A modified organosilicon, its preparation method and application
By introducing octamethylcyclotetrasiloxane into the silicone-based conformal coating and reacting it with amino-containing siloxane monomers to generate side-amino silicone oil, which then reacts with isocyanate groups to form a urea network, the microphase separation problem is solved, tensile strength and overall performance are improved, and it is suitable for the protection of high-density electronic components.
Patent Information
- Application Number
- CN202611205601.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-17
AI Technical Summary
The existing UV/moisture dual-curing silicone conformal coatings, after introducing alkoxysilane groups, result in severe thermodynamic incompatibility between the polyurethane and silicone segments, causing microphase separation and a significant reduction in tensile strength, making it difficult to meet the mechanical requirements of precision electronic circuit boards.
The side-amino silicone oil is generated by the dehydration condensation reaction of octamethylcyclotetrasiloxane with amino-containing siloxane monomers under the action of a catalyst. It then undergoes a nucleophilic addition reaction with isocyanate-containing siloxanes and acrylates to introduce acryloyloxy and urea groups, forming a strong hydrogen bond network, which avoids microphase separation and improves tensile strength.
While achieving UV/moisture dual curing, it significantly improves the tensile strength of silicone-based conformal coatings, possesses suitable system viscosity, hardness, and elongation at break, and exhibits excellent salt spray corrosion resistance and high and low temperature cyclic impact resistance, making it suitable for the protection of high-density electronic components.
Smart Images

Figure CN123107092A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer materials technology, and more specifically, to a modified organosilicon, its preparation method, and its application. Background Technology
[0002] Conformal coating is a type of paint applied to the surface of printed circuit boards (PCBs) to form a protective film, used for moisture protection, salt spray protection, and mildew prevention, while also providing insulation protection. As electronic components become increasingly miniaturized and denser, the performance requirements for conformal coatings are constantly increasing, particularly demanding a balance between rapid curing, complete curing (no shaded areas), good adhesion, a suitable balance between hardness and flexibility, and excellent weather resistance and electrical insulation.
[0003] Currently, commercially available conformal coatings are mainly divided into three categories: acrylic, polyurethane, and silicone.
[0004] Acrylic conformal coatings have fast UV curing speeds, but they suffer from incomplete curing in shaded areas and exhibit poor flexibility and insufficient temperature resistance. Polyurethane conformal coatings have good adhesion and high toughness, but their curing speed is slow and their weather resistance is poor. To address the shortcomings of single-curing systems, UV / moisture dual-curing systems have been reported in the literature. For example, a Chinese patent discloses a polyurethane acrylate containing isocyanate and (meth)acrylate, which can be used to formulate light / moisture dual-curing conformal coatings. However, its main structure is a pure carbon chain, lacking organosilicon segments, resulting in insufficient flexibility and hydrophobicity.
[0005] Silicone-based conformal coatings possess excellent weather resistance, low surface energy, and hydrophobic and moisture-proof properties, but they generally suffer from poor adhesion to PCB substrates. Research indicates that introducing polyurethane segments or urethane structures into the silicone molecular framework can effectively improve the interfacial adhesion between the resin and the substrate. Furthermore, introducing acryloyloxy functional groups can construct a UV / moisture dual-curing system, balancing rapid UV curing with deep moisture cross-linking capabilities.
[0006] In the preparation of this type of dual-curing resin, isocyanate groups are often used to construct polyurethane segments. However, free isocyanate groups are highly chemically reactive and readily react with trace amounts of moisture in the system, causing a deterioration in the storage stability of the conformal coating. The current mainstream solution is to use aminosilanes to perform end-capping reactions with isocyanates, converting the reactive isocyanate into alkoxysilyl groups. The alkoxysilyl groups can undergo hydrolysis and condensation in a humid environment to achieve cross-linking and curing, thereby eliminating free NCO while retaining the moisture curing ability, and achieving stable storage of the UV / moisture dual-curing resin system.
[0007] However, the solubility parameters of the polar hard segments of polyurethane and the non-polar soft segments of organosilicon differ significantly. Further introduction of alkoxysilane groups into the molecule exacerbates the thermodynamic incompatibility between the polyurethane and organosilicon segments, inducing severe microphase separation and ultimately resulting in a significant decrease in the tensile strength of the cured film. Existing studies have confirmed that the higher the amount of alkoxysilane groups introduced into the system, the more severe the microphase separation and the more significant the decrease in the mechanical strength of the cured material. The organosilicon matrix itself has relatively weak mechanical properties, and the strength deficiency caused by the aforementioned phase separation makes it difficult for traditional UV / moisture dual-curing organosilicon conformal coatings to meet the mechanical requirements of applications such as precision electronic circuit boards.
[0008] Therefore, how to improve the tensile strength of silicone-based conformal coatings to meet practical application scenarios while achieving UV / moisture dual curing through acryloyloxy and alkoxysilane groups is a current research challenge. Summary of the Invention
[0009] The primary objective of this invention is to overcome the problem of how to improve the tensile strength of silicone-based conformal coatings when UV / moisture dual curing is achieved through acryloyloxy and alkoxysilane groups, and to provide a method for preparing modified silicone.
[0010] Another objective of this invention is to provide the application of the modified organosilicon prepared by the above-described preparation method in the preparation of UV / moisture dual-curing paints.
[0011] A further objective of this invention is to provide a UV / moisture dual-curing paint.
[0012] Another objective of this invention is to provide a conformal coating for UV / moisture dual-curing paint.
[0013] The above-mentioned objective of the present invention is achieved through the following technical solution: A method for preparing modified organosilicon includes the following steps: S1. Octamethylcyclotetrasiloxane, a siloxane monomer containing one amino group, and an amino-containing end-capping agent undergo a dehydration condensation reaction under the action of a catalyst to obtain a side-amino silicone oil; S2. Under conditions not exceeding 72°C, the amino silicone oil described in S1 first undergoes a nucleophilic addition reaction with a siloxane containing an isocyanate group, and then undergoes a nucleophilic addition reaction with an acrylate containing an isocyanate group to obtain the modified organosilicon. The molar ratio of the octamethylcyclotetrasiloxane to the siloxane monomer containing one amino group is 1:(0.030-0.042).
[0014] To enable modified organosilicon to exhibit UV / moisture curing properties, this invention introduces acryloyloxy and siloxane groups through isocyanate-containing siloxanes and isocyanate-containing acrylates. Simultaneously, the isocyanate-containing siloxanes and isocyanate-containing acrylates react with the amino groups of specific side-amino silicone oils to generate a certain amount of urea groups. These urea groups form a strong hydrogen bond network that effectively "anchors" the siloxane groups, effectively avoiding the microphase separation problem between polyurethane and organosilicon segments that occurs with the introduction of urethane bonds. Therefore, while achieving UV / moisture curing of the paint made from modified organosilicon, it also achieves a significant improvement in the tensile strength of the paint made from modified organosilicon.
[0015] In the preparation of side-amino silicone oil, the ratio of octamethylcyclotetrasiloxane to a siloxane monomer containing one amino group is particularly critical. If the amount of the siloxane monomer containing one amino group is too high, the number of amino groups on the side-amino silicone oil molecular chain will be excessive, resulting in an excessive number of urea groups formed in step S2. This leads to excessive hydrogen bonding, causing the side-amino silicone oil to gel and rendering it unusable for paint preparation. The reaction temperature in step S2 is also critical. If the temperature is too high, after the amino group of the side-amino silicone oil completes the primary addition with the isocyanate monomer to form a urea bond, the secondary amine of the urea bond still contains active NH bonds. These NH bonds continue to undergo secondary addition with the isocyanate monomer, easily forming excessively long branches. Under the influence of branch entanglement and strong hydrogen bonding, the side-amino silicone oil undergoes irreversible gelation, also rendering it unusable for paint preparation.
[0016] Preferably, the molar ratio of the octamethylcyclotetrasiloxane to the siloxane monomer containing one amino group is 1:0.032 to 0.040.
[0017] More preferably, the molar ratio of the octamethylcyclotetrasiloxane to the siloxane monomer containing one amino group is 1:0.036~0.040.
[0018] Preferably, the molar ratio of octamethylcyclotetrasiloxane to the amino-containing capping agent in step S1 is 1:(0.09~0.2).
[0019] Preferably, the siloxane monomer containing one amino group in step S1 is 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, aminoethylmethyldimethoxysilane, or aminoethylmethyldiethoxysilane.
[0020] Preferably, the amino-containing end-capping agent in step S1 is an amino double-end-capping agent.
[0021] Preferably, the catalyst in step S1 is tetramethylammonium hydroxide.
[0022] Preferably, the mass ratio of octamethylcyclotetrasiloxane to catalyst in step S1 is 1:(0.01~0.06).
[0023] Preferably, the temperature of the dehydration condensation reaction in step S1 is 105~120℃ and the time is 5~7 hours.
[0024] Preferably, after the dehydration condensation reaction described in step S1, a step of removing impurities is also included.
[0025] Preferably, the specific process of removing impurities is as follows: heating to 130~150℃ and maintaining it in a vacuum environment for 0.5~1.5 hours.
[0026] Preferably, the side-amino silicone oil in step S1 is a double-amino-terminated side-amino silicone oil.
[0027] Preferably, the siloxane containing the isocyanate group in step S2 is at least one of propyltriethoxysilane, propyltrimethoxysilane, methyltriethoxysilane, methyltrimethoxysilane, propylmethyldimethoxysilane, or propylmethyldiethoxysilane.
[0028] Preferably, the acrylate containing the isocyanate group in step S2 is at least one of ethyl isocyanate acrylate, 2-isocyanate-ethyl methacrylate, isocyanate-ethyl methacrylate, 1-(isocyanate-methyl)-4-(meth)acryloyloxycyclohexane, 3-isocyanate-propyl acrylate, or 3-isocyanate-propyl methacrylate.
[0029] Preferably, the mass ratio of the side-amino silicone oil to the isocyanate-containing siloxane in step S2 is 1:(0.14~0.18).
[0030] Preferably, the mass ratio of the side-amino silicone oil to the acrylate containing isocyanate groups in step S2 is 1:(0.03~0.04).
[0031] Preferably, step S2 is carried out in the presence of an organic solvent.
[0032] More preferably, the organic solvent in step S2 is at least one of toluene or isopropanol.
[0033] More preferably, the organic solvent is toluene and isopropanol in a volume ratio of 2 to 4:1.
[0034] Preferably, the nucleophilic addition reaction with the isocyanate-containing acrylate in step S2 is carried out in the presence of a polymerization inhibitor.
[0035] In this invention, the reaction in step S2 is carried out at a temperature not exceeding 72°C, as long as the reaction temperature is sufficient for NCO to react with the amino group. Those skilled in the art can set the lower limit of the temperature according to this requirement.
[0036] Preferably, step S2 is as follows: under conditions of 65~72°C, the side-amino silicone oil mentioned in S1 first undergoes a nucleophilic addition reaction with a siloxane containing isocyanate groups, and then undergoes a nucleophilic addition reaction with an acrylate containing isocyanate groups to obtain the modified organosilicon.
[0037] Preferably, the reaction in step S2 is carried out in an inert atmosphere.
[0038] More preferably, the inert atmosphere is nitrogen.
[0039] Preferably, after the reaction in step S2 is completed, the step further includes removing the solvent by vacuum distillation and / or cooling.
[0040] This invention also protects the application of a modified organosilicon prepared by the above method in the preparation of UV / moisture dual-curing paints.
[0041] The present invention also protects a UV / moisture dual-curing paint, comprising the following components in parts by weight: 80-100 parts modified organosilicon, 20-30 parts reactive diluent, 3-5 parts photoinitiator, and 0.2-0.5 parts curing catalyst.
[0042] Preferably, the reactive diluent is at least one selected from isobornyl acrylate, isobornyl methacrylate, trimethylolpropane triacrylate, 1,6-hexanediol diacrylate, dipentaerythritol hexaacrylate, or tetrahydrofuran acrylate.
[0043] Preferably, the photoinitiator is at least one of 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 4-chlorobenzophenone, phenylbis(2,4-trimethylbenzoyl)phosphine oxide, 2,4,6-trimethylbenzoyl diphenylphosphine oxide, or isopropylthioxanthraphenone.
[0044] Preferably, the curing catalyst is at least one of dibutyltin dilaurate, dioctyltin dilaurate, stannous octoate, dibutyltin diacetate, tetrabutyl titanate, or isopropyl titanate.
[0045] Preferably, the UV / moisture dual-curing paint is a conformal coating.
[0046] Compared with the prior art, the beneficial effects of the present invention are: (1) The present invention can achieve UV / moisture curing of paint made of modified organosilicon, and at the same time, it can also achieve a leapfrog improvement in the tensile strength of paint made of modified organosilicon.
[0047] (2) The paint made of modified organosilicon of the present invention also has suitable system viscosity, good hardness and elongation at break, high volume resistivity, and excellent salt spray corrosion resistance and high and low temperature cycle impact resistance. It can be widely used in high reliability protection scenarios of high-density electronic components (e.g., protective coating of electronic circuit boards). Attached Figure Description
[0048] Figure 1 Fourier transform infrared spectrum of the modified organosilicon prepared in Example 1. Detailed Implementation
[0049] To more clearly and completely describe the technical solution of the present invention, the present invention will be further described in detail below through specific embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the present invention. Various changes can be made within the scope of the claims of the present invention.
[0050] Example 1 This embodiment provides a method for preparing modified organosilicon, comprising the following steps: S1. In a reaction flask equipped with a stirrer, thermometer, and condenser, add 183.9 g of octamethylcyclotetrasiloxane, 16.1 g of amino-double-ended siloxane, 4.05 g of 3-aminopropylmethyldimethoxysilane, and 1 g of tetramethylammonium hydroxide catalyst, and heat to 110 °C. o C, react for 6 hours, after the reaction is complete, raise the temperature to 140°C. o C. Keep under vacuum for 1 hour to decompose the catalyst and remove unreacted monomers. After cooling, a transparent liquid is obtained, which is the side-amino silicone oil. The molar ratio of octamethylcyclotetrasiloxane to 3-aminopropylmethyldimethoxysilane is 1:0.04, and the molar ratio of octamethylcyclotetrasiloxane to amino-terminated siloxane is 1:0.105. S2. Add 66 mL of toluene, 33 mL of isopropanol, and 100 g of aminopropyl silicone oil to a dry reaction vessel, and heat to 70°C under nitrogen protection. o C. Slowly add 16.055 g of propyltriethoxysilane isocyanate dropwise, and react for 2 hours; maintain the temperature at 70°C. o C. Add 3.5 g of ethyl isocyanate acrylate and 0.35 mg of polymerization inhibitor MEHQ, and react for 2 hours. After the reaction is complete, remove the mixed solvent by vacuum distillation, and cool to obtain the modified organosilicon. Fourier transform infrared spectroscopy characterization shows that all NCO in the modified organosilicon has reacted. Figure 1 .
[0051] Example 2 This embodiment provides a method for preparing modified organosilicon. Unlike Example 1, in step S1, the amount of 3-aminopropylmethyldimethoxysilane is adjusted to 3.24 g, that is, the molar ratio of octamethylcyclotetrasiloxane to 3-aminopropylmethyldimethoxysilane is 1:0.032.
[0052] Example 3 This embodiment provides a method for preparing modified organosilicon. Unlike Example 1, in step S1, the amount of 3-aminopropylmethyldimethoxysilane is adjusted to 3.645g, that is, the molar ratio of octamethylcyclotetrasiloxane to 3-aminopropylmethyldimethoxysilane is 1:0.036.
[0053] Example 4 This embodiment provides a UV / moisture dual-curing conformal coating, comprising the following components in parts by weight: 80g of modified organosilicon prepared in Example 1, 20g of isobornyl acrylate, 3g of 1-hydroxycyclohexylphenyl ketone, and 0.3g of dibutyltin dilaurate.
[0054] The preparation method of the UV / moisture dual-curing conformal coating in this embodiment includes the following steps: adding modified silicone resin and isobornyl acrylate into a reaction vessel and stirring and mixing evenly at room temperature; then adding photoinitiator 1-hydroxycyclohexylphenyl ketone and catalyst dibutyltin dilaurate, and stirring continuously until the system is completely homogeneous and transparent, filtering out the material to obtain the UV / moisture dual-curing conformal coating.
[0055] Example 5 This embodiment provides a UV / moisture dual-curing conformal coating, which differs from Embodiment 4 in that the modified organosilicon prepared in Embodiment 1 is replaced with the modified organosilicon prepared in Embodiment 2.
[0056] Example 6 This embodiment provides a UV / moisture dual-curing conformal coating, which differs from Embodiment 4 in that the modified organosilicon prepared in Embodiment 1 is replaced with the modified organosilicon prepared in Embodiment 3.
[0057] Comparative Example 1 This comparative example provides a method for preparing modified organosilicon. Unlike Example 1, in step S1, the amount of 3-aminopropylmethyldimethoxysilane is adjusted to 4.86 g, that is, the molar ratio of octamethylcyclotetrasiloxane to 3-aminopropylmethyldimethoxysilane is 1:0.048.
[0058] Comparative Example 2 This comparative example provides a method for preparing modified organosilicon. Unlike Example 1, in step S2, the temperature is raised to 75°C under inert gas protection.
[0059] Comparative Example 3 Commercially available UV / moisture-curing silicone conformal coating 916 was selected as a comparison sample and designated as Conformal Coating 1.
[0060] Comparative Example 4 Commercially available UV / moisture-curing silicone conformal coating 953 was selected as a comparison sample and designated as conformal coating 2.
[0061] Characterization and performance testing 1. Appearance condition record The modified organosilicones obtained in Examples 1-3 were clear, transparent, and viscous liquids with good fluidity, and could be used for further preparation of paints. Comparative Examples 1 and 2 experienced irreversible gelation during the reaction with ethyl isocyanate acrylate in step S2, resulting in a loss of fluidity and making further paint preparation impossible.
[0062] 2. Adhesion test According to GB / T 9286-2021 "Adhesion Test of Paints and Varnishes by Cross-cut Method", the adhesion of the coatings formed by the paints in Examples 4-6 and Comparative Examples 3-4 was tested using a single-edged cutting tool. The cuts were made manually with uniform force, and the grid spacing was 2 mm. After cutting, a soft brush was used to gently brush back and forth 10 times along the two diagonals of the grid. Then, 3M tape was applied and peeled off at the required rate. The coating adhesion was then assessed according to the specified rating.
[0063] 3. Pencil hardness test According to GB / T 6739-2006 "Determination of Hardness of Paints and Varnishes by Pencil Method", a cart-type pencil hardness tester was used to test the hardness of the paint coatings formed in Examples 4-6 and Comparative Examples 3-4. The pencil hardness grades ranged from 6B to 6H, from lowest to highest. A 45... o When a pencil with a fixed tilt angle is used to perform three parallel scratch tests on the coating surface, if a certain hardness grade (such as 3H) scratches the coating twice or more, the hardness of the coated pencil is determined to be the next lower grade (2H).
[0064] 4. Tensile strength test The test was conducted using the STD 5000 electronic universal tensile testing machine from Guangdong Lugong Precision Instruments Co., Ltd., according to the test standard GB / T1040.1-2018.
[0065] 5. Viscosity test Viscosity was tested using a ThermoFisher Scientific HAAKE MARS 60 rotational rheometer with a diameter of 20 mm, a temperature of 25 °C, an equilibration time of 120 s, and a rotational speed range of 0.01-1000 r / s.
[0066] 6. Moisture curing effect test The conformal coating was evenly applied to the glass plate surface, with a film thickness controlled at 50±5 μm. Half of the coating area was completely shielded from light by aluminum foil, while the other half was exposed to ultraviolet light (UV energy 1000 mJ / cm², wavelength 365 nm). After UV irradiation, the sample was placed in a constant temperature and humidity chamber at 25℃ and 90% relative humidity for 72 hours. Subsequently, the curing degree of the shielded and illuminated areas was tested using the fingernail scratching method and the acetone wiping method (50 back-and-forth wipings) respectively. If the coating surface in the shielded area showed no indentations, no stickiness, and no dissolution or bubbling after wiping, and exhibited the same behavior as the illuminated area, the moisture curing effect was deemed acceptable.
[0067] 7. Salt spray resistance test The test was conducted according to GB / T 1771-2007 "Determination of resistance to neutral salt spray of paints and varnishes". A steel plate (150 mm × 75 mm × 1 mm) coated with conformal coating was placed in a salt spray test chamber. A 5 wt% NaCl solution (pH 6.5~7.2) was used, with a spray pressure of 0.07~0.17 MPa and a test temperature of (35±2)℃, and continuous spraying was performed. Every 24 hours, the plate was removed and the coating surface was observed for blistering, rust, peeling, etc. The time (h) at which the first corrosion mark appeared was recorded. At least three parallel samples were tested in each group, and the average value was taken.
[0068] 8. Volume resistivity test According to GB / T 1410-2006 "Test Methods for Volume Resistivity and Surface Resistivity of Solid Insulating Materials", a high-resistivity meter (ZC-90G type) was used for testing. Conformal coating was applied to the standard electrode system with a film thickness of (100±5) μm. The test voltage was 500 V, the charging time was 60 s, and the system was allowed to stand for 24 hours at a temperature of (23±2)℃ and a relative humidity of (50±5)%. The volume resistivity ρv was calculated using the formula ρv=Rv×(S / d), where Rv is the volume resistivity (Ω), S is the effective electrode area (m²), and d is the coating thickness (m). Five tests were performed on each sample group, and the average value was taken.
[0069] 9. High and low temperature impact test The test was conducted according to GJB 150.5A-2009 "Laboratory Environmental Test Methods for Military Equipment - Part 5: Temperature Shock Test". Printed circuit boards coated with conformal coating were placed in a high and low temperature shock test chamber. The chamber was set to a low temperature of 40℃ for 2 hours, followed by a high temperature of 85℃ for 2 hours. The transition time between high and low temperatures was ≤5 minutes, constituting one cycle. After every 50 cycles, the samples were removed and left at room temperature for 2 hours. The coating was then inspected using a 20x magnifying glass for cracking, blistering, peeling, or discoloration. Simultaneously, the adhesion (according to GB / T 9286-2021) was tested to ensure it remained at grade 0. The number of cycles at which failure occurred was recorded.
[0070] Table 1. Test results of conformal coatings in Examples 4-6 and Comparative Examples 3 and 4
[0071] As shown in Table 1, the UV / moisture dual-curing conformal coating of the present invention (Examples 4-6) has comprehensive and significant advantages in overall performance compared with commercially available dual-curing conformal coating products (Comparative Examples 3 and 4).
[0072] Comparative examples and comparative examples show that the tensile strength (above 1.30 MPa) of the UV / moisture dual-curing conformal coating prepared by the modified organosilicon of the present invention is significantly better than that of commercially available organosilicon conformal coatings. Furthermore, as shown in Examples 5, 6, and 4, the tensile strength of the UV / moisture dual-curing conformal coating prepared by the modified organosilicon of the present invention gradually increases with the increase of the amount of 3-aminopropylmethyldimethoxysilane used in the preparation process. In addition, the elongation at break and hardness of the UV / moisture dual-curing conformal coating prepared by the modified organosilicon of the present invention also gradually increase with the increase of the amount of 3-aminopropylmethyldimethoxysilane used in the preparation process.
[0073] Furthermore, the UV / moisture dual-curing conformal coating made from the modified organosilicon of this invention exhibits superior salt spray resistance (over 168 hours) and volume resistivity (2.1 × 10⁻⁶). 15 The modified silicone UV / moisture dual-curing conformal coating of this invention has better electrical insulation, salt spray resistance, and high and low temperature impact resistance (above Ω·cm) than commercially available silicone conformal coatings, indicating that the modified silicone UV / moisture dual-curing conformal coating of this invention has good electrical insulation, salt spray resistance, and high and low temperature impact resistance.
[0074] In the moisture curing test in the shaded area, Examples 4-6 achieved complete drying, while Comparative Examples 3 and 4 showed slight stickiness and surface tackiness, respectively. This indicates that the material of the present invention not only effectively overcomes the industry pain point of traditional UV conformal coatings failing to cure in the shaded area, but also solves the problem of incomplete curing of commercially available products in the shaded area.
[0075] Based on the above test data, the UV / moisture dual-curing conformal coating prepared by the modified organosilicon of the present invention achieves a significant improvement in tensile strength while simultaneously achieving UV / moisture curing. Furthermore, the UV / moisture dual-curing conformal coating prepared by the modified organosilicon of the present invention exhibits excellent application value in core indicators such as hardness, elongation at break, electrical insulation, salt spray resistance, high and low temperature impact resistance, and deep curing, fully meeting the stringent requirements of high-density, high-reliability electronic components for conformal coatings.
[0076] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. Those skilled in the art can make other variations or modifications based on the above description. It is neither necessary nor possible to exhaustively describe all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing modified organosilicon, characterized in that, Includes the following steps: S1. Octamethylcyclotetrasiloxane, a siloxane monomer containing one amino group, and an amino-containing end-capping agent undergo a dehydration condensation reaction under the action of a catalyst to obtain a side-amino silicone oil; S2. Under conditions not exceeding 72°C, the amino silicone oil described in S1 first undergoes a nucleophilic addition reaction with a siloxane containing isocyanate groups, and then undergoes a nucleophilic addition reaction with an acrylate containing isocyanate groups to obtain the modified organosilicon. The molar ratio of the octamethylcyclotetrasiloxane to the siloxane monomer containing one amino group is 1:(0.030-0.042).
2. The preparation method according to claim 1, characterized in that, The siloxane monomer containing one amino group in step S1 is at least one of 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, aminoethylmethyldimethoxysilane, or aminoethylmethyldiethoxysilane.
3. The preparation method according to claim 1, characterized in that, The amino-containing end-capping agent mentioned in step S1 is an amino-double-ended end-capping agent.
4. The preparation method according to claim 1, characterized in that, The temperature of the dehydration condensation reaction in step S1 is 105~120℃ and the time is 5~7 hours.
5. The preparation method according to claim 1, characterized in that, The time for the nucleophilic addition reaction with the isocyanate-containing siloxane in step S2 is 1-3 hours; the time for the nucleophilic addition reaction with the isocyanate-containing acrylate in step S2 is 1-3 hours.
6. The preparation method according to claim 1, characterized in that, The mass ratio of the side-amino silicone oil to the isocyanate-containing siloxane in step S2 is 1:(0.14~0.18); the mass ratio of the side-amino silicone oil to the isocyanate-containing acrylate in step S2 is 1:(0.03~0.04).
7. The application of the modified organosilicon prepared by the preparation method according to any one of claims 1 to 6 in the preparation of UV / moisture dual-curing paints.
8. A UV / moisture dual-curing paint, characterized in that, The product comprises the following components in parts by weight: 80-100 parts of modified organosilicon prepared by the preparation method according to any one of claims 1 to 6, 20-30 parts of reactive diluent, 3-5 parts of photoinitiator, and 0.2-0.5 parts of curing catalyst.
9. The UV / moisture dual-curing paint according to claim 8, characterized in that, The active diluent is at least one of isobornyl acrylate, isobornyl methacrylate, trimethylolpropane triacrylate, 1,6-hexanediol diacrylate, dipentaerythritol hexaacrylate, or tetrahydrofuran acrylate. The photoinitiator is at least one of 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 4-chlorobenzophenone, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2,4,6-trimethylbenzoyl diphenylphosphine oxide, or isopropylthioxanthrone. The curing catalyst is at least one of dibutyltin dilaurate, dioctyltin dilaurate, stannous octoate, dibutyltin diacetate, tetrabutyl titanate, or isopropyl titanate.
10. The UV / moisture dual-curing paint according to claim 8, characterized in that, The UV / moisture dual-curing paint is a conformal coating.