A high-performance composite polymer encapsulation material and its preparation method
By treating polyphenylene sulfide with carboxyl disulfide and introducing an aminosiloxane structure interface modifier, combined with the melt mixing of aluminum nitride, boron nitride and glass fiber, the problem of poor interfacial state of multiphase resin and resin/inorganic filler was solved, and the thermal conductivity, mechanical properties and thermal stability of high-performance composite materials were achieved.
Patent Information
- Application Number
- CN202611627381.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-17
AI Technical Summary
When existing composite polymer encapsulation materials are used in combination with various high-performance thermoplastic resins and high-content inorganic thermally conductive fillers, the interfacial state between multiphase resins and between resins and inorganic fillers is not good, making it difficult to achieve a balance between thermal conductivity, mechanical properties, thermal cycling stability and high-temperature deformation resistance.
A PPS/LCP resin system was constructed by melting polyphenylene sulfide with carboxyl disulfide and introducing an interface modifier with an aminosiloxane structure. Combined with the melt mixing of aluminum nitride, boron nitride and chopped glass fiber, a multi-level regulation was formed to improve the interfacial contact and filler dispersion.
It improves the thermal conductivity of the material while taking into account its mechanical properties, thermal cycling stability and high-temperature deformation resistance, ensuring that the material maintains good dimensional stability and performance retention under continuous high-temperature loads.
Smart Images

Figure CN123107130A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite materials technology, specifically to a high-performance composite polymer encapsulation material and its preparation method. Background Technology
[0002] Composite polymer encapsulation materials are a type of composite material formed by using polymer materials as the matrix and introducing thermally conductive fillers, reinforcing materials, and other functional components according to the needs of encapsulation applications. They are mainly used for the encapsulation, support, insulation, and protection of electronic components, power devices, semiconductor devices, and related components. As electronic devices develop towards higher integration, higher power density, and miniaturization, the heat generated during device operation is constantly increasing, placing higher demands on the thermal conductivity, mechanical properties, dimensional stability, and long-term reliability of encapsulation materials. Especially for encapsulation components that need to be used under repeated temperature changes or long-term high-temperature loads, in addition to requiring high thermal conductivity, the materials also need to have good mechanical properties, thermal cycling stability, and dimensional stability under high-temperature conditions.
[0003] In existing technologies, to improve the heat resistance, mechanical properties, and processability of polymer encapsulation materials, one or more high-temperature resistant thermoplastic resins such as polyetheretherketone, polyphenylene sulfide, and liquid crystal polymers can be used as the resin matrix. Inorganic thermally conductive fillers such as aluminum nitride, boron nitride, and alumina can be added to improve the material's thermal conductivity. Reinforcing materials such as glass fiber can also be added to improve the material's mechanical properties. For composite systems containing multiple resins and a high content of inorganic fillers, it is usually necessary to adjust the resin composition, filler system, and melt blending process to improve the compatibility and dispersion of the components.
[0004] However, in composite systems containing multiple high-performance thermoplastic resins and a high proportion of inorganic thermally conductive fillers, differences in molecular structure, melt rheological properties, and interfacial properties exist among the different resins. Even after melt blending, a multiphase structure with relatively weak interfacial bonding may still form. The addition of a large amount of inorganic filler also increases the number of interfaces in the system and may lead to increased melt viscosity, affecting filler dispersion and interfacial contact between resin and filler. When the composite material undergoes long-term thermal cycling, the differences in thermal expansion behavior between different components may cause the interfacial region to be repeatedly subjected to thermal stress, leading to changes in the interfacial state and a gradual decrease in the material's thermal conductivity and mechanical properties. Under sustained high-temperature loads, relative slippage and cumulative deformation may also occur near the interface. Furthermore, while increasing the content of thermally conductive fillers is beneficial for improving the material's thermal conductivity, a high filler content may also adversely affect the material's mechanical properties, moldability, and interfacial integrity. Therefore, there is still room for further coordination and improvement in existing composite polymer encapsulation materials regarding thermal conductivity, mechanical properties, interfacial stability, thermal cycling stability, and high-temperature deformation resistance. Summary of the Invention
[0005] To address the aforementioned shortcomings of existing technologies, this invention provides a high-performance composite polymer encapsulation material and its preparation method. The aim is to solve the problem that when multiple high-performance thermoplastic resins are used together with a high content of inorganic thermally conductive fillers, the interfacial state between the multiphase resins and between the resin and the inorganic filler is poor, making it difficult to simultaneously achieve the desired thermal conductivity, mechanical properties, thermal cycling stability, and high-temperature deformation resistance of the material.
[0006] To achieve the above objectives, the present invention provides the following technical solution:
[0007] In a first aspect, the present invention provides a method for preparing a high-performance composite polymer encapsulation material, comprising the following steps:
[0008] (1) Polyphenylene sulfide is melt-mixed with a carboxyl disulfide to obtain a polyphenylene sulfide melt treated with a carboxyl disulfide;
[0009] (2) Add a fully aromatic polyester liquid crystal polymer to the polyphenylene sulfide melt treated with carboxyl disulfide, and after the fully aromatic polyester liquid crystal polymer softens and melts, perform a first mixing treatment and a second mixing treatment in sequence to obtain a PPS / LCP resin melt.
[0010] (3) Polyether ether ketone is added to the PPS / LCP resin melt for melt mixing. After the polyether ether ketone melts, an interface modifier containing an aminosiloxane structure is added and melt mixing is continued to obtain a PEEK / PPS / LCP ternary resin melt. The interface modifier containing an aminosiloxane structure is obtained by partial hydrolysis and limited condensation of an aminoalkoxysilane.
[0011] (4) Aluminum nitride and boron nitride are added sequentially to the PEEK / PPS / LCP ternary resin melt and melt-mixed to obtain a thermally conductive composite melt;
[0012] (5) Add short glass fibers to the thermally conductive composite melt for melting and mixing, discharge the resulting composite melt, cool and crush it to obtain the high-performance composite polymer encapsulation material.
[0013] Furthermore, in step (1), 12 to 18 parts of polyphenylene sulfide and 0.15 to 0.60 parts of carboxyl disulfide are melt-mixed at 300 to 320°C to form a continuous melt of polyphenylene sulfide. Then, the mixing speed is increased and the melt mixing continues.
[0014] Furthermore, the carboxyl-containing disulfide is selected from one or more of 2,2′-dithiodibenzoic acid, 3,3′-dithiodipropionic acid, and 4,4′-dithiodibenzoic acid.
[0015] Further, in step (2), 5 to 9 parts of the fully aromatic polyester liquid crystal polymer are added to the polyphenylene sulfide melt treated with carboxyl disulfide at 310 to 330°C; after the fully aromatic polyester liquid crystal polymer softens and melts, the first mixing treatment time is 5 to 15 s, the second mixing treatment time is 15 to 40 s, and the rotor speed during the second mixing treatment is lower than the rotor speed during the first mixing treatment.
[0016] Furthermore, in step (3), 20 to 28 parts of polyether ether ketone are added to the PPS / LCP resin melt for melt mixing. After the polyether ether ketone melts, 0.20 to 0.80 parts of the interface modifier containing aminosiloxane structure are added to continue melt mixing.
[0017] Furthermore, the preparation of the interface modifier containing the aminosiloxane structure includes: adding an aminoalkoxysilane to an ethanol-water mixture, performing partial hydrolysis and limited condensation at 25-50°C for 1-6 h under acidic conditions of pH 4-6; after the reaction is completed, performing vacuum treatment to remove volatile components in the system, thereby obtaining the interface modifier containing the aminosiloxane structure.
[0018] Furthermore, the aminoalkoxysilane is selected from one or more of N-phenyl-γ-aminopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-aminopropyltriethoxysilane; the temperature of the depressurization treatment is 40-70°C, and the absolute pressure is 10-40 kPa.
[0019] Furthermore, in step (4), the amount of aluminum nitride is 25 to 35 parts, and the amount of boron nitride is 10 to 18 parts; the aluminum nitride is spherical or near-spherical aluminum nitride, and the boron nitride is plate-shaped boron nitride or secondary particles formed from plate-shaped boron nitride.
[0020] Furthermore, in step (5), the amount of the chopped glass fiber is 5 to 10 parts, the length is 2 to 6 mm, and the diameter is 7 to 15 μm; the rotor speed when the chopped glass fiber is added and then melted and mixed is lower than the rotor speed when all the aluminum nitride is added and then melted and mixed.
[0021] In a second aspect, the present invention also provides a high-performance composite polymer encapsulation material, which is prepared by the preparation method described in the first aspect; the raw materials for preparing the high-performance composite polymer encapsulation material, by weight, include: 20-28 parts of polyetheretherketone, 12-18 parts of polyphenylene sulfide, 5-9 parts of a fully aromatic polyester liquid crystal polymer, 0.15-0.60 parts of a carboxyl disulfide, 0.20-0.80 parts of an interface modifier containing an aminosiloxane structure, 25-35 parts of aluminum nitride, 10-18 parts of boron nitride, and 5-10 parts of chopped glass fiber;
[0022] The interface modifier containing an aminosiloxane structure is obtained by partial hydrolysis and limited condensation of an aminoalkoxysilane.
[0023] The technical solution provided by this invention has the following advantages compared with the known prior art:
[0024] 1. This invention involves melting PPS with carboxyl disulfide and sequentially constructing a PPS / LCP resin system and a PEEK / PPS / LCP ternary resin system. Simultaneously, an interface modifier containing an aminosiloxane structure is introduced, and AlN, BN, and chopped glass fibers are added sequentially for melt mixing. This allows for the synergistic effect of resin phase regulation, interface adjustment, thermal conductivity filling, and fiber reinforcement, thereby improving the interfacial contact and filler dispersion in the highly filled multiphase composite system. While enhancing the material's thermal conductivity, this also helps to balance its mechanical properties, thermal cycling stability, and dimensional stability under sustained high-temperature loads.
[0025] 2. In this invention, PPS is first subjected to a carboxyl disulfide melt treatment, and then LCP is introduced to construct a PPS / LCP resin system. This is beneficial for adjusting the interfacial state between PPS and LCP, and provides a basic resin melt for the subsequent construction of a PEEK / PPS / LCP ternary resin system.
[0026] 3. This invention prepares an interface modifier containing an aminosiloxane structure by partially hydrolyzing and limiting the condensation of an aminoalkoxysilane in an acidic ethanol-water system. The resulting interface modifier retains the amino organic structure and forms certain silanol and siloxane structures, which helps to improve the wetting and interfacial contact state between multiphase resins and between resins and inorganic fillers, reduces interfacial defects such as local agglomeration of fillers, interfacial gaps and particle pull-out, and improves the interfacial stability of the composite system.
[0027] 4. This invention uses spherical or near-spherical AlN and sheet-like BN or their secondary particles for composite thermal conductive filling, adding AlN first and then BN, followed by the addition of chopped glass fibers in a subsequent stage. This allows the thermally conductive fillers of different morphologies to complement each other in the composite system and reduces excessive breakage of glass fibers during the initial strong mixing process. This facilitates the formation of a more effective heat transfer path while maintaining the reinforcing effect of glass fibers, thus achieving a good balance between the material's thermal conductivity, mechanical load-bearing capacity, and high-temperature deformation resistance. Attached Figure Description
[0028] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without any creative effort.
[0029] Figure 1 This is a process flow diagram of the present invention;
[0030] Figure 2 This is a comparison of the Fourier transform infrared spectra of N-phenyl-γ-aminopropyltrimethoxysilane and the interface modifier containing aminosiloxane structure of the present invention.
[0031] Figure 3 These are comparative images of the cross-sectional scanning electron microscope (SEM) morphology of the composite materials obtained in Example 1, Comparative Example 3 and Comparative Example 4 of the present invention. The left image is Example 1, the middle image is Comparative Example 3 and the right image is Comparative Example 4. Detailed Implementation
[0032] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are some embodiments of the present invention, but not all embodiments.
[0033] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail. The terms “comprising,” “including,” “having,” “containing,” etc., as used herein are open-ended terms, meaning that they include but are not limited to. Unless the context clearly indicates otherwise, the expressions “a” and “an” as used herein include plural references. It should be noted that “first,” “second,” etc., are used merely for convenience of description and distinction and should not be construed as indicating or implying relative importance. The term “about” as used herein indicates a range of ±20% of the following numerical value. In some embodiments, the term “about” indicates a range of ±10% of the following numerical value. In some embodiments, the term “about” indicates a range of ±5% of the following numerical value. The invention is further described below with reference to embodiments.
[0034] Unless otherwise stated, all "parts" in this invention refer to parts by weight. Polyphenylene sulfide (PPS) should be dried at 135°C for 6 hours before use; polyetheretherketone (PEEK) should be dried at 150°C for 6 hours before use; fully aromatic polyester liquid crystal polymer (LCP) should be dried at 130°C for 4 hours before use; 2,2′-dithiodibenzoic acid (2,2′-dithiobenzoic acid) with a purity of not less than 98.0% should be sealed and dried before use; N-phenyl-γ-aminopropyltrimethoxysilane with a purity of not less than 98.0% should be sealed and kept away from moisture before use; aluminum nitride (AlN) consists of nearly spherical particles with a median particle size (D50) of approximately 25 μm, and should be dried at 130°C for 3 hours before use; boron nitride (BN) consists of secondary particles formed from plate-like boron nitride with a median particle size (D50) of approximately 35 μm, and should be dried at 130°C for 3 hours before use; chopped glass fibers with an initial length of approximately 3 mm and a diameter of approximately 10 μm should be dried at 120°C for 3 hours before use. h; anhydrous ethanol and acetic acid, both analytical grade; deionized water. The dried raw materials were stored separately in sealed containers for later use.
[0035] Example 1
[0036] This invention provides a method for preparing a high-performance composite polymer encapsulation material, the process flow of which is as follows: Figure 1 As shown, the specific steps include the following.
[0037] Step 1: Raw material pretreatment
[0038] PPS was dried at 135℃ for 6 hours; PEEK was dried at 150℃ for 6 hours; LCP was dried at 130℃ for 4 hours. AlN and BN were dried at 130℃ for 3 hours each; chopped glass fibers were dried at 120℃ for 3 hours. After drying, each raw material was sealed and stored separately for later use.
[0039] Step 2: Preparation of amino-siloxane-containing interface modifiers
[0040] Take 100 parts of N-phenyl-γ-aminopropyltrimethoxysilane, add 100 parts of ethanol and 15 parts of deionized water, and stir to mix. Adjust the pH of the mixture to 5.0 with acetic acid, and stir at 40°C for 3 h to allow N-phenyl-γ-aminopropyltrimethoxysilane to undergo partial hydrolysis accompanied by limited condensation.
[0041] After the reaction was completed, the volatile components such as ethanol, free water and methanol generated during hydrolysis were removed under reduced pressure at 55℃ and 20 kPa until there was no obvious free ethanol-water liquid phase in the system and the product remained fluid. An interface modifier containing an aminosiloxane structure was obtained and stored in a sealed container for later use.
[0042] Step 3: PPS Melting Treatment
[0043] Weigh out 15 parts of PPS and 0.35 parts of 2,2′-dithiodibenzoic acid, and mix them thoroughly beforehand.
[0044] The high-temperature internal mixer was preheated to 310°C, and the rotor speed was set to 45 rpm. PPS and 2,2′-dithiobenzoic acid were added to the mixing chamber and mixed for 2.5 min to form a continuous melt of PPS. Then, the rotor speed was increased to 65 rpm, and mixing was continued at 310°C for 30 s to obtain a PPS melt treated with 2,2′-dithiobenzoic acid.
[0045] Step 4: Preparation of PPS / LCP resin melt
[0046] Adjust the mixing temperature to 320°C and add 7 parts of LCP to the above PPS melt.
[0047] First, the LCP is mixed at 45 rpm for 60 s to soften it and bring it into a molten state. Then, while maintaining the mixing temperature at 320°C, the rotor speed is increased to 100 rpm for the first mixing treatment, which lasts for 10 s. After the first mixing treatment, the rotor speed is reduced to 45 rpm for the second mixing treatment, which lasts for 25 s, to obtain the PPS / LCP resin melt.
[0048] The first and second mixing processes described above are carried out continuously in the same internal mixer. Specifically, the stage of mixing at 45 rpm for 60 s after adding LCP is the softening and melting stage; the stage of mixing at 100 rpm for 10 s is the first mixing process; and the subsequent stage of mixing at 45 rpm for 25 s is the second mixing process.
[0049] Step 5: Melt and interface conditioning of PEEK / PPS / LCP ternary resin
[0050] Set the internal mixer temperature to 360°C and maintain a low mixing speed of 35 rpm during the heating process.
[0051] After the temperature of the mixing chamber reaches 360℃, add 24 parts of PEEK. The PEEK is added in two batches of 12 parts each time, with a 60-second interval between the two additions.
[0052] After all the PEEK is added, adjust the rotor speed to 60 rpm and continue mixing at 360℃ for 3 minutes to allow the PEEK to basically melt and form a ternary resin melt with the PPS / LCP system.
[0053] Then, slowly add 0.50 parts of the above-mentioned amino-siloxane-containing interface modifier, controlling the addition process to be completed within approximately 10 seconds. After the interface modifier is added, adjust the rotor speed to 70 rpm and continue mixing at 360°C for 30 seconds.
[0054] Step 6: Add AlN and BN
[0055] Adjust the mixing temperature to 355℃. Add 30 parts AlN. Divide the AlN into 3 batches of 10 parts each, maintain the rotor speed at 45 rpm, and mix for 30 seconds between adjacent batches.
[0056] After all AlN was added, the rotor speed was adjusted to 60 rpm, and mixing continued at 355°C for 2 minutes. Then, the rotor speed was reduced to 40 rpm, and 14 parts of BN were added. The BN was added in two equal batches of 7 parts each, with a 30-second mixing interval between batches. After all BN was added, mixing continued at 355°C and 40 rpm for 2 minutes.
[0057] Step 7: Adding and discharging chopped glass fibers
[0058] Reduce the rotor speed to 30 rpm, add a total of 7 parts of chopped glass fiber in two batches, 3.5 parts per batch, and mix the two batches for 30 seconds.
[0059] After adding all the chopped glass fibers, continue mixing at 355°C and 30 rpm for 60 seconds. Then adjust the temperature to 350°C and continue mixing at 30 rpm for 60 seconds. Then stop heating and rotor operation, and remove the composite melt from the mixing chamber.
[0060] The resulting composite melt was cooled and then crushed to obtain a granular high-performance composite polymer encapsulation material.
[0061] Example 1 uses PPS, PEEK and LCP to construct a multiphase high-temperature resistant resin system. During the melt mixing process, the interface state between different resin phases and between the resin and inorganic filler is adjusted step by step by treating with carboxyl disulfide and introducing an amino-siloxane structure interface modifier. At the same time, AlN, BN and chopped glass fiber are used to undertake the functions of thermal conductivity filling and structural reinforcement, respectively, thereby forming a composite material system that takes into account thermal conductivity, mechanical properties, high-temperature dimensional stability and long-term load stability.
[0062] PPS, possessing high-temperature resistance, chemical resistance, and good melt processing properties, serves not only as a heat-resistant resin component in this system but also undergoes initial treatment with carboxyl-containing disulfides. 2,2′-Dithiodibenzoic acid, possessing both disulfide bonds and carboxyl functional groups, interacts with PPS segments in the molten state, causing some PPS segments to form structures with reactive or polar end groups, thereby altering the interfacial state between PPS and the subsequent LCP. This treatment is not simply the addition of low-molecular-weight additives but rather a pre-conditioning of the interfacial chemical environment of PPS before constructing the PPS / LCP system, which is beneficial for improving the interaction between the two resins and the interfacial stress transfer capability.
[0063] Based on this, LCP is added, first softened and melted, and then subjected to a first mixing treatment and a second mixing treatment in sequence. The first mixing treatment uses a higher rotor speed to promote the mixing of LCP and PPS; then the rotor speed is reduced for the second mixing treatment, and mixing continues to obtain the PPS / LCP base resin melt for subsequent addition of PEEK. The mixing conditions in the above two stages are consistent in Example 1 and Comparative Examples 1-4.
[0064] PEEK possesses high heat resistance, mechanical strength, and dimensional stability. Introducing it into the PPS / LCP system can improve the structural stability of the composite material under high temperature and sustained load conditions. Adding PEEK in batches while maintaining a low to medium mixing speed avoids the rapid increase in local melt viscosity caused by adding high-viscosity PEEK all at once. This allows PEEK to gradually melt and integrate into the existing PPS / LCP dispersion system, thus forming a PEEK / PPS / LCP ternary resin melt.
[0065] The amino-siloxane-containing interface modifier is obtained by pre-partial hydrolysis and limited condensation of aminoalkoxysilanes. Compared with the direct addition of untreated aminoalkoxysilanes, pre-partial hydrolysis can form a certain amount of silanol groups and oligomeric siloxane structures, giving the interface modifier both amino-containing organic structures and siloxane structures. After being added to a ternary resin melt, this interface modifier can improve the interfacial contact state between resin phases and between the resin and subsequent inorganic fillers through polar interactions, interfacial wetting, and the interaction between the siloxane structure and the surface of the inorganic filler. It also reduces the tendency of inorganic fillers to locally agglomerate and form interfacial defects under high-filling conditions.
[0066] AlN possesses high intrinsic thermal conductivity and electrical insulation properties. In this embodiment, near-spherical AlN is used as the main thermally conductive filler, which helps to maintain a high thermal conductivity filler content while ensuring melt flow and filling uniformity. BN also has good thermal conductivity and electrical insulation properties. Using plate-shaped secondary BN particles can form supplementary heat transfer contacts between AlN particles, allowing the thermally conductive fillers with different morphologies to work together and increasing the possibility of forming effective heat transfer paths. Therefore, in this embodiment, AlN is added first to form the main thermally conductive filler framework, and then BN is added to supplement the contact state between particles, rather than adding the two highly filled inorganic fillers at once. This helps to control the melt viscosity increase process and the dispersion state of the inorganic fillers.
[0067] Short-cut glass fibers are added in the final stage at lower rotational speeds, primarily to improve the mechanical load-bearing capacity and high-temperature dimensional stability of the composite material. Adding the glass fibers after the thermally conductive filler and reducing the rotor speed can minimize excessive breakage of the fibers during prolonged high-shear processes, ensuring they maintain a certain effective reinforcing length in the composite system. This further suppresses excessive deformation of the material under sustained high-temperature loads.
[0068] Therefore, the various technical measures in Example 1 do not function in isolation, but rather form a multi-level control process that unfolds sequentially from resin phase regulation, resin interphase interface regulation, resin / inorganic filler interface regulation, thermally conductive filler construction, and fiber reinforcement. The carboxyl disulfide treatment mainly acts on the PPS and PPS / LCP interfaces, while the amino-siloxane structural interface modifier further acts on the interface between the ternary resin system and the inorganic filler. AlN, BN, and chopped glass fibers respectively undertake the functions of thermal conduction and structural support. The various technical measures are interconnected in terms of their target and stage of action.
[0069] Through the aforementioned multi-level interface control, the local weak bonding regions at the resin / filler interface and in the multiphase resin system can be reduced, allowing the applied load to be transferred more uniformly among the resin phase, inorganic filler, and glass fiber. Simultaneously, it reduces interfacial thermal resistance and the tendency for relative slippage and cumulative deformation near the interface during sustained high-temperature stress. Therefore, this embodiment improves the thermal conductivity of the composite material while maintaining high tensile strength, flexural strength, and impact performance, and enhances the material's ability to retain performance after repeated thermal cycling and its creep resistance under sustained high-temperature compressive loads.
[0070] This embodiment does not simply address the problem of improving a single thermal conductivity or mechanical property. Rather, it aims to alleviate issues such as insufficient compatibility between resin phases, inadequate contact between inorganic fillers and resin interfaces, decreased mechanical properties due to high filler content, and easy relative slippage at the interface under long-term high-temperature loads when PEEK / PPS / LCP high-temperature multiphase resin and high-content inorganic thermally conductive fillers coexist. This allows for a better balance between thermal conductivity, mechanical enhancement, and high-temperature stability within the same composite system.
[0071] Comparative Example 1
[0072] This comparative example is used to investigate the effect of treatment with carboxyl disulfide.
[0073] Except for the absence of 2,2′-dithiodibenzoic acid, the composition of the raw materials, the composition of the interface modifier, and the preparation conditions were the same as in Example 1.
[0074] Specifically, 15 parts of PPS were added to a mixer preheated to 310°C and mixed at 45 rpm for 2.5 min to form a continuous melt of PPS; then the mixture was continued to be mixed at 65 rpm for 30 s.
[0075] Then, following the method of Example 1, 7 parts LCP, 24 parts PEEK, 0.50 parts amino-siloxane structure interface modifier, 30 parts AlN, 14 parts BN and 7 parts chopped glass fiber were added in sequence, and the same temperature, rotor speed, feeding sequence and mixing time as in Example 1 were used for processing.
[0076] After mixing, the mixture was cooled and crushed to obtain the composite material of Comparative Example 1.
[0077] Comparative Example 1, which eliminated the carboxyl disulfide, was used to investigate the effect of PPS treatment with carboxyl disulfide on the properties of the composite material.
[0078] Comparative Example 2
[0079] This comparative example is used to investigate the role of interface modifiers containing aminosiloxane structures.
[0080] The amounts of PPS, 2,2′-dithiodibenzoic acid, LCP, PEEK, AlN, BN, and chopped glass fibers were 15 parts, 0.35 parts, 7 parts, 24 parts, 30 parts, 14 parts, and 7 parts, respectively.
[0081] PPS and 2,2′-dithiodibenzoic acid were melt-treated according to the method of Example 1, and the PPS / LCP resin melt and the PEEK / PPS / LCP ternary resin melt were prepared according to the method of Example 1.
[0082] After the PEEK is basically melted, without adding an amino-siloxane structure interface modifier, continue mixing at 360℃ and 70 rpm for 30 seconds, and then adjust the mixing temperature to 355℃.
[0083] Then, following the method in Example 1, 30 parts AlN, 14 parts BN, and 7 parts chopped glass fibers were added sequentially.
[0084] The remaining mixing temperature, rotor speed and mixing time are the same as in Example 1.
[0085] After mixing, the mixture was cooled and crushed to obtain the composite material of Comparative Example 2.
[0086] Comparative Example 2 eliminated the amino-siloxane-containing interface modifier to investigate the effect of the interface modifier on the interface of multiphase resin and resin / inorganic filler.
[0087] Comparative Example 3
[0088] This comparative example simultaneously eliminated carboxyl disulfide and amino-siloxane-containing interface modifiers, which were used as a basic control.
[0089] Weigh 15 parts of PPS and add them to a mixer preheated to 310°C. Mix at 45 rpm for 2.5 min until the PPS is basically melted, and then continue mixing at 65 rpm for 30 s.
[0090] Then, 7 parts of LCP were added according to the method in Example 1, and the mixture was kneaded at 45 rpm for 60 s, 100 rpm for 10 s, and 45 rpm for 25 s in sequence.
[0091] Raise the mixing temperature to 360℃, add 24 parts of PEEK in two batches, and mix at 60 rpm for 3 minutes after adding all the PEEK.
[0092] After the PEEK is basically melted, without adding an interface modifier, continue mixing at 360℃ and 70 rpm for 30 seconds, and then adjust the mixing temperature to 355℃.
[0093] Following the method of Example 1, 30 parts AlN, 14 parts BN, and 7 parts chopped glass fiber were added sequentially, and the same feeding method, rotor speed, and mixing time as in Example 1 were used for mixing.
[0094] After mixing, the mixture was cooled and crushed to obtain the composite material of Comparative Example 3.
[0095] Comparative Example 3 simultaneously eliminated both the carboxyl disulfide-containing and amino-siloxane-containing interface modifiers, serving as a baseline control system. By comparing Example 1 with Comparative Examples 1-3, further analysis can be conducted to determine whether there is a synergistic or cooperative effect between the carboxyl disulfide treatment and the amino-siloxane-containing interface modifier.
[0096] Comparative Example 4
[0097] This comparative example was used to investigate the effects of pre-partial hydrolysis and limited condensation treatment of aminoalkoxysilanes. The raw material composition and all preparation processes were the same as in Example 1, except that the aminosiloxane-containing interface modifier described in Example 1 was not prepared.
[0098] After the PEEK is basically melted to form a PEEK / PPS / LCP ternary resin melt, 0.50 parts of unhydrolyzed N-phenyl-γ-aminopropyltrimethoxysilane are added directly.
[0099] Continue mixing at 360°C and 70 rpm for 30 seconds.
[0100] Subsequently, following the method in Example 1, 30 parts AlN, 14 parts BN, and 7 parts chopped glass fiber were added sequentially, and the subsequent mixing and discharge were completed.
[0101] The composite material of Comparative Example 4 was obtained.
[0102] Comparative Example 4 replaced the amino-siloxane-containing interface modifier prepared by partial hydrolysis and limited condensation with the same aminoalkoxysilane that was not pre-hydrolyzed, in order to compare the effects of the interface modifier obtained by pre-partial hydrolysis and limited condensation and the untreated silane on the properties of the composite material under the same addition mass conditions.
[0103] In both the embodiments and comparative examples of this invention, the same high-temperature internal mixer was used for melt mixing. Each group used the same batch of PPS, PEEK, LCP, AlN, BN, and chopped glass fibers. In Examples 1 and Comparative Examples 1-4, the same first and second mixing conditions were used in the mixing stage after the addition of LCP to investigate the effects of carboxyl disulfide treatment, the addition of amino-siloxane structure interface modifiers, and their pre-partial hydrolysis and limited condensation treatments on material properties.
[0104] Performance testing
[0105] Before performance testing, the composite material particles obtained in each group were dried at 150℃ for 4 h, and corresponding test specimens were prepared under the same high-temperature injection molding conditions. All test specimens were subjected to the same molding temperature, mold temperature, injection pressure, and cooling conditions to minimize the impact of differences in molding processes on the performance test results.
[0106] Before testing, the obtained samples were placed in an environment of 23±2℃ for conditioning. Then, their thermal conductivity, tensile properties, bending properties, notched impact properties, thermal cycling stability, and high-temperature compression creep properties were tested according to the following methods.
[0107] 1. Thermal conductivity test
[0108] The thermal conductivity of composite materials was determined using the transient planar heat source method. Each group of composite materials was prepared into identical flat plate specimens. A planar heat source sensor was placed between two specimens of the same material, and tests were conducted at room temperature. Each group consisted of five independent test units. The arithmetic mean and standard deviation of the thermal conductivity were calculated from the five valid test results, i.e., n=5.
[0109] 2. Tensile property test
[0110] Each composite material was prepared into a standard dumbbell-shaped tensile specimen of the same size. After conditioning, tensile tests were performed using a universal testing machine. The same clamping method and loading speed were used for each group. Five independent parallel specimens were tested for each group, and the arithmetic mean and standard deviation of the tensile strength were calculated based on the five valid test results.
[0111] 3. Bending performance test
[0112] Each group of composite materials was prepared into strip specimens of the same size and tested using a three-point bending method after conditioning. Each group used the same span and loading speed, and five independent parallel specimens were tested in each group. The arithmetic mean and standard deviation of the bending strength were calculated from the five valid test results.
[0113] 4. Notched impact performance test
[0114] Each group of composite materials was prepared into simply supported beam impact specimens of the same size, and notches of the same size were machined. After condition conditioning, the specimens were subjected to notched impact tests. Five independent parallel specimens were tested in each group, and the arithmetic mean and standard deviation of the notched impact strength were calculated based on the five valid test results.
[0115] 5. Thermal cycling stability test
[0116] Thermal cycling stability tests were conducted on Example 1 and the corresponding comparative example.
[0117] For thermal conductivity testing, five independent testing units were set up for each group of materials. Thermal conductivity tests were performed before thermal cycling, and the corresponding samples were subjected to subsequent thermal cycling treatment so that their thermal conductivity could be measured again after the thermal cycling was completed.
[0118] For the bending strength test, 10 independent parallel specimens prepared in the same batch were used for each group of materials. Five of them were used as pre-cycle specimens to directly determine the bending strength before cycling. The other five were used as thermal cycling specimens to determine the bending strength after 200 cycles of hot and cold cycling.
[0119] The samples used for thermal cycling were placed in a thermal cycling test chamber and cooled from room temperature to -40°C, held at -40°C for 30 min; then heated to 150°C and held at 150°C for 30 min; then cooled to -40°C again, which constituted one thermal cycle, and a total of 200 thermal cycles were performed. All groups of samples used the same heating and cooling procedures.
[0120] After the thermal cycling was completed, the samples were allowed to return to room temperature and left for 24 hours. The surface of the samples was then observed for obvious cracking, warping, or delamination. The thermal conductivity and flexural strength after cycling were measured. The arithmetic mean and standard deviation of the thermal conductivity and flexural strength before and after cycling were calculated using five valid test results.
[0121] Performance retention rate is calculated using the following formula:
[0122] Performance retention rate = Average performance after thermal cycling / Average performance before thermal cycling × 100%.
[0123] The thermal conductivity and flexural strength before and after cycling in Table 2 are expressed as arithmetic mean ± standard deviation (mean ± SD), n=5; the thermal conductivity retention rate and flexural strength retention rate are calculated based on the corresponding average performance before and after cycling.
[0124] 6. High-Temperature Compression Creep Performance Test
[0125] Example 1 and the corresponding comparative example were selected for high-temperature compression creep performance testing.
[0126] Five independent parallel block specimens were prepared for each group for testing. The composite materials of each group were processed into block specimens of the same size, and their initial height h0 was measured. The specimens were placed in a high-temperature compression creep testing device, preheated at 150°C for 30 min, and then a constant compressive stress of 20 MPa was applied and maintained for 100 h. The height change of the specimens under continuous compressive load was recorded.
[0127] The compressive creep strain at 100 h is calculated according to the following formula:
[0128] Compressive creep strain = (h0 - h) 100 ) / h0×100%;
[0129] Among them, h 100 The height of the sample after being subjected to a compressive stress of 20 MPa at 150℃ for 100 h is given.
[0130] After 100 hours, the sample was unloaded and placed at 23±2℃ for 24 hours to recover. The sample height h was then measured again. r The compressive permanent deformation rate is calculated according to the following formula:
[0131] Compression permanent deformation rate = (h0 - h) r ) / h0×100%.
[0132] The compressive creep strain and compressive permanent deformation rate were calculated for each specimen, and the arithmetic mean of 5 valid test results was taken as the test result for the material group, i.e., n=5. The compressive creep strain and permanent deformation rate listed in Table 3 are expressed as the arithmetic mean ± standard deviation (mean ± SD) of 5 valid test results, i.e., n=5.
[0133] The basic performance test results of each group of composite materials are shown in Table 1 after the above tests.
[0134] The test results in Table 1 are expressed as arithmetic mean ± standard deviation (mean ± SD). The effective sample size for thermal conductivity, tensile strength, flexural strength and notched impact strength tests is n=5.
[0135] Table 1. Basic performance of Example 1 and each comparative example
[0136]
[0137] As can be seen from the results in Table 1, Example 1 is superior to the comparative examples in terms of thermal conductivity, tensile strength, flexural strength and notched impact strength.
[0138] Comparative Example 3, which simultaneously eliminated both the carboxyl disulfide-containing and amino-siloxane-containing interface modifiers, exhibited the lowest thermal conductivity and mechanical properties. Compared to Comparative Example 3, Comparative Example 1 retained the amino-siloxane-containing interface modifier, and Comparative Example 2 retained the carboxyl disulfide-containing material; both groups showed improved thermal conductivity and mechanical properties. Example 1, which employed both the carboxyl disulfide-containing and amino-siloxane-containing interface modifiers, demonstrated even better overall performance.
[0139] Comparative Example 4 directly used aminoalkoxysilane without partial hydrolysis and limited condensation treatment. Although its performance was better than the system without any added interface modifier, it was still lower than that of Example 1. This shows that pre-treatment of aminoalkoxysilane with partial hydrolysis and limited condensation is beneficial to exert the interface modifier effect.
[0140] Table 2 Properties of composite materials before and after thermal cycling
[0141]
[0142] In Table 2, thermal conductivity and flexural strength are expressed as arithmetic mean ± standard deviation (mean ± SD), n=5; thermal conductivity retention rate and flexural strength retention rate are calculated based on the ratio of the average value of the corresponding performance after cycling to the average value of the corresponding performance before cycling.
[0143] Example 1 showed no visible cracking or delamination after 200 thermal cycles, and its thermal conductivity and flexural strength retention were both above 94%. In contrast, Comparative Example 3, lacking carboxyl disulfide treatment and interface conditioning, exhibited a greater performance degradation after thermal cycling. Although Comparative Example 4 used the same type of aminoalkoxysilane, it did not undergo pre-partial hydrolysis and limited condensation, resulting in lower thermal cycling stability than Example 1.
[0144] This set of tests is mainly used to evaluate the ability of different interface construction methods to maintain effective contact between resin phases and between resin and inorganic fillers under repeated thermal expansion and contraction conditions. Compared with testing only the initial tensile strength, it can better reflect the long-term stability of the interface structure.
[0145] Table 3. High-temperature compressive creep properties of different composite materials
[0146]
[0147] As shown in Table 3, the high-temperature compression creep strain and the permanent deformation rate after unloading in Example 1 were both lower than those in the comparative examples. In Comparative Examples 1 and 2, the compression creep increased after either the carboxyl disulfide treatment or the amino-siloxane interface modifier was removed; the increase was most significant in Comparative Example 3 after both treatments were removed.
[0148] This indicates that in the highly filled multiphase composite system of the present invention, improving the interfacial state between PEEK / PPS / LCP multiphase resins and between the resin and inorganic filler can not only improve the initial mechanical properties of the material, but also help to suppress the cumulative deformation caused by relative slippage near the interface under sustained high temperature load.
[0149] like Figure 2 As shown, Fourier transform infrared spectroscopy (FTIR) analysis was performed on N-phenyl-γ-aminopropyltrimethoxysilane and the amino-siloxane-containing interface modifier obtained after partial hydrolysis and limited condensation treatment. Untreated N-phenyl-γ-aminopropyltrimethoxysilane showed a wavelength of approximately 2900 cm⁻¹. -1 CH stretching vibration-related absorption can be observed nearby, at approximately 1600 cm⁻¹. -1 Aromatic ring skeletal vibrations and NH-related absorptions can be observed in the vicinity, at approximately 1000–1100 cm⁻¹. -1 The region exhibits absorption characteristics associated with the Si-OC structure.
[0150] After partial hydrolysis and limited condensation treatment, the resulting interface modifier was obtained at approximately 3400 cm⁻¹. -1 The broad OH / NH absorption band is more pronounced in the vicinity, particularly at approximately 1000–1150 cm⁻¹. -1 The absorption peak shape and intensity changed in the region, with enhanced absorption features related to the Si-O-Si structure. These changes in absorption bands are consistent with the structural changes caused by the hydrolysis and silanol condensation of aminoalkoxysilanes, providing support for the formation of products containing siloxane structures after treatment.
[0151] Meanwhile, the treated spectrum still retains the absorption characteristics related to CH, aromatic rings, and amino-containing structures, indicating that the partial hydrolysis and limited condensation processes did not completely destroy the N-phenyl-γ-aminopropyl organic structure. Therefore, it can be concluded that the treatment conditions adopted in this invention can introduce a certain amount of silanol and siloxane structures while preserving the amino organic functional structure, providing a structural basis for subsequently improving the multiphase resin system and the interfacial contact between the resin and inorganic fillers.
[0152] In the cross-section of the composite material, the near-spherical particles mainly correspond to AlN filler, the lamellar stacked structure mainly corresponds to BN secondary particles formed from lamellar boron nitride, and the short rod-shaped or fibrous structure mainly corresponds to chopped glass fibers. The initial median particle size (D50) of AlN is approximately 25 μm, the initial median particle size (D50) of BN secondary particles is approximately 35 μm, and the initial length of the chopped glass fibers is approximately 3 mm and the diameter is approximately 10 μm. Because glass fibers may break to varying degrees during melt mixing, and cross-sectional observation only shows the localized exposed length of some fibers, the visible fiber length in the cross-section is not equivalent to the initial length of the raw material.
[0153] like Figure 3 As shown, the cross-sectional morphology of the composite materials obtained in Example 1, Comparative Example 3, and Comparative Example 4 was observed by scanning electron microscopy. The cross-section of Example 1 was relatively dense overall, with nearly spherical particles, lamellar fillers, and fibrous reinforcing phases distributed relatively evenly in the resin matrix. The resin matrix exhibited a relatively continuous connection morphology around some fillers, and there were relatively few large local stacked areas of fillers and obvious local interfacial gaps, indicating that the fillers and the resin matrix maintained a relatively good interfacial contact state.
[0154] Comparative Example 3 did not employ treatment with carboxyl disulfide or an interface modifier containing aminosiloxane. Its cross-section showed significant localized packing aggregation, numerous irregular dark areas, and localized interfacial gaps around the packing. Some areas exhibited obvious fracture and depression morphology, and the uniformity of the local cross-sectional morphology was lower than that of Example 1. This indicates that in the absence of the aforementioned interface modulation measures, highly packed multiphase systems are more prone to forming localized weak interfaces and packing aggregation regions.
[0155] Comparative Example 4 used N-phenyl-γ-aminopropyltrimethoxysilane that had not undergone prior partial hydrolysis and limited condensation treatment. Its cross-sectional morphology was improved compared to Comparative Example 3, with a relative reduction in localized packing and obvious irregular dark areas. However, some localized packing and interfacial gaps were still observed. The continuous contact between the resin matrix and the packing and the degree of localized dispersion uniformity in its cross-section were still not as good as in Example 1.
[0156] The morphological differences between Example 1 and Comparative Example 4 indicate that, when using the same type of aminoalkoxysilane, the amino-siloxane-containing interface modifier obtained after pre-treatment with partial hydrolysis and limited condensation is more beneficial for improving the filler dispersion and interfacial contact state in highly filled composite systems. A comparison of Example 1 with Comparative Examples 3 and 4 suggests that, under the same melt-mixing process conditions, the combined use of carboxyl disulfide treatment and the amino-siloxane-containing interface modifier is beneficial for reducing localized interfacial defects between multiphase resins and inorganic fillers. Figure 3 The trends in interface morphology shown are consistent with the trends in thermal conductivity, mechanical properties, thermal cycling stability, and high-temperature compression creep properties of the material, further supporting the role of improved interface state in enhancing the overall performance of the material from a morphological perspective.
[0157] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions will not cause the essence of the corresponding technical solutions to deviate from the protection scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a high-performance composite polymer encapsulation material, characterized in that, Includes the following steps: (1) Polyphenylene sulfide is melt-mixed with a carboxyl disulfide to obtain a polyphenylene sulfide melt treated with a carboxyl disulfide; (2) Add a fully aromatic polyester liquid crystal polymer to the polyphenylene sulfide melt treated with carboxyl disulfide, and after the fully aromatic polyester liquid crystal polymer melts, perform a first mixing treatment and a second mixing treatment in sequence to obtain a PPS / LCP resin melt. (3) Polyether ether ketone is added to the PPS / LCP resin melt for melt mixing. After the polyether ether ketone melts, an interface modifier containing an aminosiloxane structure is added and melt mixing is continued to obtain a PEEK / PPS / LCP ternary resin melt. The interface modifier containing an aminosiloxane structure is obtained by partial hydrolysis and limited condensation of an aminoalkoxysilane. (4) Add aluminum nitride and boron nitride to the PEEK / PPS / LCP ternary resin melt in sequence and melt mix to obtain a thermally conductive composite melt; (5) Add short glass fibers to the thermally conductive composite melt for melting and mixing, discharge the resulting composite melt, cool and crush it to obtain the high-performance composite polymer encapsulation material.
2. The method for preparing a high-performance composite polymer encapsulation material according to claim 1, characterized in that, In step (1), 12 to 18 parts of polyphenylene sulfide and 0.15 to 0.60 parts of carboxyl disulfide are melt-mixed at 300 to 320°C to form a continuous melt of polyphenylene sulfide. Then the mixing speed is increased and the melt mixing continues.
3. The method for preparing a high-performance composite polymer encapsulation material according to claim 1 or 2, characterized in that, The carboxyl-containing disulfide is selected from one or more of 2,2′-dithiodibenzoic acid, 3,3′-dithiodipropionic acid, and 4,4′-dithiodibenzoic acid.
4. The method for preparing a high-performance composite polymer encapsulation material according to claim 1, characterized in that, In step (2), 5 to 9 parts of the fully aromatic polyester liquid crystal polymer are added to the polyphenylene sulfide melt treated with carboxyl disulfide at 310 to 330°C. After the fully aromatic polyester liquid crystal polymer softens and melts, the first mixing treatment takes 5 to 15 seconds, and the second mixing treatment takes 15 to 40 seconds.
5. The method for preparing a high-performance composite polymer encapsulation material according to claim 1, characterized in that, In step (3), 20 to 28 parts of polyether ether ketone are added to the PPS / LCP resin melt for melt mixing. After the polyether ether ketone melts, 0.20 to 0.80 parts of the interface modifier containing aminosiloxane structure are added to continue melt mixing.
6. The method for preparing a high-performance composite polymer encapsulation material according to claim 5, characterized in that, The preparation of the interface modifier containing the aminosiloxane structure includes: Aminoalkoxysilanes were added to an ethanol-water mixture and subjected to partial hydrolysis and limited condensation at 25–50 °C under acidic conditions of pH 4–6. After the reaction is complete, a reduced pressure treatment is performed to obtain the interface modifier containing the aminosiloxane structure.
7. The method for preparing a high-performance composite polymer encapsulation material according to claim 6, characterized in that, The aminoalkoxysilane is selected from one or more of N-phenyl-γ-aminopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-aminopropyltriethoxysilane.
8. The method for preparing a high-performance composite polymer encapsulation material according to claim 1, characterized in that, In step (4), the amount of aluminum nitride is 25 to 35 parts and the amount of boron nitride is 10 to 18 parts.
9. The method for preparing a high-performance composite polymer encapsulation material according to claim 1, characterized in that, In step (5), the amount of chopped glass fiber used is 5 to 10 parts.
10. A high-performance composite polymer encapsulation material, characterized in that, The high-performance composite polymer encapsulation material is prepared by the preparation method according to any one of claims 1 to 9. The raw materials for preparing the high-performance composite polymer encapsulation material, by weight, include: 20-28 parts of polyetheretherketone, 12-18 parts of polyphenylene sulfide, 5-9 parts of a fully aromatic polyester liquid crystal polymer, 0.15-0.60 parts of a carboxyl disulfide, 0.20-0.80 parts of an interface modifier containing an aminosiloxane structure, 25-35 parts of aluminum nitride, 10-18 parts of boron nitride, and 5-10 parts of chopped glass fiber. The interface modifier containing an aminosiloxane structure is obtained by partial hydrolysis and limited condensation of an aminoalkoxysilane.