A thermally induced phase separation-based porous PTFE material and its preparation method

The preparation of PTFE porous membranes by thermally induced phase separation method solves the safety hazards and pore size control problems in the existing technology, and realizes the preparation of porous membranes with excellent pore size uniformity and interconnection, which is suitable for membrane distillation, oil-water separation and air filtration.

CN123107166APending Publication Date: 2026-11-17HENAN NAQING NEW MATERIAL MANUFACTURING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611288109.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for preparing PTFE porous membranes have safety hazards, difficulty in uniformly controlling pore size, and problems such as wide pore size distribution and poor permeability.

Method used

The thermally induced phase separation method is adopted. Lauric acid is mixed with PTFE dispersion resin powder, and after curing, it is heat-treated in an inert gas atmosphere to remove the pore-forming agent in three stages to form a porous material.

Benefits of technology

It achieves safe, green and environmentally friendly uniform and controllable pore size, highly uniform pore structure, and excellent pore connectivity, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107166A_ABST
    Figure CN123107166A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of polymer functional membrane materials technology, specifically relating to a PTFE porous material based on thermally induced phase separation and its preparation method. The method of this invention is as follows: (1) a pore-forming agent solution is mixed evenly with PTFE dispersion resin powder to obtain a wet powder. Under sealed conditions, the wet powder is cured to obtain a cured mixture. The pore-forming agent solution is prepared by dissolving lauric acid in anhydrous ethanol. (2) The cured mixture is pre-pressed into a green body, and then the green body is extruded to obtain a raw material. (3) The raw material is heat-treated in an inert gas atmosphere to remove the pore-forming agent and complete the shaping, thereby obtaining the PTFE porous material. This invention provides a PTFE porous material preparation method with high process safety, no pore-forming agent residue, and uniform and controllable pore size. It particularly solves the problems of flammable organic solvents, solid pore-forming agent agglomeration, and difficulty in pore size control in traditional methods.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer functional membrane materials technology, specifically relating to a PTFE porous material based on thermally induced phase separation and its preparation method. Background Technology

[0002] Polytetrafluoroethylene (PTFE) is an ideal membrane material for membrane distillation, oil-water separation, and air filtration due to its excellent chemical stability, thermal stability, low surface energy, and hydrophobicity. However, PTFE is extremely difficult to dissolve in common solvents, and its porous membrane manufacturing methods are very limited.

[0003] Currently, the main preparation routes for industrialized PTFE porous membranes include: Mechanical stretching, where PTFE dispersion resin is mixed with a lubricant, extruded as a paste, degreased, and then stretched unidirectionally or bidirectionally to form a "fiber-node" microporous structure. This method requires precision stretching equipment, and the pore size is usually elongated and difficult to control uniformly; the lubricant is often a flammable organic solvent such as naphtha, posing significant safety hazards. Electrospinning, where a small amount of PTFE is co-spun with a sacrificial carrier polymer, and then the carrier is removed by sintering. This method is less efficient and is mostly used for preparing thin-layer membranes, limiting its industrialization. Solid pore-forming agent method, where inorganic salts or organic particles are added to the PTFE matrix to create pores through leaching or decomposition. Solid particles are prone to agglomeration, resulting in large and widely distributed pores with poor permeability.

[0004] In view of this, developing a new method for preparing PTFE porous membranes that is safe, environmentally friendly, and can precisely control pore size and distribution is a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0005] In view of the problems and shortcomings of the existing technology, the present invention aims to provide a PTFE porous material based on thermally induced phase separation and its preparation method.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: This invention provides a method for preparing PTFE porous materials based on thermally induced phase separation, comprising the following steps: (1) The pore-forming agent solution is mixed evenly with PTFE dispersion resin powder to obtain wet powder. Under closed conditions, the wet powder is subjected to aging treatment to obtain aging mixture; wherein, the pore-forming agent solution is prepared by dissolving lauric acid in a solvent; (2) The matured mixture is pre-pressed into a blank, and then the blank is extruded to obtain raw material; (3) In an inert gas atmosphere, the raw material is heat-treated to remove the pore-forming agent and complete the shaping to obtain PTFE porous material.

[0007] Preferably, in step (1), the mass ratio of lauric acid to anhydrous ethanol in the pore-forming agent solution is 1:(1.5-10).

[0008] More preferably, in step (1), the mass ratio of lauric acid to anhydrous ethanol in the pore-forming agent solution is 1:(2-5).

[0009] Preferably, in step (1), the mass ratio of lauric acid to PTFE dispersion resin powder is (10-40):100.

[0010] More preferably, in step (1), the mass ratio of lauric acid to PTFE dispersion resin powder is (18-25):100.

[0011] Preferably, in step (3), the heat treatment includes three stages; the first stage heat treatment is: heating the raw material to 48-85°C and holding it for 15-180 minutes to melt and remove the pore-forming agent from the raw material; the second stage heat treatment is: heating the raw material after the first stage heat treatment to 280-350°C and holding it for 5-60 minutes to vaporize the residual pore-forming agent in the raw material; the third stage heat treatment is: heating the raw material after the second stage heat treatment to 350-400°C and holding it for 5-120 seconds to complete the shaping.

[0012] Preferably, the heating rate of the first stage heat treatment process is 0.1–3 °C / min; the heating rate of the second stage heat treatment process is 0.5–8 °C / min. Preferably, during the first stage of heat treatment, the heat preservation process can be carried out by centrifugation or pressurized gas to remove the pore-forming agent from the raw material.

[0013] Preferably, the centrifugation speed is 300 to 3000 rpm.

[0014] Preferably, in step (1), the mixing speed is 50 to 500 rpm and the mixing time is 5 to 30 minutes.

[0015] Preferably, in step (1), the specific operation of the maturation treatment is to mature the wet powder at 25-55°C for 6-48 hours.

[0016] More preferably, in step (1), the specific operation of the maturation treatment is: to let the wet powder material stand and mature at 35-45°C for 12-24 hours.

[0017] Preferably, in step (2), the raw material is a pipe, sheet, plate or rod.

[0018] Preferably, the pre-compression pressure is 1 to 5 MPa.

[0019] Preferably, the extrusion molding temperature is 25-55°C and the extrusion pressure is 2-20 MPa.

[0020] More preferably, the extrusion molding temperature is 35-45°C and the extrusion pressure is 6-12 MPa.

[0021] Preferably, in step (1), the solvent is any one of anhydrous ethanol, diethyl ether, chloroform, and acetone.

[0022] The present invention also provides a PTFE porous material prepared by the preparation method described in the first aspect above.

[0023] Preferably, the PTFE porous material has an average pore size of 0.05–0.8 μm and a porosity of 40%–75%.

[0024] More preferably, the PTFE porous material has an average pore size of 0.1 μm to 0.5 μm and a porosity of 50% to 65%.

[0025] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) Intrinsically safe process: The use of non-toxic, high-flash-point lauric acid and ethanol completely avoids the risks of flammable and explosive solvents such as naphtha.

[0026] (2) Highly uniform and controllable pore structure: Molecular-level dispersion is achieved by “in-situ solution mixing”, overcoming the stubborn problem of solid pore-forming agent agglomeration. By precisely controlling the concentration of lauric acid solution, heating rate and external driving force, the average pore size can be precisely adjusted at the nanometer to micrometer scale.

[0027] (3) Thorough removal of pore-forming agents: The two-step method of "low-temperature effluent + high-temperature decomposition" is adopted, which is far more efficient than single solvent extraction or high-temperature decomposition. The decomposition products of lauric acid are water and carbon dioxide, with no residual carbon, ensuring the intrinsic purity of the membrane.

[0028] (4) Easy to scale up: The discharge of molten lauric acid is a macroscopic fluid flow, which is less affected by the wall thickness, has low equipment requirements, and has good industrialization prospects. Attached Figure Description

[0029] Figure 1 This is a process flow diagram of Embodiment 1 of the present invention; Figure 2 A scanning electron microscope (SEM) image of the porous membrane surface obtained in Embodiment 1 of the present invention; Figure 3 This is a pore size distribution diagram of Embodiment 1 of the present invention; Figure 4 This is a pore size distribution diagram of Comparative Example 1 of the present invention; Figure 5 This is a scanning electron microscope image of the porous membrane in Comparative Example 1 of the present invention. Detailed Implementation

[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Example 1:

[0031] A method for preparing a PTFE porous membrane based on thermally induced phase separation, the process flow of which is as follows: Figure 1 As shown, the specific steps are as follows: (1) In-situ solution mixing and aging: Dissolve 20g of lauric acid (purity ≥99%) in 60g of anhydrous ethanol and stir until completely dissolved to obtain a pore-forming agent solution. Mix the pore-forming agent solution with 100g of PTFE dispersion resin powder (Daikin F-104, molecular weight 4-6 million) in a high-speed mixer at 150rpm for 15 minutes to obtain a wet powder. Place the wet powder into a sealed container and allow it to stand and mature at 35℃ for 18 hours to allow the lauric acid to be uniformly dispersed at the molecular level on the surface of the PTFE particles, obtaining a matured mixture.

[0032] (2) Paste extrusion molding: The matured mixture is pre-compressed into a φ50mm billet at 2MPa to remove gas. The billet is then loaded into a press and extruded into a tubular shape through an annular die with an outer / inner diameter of 4mm / 2.5mm at a material chamber temperature of 38℃ and an extrusion pressure of 9MPa to obtain a pipe.

[0033] (3) Thermally induced phase separation to remove lauric acid and sintering for shaping: The tubing is suspended vertically in a tube furnace under nitrogen protection. The following procedure is set: In the first stage, the pipe is heated to 65°C at a rate of 1°C / min and kept at that temperature for 90 minutes. The solid lauric acid melts into a low-viscosity liquid and flows out of the PTFE matrix under gravity, forming primary channels. In the second stage, the pipes that have undergone the first stage heat treatment are heated to 320°C at 2°C / min and held for 20 minutes to completely vaporize and decompose the residual lauric acid, forming secondary nanopores. In the third stage, the pipes that have undergone the second stage of heat treatment are heated to 380°C, sintered for 25 seconds, and then naturally cooled. The PTFE fiber nodes are fused together, and the porous structure is permanently fixed, thus obtaining the PTFE porous membrane.

[0034] Figure 2 This is a scanning electron microscope (SEM) image of the surface of the PTFE porous membrane obtained in Example 1. Figure 2As can be seen, the membrane exhibits a typical three-dimensional network hierarchical porous structure, with pore walls composed of interwoven PTFE fibrils and nodes. The pores are evenly distributed and have clear outlines, with no obvious macropore defects or closed-pore regions observed. This microstructure directly verifies that the "in-situ solution mixing + low-temperature melt flowout" technical route described in this invention can effectively construct a porous network with good connectivity and uniform structure, providing structural assurance for high porosity and excellent permeability.

[0035] Figure 3 The pore size distribution diagram for Example 1 shows a narrow single-peak shape with an average pore size of approximately 0.32 μm, and over 90% of the pore size is concentrated in the 0.25–0.40 μm range. This result demonstrates that even under conditions where lauric acid is discharged solely by gravity, the present invention achieves pore size uniformity far superior to traditional solid porogen methods, fully proving the precise control over pore size distribution achieved by the molecular-level dispersed porogen strategy. Example 2:

[0036] A method for preparing a PTFE porous membrane based on thermally induced phase separation, the specific steps of which are as follows: (1) In-situ solution mixing and aging: Dissolve 20g of lauric acid (purity ≥99%) in 60g of anhydrous ethanol and stir until completely dissolved to obtain a pore-forming agent solution. Mix the pore-forming agent solution with 100g of PTFE dispersion resin powder (Daikin F-104, molecular weight 4-6 million) in a high-speed mixer at 150rpm for 15 minutes to obtain a wet powder. Place the wet powder into a sealed container and allow it to stand and mature at 35℃ for 18 hours to allow the lauric acid to be uniformly dispersed at the molecular level on the surface of the PTFE particles, obtaining a matured mixture.

[0037] (2) Paste extrusion molding: The matured mixture is pre-compressed into a φ50mm billet at 2MPa to remove gas. The billet is then loaded into a press and extruded into a tubular shape through an annular die with an outer / inner diameter of 4mm / 2.5mm at a material chamber temperature of 38℃ and an extrusion pressure of 9MPa to obtain a pipe.

[0038] (3) Thermally induced phase separation to remove lauric acid and sintering for shaping: Place the pipe horizontally into the nitrogen-filled centrifuge drum. Set the following program: In the first stage, the pipe is heated to 65°C at a rate of 1°C / min and kept at a centrifugal speed of 800 rpm throughout the process to remove the molten lauric acid.

[0039] In the second stage, the pipes that have undergone the first stage of heat treatment are heated to 320°C at 2°C / min, without centrifugation, and kept at this temperature for 20 minutes. The residual lauric acid is completely vaporized and decomposed to form secondary nanopores. In the third stage, the pipes that have undergone the second stage of heat treatment are heated to 380°C, sintered for 25 seconds without centrifugation, and then cooled naturally. The PTFE fibril nodes are fused together, and the porous structure is permanently fixed, thus obtaining the PTFE porous membrane.

[0040] The porosity, average pore size, and tensile strength of the PTFE porous membranes from Examples 1 and 2 were tested using a porosity meter, a membrane pore size analyzer, and a tensile testing machine, respectively. The test results are shown in Table 1.

[0041] Table 1. Porosity, average pore size, and tensile strength of the PTFE porous membranes in Examples 1 and 2

[0042] As shown in Table 1, centrifugation can remove molten lauric acid to obtain PTFE porous membranes with higher porosity and lower pore size. Centrifugation can remove molten lauric acid more quickly, so that some pores are retained to the greatest extent, resulting in membrane materials with higher porosity. Example 3:

[0043] The content of Example 3 is basically the same as that of Example 2, except that the amount of lauric acid used in step (1) is 10g. Example 4:

[0044] The content of Example 4 is basically the same as that of Example 2, except that in step (1), the amount of lauric acid used is 18g. Example 5:

[0045] The content of Example 5 is basically the same as that of Example 2, except that the amount of lauric acid used in step (1) is 22g. Example 6:

[0046] The content of Example 6 is basically the same as that of Example 2, except that the amount of lauric acid used in step (1) is 28g. Example 7:

[0047] The content of Example 7 is basically the same as that of Example 2, except that the amount of lauric acid used in step (1) is 35g.

[0048] The porosity, average pore size, and tensile strength of the PTFE porous membranes from Examples 2, 3-7 were tested. The results are shown in Table 2.

[0049] Table 2. Porosity, average pore size, and tensile strength of the PTFE porous membranes in Examples 2, 3-7.

[0050] As shown in Table 2, with the gradual increase of lauric acid content, the tensile strength of the resulting membrane material gradually decreases while the porosity gradually increases. This is because with the increase in lauric acid content, subsequent processing removes more pores and fewer nodes, resulting in a corresponding decrease in tensile strength. Example 8:

[0051] The content of Example 8 is basically the same as that of Example 5, except that: in step (1), the amount of lauric acid used is 22g, and the mass ratio of lauric acid to anhydrous ethanol is 1:1.5; in step (2), the extrusion pressure is 10.5MPa. Example 9:

[0052] The content of Example 9 is basically the same as that of Example 5, except that: in step (1), the amount of lauric acid used is 22g, and the mass ratio of lauric acid to anhydrous ethanol is 1:2; in step (2), the extrusion pressure is 9.5MPa.

[0053] Example 10: The content of Example 10 is basically the same as that of Example 5, except that: in step (1), the amount of lauric acid used is 22g, and the mass ratio of lauric acid to anhydrous ethanol is 1:5; in step (2), the extrusion pressure is 8.5MPa.

[0054] Example 11: The content of Example 11 is basically the same as that of Example 5, except that: in step (1), the amount of lauric acid used is 22g, and the mass ratio of lauric acid to anhydrous ethanol is 1:10; in step (2), the extrusion pressure is 7MPa.

[0055] The porosity, average pore size, and tensile strength of the PTFE porous membranes from Examples 5, 8-11 were tested. The results are shown in Table 3.

[0056] Table 3. Porosity, average pore size, and tensile strength of the PTFE porous membranes in Examples 5, 8-11

[0057] As shown in Table 3, when the proportion of anhydrous ethanol is too low (mass ratio 1:1.5), the solvent is insufficient to fully dissolve and disperse lauric acid, resulting in particle agglomeration in the wet powder and generally poor mixing uniformity. The powder is generally dry, leading to high extrusion resistance, increased extrusion pressure, poor extrusion continuity, and a decrease in the tensile strength of the final product. When the solvent ratio is in the range of 1:2 to 1:5, the wet powder exhibits excellent mixing uniformity, moderate extrusion pressure, and a continuous and stable extrusion molding process. The resulting PTFE porous material possesses good porosity, pore size, and tensile strength, which is the preferred ratio range for this invention. Further increasing the anhydrous ethanol ratio to 1:10, although the powder mixing uniformity is acceptable, results in an excessively high total solvent volume. During extrusion, the solvent occupies a large volume of the system, deteriorating the uniformity of the extruded preform and causing a significant decrease in the tensile strength of the product, which is detrimental to obtaining high-performance porous products. In this system, anhydrous ethanol serves as a solvent for lauric acid, enabling molecular-level dispersion of the pore-forming agent. Simultaneously, it acts as an extrusion booster. As the amount of solvent added decreases, the required extrusion pressure increases, and as the amount of solvent increases, the required extrusion pressure decreases.

[0058] Example 12: The content of Example 12 is basically the same as that of Example 2, except that in step (3), the heating rate of the first stage heat treatment is 0.3℃ / min.

[0059] Example 13: The content of Example 13 is basically the same as that of Example 2, except that in step (3), the heating rate of the first stage heat treatment is 0.8℃ / min.

[0060] Example 14: The content of Example 14 is basically the same as that of Example 2, except that in step (3), the heating rate of the first stage heat treatment is 1.5℃ / min.

[0061] Example 15: The content of Example 15 is basically the same as that of Example 2, except that in step (3), the heating rate of the first stage heat treatment is 3℃ / min.

[0062] Example 16: The content of Example 16 is basically the same as that of Example 2, except that in step (3), the heating rate of the first stage heat treatment is 5℃ / min.

[0063] The porosity, average pore size, and tensile strength of the PTFE porous membranes from Examples 2, 12-16 were tested. The results are shown in Table 4.

[0064] Table 4. Porosity, average pore size, and tensile strength of the PTFE porous membranes in Examples 2, 12-16

[0065] As shown in Table 4, the membrane structure begins to deteriorate when the heating rate in the first stage exceeds 3°C / min. This is because the excessively rapid heating rate leads to the rapid decomposition of lauric acid, resulting in the rapid release of a large amount of gas, which damages the membrane, causing the membrane tube to rupture and reducing its tensile strength.

[0066] Example 17: The content of Example 17 is basically the same as that of Example 2, except that in step (3), the centrifugation speed is 300 rpm.

[0067] Example 18: The content of Example 18 is basically the same as that of Example 2, except that in step (3), the centrifugation speed is 1500 rpm.

[0068] Example 19: The content of Example 19 is basically the same as that of Example 2, except that in step (3), the centrifugation speed is 3000 rpm.

[0069] The porosity, average pore size, and tensile strength of the PTFE porous membranes from Examples 1, 2, and 17-19 were tested. The results are shown in Table 5.

[0070] Table 5. Porosity, average pore size, and tensile strength of Examples 1, 2, and 17-19

[0071] As shown in Table 5, centrifugal force can effectively overcome the capillary force of liquid lauric acid and significantly improve the uniformity of pore distribution. The effect tends to stabilize when the centrifugal speed reaches above 800 rpm.

[0072] Example 20: The content of Example 20 is basically the same as that of Example 2, except that in step (1), the PTFE dispersion resin used is DuPont 601A.

[0073] Example 21: The content of Example 21 is basically the same as that of Example 2, except that in step (1), the PTFE dispersion resin used is Chenguang SFN-01.

[0074] Example 22: The content of Example 22 is basically the same as that of Example 2, except that in step (1), the PTFE dispersion resin used is Chenguang SFN-03.

[0075] The porosity, average pore size, and tensile strength of the PTFE porous membranes from Examples 2, 21-22 were tested. The results are shown in Table 6.

[0076] Table 6. Porosity, average pore size, and tensile strength of the PTFE porous membranes in Examples 2, 21-22

[0077] As shown in Table 7, the method of the present invention is applicable to all commercially available PTFE dispersion resins, and some parameters need to be finely adjusted according to the molecular weight.

[0078] Example 23: The content of Example 23 is basically the same as that of Example 2, except that in step (2), a T-shaped slit die is used and the extruded product is a flat film.

[0079] Example 24: The content of Example 24 is basically the same as that of Example 2, except that in step (2), a circular die is used and the extruded product is in the form of a rod.

[0080] The porosity, average pore size, and tensile strength of the PTFE porous membranes from Examples 2, 23, and 24 were tested. The results are shown in Table 7.

[0081] Table 7. Porosity, average pore size, and tensile strength of the PTFE porous membranes in Examples 2, 23, and 24

[0082] As shown in Table 7, the method of the present invention can be used for various shapes such as covers, tubes, and plates.

[0083] Comparative Example 1: A method for preparing a PTFE porous membrane, the specific steps of which are as follows: (1) In-situ solution mixing and aging: 22g of commercially available naphtha (Exxsol D60) and 100g of PTFE dispersion resin powder (Daikin F-104, molecular weight 4 million-6 million) were mixed in a high-speed mixer at 150 rpm for 15 minutes to obtain a wet powder. The wet powder was placed in a sealed container and allowed to stand and mature at 35°C for 18 hours to obtain a matured mixture.

[0084] (2) Paste extrusion molding: The matured mixture is pre-compressed into a φ50mm billet at 2MPa to remove gas. The billet is then loaded into a press and extruded into a tubular shape through an annular die with an outer / inner diameter of 4mm / 2.5mm at a material chamber temperature of 38℃ and an extrusion pressure of 9MPa to obtain a pipe.

[0085] (3) Defatting: The tubing is suspended vertically in a tube furnace under nitrogen protection. The following procedure is set: In the first stage, the pipe is heated to 65°C at a rate of 1°C / min and kept at that temperature for 90 minutes.

[0086] In the second stage, the pipes that have undergone the first stage of heat treatment are degreased at 2℃ / min to 180℃. After degreasing, the membrane is rapidly stretched to twice its length at 180℃ using a stretching machine.

[0087] In the third stage, the pipes that have undergone the second stage of heat treatment are heated to 380°C, sintered for 25 seconds, and then naturally cooled. The PTFE fiber nodes are fused together, and the porous structure is permanently fixed, thus obtaining the PTFE porous membrane.

[0088] Figure 4 The image shows the pore size distribution of Comparative Example 1 (traditional naphtha stretching method). The curve exhibits a distinct bimodal distribution, with pore sizes ranging from 0.1 to 1.2 μm and an average pore size of 0.55 μm. Many pores are elongated and narrow, characteristic of the anisotropic structure of the "fiber-node" structure obtained through the stretching method. Figure 4 and Figure 3 As can be seen from the comparison, the pore size distribution of the present invention is significantly narrower and more concentrated than that of the comparative example, indicating that the thermally induced phase separation pore-forming method of the present invention has outstanding progress in terms of pore size controllability.

[0089] Figure 5 The image shown is a scanning electron microscope (SEM) image of the porous membrane in Comparative Example 1. The pores exhibit a directional, elongated, slit-like morphology with poor inter-pore connectivity and significant structural asymmetry along the membrane thickness direction. In contrast... Figure 2 The membrane structure of the present invention, as shown, has an isotropic three-dimensional network of pores, exhibiting significantly superior connectivity and symmetry. This comparison further highlights the adaptability of the membrane structure of the present invention in isotropic mass transfer applications such as membrane distillation and gas filtration.

[0090] comprehensive Figures 2 to 5Comparative analysis shows that the PTFE porous membrane prepared by this invention has three-dimensional isotropic microstructure characteristics, concentrated pore size distribution, and excellent pore connectivity. Compared with the traditional stretching method, it has achieved substantial improvements in pore size distribution width, pore shape regularity, and structural symmetry. The above-mentioned figures and data fully support the technical effects described in the specification of this invention, such as "uniform and controllable pore size, no residue of pore-forming agent, and symmetrical membrane structure," and also provide intuitive morphological and statistical basis for the product parameter range described in the claims of this invention.

[0091] Comparative Example 2: A method for preparing a PTFE porous membrane, the specific steps of which are as follows: (1) In-situ solution mixing and aging: Dissolve 20g of lauric acid (purity ≥99%) in 60g of anhydrous ethanol and stir until completely dissolved to obtain a pore-forming agent solution. Mix the pore-forming agent solution with 100g of PTFE dispersion resin powder (Daikin F-104, molecular weight 4-6 million) in a high-speed mixer at 150rpm for 15 minutes to obtain a wet powder. Place the wet powder into a sealed container and allow it to stand and mature at 35℃ for 18 hours to allow the lauric acid to be uniformly dispersed at the molecular level on the surface of the PTFE particles, obtaining a matured mixture.

[0092] (2) Paste extrusion molding: The matured mixture is pre-compressed into a φ50mm billet at 2MPa to remove gas. The billet is then loaded into a press and extruded into a tubular shape through an annular die with an outer / inner diameter of 4mm / 2.5mm at a material chamber temperature of 38℃ and an extrusion pressure of 9MPa to obtain a pipe.

[0093] (3) The pipe is vertically suspended in a tube furnace with nitrogen protection and sintered at 10℃ / min from room temperature to 380℃. After sintering, a PTFE porous membrane is obtained.

[0094] Test results: The PTFE porous membrane prepared in this comparative example showed severe bubbling, deformation, and partial rupture. Carbonized residues were detected inside. This verifies the necessity of establishing a slow melt flow stage.

[0095] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit the scope of protection of the present invention. Those skilled in the art can modify or make equivalent substitutions to the technical solutions of the present invention based on the concept of the present invention, without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A method for producing a PTFE porous material based on thermally induced phase separation, characterized in that, Includes the following steps: (1) The pore-forming agent solution is mixed evenly with PTFE dispersion resin powder to obtain wet powder. Under closed conditions, the wet powder is subjected to aging treatment to obtain aging mixture; wherein, the pore-forming agent solution is prepared by dissolving lauric acid in a solvent; (2) The matured mixture is pre-pressed into a green body, and then the green body is extruded to obtain raw material; (3) In an inert gas atmosphere, the raw material is heat-treated to remove the pore-forming agent and complete the shaping to obtain PTFE porous material.

2. The production method according to claim 1, characterized by, In step (1), the mass ratio of lauric acid to anhydrous ethanol in the pore-forming agent solution is 1:(1.5-10).

3. The production method according to claim 1, characterized by, In step (1), the mass ratio of lauric acid to PTFE dispersion resin powder is (10-40):

100.

4. The method of claim 1, wherein, In step (3), the heat treatment includes three stages: the first stage heat treatment is to heat the raw material to 48-85°C and hold it for 15-180 minutes; the second stage heat treatment is to heat the raw material after the first stage heat treatment to 280-350°C and hold it for 5-60 minutes; the third stage heat treatment is to heat the raw material after the second stage heat treatment to 350-400°C and hold it for 5-120 seconds.

5. The preparation method according to claim 4, characterized in that, The heating rate of the first stage heat treatment process is 0.1 to 3 °C / min; the heating rate of the second stage heat treatment process is 0.5 to 8 °C / min; during the first stage heat treatment, the heat preservation process can be carried out by centrifugation or pressurized gas to remove the pore-forming agent from the raw material.

6. The production method according to claim 5, wherein The centrifuge speed is 300-3000 rpm.

7. The preparation method according to claim 1, characterized in that, In step (1), the mixing speed is 50-500 rpm and the mixing time is 5-30 minutes; the specific operation of the maturation treatment is: the wet powder is left to stand and mature at 25-55℃ for 6-48 hours; the raw material in step (2) is pipe, sheet, plate or rod.

8. The method of claim 1, wherein, In step (2), the pre-pressing pressure is 1-5 MPa; the extrusion molding temperature is 25-55℃ and the extrusion pressure is 2-20 MPa; in step (1), the solvent is any one of anhydrous ethanol, diethyl ether, chloroform and acetone.

9. A porous PTFE material prepared by any one of the preparation methods described in claims 1-8.

10. The PTFE porous material of claim 9, wherein, The PTFE porous material has an average pore size of 0.05–0.8 μm and a porosity of 40%–75%.