric acid, and p-toluenesulfonic acid monohydrate, and base catalysts such as ammonia, triethylamine, cyclohexylamine, and tetramethylammonium hydroxide can be used as polymerization catalysts.

[0103] As for the amount of the above-mentioned polymerization catalyst, it is preferable that the number of molecules of the polymerization catalyst is about 0.05 to 0.2 times the total number of molecules in the above formulas (1) to (3).

[0104] The preferred reaction temperature is 60–80°C, and the preferred reaction time is approximately 2–24 hours, so that the reaction can proceed fully.

[0105] Step 2 described above involves adding a diluent after step 1 and then evaporating the solvent. Step 2 stabilizes the terminal silanol groups.

[0106] As the diluent mentioned above, amide compounds are preferred, such as N,N-dimethylacetamide and N,N-dimethylformamide.

[0107] The amount of the diluent added is approximately 15% to 30% by mass relative to the total mass of the polysiloxane compound.

[0108] It is preferable to stir after adding the above-mentioned diluent.

[0109] The preferred stirring temperature at this time is 10–40°C, and the stirring time is preferably 0.5–1 hour.

[0110] In addition, step 2 above may also include a step of adding orthoester for dehydration.

[0111] Examples of the aforementioned orthoesters include triethyl orthoacetate, trimethyl orthoformate, and triethyl orthoformate.

[0112] By using the above-mentioned orthoester, the water produced by the reaction can be removed.

[0113] In addition, from the viewpoint of preventing side reactions, it is preferable to add the above-mentioned orthoesters dropwise at a temperature not exceeding 30°C.

[0114] There are no particular limitations on the method for solvent removal mentioned above; any known method can be used, such as removal under reduced pressure.

[0115] The reaction between the above-mentioned polysiloxane compounds and amide compounds can stabilize polysiloxane compounds with silanol groups at the ends.

[0116] Step 3 above is a process in which, after dissolving the polysiloxane compound with silanol groups at the end in an organic solvent, a protective agent with trimethylsilyl groups is added in addition to at least one selected from acids, acid anhydrides, acyl chlorides and esters, thereby obtaining a capped polysiloxane compound.

[0117] As the organic solvent mentioned above, the organic solvent described in step 1 above can be appropriately selected.

[0118] In step 3 above, it is preferable to add the capping agent after adding at least one selected from acids, acid anhydrides, acyl chlorides and esters.

[0119] Examples of acids, anhydrides, acyl chlorides, and esters mentioned above include acetic anhydride, acetic acid, and succinic acid.

[0120] The amount of at least one of the above-mentioned acids, anhydrides, acyl chlorides and esters added is about 50 to 100% by mass relative to the total mass of the above-mentioned protective reagents.

[0121] Therefore, it is possible to remove the ammonia generated during end-capping using the aforementioned protective reagent, which may also generate ammonia.

[0122] Furthermore, the step of adding at least one of the above-mentioned acids, anhydrides, acyl chlorides, and esters may be omitted as it may not be accompanied by the formation of ammonia, depending on the type of protective reagent.

[0123] Examples of protective agents mentioned above include hexamethyldisilazane, trimethylsilane chloride, trimethylsilyl acetate, N-(trimethylsilyl)diethylamine, N-trimethylsilylacetamide, and N-(trimethylsilyl)dimethylamine.

[0124] From a cost perspective, hexamethyldisilazane is preferred.

[0125] Furthermore, the amount of the protective agent added is preferably 70 to 150% by mass, more preferably 80 to 100% by mass, relative to the total mass of the polysiloxane compound.

[0126] In step 3 above, from the viewpoint of preventing side reactions, the reaction temperature is preferably 10 to 50°C.

[0127] In step 3 above, the reaction time is preferably about 3 to 15 hours to allow the reaction to proceed fully.

[0128] After step 3 above, it is preferable to remove by-products and residues, and to evaporate organic solvents and water.

[0129] As a method for removing the aforementioned byproducts and residues, known methods can be used, such as neutralization or mixing with water to remove the byproducts and residues.

[0130] For the removal of the aforementioned organic solvents and water, known methods can be used, such as removing water with sodium sulfate or removing solvents by vacuum drying.

[0131] By removing the organic solvent and water as described above, solvent-free polysiloxane compounds can be obtained.

[0132] (Solvent-free polysiloxane composition)

[0133] The solvent-free polysiloxane composition of the present invention will be described.

[0134] In this specification, "solvent-free" means that the mass reduction is less than 1% under reduced pressure (below 5 hPa) at 160°C for 2 hours.

[0135] The solvent-free polysiloxane composition of the present invention may contain a leveling agent.

[0136] Examples of leveling agents mentioned above include silicone surfactants and fluorinated surfactants.

[0137] Among them, organosilicon surfactants are more suitable as leveling agents in this invention.

[0138] The content of the leveling agent is preferably 0.05 to 1 part by mass relative to 100 parts by mass of the polysiloxane compound.

[0139] The solvent-free polysiloxane composition of the present invention may contain photopolymerizable compounds.

[0140] As the aforementioned photopolymerizable compound, a photopolymerizable compound having a free radical polymerizable unsaturated double bond is preferred.

[0141] Examples of photopolymerizable compounds having two or more free radical polymerizable unsaturated double bonds include ester compounds formed by di- or more hydroxyl-containing compounds and (meth)acrylic acid, such as 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tricyclodecanediethanol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate. Esters, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, bisphenol A di(meth)acrylate, tri(2-hydroxyethyl)isocyanurate di(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tri(2-hydroxyethyl)isocyanurate tri(meth)acrylate, bis(trimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, bispentaerythritol penta(meth)acrylate, bispentaerythritol hexa(meth)acrylate, etc.

[0142] From the viewpoint of improving crosslinking density and imparting excellent hardness to the cured film, compounds having three or more reactive functional groups are preferred, such as trimethylolpropane tri(meth)acrylate, glycerol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tri(2-hydroxyethyl)isocyanurate tri(meth)acrylate, bis(trimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, bispentaerythritol penta(meth)acrylate, bispentaerythritol hexa(meth)acrylate, and more preferably tri(2-hydroxyethyl)isocyanurate tri(meth)acrylate and bispentaerythritol hexa(meth)acrylate.

[0143] Relative to 100 parts by mass of the above-mentioned polysiloxane compound, it is preferable to contain 10 to 50 parts by mass of the above-mentioned photopolymerizable compound.

[0144] Regarding the content of the aforementioned photopolymerizable compound, if it is less than 10 parts by mass relative to 100 parts by mass of the aforementioned polysiloxane compound, the curability, light transmittance, and adhesion to the ITO electrode of the cured film may sometimes become insufficient; if it is more than 50 parts by mass relative to 100 parts by mass of the aforementioned polysiloxane compound, the solubility of the uncured film in the developer may sometimes become insufficient.

[0145] The solvent-free polysiloxane composition of the present invention may contain a polymerization initiator.

[0146] As the polymerization initiator mentioned above, it is preferable to use a polymerization initiator that can achieve a sufficient photocuring reaction when forming a cured film.

[0147] Examples of polymerization initiators include: benzoyl, benzoin, benzophenone, camphorquinone, 2,2-dimethoxy-1,2-diphenylethane-1-one, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-hydroxycyclohexylphenyl ketone, 2,2-dimethoxy-2-phenylacetophenone, 2-methyl-[4'-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butane-1-one, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl-diphenylphosphine oxide, etc.). Carbonyl compounds such as acyl)-phenylphosphine oxide; trihalomethanes such as 1,3-bis(trichloromethyl)-5-(2'-chlorophenyl)-1,3,5-triazine and 2-[2-(2-furanyl)vinyl]-4,6-bis(trichloromethyl)-1,3,5-triazine; imidazole dimers such as 2,2'-bis(2-chlorophenyl)4,5,4',5'-tetraphenyl1,2'-biimidazole; thioxanthone compounds such as 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone; biguanide compounds such as 1,2-diisopropyl-3-[bis(dimethylamino)methylene]guanidinium=2-(3-benzoylphenyl)propionate; and so on.

[0148] These polymerization initiators can be used alone or in combination of two or more. They can also be used in combination with any photosensitizer.

[0149] In addition, as a catalyst to promote the condensation reaction of the above-mentioned polysiloxane compounds, it can also be combined with photoacid generators and photoalkali generators.

[0150] When the total amount of the above-mentioned polysiloxane compound and the above-mentioned photopolymerizable compound is set to 100 parts by mass, it is preferable to contain 0.5 to 40 parts by mass of the above-mentioned polymerization initiator.

[0151] If the content of the above polymerization initiator is less than 0.5 parts by mass, the photopolymerization property will be reduced, resulting in insufficient curing (hardening) of the film; if the content of the above polymerization initiator exceeds 40 parts by mass, the storage stability of the solvent-free polysiloxane composition may be reduced.

[0152] When the total amount of the above-mentioned polysiloxane compound and the above-mentioned polymerizable monomer having two or more free radical polymerizable unsaturated double bonds is set to 100 parts by mass, the above-mentioned polymerization initiator is more preferably 1 to 20 parts by mass.

[0153] (Other materials)

[0154] Without diminishing the effectiveness of the invention, the solvent-free polysiloxane composition of the present invention may contain the following substances: chelating compounds of metals such as aluminum, zirconium, and titanium; crosslinking agents such as carbodiimides, isocyanates, and crosslinking functional groups having epoxy or thiol groups; surfactants such as organosilicones and fluorine compounds; photosensitizers such as aromatic hydrocarbons, amino compounds, nitro compounds, quinones, and xanthones; polymerization inhibitors such as hydroquinone, p-methoxyphenol, hindered amines, hindered phenols, di-tert-butylhydroquinone, 4-methoxyphenol, 2,6-di-tert-butyl-p-cresol, and nitrosamine salts; and fillers such as inorganic metal oxides and organic microparticles.

[0155] (Preparation method of solvent-free polysiloxane composition)

[0156] As a method for preparing the solvent-free polysiloxane composition of the present invention, the following method can be used: placing an organic solvent in a suitable container, for example, adding the above-mentioned polysiloxane compound while stirring with a high-speed mixer or the like, and adding the above-mentioned photopolymerizable compound having two or more free radical polymerizable unsaturated double bonds, the above-mentioned polymerization initiator, and other materials as needed, and mixing them.

[0157] Furthermore, the preparation method of the solvent-free polysiloxane composition of the present invention is not limited to the above method, and the order in which the various materials are added can be arbitrary.

[0158] In addition, for solid materials, if they are soluble in organic solvents, they can be pre-dissolved in organic solvents before being placed in them; if they can be directly or dispersed in organic solvents using dispersants, they can be pre-dispersed in organic solvents before being placed in them.

[0159] (Methods for forming a cured film)

[0160] As a method for forming a cured film using the solvent-free polysiloxane composition of the present invention, it preferably includes: a coating step of coating the solvent-free polysiloxane composition onto a substrate; an exposure step of irradiating an exposed portion with active energy lines to form a cured film; and a developing step of dissolving and removing the coating liquid from the unexposed portion with a developing solution.

[0161] In addition, heat curing can be performed after the above coating process.

[0162] The coating method in the above coating process, the active energy line and irradiation method for irradiating the exposed part in the above exposure process, and the developing solution for removing the coating solution from the exposed part can be appropriately selected and the substances and methods used in conventional photolithography can be used.

[0163] For example, the solvent-free polysiloxane composition is diluted to a concentration of 20% by mass, coated using a spin coater, and then pre-baked at 80°C for 3 minutes. Finally, it is lithographically applied using a mask aligner at 100 mJ / cm². 2 The test pattern is printed under the irradiation conditions, immersed in the developer for 1 minute, and then heated (post-baked) at 150°C for 30 minutes to obtain a cured film.

[0164] The preferred pre-drying conditions are 60–130°C for 1–3 minutes.

[0165] The preferred irradiation conditions are 50–260 mJ / cm². 2 .

[0166] The preferred conditions for the post-drying process are 120–230°C and 30–60 minutes.

[0167] The aforementioned thermosetting process can be performed, for example, by heating at 130°C for 10 minutes followed by heating at 180°C for 60 minutes to cure the material.

[0168] (Physical properties of solvent-free polysiloxane compositions)

[0169] The solvent-free polysiloxane composition of the present invention exhibits excellent stability over time.

[0170] In this specification, stability over time is evaluated using the following methods.

[0171] The viscosity and weight-average molecular weight of solvent-free polysiloxane compositions were compared immediately after preparation and after storage at 60°C for one week.

[0172] If the increase in viscosity and weight-average molecular weight is less than 15%, it is judged to have excellent stability over time.

[0173] In addition, the viscosity was measured using an R115 type viscometer RE-105L (E type viscometer, manufactured by Toki Sangyo Co., Ltd.) (measurement temperature 25°C), and the weight-average molecular weight was measured using the method described above.

[0174] The refractive index of the cured film of the solvent-free polysiloxane composition of the present invention is 1.48 or less.

[0175] The refractive index of the cured film is preferably 1.47 or less, more preferably 1.46 or less.

[0176] The refractive index of the cured film was measured by the following method.

[0177] The above-mentioned polysiloxane compound and a polymerization initiator (Omnirad 184, manufactured by TIANJIN NEW MATERIALS) at 5% by mass relative to the above-mentioned polysiloxane compound were dissolved in tetrahydrofuran (THF), and the tetrahydrofuran was removed by vacuum distillation to prepare a solvent-free polysiloxane composition.

[0178] Next, 1.5 g of the above solvent-free polysiloxane composition was coated onto a glass substrate at 3000 rpm for 60 seconds using spin coating. The substrate was then placed in a plastic bag, and the air inside was replaced with nitrogen gas to achieve a cumulative light intensity of 3000 mJ / cm². 2 The film is formed by irradiating it with 365nm UV light.

[0179] Finally, the refractive index of the cured film at a wavelength of 550 nm was measured using the OPTM series microspectrophotometer (manufactured by Otsuka Electronics Co., Ltd.).

[0180] In addition, the thickness of the cured film can also be measured using a microspectral film thickness gauge of the OPTM series (manufactured by Otsuka Electronics Co., Ltd.).

[0181] The cured film of the solvent-free polysiloxane composition of the present invention has excellent pencil hardness.

[0182] The pencil hardness of the above-mentioned cured film was measured by the following method.

[0183] The above-mentioned polysiloxane compound and a polymerization initiator (Omnirad 184, manufactured by TIANJIN NEW MATERIALS) at 5% by mass relative to the above-mentioned polysiloxane compound were dissolved in tetrahydrofuran (THF), and the tetrahydrofuran was removed by vacuum distillation to prepare a solvent-free polysiloxane composition.

[0184] Next, 1.5 g of the above solvent-free polysiloxane composition was coated onto a glass substrate at 3000 rpm for 60 seconds using spin coating. The substrate was then placed in a plastic bag, and the air inside was replaced with nitrogen gas to achieve a cumulative light intensity of 3000 mJ / cm². 2 The film is formed by irradiating it with 365nm UV light.

[0185] Finally, the hardness of the pencil [Mitsubishi Pencil Co., Ltd., Uni] was measured according to JIS K 5400-5-4.

[0186] If the pencil hardness of the cured film measured by the above method is 3H or higher, it is considered to have excellent pencil hardness.

[0187] The preferred hardness of the pencil is 4H or higher, and more preferably 5H or higher.

[0188] The following technical solutions are disclosed in this specification.

[0189] This disclosure (1) is a solvent-free polysiloxane composition comprising a polysiloxane compound and satisfying conditions 1 and 2 below, wherein the polysiloxane compound has at least a structural unit derived from the following formula (1) and at least one terminal silanol group is capped with a trimethylsilyl group.

[0190]

[0191] In equation (1), A 1 A represents a monovalent organic group with a double bond that exhibits free radical polymerization. 2 R indicates alkyl or siloxy groups. 1 Indicates alkyl group, multiple R 1 They can be the same or different, and 'a' can be 0 or 1. [Condition 1] The refractive index of the cured film is below 1.48; [Condition 2] In the above polysiloxane compounds, when the molar ratio of the structural units derived from the above formula (1) relative to all structural units is set to M1, M1 is 40 to 100.

[0192] This disclosure (2) is the solvent-free polysiloxane composition described in this disclosure (1), wherein the molar ratio M1 of the structural units derived from the above formula (1) of the polysiloxane compound is 60 or more.

[0193] This disclosure (3) is a solvent-free polysiloxane composition as described in disclosure (1) or (2), wherein the polysiloxane compound further contains a structural unit derived from at least one of the group consisting of the following formulas (2) and (3), and satisfies the following condition 3.

[0194]

[0195] In equation (2), B 1 B indicates alkyl group. 2 R represents the silicon-oxygen group. 2 Indicates alkyl group, multiple R 2 They can be the same or different, and b is 0 or 1;

[0196] In equation (3), C 1 Indicates alkyl, C 2 R represents the silicon-oxygen group. 3 Indicates alkyl; two carbon atoms 1 They can be the same or different, multiple Rs 3 They can be the same or different, and c can be 0 or 1; [Condition 3] For the above polysiloxane compounds, when the molar ratio of structural units derived from the above formula (2) relative to all structural units is set to M2 and the molar ratio of structural units derived from the above formula (3) is set to M3, M2 is 0 to 40 and M3 is 0 to 40.

[0197] This disclosure (4) is a solvent-free polysiloxane composition as described in any one of (1) to (3) of this disclosure, wherein the weight-average molecular weight of the polysiloxane compound is 800 to 10000.

[0198] This disclosure (5) is a method for preparing a polysiloxane compound, which sequentially includes the following steps 1, 2 and 3, and satisfies the following condition 4.

[0199] (Process 1)

[0200] The process of reacting a silane compound containing at least one of the following formula (1) to prepare a polysiloxane compound with a terminal silanol group,

[0201] In equation (1), A 1 A represents a monovalent organic group with a double bond that exhibits free radical polymerization. 2 R indicates alkyl or siloxy groups. 1 Indicates alkyl group, multiple R 1 They can be the same or different, and 'a' can be 0 or 1. (Process 2) The process of removing the solvent after adding the diluent; (Process 3) The process involves dissolving the aforementioned polysiloxane compound with terminal silanol groups in an organic solvent and then adding a protective agent with trimethylsilyl groups to obtain a polysiloxane compound with at least one terminal silanol group capped. [Condition 4] In the above polysiloxane compounds, when the molar ratio of the structural units derived from the above formula (1) relative to all structural units is set to M1, M1 is 40 to 100.

[0202] This disclosure (6) is a method for preparing the polysiloxane compound described in this disclosure (5), wherein step 1 includes a step of further reacting at least one silane compound selected from the group consisting of the following formulas (2) to (3) to prepare a polysiloxane compound having a silanol group at the end, and satisfies the following condition 5.

[0203]

[0204] In equation (2), B1 B indicates alkyl group. 2 R represents the silicon-oxygen group. 2 Indicates alkyl group, multiple R 2 They can be the same or different, and b is 0 or 1;

[0205] In equation (3), C 1 Indicates alkyl, C 2 R represents the silicon-oxygen group. 3 Indicates alkyl; two carbon atoms 1 They can be the same or different, multiple Rs 3 They can be the same or different, and c can be 0 or 1; [Condition 5] In the above-mentioned polysiloxane compound, M1 is 60 or more. When the molar ratio of structural units derived from the above formula (2) relative to all structural units is set to M2 and the molar ratio of structural units derived from the above formula (3) is set to M3, M2 is 0 to 40 and M3 is 0 to 40.

[0206] Example

[0207] The present invention will be further described in detail below by way of examples, but the present invention is not limited to these examples. In addition, unless otherwise stated, "%" means "percentage by mass" and "parts" means "parts by mass".

[0208] The materials used in the embodiments and comparative examples are described below.

[0209] (The compound of formula (1) above)

[0210] 3-Acryloyloxypropyltrimethoxysilane

[0211] (The compound of formula (2) above)

[0212] Methyltriethoxysilane

[0213] (The compound of formula (3) above)

[0214] dimethyldimethoxysilane

[0215] (Polymerization catalyst)

[0216] p-Toluenesulfonic acid monohydrate

[0217] (water)

[0218] Ion-exchanged water

[0219] (Amide compounds)

[0220] N,N-Dimethylacetamide

[0221] (orthoester)

[0222] Trimethyl orthoacetate

[0223] (Protective reagent)

[0224] Hexamethyldisilazane

[0225] (Example 1)

[0226] Add 28.38 g of 3-acryloyloxypropyltrimethoxysilane, 19.79 g of methyltriethoxysilane, and 6.07 g of dimethyldimethoxysilane to a flask and stir.

[0227] On the other hand, a solution was prepared by mixing 0.03 g of p-toluenesulfonic acid monohydrate with 11.48 g of deionized water. This solution was added dropwise to the flask over 15 minutes at a temperature not exceeding 60°C. After the addition, stirring was performed at 60°C for 3 hours (Step 1).

[0228] After cooling, 10.8 g of N,N-dimethylacetamide was added as a diluent and stirred. Next, 22.8 g of trimethyl orthoacetate was added dropwise while maintaining a temperature not exceeding 30°C. Then, methanol, ethanol, and water, which were byproducts, were removed by vacuum distillation to obtain a concentrated solution of a polysiloxane compound with terminal silanol groups (step 2).

[0229] 23.2 g of ethyl acetate and 23.5 g of acetic anhydride were added to a concentrated solution of a polysiloxane compound with silanol groups at the ends, and the mixture was stirred. Then, 34.25 g of hexamethyldisilazane was added dropwise while maintaining a temperature not exceeding 30°C, resulting in a solution of a polysiloxane compound capped with hexamethyldisilazane (step 3).

[0230] A solution of a polysiloxane compound capped with hexamethyldisilazane was added to 34.8 g of hexane and 11.6 g of deionized water. The mixture was stirred using a separatory funnel and allowed to stand until an organic layer and an aqueous layer separated. The aqueous layer was then removed. After removing the aqueous layer, the organic layer was extracted using deionized water and a saturated sodium bicarbonate solution.

[0231] 10.0 g of sodium sulfate was added to the extracted organic layer and the mixture was stirred for 10 minutes to dehydrate it. The solution was then filtered using a filter.

[0232] Next, the solution was subjected to vacuum distillation at 60°C for 1 hour, followed by vacuum distillation at 120°C for 3 hours to remove low-boiling-point components other than the polysiloxane compound, resulting in a solvent-free polysiloxane composition containing the polysiloxane compound.

[0233] In addition, the molar ratio of the structural units derived from formula (1) is set as M1, the molar ratio of the structural units derived from formula (2) is set as M2, and the molar ratio of the structural units derived from formula (3) is set as M3, as shown in Table 1.

[0234] (Examples 2-4, Comparative Examples 1-2)

[0235] Except for changing the amount of various materials added as shown in Table 1, the solvent-free polysiloxane composition was obtained by operating in the same manner as in Example 1.

[0236] In addition, Table 1 records the amount of each material added in step 1 above and the amount of hexamethyldisilazane added in step 3 above.

[0237] Furthermore, the molar ratio of the structural units derived from formula (1) is set as M1, the molar ratio of the structural units derived from formula (2) is set as M2, and the molar ratio of the structural units derived from formula (3) is set as M3, as shown in Table 1.

[0238] [Table 1]

[0239] <Stability over time>

[0240] For the polysiloxane compositions of the Examples and Comparative Examples, the viscosity and weight-average molecular weight were measured immediately after preparation and after storage at 60°C for one week, and evaluated according to the following criteria. The results are shown in Table 2.

[0241] In addition, viscosity was measured using an R115 type viscometer RE-105L (E type viscometer, manufactured by Toki Sangyo Co., Ltd.) (measurement temperature 25°C), and weight-average molecular weight was measured using the method described in this manual.

[0242] (Evaluation Criteria)

[0243] 〇: The increase in viscosity and weight-average molecular weight is less than 15%; △: The increase in viscosity and weight-average molecular weight is more than 15%; ×: It has gelled.

[0244] <Measurement of the refractive index of the cured film>

[0245] The polysiloxane compositions of the examples and comparative examples, along with a polymerization initiator (Omnirad 184, manufactured by TIANJIN NEW MATERIALS) at 5% by mass relative to the polysiloxane compound, were dissolved in tetrahydrofuran (THF), and the tetrahydrofuran was removed by vacuum distillation.

[0246] Next, 1.5 g of the above solvent-free polysiloxane composition was applied onto a glass substrate under spin coating conditions of 3000 rpm for 60 seconds, then placed in a plastic bag, the internal air was replaced with nitrogen, and UV light at 365 nm was irradiated so that the cumulative light amount reached 3000 mJ / cm 2 , thereby forming a cured film.

[0247] Finally, the refractive index of the cured film at a wavelength of 550 nm was measured using a microspectroscopic film thickness meter OPTM series (manufactured by Otsuka Electronics Co., Ltd.). The results are shown in Table 2.

[0248] <Evaluation of Pencil Hardness of Cured Film>

[0249] The polysiloxane compositions of Examples and Comparative Examples, and a polymerization initiator (Omnirad 184, manufactured by TIANJIN NEW MATERIALS Co., Ltd.) in an amount of 5% by mass relative to the above polysiloxane compound were dissolved in tetrahydrofuran (THF), and tetrahydrofuran was removed by distillation under reduced pressure.

[0250] Next, 1.5 g of the above solvent-free polysiloxane composition was applied onto a glass substrate under spin coating conditions of 3000 rpm for 60 seconds, then placed in a plastic bag, the internal air was replaced with nitrogen, and UV light at 365 nm was irradiated so that the cumulative light amount reached 3000 mJ / cm 2 , thereby forming a cured film.

[0251] Finally, the hardness of a pencil [Mitsubishi Pencil Co., Ltd., Uni] was measured in accordance with JIS K 5400-5-4. A pencil hardness of 3H or higher was judged as acceptable.

[0252] [Table 2]

[0253] It can be confirmed from Table 2 that the solvent-free polysiloxane compositions in the Examples have excellent temporal stability, the cured films have a refractive index of 1.48 or less, and also have excellent pencil hardness.

[0254] Industrial Applicability

[0255] Based on the present invention, it is possible to provide a solvent-free polysiloxane composition that is solvent-free, has excellent temporal stability, gives a cured film with a low refractive index, and also has excellent pencil hardness.

Claims

1. A solvent-free polysiloxane composition comprising a polysiloxane compound and satisfying conditions 1 and 2 below, wherein the polysiloxane compound has at least a structural unit derived from the following formula (1) and at least one terminal silanol group is capped with a trimethylsilyl group. In equation (1), A 1 A represents a monovalent organic group with a double bond that exhibits free radical polymerization. 2 R indicates alkyl or siloxy groups. 1 Indicates alkyl group, multiple R 1 They can be the same or different, and 'a' can be 0 or 1. Condition 1: The refractive index of the cured film is below 1.48; Condition 2: In the polysiloxane compound, when the molar ratio of the structural units derived from the above formula (1) relative to all structural units is set to M1, M1 is 40 to 100.

2. The solvent-free polysiloxane composition according to claim 1, wherein, The molar ratio M1 of the structural units derived from formula (1) of the polysiloxane compound is 60 or more.

3. The solvent-free polysiloxane composition according to claim 1 or 2, wherein, The polysiloxane compound further contains a structural unit derived from at least one of the following formulas (2) and (3), and satisfies the following condition 3; In equation (2), B 1 B indicates alkyl group. 2 R represents the silicon-oxygen group. 2 Indicates alkyl group, multiple R 2 They can be the same or different, and b is 0 or 1; In equation (3), C 1 Indicates alkyl, C 2 R represents the silicon-oxygen group. 3 Indicates alkyl; two carbon atoms 1 They can be the same or different, multiple Rs 3 They can be the same or different, and c can be 0 or 1; Condition 3: For the polysiloxane compound, when the molar ratio of structural units derived from formula (2) relative to all structural units is set to M2 and the molar ratio of structural units derived from formula (3) is set to M3, M2 is 0 to 40 and M3 is 0 to 40.

4. The solvent-free polysiloxane composition according to claim 1 or 2, wherein, The weight-average molecular weight of the polysiloxane compound is 800 to 10,000.

5. A method for preparing a polysiloxane compound, comprising the following steps 1, 2 and 3 in sequence, and satisfying the following condition 4; Process 1: The process of reacting a silane compound containing at least one of the following formula (1) to prepare a polysiloxane compound with a terminal silanol group, In equation (1), A 1 A represents a monovalent organic group with a double bond that exhibits free radical polymerization. 2 R indicates alkyl or siloxy groups. 1 Indicates alkyl group, multiple R 1 They can be the same or different, and 'a' can be 0 or 1. Process 2: The process of removing the solvent after adding the diluent; Process 3: The process of diluting the polysiloxane compound with silanol groups at the ends with an organic solvent and adding a protective agent with trimethylsilyl groups to obtain a polysiloxane compound with at least one silanol group at the end. Condition 4: In the polysiloxane compound, when the molar ratio of the structural units derived from the above formula (1) relative to all structural units is set to M1, M1 is 40 to 100.

6. The method for preparing the polysiloxane compound according to claim 5, wherein, The step 1 includes a step of further reacting at least one silane compound selected from the group consisting of the following formulas (2) to (3) to prepare a polysiloxane compound with a silanol group at the end, and satisfies the following condition 5; In equation (2), B 1 B indicates alkyl group. 2 R represents the silicon-oxygen group. 2 Indicates alkyl group, multiple R 2 They can be the same or different, and b is 0 or 1; In equation (3), C 1 Indicates alkyl, C 2 R represents the silicon-oxygen group. 3 Indicates alkyl; two carbon atoms 1 They can be the same or different, multiple Rs 3 They can be the same or different, and c can be 0 or 1; Condition 5: The M1 of the polysiloxane compound is 60 or more. When the molar ratio of structural units derived from the formula (2) relative to all structural units is set to M2 and the molar ratio of structural units derived from the formula (3) is set to M3, M2 is 0 to 40 and M3 is 0 to 40.

Citation Information

Patent Citations

  • Composition for forming low-refractive index film, method for manufacturing low-refractive index thin film, and component with Anti-reflection film