Preparation method and application of silk fibroin-based piezoelectric hydrogel
By preparing silk fibroin-based piezoelectric hydrogels and combining high β-folded grains with AMPS hydrogels, a piezoelectric-ion synergistic sensing system was constructed, which solved the performance degradation problem of hydrogel sensors under extreme strain and achieved a self-powered and highly sensitive flexible sensing effect.
Patent Information
- Application Number
- CN202611482745.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing hydrogel sensors struggle to simultaneously achieve high voltage and soft elasticity, composite fillers pose safety hazards, silk fibroin particles fail to exert their piezoelectric effect, and single sensors experience performance degradation under extreme strain.
Silk fibroin solution was induced to form highly β-folded crystals by anhydrous ethanol, which were then mixed with AMPS hydrogel precursors and irradiated with ultraviolet light to prepare silk fibroin-based piezoelectric hydrogels. This constructed a piezoelectric-ion synergistic sensing system, avoiding the mutual constraint between piezoelectric properties and modulus in traditional processes.
It achieves self-powered, high-sensitivity sensing over a wide strain range, high biosafety, and is suitable for flexible skin sensing applications. It also improves the tensile and adhesive strength of the hydrogel and reduces noise interference.
Smart Images

Figure CN123107119A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of hydrogel materials technology, specifically to a method for preparing and applying a silk fibroin-based piezoelectric hydrogel. Background Technology
[0002] Hydrogel materials are considered ideal matrix materials for constructing flexible strain sensors due to their high water content, three-dimensional network structure, and tissue-like mechanical properties. However, traditional hydrogel sensors mostly rely on resistance changes to achieve strain response, usually requiring an external power supply, which is difficult to meet the needs of portable and self-powered applications.
[0003] Silk fibroin (SF) is a natural high-molecular-weight protein extracted from natural silkworm silk, possessing good biocompatibility, biodegradability, and excellent mechanical properties. However, in its natural state or in regenerated silk fibroin without special treatment, the β-sheet content is low and the molecular chain arrangement is relatively disordered, resulting in weak intrinsic piezoelectric output, which is difficult to meet the needs of practical strain sensing.
[0004] Currently, improving the piezoelectric properties of silk fibroin generally faces key bottlenecks such as the strong coupling between piezoelectric activity and mechanical properties, poor biosafety, or complex processes. Of particular concern is that although silk fibroin particles have been attempted for hydrogel modification, existing technologies only treat them as inert reinforcing phases, failing to activate their piezoelectric potential. Furthermore, traditional hydrogel strain sensors mostly rely on a single resistance signal, resulting in limited resolution when facing deformations over a wide strain range. Summary of the Invention
[0005] In view of the technical problems existing in the background art, this application provides a method for preparing and applying a silk fibroin-based piezoelectric hydrogel. First, the prepared silk fibroin solution is induced to undergo treatment with anhydrous ethanol to obtain regenerated silk fibroin blocks, which are then crushed and mixed with a prepared 2-acrylamide-2-methylpropanesulfonic acid (AMPS) hydrogel precursor solution. The mixture is then cured by ultraviolet light irradiation to obtain a silk fibroin-based piezoelectric hydrogel. This method solves the technical problems of existing piezoelectric hydrogels, such as the difficulty in simultaneously achieving high voltage and soft elasticity, safety hazards of composite fillers, failure of silk fibroin particles to exert piezoelectric effect, and performance degradation of single sensors under extreme strain.
[0006] To achieve the above objectives, in a first aspect, embodiments of this application provide a method for preparing a silk fibroin-based piezoelectric hydrogel, comprising the following steps: S1. After degumming the silk, dissolve it in a solvent, heat and stir to obtain a mixed solution; the mixed solution is then subjected to dialysis, centrifugation and freeze-drying to obtain silk fibroin. S2. Prepare the silk fibroin into a silk fibroin solution, induce the regeneration of silk fibroin with anhydrous ethanol at room temperature, remove the anhydrous ethanol to obtain regenerated silk fibroin blocks, and crush the regenerated silk fibroin blocks. S3. Prepare a 2-acrylamide-2-methylpropanesulfonic acid hydrogel precursor solution; S4. The pulverized regenerated silk fibroin is added to the 2-acrylamide-2-methylpropanesulfonic acid hydrogel precursor solution, and after being mixed evenly, a composite hydrogel precursor solution is obtained. The silk fibroin-based piezoelectric hydrogel is obtained by irradiation with ultraviolet light.
[0007] Further, the silk fibroin in the solvent has a mass-volume fraction of 1% to 5%; the solvent includes a lithium bromide solution with a lithium bromide molar concentration of 9.1 to 9.5 M; the heating temperature is 58 to 62 °C; and the dialysis time is 46 to 50 h.
[0008] In some embodiments, the mass-volume fraction of silk fibroin in the lithium bromide solution is 3.5%; the molar concentration of lithium bromide in the lithium bromide solution is 9.3 M; the heating temperature is 60 °C; and the dialysis time is 48 h.
[0009] Furthermore, the silk fibroin solution contains 6%~10% w / v of silk fibroin by mass; the volume ratio of anhydrous ethanol to the silk fibroin solution is (1~3):1.
[0010] Furthermore, the particle size of the pulverized regenerated silk fibroin is 125~450μm.
[0011] Further, the method for preparing the 2-acrylamide-2-methylpropanesulfonic acid hydrogel precursor solution is as follows: N,N'-methylenebisacrylamide and phenyl-(2,4,6-trimethylbenzoyl)lithium phosphate are added sequentially to pure water and stirred in the dark until completely dissolved. Then, sodium carboxymethyl cellulose is added and stirred in the dark until uniformly mixed. Next, 2-acrylamide-2-methylpropanesulfonic acid is added and stirred in the dark until uniformly mixed. Finally, glycerol is added and stirred in the dark until uniformly mixed to obtain the 2-acrylamide-2-methylpropanesulfonic acid hydrogel precursor solution.
[0012] Further, the molar ratio of N,N'-methylenebisacrylamide, phenyl-(2,4,6-trimethylbenzoyl)lithium phosphate, and 2-acrylamide-2-methylpropanesulfonic acid is (0.005~0.007):(0.001~0.003):1.
[0013] In some embodiments, the molar ratio of N,N'-methylenebisacrylamide, phenyl-(2,4,6-trimethylbenzoyl)lithium phosphate, and 2-acrylamide-2-methylpropanesulfonic acid is (0.005~0.007):0.002:1.
[0014] Further, the mass ratio of the pure water to the 2-acrylamide-2-methylpropanesulfonic acid is (0.3~0.5):1; the mass ratio of the sodium carboxymethyl cellulose to the 2-acrylamide-2-methylpropanesulfonic acid is (0.03~0.04):1; and the mass ratio of the glycerol to the 2-acrylamide-2-methylpropanesulfonic acid is (0.9~1.1):1.
[0015] Furthermore, the mass-volume fraction of regenerated silk fibroin in the composite hydrogel precursor solution is 5%~10% w / v.
[0016] Furthermore, the ultraviolet light used for irradiation has a wavelength of 365 nm and a light intensity of 30 m / Wcm². 2 The duration is 140~160s.
[0017] In some embodiments, the wavelength of the ultraviolet light irradiated is 365 nm, and the light intensity is 30 m / Wcm. 2 The time is 150 seconds.
[0018] Secondly, embodiments of this application provide an application of silk fibroin-based piezoelectric hydrogel prepared by the preparation method described in the first aspect in a flexible strain sensor.
[0019] The beneficial technical effects of this application are as follows: 1. In the technical solution of this application, a "piezoelectric-ion" dual-modal synergistic sensing system is constructed by utilizing silk fibroin piezoelectric grains (SF) and AMPS ion-conductive network. The AMPS hydrogel, relying on its internal sulfonate groups and free ions, changes the output resistance sensing signal through ion migration paths under low and medium strain. In this application, the silk fibroin piezoelectric grains dispersed within the AMPS matrix continuously generate polarization charges under large deformation due to their highly ordered β-sheet crystals. The piezoelectric signal steadily increases with increasing deformation, effectively complementing the ion signal. After the SF and AMPS are combined, the hydrogel sensor maintains good linearity and high sensing sensitivity across the entire strain range from small to large deformations. It can also convert mechanical energy into electrical energy, possessing self-powered characteristics. Furthermore, the entire preparation process does not use toxic crosslinking agents or add non-degradable inorganic fillers, resulting in high biosafety and suitability for flexible sensing applications such as human motion monitoring and health monitoring.
[0020] 2. In the technical solution of this application, a decoupled preparation approach of "inducing crystallization first, then compounding" is adopted. This involves combining pre-induced high-β-sheet structure SF and AMPS ion-conductive hydrogels, overcoming the limitation of simultaneous β-sheet formation and gel network cross-linking in traditional in-situ induction processes. This solves the technical problem that high voltage performance inevitably leads to a sharp increase in hydrogel modulus. Even with a high level of β-sheet in silk fibroin, the AMPS hydrogel matrix can still maintain a low Young's modulus. The material exhibits excellent skin compliance, allowing it to adhere closely to uneven skin surfaces, effectively reducing noise interference during human movement, and making it more suitable for flexible skin sensing applications.
[0021] 3. In the technical solution of this application, large-particle-size silk fibroin crystals are selected as functional fillers. These crystals have a more complete internal crystalline structure and a higher degree of β-sheet orientation, enabling the material to generate a larger cooperative dipole moment when subjected to external forces, thus giving the composite hydrogel superior piezoelectric output performance. Simultaneously, the numerous amino, carboxyl, hydroxyl, and charged side chain groups on the silk fibroin polypeptide chains can form various non-covalent physical crosslinks with the sulfonic acid groups on the AMPS segments, such as hydrogen bonds, electrostatic interactions, and hydrophobic interactions, significantly increasing the crosslink density of the network and making the crosslinked structure more compact than pure AMPS. Furthermore, the flexible AMPS network is responsible for transmitting stress, while the high β-sheet rigid crystals bear and disperse the load. SF and AMPS can synergistically dissipate external forces, inhibit crack propagation, resist structural collapse, and significantly improve the tensile and compressive strength of the composite hydrogel.
[0022] 4. In the technical solution of this application, multiple non-covalent interfacial interactions are formed between SF and AMPS matrix. On the one hand, the cohesive strength of the hydrogel itself is improved. On the other hand, the abundant polar groups on the surface of SF can enhance the interfacial bonding force between the hydrogel and skin tissue, effectively improving the adhesion strength of the material. At the same time, the rigid silk fibroin grains embedded in the AMPS network can disperse the compressive stress, suppress local stress concentration, and significantly improve the burst pressure of the hydrogel.
[0023] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description
[0024] To more clearly illustrate the technical solutions of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.
[0025] Figure 1 Infrared spectra and secondary structure content diagrams of freeze-dried silk fibroin with different particle sizes and regenerated silk fibroin with different particle sizes; Figure 2 Infrared spectra and secondary structure content diagrams of different regenerated silk fibroin particles; Figure 3 For AMPS, AMPS / SF5, AMPS / SF 10 Time-scan and frequency-scan graphs of the hydrogel; Figure 4 For AMPS, AMPS / SF5, AMPS / SF 10 Tensile strength diagram of hydrogel; Figure 5 For AMPS, AMPS / SF5, AMPS / SF 10 Compressive strength diagram of hydrogel; Figure 6 For AMPS, AMPS / SF5, AMPS / SF 10 Young's modulus diagram of hydrogels; Figure 7 For AMPS, AMPS / SF5, AMPS / SF 10 Adhesion strength diagram of hydrogel; Figure 8 For AMPS, AMPS / SF5, AMPS / SF 10 Burst compression pattern of hydrogel; Figure 9 For AMPS, AMPS / SF5, AMPS / SF 10 Conductivity diagram of hydrogel; Figure 10 For AMPS, AMPS / SFNC 10 AMPS / SF 10 The piezoelectric output curve of the hydrogel; Figure 11 For AMPS, AMPS / SF 10 Sensitivity curve of hydrogel; Figure 12 This is a diagram of the solid blocks formed after drying anhydrous ethanol-induced SF solution. Figure 13 This is a gelation diagram of the mixture of lyophilized silk fibroin powder and AMPS. Figure 14 AMPS / SF under piezoelectric output 10 A schematic diagram of the internal structure of a hydrogel. Detailed Implementation
[0026] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.
[0028] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0029] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0030] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0031] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0032] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0033] Unless otherwise specified, the terms "comprising" and "including" as used in this application are open-ended. For example, "comprising" and "including" may mean that other components not listed may also be included or contained.
[0034] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.
[0035] The embodiments of this application will be described in further detail below with reference to the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to illustrate the principles of this application by way of example, but should not be used to limit the scope of this application, that is, this application is not limited to the described embodiments.
[0036] To address the technical problems of existing piezoelectric hydrogels, such as the difficulty in simultaneously achieving high piezoelectricity and soft elasticity, safety hazards associated with composite fillers, failure of silk fibroin particles to exert piezoelectric effects, and performance degradation of single sensors under extreme strain, this application provides, in a first aspect, a method for preparing a silk fibroin-based piezoelectric hydrogel, comprising the following steps: S1. After degumming the silk, dissolve it in a solvent, heat and stir to obtain a mixed solution; perform dialysis, centrifugation and freeze-drying on the mixed solution in sequence to obtain silk fibroin. S2. Prepare a silk fibroin solution, induce the regeneration of silk fibroin with anhydrous ethanol at room temperature, remove the anhydrous ethanol to obtain regenerated silk fibroin blocks, and crush the regenerated silk fibroin blocks. S3. Prepare a 2-acrylamide-2-methylpropanesulfonic acid hydrogel precursor solution; S4. The pulverized regenerated silk fibroin is added to the 2-acrylamide-2-methylpropanesulfonic acid hydrogel precursor solution and mixed evenly to obtain a composite hydrogel precursor solution. The silk fibroin-based piezoelectric hydrogel is obtained by irradiation with ultraviolet light.
[0037] In the technical solution of this application, high β-sheet silk fibroin crystals (SF) obtained by pre-induced crystallization and pulverization with ethanol are combined with AMPS hydrogel precursors to achieve an effective combination of piezoelectric function and ion-conductive matrix. This composite method introduces SF as a piezoelectric functional filler into the AMPS network, forming multiple non-covalent interactions through hydrogen bonding, electrostatics, and hydrophobic interactions. It retains the advantages of low modulus and ion conductivity of the AMPS matrix while introducing the piezoelectric properties of silk fibroin, thus constructing a piezoelectric-ion synergistic response system. At the same time, the composite can also simultaneously improve the mechanical properties, tissue adhesion, and pressure resistance of the hydrogel, avoiding the problem of mutual restriction between piezoelectric performance and modulus in in-situ induction process. It does not require the introduction of inorganic fillers and can obtain a silk fibroin-based piezoelectric hydrogel with self-powered, wide strain range, high sensitivity, and good biocompatibility.
[0038] In some embodiments, the mass-volume fraction of silk fibroin in the solvent is 1% to 5%; the solvent includes a lithium bromide solution with a lithium bromide molar concentration of 9.1 to 9.5 M; the heating temperature is 58 to 62°C; and the dialysis time is 46 to 50 hours.
[0039] In this embodiment, the silk can be fully dissolved, the high-temperature degradation of silk fibroin can be inhibited, the residual impurities of lithium bromide can be fully removed, the quality of the raw solution can be guaranteed, and qualified raw materials can be provided for the subsequent preparation of silk fibroin crystals and composite with AMPS.
[0040] In one specific embodiment, the mass-volume fraction of silk fibroin in the lithium bromide solution is 3.5%; the molar concentration of lithium bromide in the lithium bromide solution is 9.3M; the heating temperature is 60°C; and the dialysis time is 48 hours.
[0041] With this setting, the silk is completely dissolved under these optimal parameters, the silk fibroin molecular chains are intact, and lithium bromide salt impurities are removed more thoroughly, resulting in a silk fibroin stock solution with excellent uniformity. Subsequently, when induced by anhydrous ethanol, it is easier to generate a regularly arranged β-sheet crystal form, resulting in SF with higher piezoelectric activity.
[0042] In some embodiments, the mass-volume fraction of silk fibroin in the silk fibroin solution is 6%~10% w / v; the volume ratio of anhydrous ethanol to silk fibroin solution is (1~3):1.
[0043] In this embodiment, the rearrangement of silk fibroin molecular chains can be effectively promoted to form a β-sheet crystal structure, thereby obtaining regenerated silk fibroin blocks with excellent piezoelectric activity. The blocks have good crushing and processing performance, which facilitates the subsequent preparation of micro and nano crystals and can be directly used for composite with AMPS hydrogel.
[0044] In some embodiments, the particle size of the pulverized regenerated silk fibroin is 125~450μm.
[0045] In this embodiment, the regenerated silk fibroin crystals within this particle size range possess a more complete β-sheet crystalline region structure, which can generate a stronger piezoelectric response. At the same time, the crystals can be uniformly dispersed in the AMPS hydrogel precursor, ensuring sufficient contact between the two phases and facilitating the formation of abundant non-covalent interactions. This effectively plays a role in physical crosslinking and stress dispersion in the composite hydrogel, synergistically improving the mechanical, adhesive, and sensing piezoelectric properties of the composite hydrogel.
[0046] In some embodiments, the steps for preparing the 2-acrylamide-2-methylpropanesulfonic acid hydrogel precursor solution are as follows: N,N'-methylenebisacrylamide and phenyl-(2,4,6-trimethylbenzoyl)lithium phosphate are added sequentially to pure water and stirred in the dark until completely dissolved. Then, sodium carboxymethyl cellulose is added and stirred in the dark until homogeneous. Next, 2-acrylamide-2-methylpropanesulfonic acid is added and stirred in the dark until homogeneous. Finally, glycerol is added and stirred in the dark until homogeneous to obtain the 2-acrylamide-2-methylpropanesulfonic acid hydrogel precursor solution.
[0047] In this embodiment, the components can be fully dissolved and mixed to avoid premature photodegradation failure of the photoinitiator; the addition of sodium carboxymethyl cellulose and glycerol can improve the compatibility and water retention of the system, and can form a good interface with the subsequently added silk fibroin crystals to obtain a uniform and stable AMPS precursor, which ensures subsequent UV curing and molding, and is conducive to obtaining a composite hydrogel matrix with uniform structure and good ionic conductivity.
[0048] In some embodiments, the molar ratio of N,N'-methylenebisacrylamide, phenyl-(2,4,6-trimethylbenzoyl)lithium phosphate, and 2-acrylamide-2-methylpropanesulfonic acid is (0.005~0.007):(0.001~0.003):1.
[0049] In this embodiment, the molar ratio can control the relative amounts of crosslinking agent and photoinitiator, ensuring the photopolymerization reaction proceeds smoothly and forming a moderately crosslinked AMPS three-dimensional network. This network can maintain sufficient ion transport channels in the matrix, retain good ion conductivity, and also possess suitable network toughness. When combined with silk fibroin grains, it can fully exert its stress transfer function.
[0050] In some embodiments, the mass ratio of pure water to 2-acrylamide-2-methylpropanesulfonic acid is (0.3~0.5):1; the mass ratio of sodium carboxymethyl cellulose to 2-acrylamide-2-methylpropanesulfonic acid is (0.03~0.04):1; and the mass ratio of glycerol to 2-acrylamide-2-methylpropanesulfonic acid is (0.9~1.1):1.
[0051] In this embodiment, the mass ratio range ensures that each component is fully dissolved, resulting in a precursor solution with suitable flowability; water provides a medium for ion transport, sodium carboxymethyl cellulose optimizes the system viscosity and improves the interfacial compatibility with silk fibroin grains, and glycerol imparts excellent water retention and anti-drying ability to the hydrogel; after composite, it can maintain a suitable network structure of the AMPS matrix, taking into account ion conductivity and flexible mechanical properties, ensuring the overall adhesion performance of the hydrogel after composite with silk fibroin grains and the stability of piezoelectric-ion synergistic sensing output.
[0052] In some embodiments, the mass-volume fraction of regenerated silk fibroin in the composite hydrogel precursor solution is 5%~10% w / v.
[0053] In this embodiment, the regenerated silk fibroin crystals can be uniformly dispersed in the AMPS precursor at this addition amount, and the crystals and hydrogel matrix can fully form non-covalent interactions such as hydrogen bonds and electrostatics, effectively exerting physical cross-linking and piezoelectric functions.
[0054] In some embodiments, the wavelength of the ultraviolet light irradiated is 365 nm, and the light intensity is 30 m / Wcm. 2 The duration is 140~160s.
[0055] In this embodiment, suitable ultraviolet light conditions can ensure that the photoinitiator is fully excited, enabling the composite precursor to achieve sufficient and appropriate photopolymerization and curing, forming a hydrogel with a complete and uniform structure. This facilitates stress transfer between silk fibroin grains and the AMPS matrix, ensuring the mechanical and sensing properties of the composite hydrogel.
[0056] In one specific embodiment, the ultraviolet light used for irradiation has a wavelength of 365 nm and a light intensity of 30 m / Wcm. 2 The time is 150 seconds.
[0057] With this setup and the preferred illumination conditions, the photopolymerization reaction is fully controllable, the cross-linking network of the composite hydrogel is more uniform, the silk fibroin piezoelectric grains can be stably embedded in the AMPS network, and the two-phase interface bonding effect is good.
[0058] Secondly, this application also provides an application of the silk fibroin-based piezoelectric hydrogel prepared by the preparation method of the first aspect in a flexible strain sensor.
[0059] The following are some specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.
[0060] I. Preparation Method Example 1 This embodiment provides a method for preparing a silk fibroin-based piezoelectric hydrogel, including the following steps: S1. Take 5g of mulberry silk fabric and boil it in 1000mL of 0.5% w / v sodium carbonate aqueous solution for 30min. Wash with plenty of deionized water to remove sericin. Repeat the boiling-washing operation twice and dry in an oven at 60℃ for 4h to obtain dried degummed mulberry silk fabric. Take 0.7g of degummed mulberry silk fabric, cut it into pieces, dissolve it in 20mL of 9.3M LiBr solution, and stir in an oil bath at 60℃ for 3h to obtain a silk fibroin / LiBr mixed solution. Put the mixed solution into a dialysis bag with a molecular weight cutoff of 8000-14000Da and dialyze it with deionized water for 48h, changing the deionized water every 2h. After dialysis, centrifuge at 10000rpm for 20min to remove insoluble precipitate, collect the supernatant, freeze-dry the supernatant to obtain freeze-dried silk fibroin, and store it at 4℃ for later use. S2. Prepare a 10% w / v silk fibroin aqueous solution by lyophilizing silk fibroin; place 5 mL of silk fibroin solution in a petri dish, add anhydrous ethanol at a volume ratio of 3:1 to silk fibroin solution, induce at room temperature for 1 h, remove anhydrous ethanol in a 60℃ oven to obtain regenerated silk fibroin blocks; crush the blocks separately, select regenerated silk fibroin particles with a particle size of 125-450 μm as fillers, and denote them as 10%-3:1-M; S3. Weigh 0.03g N,N'-methylenebisacrylamide (MBAA) and 0.02g phenyl-(2,4,6-trimethylbenzoyl)lithium phosphate (LAP), add them to 2.5g pure water and stir in the dark for 3h; then add 0.2g sodium carboxymethyl cellulose, 6.08g AMPS and 6.3g glycerol in sequence, stirring in the dark until the mixture is homogeneous after each addition to obtain an AMPS hydrogel precursor solution; S4. Weigh 0.3g of the regenerated silk fibroin particles (10%-3:1-M) obtained in step S2, and add them to 3mL of AMPS hydrogel precursor solution to make the mass-volume fraction of regenerated silk fibroin in the composite hydrogel precursor solution 10% w / v (volume change is negligible). Stir and mix well to obtain the composite hydrogel precursor solution. Inject the composite precursor solution into a silicone sheet mold and apply light at a wavelength of 365nm and an intensity of 30mW / cm². 2 After irradiation with ultraviolet light for 150 seconds, a silk fibroin-based piezoelectric hydrogel (denoted as AMPS / SF) was obtained. 10 ).
[0061] Example 2 This embodiment provides a method for preparing a silk fibroin-based piezoelectric hydrogel. Compared with Example 1, the only difference is that in step S4, 0.15g of regenerated silk fibroin particles (10%-3:1-M) are weighed to make the mass-volume fraction of regenerated silk fibroin in the composite hydrogel precursor solution 5% w / v (volume change is negligible). Other experimental parameters and conditions are basically the same as in Example 1, and will not be repeated here.
[0062] The silk fibroin-based piezoelectric hydrogel obtained in this embodiment is designated as AMPS / SF5.
[0063] Example 3 This embodiment provides a method for preparing regenerated silk fibroin particles. Compared with the regenerated silk fibroin particles prepared in step S2 of Example 1, the only difference is that anhydrous ethanol is added at a volume ratio of 1:1 to silk fibroin solution. The resulting regenerated silk fibroin particles are denoted as 10%-1:1-M. Other experimental parameters and conditions are basically the same as those for the regenerated silk fibroin particles prepared in step S2 of Example 1, and will not be repeated here.
[0064] Example 4 This embodiment provides a method for preparing regenerated silk fibroin particles. Compared with the regenerated silk fibroin particles prepared in step S2 of Example 1, the only difference is that the freeze-dried silk fibroin is prepared into a 6% w / v silk fibroin aqueous solution, and the volume ratio of anhydrous ethanol to silk fibroin solution is 3:1. The resulting regenerated silk fibroin particles are denoted as 6%-3:1-M. Other experimental parameters and conditions are basically the same as those for the regenerated silk fibroin particles prepared in step S2 of Example 1, and will not be repeated here.
[0065] Example 5 This embodiment provides a method for preparing regenerated silk fibroin particles. Compared with Example 4, the only difference is that the volume ratio of anhydrous ethanol to silk fibroin solution is 1:1, and the resulting regenerated silk fibroin particles are denoted as 6%-1:1-M. Other experimental parameters and conditions are basically the same as in Example 4, and will not be repeated here.
[0066] Comparative Example 1 This comparative example provides a method for preparing a hydrogel. After preparing the AMPS hydrogel precursor solution according to step S3 of Example 1, the precursor solution is injected into a silicone sheet mold and placed under light with a wavelength of 365 nm and an intensity of 30 mW / cm². 2 Irradiate with ultraviolet light for 120 seconds to obtain a shaped hydrogel, denoted as AMPS.
[0067] Comparative Example 2 This comparative example provides a method for preparing freeze-dried silk fibroin particles. After preparing freeze-dried silk fibroin according to step S1 of Example 1, it is pulverized to a particle size of 125-450 μm, and the resulting freeze-dried silk fibroin particles are denoted as SFNC-M.
[0068] Comparative Example 3 This comparative example provides a method for preparing freeze-dried silk fibroin particles. Compared with Comparative Example 2, the only difference is that the freeze-dried silk fibroin is pulverized to a particle size of less than 75 μm, and the resulting freeze-dried silk fibroin particles are denoted as SFNC-S.
[0069] Comparative Example 4 This comparative example provides a method for preparing a hydrogel. The SFNC-M obtained in Comparative Example 2 is combined with the AMPS hydrogel precursor solution obtained in step S3 of Example 1, such that the mass-volume fraction of SFNC-M in the composite hydrogel precursor solution is 10% w / v, with negligible volume change. The resulting hydrogel is denoted as AMPS / SFNC. 10 .
[0070] Comparative Example 5 This comparative example provides a method for preparing regenerated silk fibroin particles. Compared with Example 3, the only difference is that the regenerated silk fibroin block is crushed into particles with a particle size of less than 75 μm. The resulting regenerated silk fibroin particles are denoted as 10%-1:1-S. Other experimental parameters and conditions are basically the same as those in Example 3, and will not be repeated here.
[0071] II. Testing Methods 1. Using a NICOLET iS50 infrared absorption spectrometer, at 32cm -1 Scanned 64 times at a resolution of 4000-400cm. -1 Infrared spectroscopy and secondary structure (β-sheet) characterization tests were performed on silk fibroin samples with different particle sizes and under different induction conditions.
[0072] 2. A Discovery HR 20 high-speed rotating rheometer was used to analyze AMPS, AMPS / SF5, and AMPS / SF5. 10 Hydrogels were subjected to time-scan (strain at 1% and frequency at 1 Hz) and frequency-scan (strain at 1%) tests.
[0073] 3. An Instron 5943 kJ / m² capacity testing machine was used to test AMPS, AMPS / SF5, and AMPS / SF5. 10 The hydrogel was tested for tensile strength, compressive strength, Young's modulus, and adhesive strength.
[0074] 4. Adopt the ATSM F2392-24 standard for AMPS, AMPS / SF5, and AMPS / SF 10 Hydrogel burst pressure test.
[0075] 5. Using a CHI600F electrochemical workstation, AMPS, AMPS / SF5, and AMPS / SF5 were analyzed. 10 Hydrogels were tested for their ionic conductivity.
[0076] 6. Using the compression mode of a universal tensile testing machine and a Keithley 2450 digital source meter, AMPS, AMPS / SF5, and AMPS / SF5 were tested. 10 Test of piezoelectric output voltage of hydrogel under different external forces.
[0077] 7. Using an Instron 594300000-ton capacity testing machine and a Keithley 2450 digital source meter, AMPS and AMPS / SF were tested. 10 Strain sensitivity testing was performed on the hydrogel.
[0078] III. Test Result Analysis Infrared spectroscopy results of lyophilized silk fibroin with different particle sizes and regenerated silk fibroin with different particle sizes ranging from 10% to 1:1 are as follows: Figure 1 As shown, the secondary structure content of different silk fibroin proteins was calculated by deconvolution, and the results are as follows. Figure 1 As shown, SFNC-S is the freeze-dried silk fibroin particles prepared in Comparative Example 3, SFNC-M is the freeze-dried silk fibroin particles prepared in Comparative Example 2, 10%-1:1-S is the regenerated silk fibroin particles prepared in Comparative Example 5, and 10%-1:1-M is the regenerated silk fibroin particles prepared in Example 3.
[0079] Depend on Figure 1 It can be seen that in the infrared spectrum, 1625 cm⁻¹ -1 1545cm -1 and 1265cm -1The absorption peaks at these locations correspond to the characteristic peaks of the β-sheet structures in the amide I (C=O stretching), amide II (NH bending / CN stretching), and amide III (CN stretching / NH bending) regions of silk fibroin, respectively. The secondary structure content of different silk fibroin proteins was calculated by deconvolution from the infrared spectra. It was found that the β-sheet content of regenerated silk fibroin induced by anhydrous ethanol in 10%-1:1-M and 10%-1:1-S (56.5% and 48.4%, respectively) was higher than that of lyophilized silk fibroin SFNC-M and SFNC-S without anhydrous ethanol induction (42.1% and 38.5%, respectively). Further comparison showed that the β-sheet content of 10%-1:1-M (56.5%) was higher than that of 10%-1:1-S (48.4%), and the β-sheet content of SFNC-M (42.1%) was higher than that of SFNC-S (38.5%). This indicates that anhydrous ethanol successfully induced the formation of β-sheets, and that after physical crushing and sieving, the content of β-sheets with larger particle sizes was high under the same conditions.
[0080] Fourier transform infrared spectroscopy was performed on different regenerated silk fibroin particles, and the results are as follows: Figure 2 As shown, the secondary structure content of different silk fibroin proteins was calculated by deconvolution, and the results are as follows. Figure 2 As shown, 6%-1:1-M is the regenerated silk fibroin particles prepared in Example 5, 6%-3:1-M is the regenerated silk fibroin particles prepared in Example 4, 10%-1:1-M is the regenerated silk fibroin particles prepared in Example 3, and 10%-3:1-M is the regenerated silk fibroin particles prepared in step S2 of Example 1.
[0081] Depend on Figure 2 It can be seen that in the infrared spectrum, 1625 cm⁻¹ -1 1545cm -1 and 1265cm -1 The absorption peaks at these locations correspond to the characteristic peaks of the β-sheet structures in the amide I (C=O stretching), amide II (NH bending / CN stretching), and amide III (CN stretching / NH bending) regions of silk fibroin, respectively. Calculations of the secondary structure content of different silk fibroin proteins using deconvolution from the infrared spectra show that the β-sheet content of 10% silk fibroin particles (62.5% and 56.5%, respectively) is higher than that of 6% silk fibroin particles (55.2% and 53.5%, respectively). Further comparison reveals that the β-sheet content of 10%-3:1-M (62.5%) is higher than that of 10%-1:1-M (56.5%), and the β-sheet content of 6%-3:1-M (55.2%) is higher than that of 6%-1:1-M (53.5%). This indicates that higher concentrations of silk fibroin solution and a higher proportion of anhydrous ethanol induce higher β-sheet content. Combined with… Figure 1 and Figure 2It can be seen that the 10%-3:1-M ratio has the highest β-sheet content, which is the optimal SF ratio for subsequent composite with hydrogel.
[0082] For AMPS, AMPS / SF5, AMPS / SF 10 The hydrogel underwent rheological testing, and the results are as follows: Figure 3 As shown, AMPS is the hydrogel prepared in Comparative Example 1, and AMPS / SF5 is the silk fibroin-based piezoelectric hydrogel prepared in Example 2. 10 The silk fibroin-based piezoelectric hydrogel prepared in Example 1.
[0083] Depend on Figure 3 It can be seen that AMPS, AMPS / SF5 and AMPS / SF 10 All systems gelled rapidly, with the storage modulus / loss modulus intersection (gel point) appearing within 10 s, followed by stable gel formation within 60 s. The addition of 5% or 10% SF did not significantly alter the gel formation time of the AMPS system, indicating that the addition of SF mainly participates in network enhancement and interfacial synergy without interfering with AMPS gel formation. In the frequency scan diagram, AMPS / SF5 and AMPS / SF... 10 The energy storage modulus (G') of both is higher than that of AMPS, and AMPS / SF 10 The storage modulus (G') is higher than that of AMPS / SF5 because SF is a protein polypeptide chain containing abundant amino, carboxyl, hydroxyl and polar charged side chain groups. It can be embedded in the AMPS network and entangled with the AMPS chain through hydrogen bonding, electrostatic interaction, hydrophobic interaction, etc., which is equivalent to increasing the physical cross-linking points and inter-chain constraints, thereby increasing the storage modulus (G') and making the gel more elastic.
[0084] For AMPS, AMPS / SF5, AMPS / SF 10 The hydrogel underwent tensile property testing, and the results are as follows: Figure 4 As shown, AMPS was prepared in Comparative Example 1, and AMPS / SF5 was prepared in Example 2. 10 It was prepared as in Example 1.
[0085] Depend on Figure 4 It can be seen that AMPS / SF5 and AMPS / SF 10 The tensile strength of all of them is greater than that of AMPS, and AMPS / SF 10The tensile strength of the SF5 is greater than that of AMPS / SF5. This indicates that the various physical interactions formed between SF and AMPS increase the crosslinking density of the network. The β-sheet grains, acting as rigid reinforcing domains and physical crosslinking points in the hydrogel network, not only increase the crosslinking density but also improve network uniformity and energy dissipation. During stretching, the AMPS network provides a flexible matrix for the SF grains, enabling effective load transfer between the soft segments and the rigid β-sheet grains. Therefore, with increasing SF content, the interaction between the β-sheet grains and the interface increases, strengthening network constraint and resulting in higher tensile strength.
[0086] For AMPS, AMPS / SF5, AMPS / SF 10 The hydrogel underwent compression performance testing, and the results are as follows: Figure 5 As shown, AMPS is the hydrogel prepared in Comparative Example 1, and AMPS / SF5 is the silk fibroin-based piezoelectric hydrogel prepared in Example 2. 10 The silk fibroin-based piezoelectric hydrogel prepared in Example 1.
[0087] Depend on Figure 5 It can be seen that AMPS / SF 10 The compressive strength of the SF5 was significantly higher than that of AMPS and AMPS / SF5, while there was no significant difference between AMPS / SF5 and pure AMPS (NS), indicating that only at higher SF contents can the introduction of silk fibroin effectively improve the compressive strength of the hydrogel. The high β-sheet SF grains induced by anhydrous ethanol exhibit strong rigidity and ordered stacking characteristics, and can be embedded in the AMPS polyelectrolyte network as physical crosslinking points and rigidity-enhancing domains. Multiple non-covalent interactions between SF and AMPS help fix the network structure, restrict polymer chain slippage, and promote stress transfer and dissipation between the flexible AMPS matrix and the rigid β-sheet crystalline region during compression. When the SF content is increased to AMPS / SF5... 10 At this time, the β-sheet grain density and the degree of interfacial synergistic cross-linking reach the enhancement threshold, making the network nodes more compact, the structure more uniform, and the compressive strength significantly improved.
[0088] For AMPS, AMPS / SF5, AMPS / SF 10 The hydrogel was subjected to Young's modulus testing, and the results are as follows: Figure 6 As shown, AMPS is the hydrogel prepared in Comparative Example 1, and AMPS / SF5 is the silk fibroin-based piezoelectric hydrogel prepared in Example 2. 10 The silk fibroin-based piezoelectric hydrogel prepared in Example 1.
[0089] Depend on Figure 6 It can be seen that AMPS / SF5 and AMPS / SF10 The Young's modulus of SF is higher than that of AMPS, primarily because the addition of SF makes the hydrogel network denser, strengthens inter-chain constraints, and increases physical cross-linking, thereby improving its resistance to deformation under tensile / compressive stress. Although the addition of high-β-sheet silk fibroin leads to an increase in Young's modulus, it is only 2.7 ± 0.05 kPa, still suitable for skin strain sensing. This also indicates that the strategy of first inducing high-β-crystallinity and then compounding it with hydrogel satisfies both the high β-sheet requirement of silk fibroin and the low modulus requirement of hydrogel, allowing it to adhere to the skin for strain sensing.
[0090] For AMPS, AMPS / SF5, AMPS / SF 10 The hydrogel underwent adhesion strength testing, and the results are as follows: Figure 7 As shown, AMPS is the hydrogel prepared in Comparative Example 1, and AMPS / SF5 is the silk fibroin-based piezoelectric hydrogel prepared in Example 2. 10 The silk fibroin-based piezoelectric hydrogel prepared in Example 1.
[0091] Depend on Figure 7 It can be seen that AMPS / SF5, AMPS / SF 10 The adhesion strength of both AMPS / SF5 and AMPS / SF5 is higher than that of pure AMPS. 10 The lack of significant differences between the samples indicates that the introduction of anhydrous ethanol-induced high β-sheet silk fibroin grains can effectively improve the adhesion properties of the hydrogel to the substrate or tissue interface. Similarly, the multiple non-covalent interfacial interactions formed between SF and AMPS, along with the continuous hydration matrix and surface wetting contact environment provided by the AMPS polyelectrolyte network, allow the SF grains to act more effectively on the substrate or tissue surface. The high β-sheet SF crystalline regions also enhance network cohesive stability and interfacial stress transfer, reducing interfacial failure during debonding.
[0092] For AMPS, AMPS / SF5, AMPS / SF 10 The hydrogel underwent burst pressure testing, and the results are as follows: Figure 8 As shown, AMPS is the hydrogel prepared in Comparative Example 1, and AMPS / SF5 is the silk fibroin-based piezoelectric hydrogel prepared in Example 2. 10 The silk fibroin-based piezoelectric hydrogel prepared in Example 1.
[0093] Depend on Figure 8 It can be seen that AMPS / SF5, AMPS / SF 10The burst pressure of the composite hydrogel is significantly higher than that of AMPS. Silk fibroin grains act as rigid physical cross-linking points, and the interfacial interactions between the sulfonic acid and amide groups on the AMPS segments and the SF groups further endow the composite hydrogel with strong compressive strength. Under pressure, the rigid grains act as the main load-bearing structure, transmitting stress, while the flexible AMPS segments dissipate energy through interfacial interactions and orientation. The strong interfacial bonding between the two effectively hinders the overall slippage of the molecular chains and network deformation, significantly reducing local stress concentration.
[0094] For AMPS, AMPS / SF5, AMPS / SF 10 The conductivity of the hydrogel was tested, and the results are as follows: Figure 9 As shown, AMPS is the hydrogel prepared in Comparative Example 1, and AMPS / SF5 is the silk fibroin-based piezoelectric hydrogel prepared in Example 2. 10 The silk fibroin-based piezoelectric hydrogel prepared in Example 1.
[0095] Depend on Figure 9 It can be seen that the conductivity of AMPS is higher than that of AMPS / SF5 and AMPS / SF5. 10 The conductivity of the composite hydrogel is lower than that of pure AMPS. This is attributed to the fact that the silk fibroin grains, which are uniformly dispersed in the network, act as a rigid dispersed phase and form steric hindrance in the ion transport channels, thus hindering ion migration to some extent.
[0096] For AMPS, AMPS / SFNC 10 AMPS / SF 10 The hydrogel was subjected to piezoelectric output testing, and the results are as follows: Figure 10 As shown, AMPS is the hydrogel prepared in Comparative Example 1, AMPS / SFNC 10 The hydrogel prepared for Comparative Example 4, AMPS / SF 10 The silk fibroin-based piezoelectric hydrogel prepared in Example 1.
[0097] Depend on Figure 10 It can be seen that within the external force range of 0.5-2.5N, AMPS / SF 10 The output voltages are significantly higher than those of AMPS and AMPS / SFNC. 10 AMPS / SFNC 10 The output voltage of AMPS is lower than that of pure AMPS within the same external force range, and the output voltage of AMPS tends to saturate at 1.0N. This is because AMPS / SFNC 10The system incorporates silk fibroin particles (SFNC-M) that have not been induced by anhydrous ethanol. Their secondary structure is dominated by random coils and α-helices, with extremely low β-sheet content, exhibiting almost no piezoelectric activity. Therefore, their output voltage originates solely from the electrical signal contribution caused by ion migration within the AMPS matrix. More importantly, the disordered silk fibroin molecular chains in SFNC-M exhibit high structural instability. During compounding with the AMPS prepolymer solution and subsequent polymerization, strong non-covalent interactions occur between the polar groups on their molecular chains and the AMPS polymer chains, inducing the in-situ formation of a double-network cross-linked structure between SFNC-M and the AMPS matrix. This double-network structure significantly shortens or blocks the migration channels of free ions within the AMPS matrix, resulting in a significant weakening of the ionic conductivity contribution. Therefore, the AMPS / SFNC... 10 The output voltage of the AMPS / SF4 hydrogel was lower than that of pure AMPS throughout the entire range of external forces tested. For pure AMPS hydrogels, the output voltage depends entirely on the electrical signal induced by changes in the migration paths of free ions under external force. However, the total number of free ions that can participate in directional migration in AMPS hydrogels is limited. When the external force increases to a certain level (approximately 1.0 N), the electrical signal contributed by ion migration reaches saturation, and the output voltage no longer increases significantly with further increases in external force. 10 The system incorporates silk fibroin (SF) crystals pre-induced by anhydrous ethanol, forming a highly ordered β-sheet crystal structure with excellent intrinsic piezoelectric activity. Under external force, the SF crystals undergo deformation polarization, generating a stable piezoelectric voltage output. Therefore, AMPS / SF... 10 The output voltage of AMPS / SF originates from the synergistic increase of ion migration electrical signals and piezoelectric electrical signals. Ion migration in the matrix provides the basic resistive response, while uniformly dispersed SF continuously generates linearly enhanced piezoelectric charges under large external forces. Due to the compensation and enhancement effect of the piezoelectric effect of silk fibroin grains, AMPS / SF... 10 This effectively overcomes the output saturation bottleneck caused by the limited total amount of free ions in pure AMPS, AMPS / SF 10 The output voltage (150-270mV) within the external force range of 0.5-2.5N is significantly better than that of AMPS (120-150mV) and AMPS / SFNC. 10 (38-96mV), demonstrating significant advantages in wide external force range and high responsiveness.
[0098] For AMPS, AMPS / SF 10 Strain sensitivity tests were performed on the hydrogel, and the results are as follows: Figure 11 As shown, AMPS is the hydrogel prepared in Comparative Example 1, and AMPS / SF 10 The silk fibroin-based piezoelectric hydrogel prepared in Example 1.
[0099] Depend on Figure 11 It can be seen that AMPS / SF in the small strain range of 0-50% 10 The strain factor (GF) of AMPS is slightly smaller than that of AMPS; while under large strain conditions of 50-250%, AMPS / SF 10 The GF of AMPS is far greater than that of AMPS. Under small strain conditions, the sensing response mainly depends on the resistance change caused by the directional migration of free ions along the electric field direction in the AMPS hydrogel matrix. At this time, the external force is small, so the deformation of the silk fibroin crystals themselves is small, and their piezoelectric output is weak; at the same time, the silk fibroin crystals uniformly dispersed in the network, as a rigid dispersed phase, will form steric hindrance in the ion transport channels, which will prolong the ion migration path and increase the transport resistance to a certain extent. The result of the combined effect of the two is that AMPS / SF 10 Within a small strain range, the contribution of ion conductivity is weaker than that of pure AMPS, hence the GF is slightly lower. However, the resistivity change rate of ion-conducting hydrogels has an upper limit, meaning the total number of free ions that can participate in directional migration within the hydrogel is limited. When network deformation continues to increase to a higher strain range, the ion transport channels undergo severe compression and distortion, leading to a sharp decline in the long-distance migration ability of ions, and the resistivity change rate tends to saturate. Consequently, the GF growth rate of pure AMPS slows down significantly. For AMPS / SF... 10 In this system, under high strain conditions, the highly β-folded silk fibroin grains undergo significant mechanical deformation, resulting in lattice polarization and a continuously increasing piezoelectric charge output that enhances with increasing deformation. This piezoelectric signal serves as an independent supplementary signal channel, forming a synergistic output with the ion resistance signal. Furthermore, the built-in electric field generated by the silk fibroin grains may modulate ion migration behavior, thus mitigating signal attenuation caused by ion channel deformation to some extent. Based on this, AMPS / SF... 10 It can still maintain a high rate of change of resistance in a large strain range, with its GF (2.789) significantly exceeding that of pure AMPS (1.955), demonstrating excellent wide strain range sensing performance. This indicates that the introduction of silk fibroin piezoelectric grains not only endows the material with self-powered characteristics, but also effectively compensates for the performance defects of traditional ion-conductive hydrogels under large strain through the piezoelectric-ion synergistic mechanism, thus achieving a high sensitivity response over a wide strain range.
[0100] Macroscopic morphology observation was performed on the samples dried after induced drying with anhydrous ethanol-induced SF solution. The results are as follows: Figure 12 As shown.
[0101] Depend on Figure 12 It can be seen that after induction with anhydrous ethanol and drying, a hard regenerated silk fibroin solid block can be obtained. This block can be further crushed and sieved to prepare piezoelectric silk fibroin crystal filler.
[0102] The macroscopic morphology of the mixed system of SFNC-M and AMPS precursors was observed, and the results are as follows: Figure 13 As shown.
[0103] Depend on Figure 13 It can be seen that when lyophilized silk fibroin powder (SFNC-M) without ethanol induction is added to the AMPS system and stirred, it can quickly gel. The disordered conformation of the lyophilized silk fibroin will have strong non-covalent interactions with the AMPS matrix, forming a cross-linked gel network in situ.
[0104] Depend on Figure 14 AMPS / SF under piezoelectric output 10 The internal structure diagram of the hydrogel shows that sodium carboxymethyl cellulose (CMC) and AMPS chains are entangled to form a semi-interpenetrating network, with regenerated silk fibroin particles dispersed within the network. Glycerol provides moisture retention and maintains the ion transport environment. Under external force, the hydrogel network undergoes compressive deformation, and the directional migration of internal free ions, along with changes in the dipole moment of the regenerated silk fibroin particles, generates an output voltage. Combined with piezoelectric output test results, it can be seen that AMPS / SF... 10 It breaks through the output saturation bottleneck of pure AMPS, and the output voltage exhibits significant advantages of wide external force range and high responsiveness within the external force range of 0.5-2.5N.
[0105] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing embodiments by combining some of the constituent elements, are also included in the scope of this application without departing from the spirit of this application.
[0106] Furthermore, although this application has been described with reference to preferred embodiments, various modifications can be made thereto and components can be replaced with equivalents without departing from the scope of this application. In particular, the technical features mentioned in the various embodiments can be combined in any manner, provided there is no structural conflict. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A method for preparing a silk fibroin-based piezoelectric hydrogel, characterized in that, Includes the following steps: S1. After degumming the silk, dissolve it in a solvent, heat and stir to obtain a mixed solution; The mixed solution was subjected to dialysis, centrifugation, and lyophilization in sequence to obtain silk fibroin. S2. Prepare the silk fibroin into a silk fibroin solution, induce the regeneration of silk fibroin with anhydrous ethanol at room temperature, remove the anhydrous ethanol to obtain regenerated silk fibroin blocks, and crush the regenerated silk fibroin blocks. S3. Prepare a 2-acrylamide-2-methylpropanesulfonic acid hydrogel precursor solution; S4. The pulverized regenerated silk fibroin is added to the 2-acrylamide-2-methylpropanesulfonic acid hydrogel precursor solution, and after being mixed evenly, a composite hydrogel precursor solution is obtained. The silk fibroin-based piezoelectric hydrogel is obtained by irradiation with ultraviolet light.
2. The method for preparing a silk fibroin-based piezoelectric hydrogel according to claim 1, characterized in that, In step S1, the silk fibroin has a mass-volume fraction of 1% to 5% in the solvent; the solvent includes a lithium bromide solution with a lithium bromide molar concentration of 9.1 to 9.5 M; the heating temperature is 58 to 62°C; and the dialysis time is 46 to 50 hours.
3. The method for preparing a silk fibroin-based piezoelectric hydrogel according to claim 1, characterized in that, In step S2, the mass-volume fraction of silk fibroin in the silk fibroin solution is 6%~10% w / v; the volume ratio of anhydrous ethanol to the silk fibroin solution is (1~3):
1.
4. The method for preparing a silk fibroin-based piezoelectric hydrogel according to claim 1, characterized in that, In step S2, the particle size of the pulverized regenerated silk fibroin is 125~450μm.
5. The method for preparing a silk fibroin-based piezoelectric hydrogel according to claim 1, characterized in that, In step S3, the method for preparing the 2-acrylamide-2-methylpropanesulfonic acid hydrogel precursor solution is as follows: N,N'-methylenebisacrylamide and phenyl-(2,4,6-trimethylbenzoyl)lithium phosphate are added sequentially to pure water and stirred in the dark until completely dissolved. Then, sodium carboxymethyl cellulose is added and stirred in the dark until uniformly mixed. Next, 2-acrylamide-2-methylpropanesulfonic acid is added and stirred in the dark until uniformly mixed. Finally, glycerol is added and stirred in the dark until uniformly mixed to obtain the 2-acrylamide-2-methylpropanesulfonic acid hydrogel precursor solution.
6. The method for preparing a silk fibroin-based piezoelectric hydrogel according to claim 5, characterized in that, The molar ratio of N,N'-methylenebisacrylamide, phenyl-(2,4,6-trimethylbenzoyl)lithium phosphate, and 2-acrylamide-2-methylpropanesulfonic acid is (0.005~0.007):(0.001~0.003):
1.
7. The method for preparing a silk fibroin-based piezoelectric hydrogel according to claim 1, characterized in that, In step S3, the mass ratio of pure water to 2-acrylamide-2-methylpropanesulfonic acid is (0.3~0.5):1; the mass ratio of sodium carboxymethyl cellulose to 2-acrylamide-2-methylpropanesulfonic acid is (0.03~0.04):1; and the mass ratio of glycerol to 2-acrylamide-2-methylpropanesulfonic acid is (0.9~1.1):
1.
8. The method for preparing a silk fibroin-based piezoelectric hydrogel according to claim 1, characterized in that, In step S4, the mass-volume fraction of regenerated silk fibroin in the composite hydrogel precursor solution is 5%~10% w / v.
9. The method for preparing a silk fibroin-based piezoelectric hydrogel according to claim 1, characterized in that, In step S4, the ultraviolet light used for irradiation has a wavelength of 365 nm and a light intensity of 30 m / Wcm. 2 The duration is 140~160s.
10. The application of a silk fibroin-based piezoelectric hydrogel prepared by the preparation method according to any one of claims 1-9 in a flexible strain sensor.