A low-dielectric polyimide microporous film and its preparation method

Low-dielectric polyimide microporous films were prepared by reacting diamine monomers with amino boron nitride, which solved the problem of high dielectric constant of polyimide films, enabling their application in high-frequency electronic devices and improving the mechanical and thermal stability of the films.

CN123107168APending Publication Date: 2026-11-17GUANGZHOU LIANMAO ELECTRONICS TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611375580.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The high dielectric constant and loss factor of existing polyimide films limit their application in high-frequency electronic devices, and traditional methods for reducing these properties suffer from performance loss or non-uniformity issues.

Method used

A polyamic acid solution was generated by reacting a diamine monomer with aminated boron nitride and hexafluorodianhydride. Low-dielectric polyimide microporous films were prepared by heat treatment. The dielectric constant was reduced by using fluorene rings and fluorine atoms, and the mechanical properties were enhanced by aminated boron nitride.

Benefits of technology

This reduces the dielectric constant and dielectric loss of the thin film while improving its mechanical properties and thermal stability, enabling its application in high-frequency electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107168A_ABST
    Figure CN123107168A_ABST
Patent Text Reader

Abstract

This invention discloses a low-dielectric polyimide microporous film and its preparation method, relating to the field of membrane technology. The invention prepares a diamine monomer with a fluorene ring and fluorine-containing groups, which undergoes a nucleophilic addition reaction with aminated boron nitride and hexafluorodianhydride to generate polyamic acid via ring-opening polymerization. Finally, it is heat-treated to imidize the polyimide, yielding a low-dielectric polyimide microporous film. The fluorene ring disrupts the close packing of molecular chains, increasing intermolecular porosity. This, combined with the strong electronegativity and large steric hindrance of fluorine atoms, reduces the dielectric constant of the film. The aminated boron nitride surface is grafted with a B-O-Si hybrid structure and reactive amino groups, improving the dispersibility of boron nitride and reducing interfacial defects. Boron nitride itself possesses intrinsically low dielectric properties, which, in conjunction with fluorine atoms, effectively reduce the dielectric constant and dielectric loss of the film. The polarizability of the B-O bond is lower than that of the Si-O bond, contributing to a synergistic effect in reducing the dielectric constant of the film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of membrane technology, specifically to a low-dielectric polyimide microporous film and its preparation method. Background Technology

[0002] Polyimide is a polymer material with high temperature resistance, high strength, and good chemical stability, and it is widely used in electronics, communications and other fields.

[0003] Traditional polyimide has a high dielectric constant and loss factor, limiting its application in high-frequency electronic devices. Currently, methods to reduce the dielectric constant of polyimide films mainly include introducing fluorinated monomers, introducing inorganic nanoparticles, and adding pore-forming agents. However, each method has limitations. For example, excessive introduction of fluorinated monomers can affect other film properties; inorganic nanoparticles have poor compatibility; and adding pore-forming agents may lead to uneven pore size and reduced mechanical properties of the film. For instance, patent CN202111008359.X discloses a low-dielectric-performance thermoplastic polyimide resin composite film and its preparation method. This involves introducing ester groups and fluorine onto polyimide and then blending it with LCP resin to obtain a composite film. However, LCP resin is a low-polarity aromatic polyester, while polyimide contains a strongly polar imide ring. Although ester groups are introduced to improve compatibility, the polarity difference between the two is significant, resulting in weak interfacial bonding during blending and easy phase separation, thus affecting film performance.

[0004] Therefore, this invention proposes a low-dielectric polyimide microporous film and its preparation method, which improves the mechanical properties and high-temperature resistance of the polyimide film while reducing its dielectric constant. Summary of the Invention

[0005] The purpose of this invention is to provide a low-dielectric polyimide microporous film and its preparation method, so as to solve the problems raised in the prior art.

[0006] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing a low-dielectric polyimide microporous film, comprising the following steps: Step 1: Mix 2,7-dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, and tetrahydrofuran. Add potassium carbonate aqueous solution and methyltrioctylammonium chloride under an argon atmosphere. Heat the mixture to react. After the reaction is complete, extract, rotary evaporate, and purify to obtain the nitrated intermediate. Step 2: Mix the nitration intermediate and anhydrous ethanol, heat to 70-80°C under an argon atmosphere, add palladium on carbon and hydrazine hydrate, reflux at a constant temperature, filter after the reaction is complete, refrigerate to crystallize, and vacuum dry to obtain the diamine monomer; Step 3: Mix the diamine monomer, aminated boron nitride, and N,N-dimethylacetamide, stir and disperse, then add hexafluorodianhydride and pore-forming agent, and react in a water bath to obtain a polyamic acid solution; Step 4: Coat the mold with polyamic acid solution, perform heat treatment, demold, and obtain a low dielectric polyimide microporous film.

[0007] Furthermore, in step 1, the ratio of 2,7-dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, tetrahydrofuran, potassium carbonate aqueous solution, and methyltrioctylammonium chloride is (1~3) g : (2.1~6.5) g : 200 mL : (3.2~10.3) g : (0.06~0.16) g; The concentration of the potassium carbonate aqueous solution is 1.8~2.2 mol / L.

[0008] Furthermore, in step 1, the process conditions for the heating reaction are: temperature 70~75℃, time 20~24h; The process conditions for rotary evaporation are: temperature 40~50℃, time 40~60min.

[0009] Furthermore, in step 2, the ratio of the nitration intermediate, anhydrous ethanol, palladium on carbon, and hydrazine hydrate is (1~2) g: 250 mL: (0.025~0.05) g: (2~4) mL; The mass fraction of palladium on carbon is 10%.

[0010] Furthermore, in step 2, the process conditions for the isothermal reflux reaction are: temperature 70~80℃, time 20~24h.

[0011] Furthermore, in step 2, the process conditions for cold crystallization are: temperature 0~4℃, time 20~24h; The vacuum drying process conditions are: temperature 60~65℃, time 20~24h.

[0012] Furthermore, in step 3, the mass ratio of diamine monomer, amino boron nitride, N,N-dimethylacetamide, hexafluorodianhydride and porogen is (3.4~4.4):(0.3~0.5):60:(3.3~3.9):(0.035~0.20).

[0013] Furthermore, the porogen is one of dimethyl phthalate and dibutyl phthalate.

[0014] Furthermore, in step 3, the process conditions for the water bath stirring reaction are: temperature 0~20℃, time 12~24h.

[0015] Furthermore, in step 4, the coating thickness of the polyamic acid solution is 150~250μm.

[0016] Furthermore, in step 4, the heat treatment process conditions are as follows: heat treatment at 75~85℃ for 2~3h; heat treatment at 110~120℃ for 0.8~1.2h; heat treatment at 170~180℃ for 0.8~1.2h; heat treatment at 240~250℃ for 0.8~1.2h; heat treatment at 290~310℃ for 0.8~1.2h; and the heating rate is 3~5℃ / min.

[0017] In the above technical solution, firstly, the palladium catalyst undergoes oxidative addition with the C-Br bond in 2,7-dibromofluorene. 3-Nitro-4-(trifluoromethoxy)phenylboronic acid is metallized under the action of potassium carbonate, replacing the bromine atom site. Finally, after reduction and elimination, the two aryl groups couple to form a new C-C bond, generating an intermediate containing trifluoromethoxy and nitro groups, which is the nitration intermediate. Then, hydrazine hydrate decomposes on the palladium carbon surface to generate active hydrogen. After the nitro group is adsorbed on the palladium surface, the active hydrogen gradually reduces it to an amino group, obtaining a diamine monomer. The diamine monomer and the amino group of aminated boron nitride attack the carbonyl carbon of the anhydride of hexafluorodianhydride, undergoing a nucleophilic addition reaction, ring-opening polymerization to generate a polyamic acid molecular chain. Finally, heat treatment is performed to imide it, obtaining a low-dielectric polyimide microporous film.

[0018] Furthermore, the aminated boron nitride is prepared by the following process: S1: Mix phenylboronic acid, phenyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, p-toluenesulfonic acid and anhydrous toluene, heat under reflux and react. After the reaction is complete, recrystallize to obtain borosilicate. S2: Hydroxylated boron nitride, boron-containing siloxane and toluene are mixed and heated under a nitrogen atmosphere and refluxed. After the reaction is completed, the mixture is filtered, washed and dried to obtain aminolated boron nitride.

[0019] Furthermore, in S1, the molar ratio of phenylboronic acid, phenyltrimethoxysilane, and γ-aminopropylmethyldiethoxysilane is 1:(1.2~1.6):(0.8~1.2). In S1, the ratio of phenylboronic acid, p-toluenesulfonic acid and anhydrous toluene is (2~5) g : (0.01~0.25) g : 50 mL.

[0020] Furthermore, in S1, the process conditions for the heating reflux reaction are: temperature 100~110℃, time 6~8h.

[0021] Furthermore, in S2, the ratio of hydroxylated boron nitride, borosilicate, and toluene is (1~3) g: (0.3~0.9) mL: 100 mL.

[0022] Furthermore, in S2, the process conditions for the heating reflux reaction are: temperature 100~110℃, time 8~12h; In S2, the drying process conditions are: temperature 50~60℃, time 8~12h.

[0023] In the above technical solution, the boron hydroxyl group of phenylboronic acid undergoes a de-alcoholization condensation reaction with the methoxysilane of phenyltrimethoxysilane and γ-aminopropylmethyldiethoxysilane to form a BO-Si covalent bond. By controlling the molar amount, the product retains hydrolyzable ethoxy groups to obtain boron-containing siloxanes. Then, the ethoxy groups are hydrolyzed to generate silanol groups, which undergo dehydration condensation with the hydroxyl groups on the surface of hydroxylated boron nitride to graft BO-Si onto the surface of boron nitride to obtain aminated boron nitride.

[0024] Compared with the prior art, the beneficial effects of the present invention are: 1. The diamine monomer prepared in this invention has a fluorene ring and a fluorine-containing group. After the fluorene ring is introduced into the main chain, it will disrupt the close packing of the molecular chain, increase the intermolecular gap, and work synergistically with the fluorine atom, which has strong electronegativity and large steric hindrance, thereby reducing the dielectric constant of the film. The fluorene ring and the imide ring also jointly endow the film with excellent thermal stability. In addition, the introduction of aminated boron nitride can not only restrict the movement of molecular chain segments, thereby reducing the dielectric constant, but also enhance and improve the mechanical properties of the film. Moreover, the surface amino group makes the compatibility of boron nitride with polyimide better, further enhancing the stability of various properties.

[0025] 2. The aminated boron nitride prepared in this invention has a BO-Si hybrid structure and reactive amino groups grafted onto its surface. The amino groups participate in the reaction of polyimide, improving the dispersibility of boron nitride and reducing interface defects. Boron nitride itself has intrinsic low dielectric properties, which can work synergistically with fluorine atoms to effectively reduce the dielectric constant and dielectric loss of the film. The polarizability of BO bonds is lower than that of Si-O bonds, which synergistically reduces the dielectric constant of the film. In addition, the BO-Si hybrid interface can also play a stress buffering role and improve the mechanical properties of the film. Attached Figure Description

[0026] Figure 1 This is a schematic diagram of the synthetic route for the diamine monomer of the present invention; Figure 2 This is a flowchart of the preparation process of the present invention. Detailed Implementation

[0027] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0028] In the following specific implementation, Palladium on carbon, mass fraction 10%; Hydroxylated boron nitride, with an average flake diameter of 0.25 μm; The pore-forming agent is dimethyl phthalate.

[0029] Example 1: A method for preparing a low-dielectric polyimide microporous film, comprising the following steps: (1) Preparation of aminated boron nitride: S1: Phenyboric acid, phenyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, p-toluenesulfonic acid, and anhydrous toluene were mixed and refluxed at 110°C for 8 hours. After the reaction, the mixture was recrystallized to obtain boron-containing siloxane. In S1, the molar ratio of phenylboric acid, phenyltrimethoxysilane, and γ-aminopropylmethyldiethoxysilane was 1:1.6:1.2. In S1, the ratio of phenylboric acid, p-toluenesulfonic acid, and anhydrous toluene was 5g:0.25g:50mL. S2: Hydroxylated boron nitride, boron-containing siloxane, and toluene were mixed at 3g:0.9mL:100mL and refluxed at 110°C for 12 hours under a nitrogen atmosphere. After the reaction, the mixture was filtered, washed, and dried at 60°C for 12 hours to obtain amino-containing boron nitride. (2) Preparation of low-dielectric polyimide microporous films: Step 1: 2,7-Dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, and tetrahydrofuran were mixed, and potassium carbonate aqueous solution and methyltrioctylammonium chloride were added under an argon atmosphere. The mixture was heated to 75°C and reacted for 24 hours. After the reaction was completed, the mixture was extracted, rotary evaporated at 50°C for 60 minutes, and then purified to obtain the nitrated intermediate. In Step 1, 2,7-Dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, tetrahydrofuran, potassium carbonate aqueous solution, and... The ratio of methyltrioctylammonium chloride was 3g:6.5g:200mL:10.3g:0.16g; the concentration of potassium carbonate aqueous solution was 2.2mol / L; Step 2: The nitration intermediate and anhydrous ethanol were mixed and heated to 80℃ under an argon atmosphere. Palladium on carbon and hydrazine hydrate were added, and the mixture was refluxed at 80℃ for 24h. After the reaction was completed, the mixture was filtered, crystallized at 4℃ for 24h, and then vacuum dried at 65℃ for 24h to obtain the diamine monomer; In Step 2, The ratio of nitration intermediate, anhydrous ethanol, palladium on carbon, and hydrazine hydrate was 2 g: 250 mL: 0.05 g: 4 mL; Step 3: The diamine monomer, aminated boron nitride, and N,N-dimethylacetamide were mixed, stirred, and dispersed. Then, hexafluorodianhydride and a porogen were added, and the mixture was stirred in a water bath at 20°C for 24 h to obtain a polyamic acid solution; In Step 3, the mass ratio of diamine monomer, aminated boron nitride, N,N-dimethylacetamide, hexafluorodianhydride, and porogen was 4.4:0. 5:60:3.9:0.20; Step 4: Coat the polyamic acid solution onto the mold, perform heat treatment, demold, and obtain a low-dielectric polyimide microporous film; The coating thickness of the polyamic acid solution is 250μm; The heat treatment process conditions are: heat treatment at 85℃ for 3h; heat treatment at 120℃ for 1.2h; heat treatment at 180℃ for 1.2h; heat treatment at 250℃ for 1.2h; heat treatment at 310℃ for 1.2h; The heating rate is 5℃ / min.

[0030] Example 2: A method for preparing a low-dielectric polyimide microporous film, comprising the following steps: (1) Preparation of aminated boron nitride: S1: Phenyboric acid, phenyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, p-toluenesulfonic acid, and anhydrous toluene were mixed and refluxed at 105°C for 7 hours. After the reaction, the mixture was recrystallized to obtain boron-containing siloxane. In S1, the molar ratio of phenylboric acid, phenyltrimethoxysilane, and γ-aminopropylmethyldiethoxysilane was 1:1.4:1.0. In S1, the ratio of phenylboric acid, p-toluenesulfonic acid, and anhydrous toluene was 3g:0.15g:50mL. S2: Hydroxylated boron nitride, boron-containing siloxane, and toluene were mixed at 2g:0.6mL:100mL and refluxed at 105°C for 10 hours under a nitrogen atmosphere. After the reaction, the mixture was filtered, washed, and dried at 55°C for 10 hours to obtain amino-containing boron nitride. (2) Preparation of low-dielectric polyimide microporous films: Step 1: 2,7-Dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, and tetrahydrofuran were mixed, and potassium carbonate aqueous solution and methyltrioctylammonium chloride were added under an argon atmosphere. The mixture was heated to 73°C and reacted for 22 hours. After the reaction was completed, the mixture was extracted, rotary evaporated at 45°C for 50 minutes, and then purified to obtain the nitrated intermediate. In Step 1, 2,7-Dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, tetrahydrofuran, potassium carbonate aqueous solution, and methyltrioctylammonium chloride were mixed. The ratio of trioctylammonium chloride was 2g:4.5g:200mL:6.5g:0.10g; the concentration of potassium carbonate aqueous solution was 2.0mol / L; Step 2: The nitration intermediate and anhydrous ethanol were mixed and heated to 75℃ under an argon atmosphere. Palladium on carbon and hydrazine hydrate were added, and the mixture was refluxed at 75℃ for 22h. After the reaction was completed, the mixture was filtered, refrigerated at 2℃ for 22h, and then vacuum dried at 63℃ for 22h to obtain the diamine monomer; In Step 2, the nitration... The ratio of intermediate, anhydrous ethanol, palladium on carbon, and hydrazine hydrate was 1.5 g: 250 mL: 0.045 g: 3 mL; Step 3: Diamine monomer, aminated boron nitride, and N,N-dimethylacetamide were mixed, stirred and dispersed, then hexafluorodianhydride and porogen were added, and the mixture was stirred in a water bath at 10 °C for 20 h to obtain a polyamic acid solution; In Step 3, the mass ratio of diamine monomer, aminated boron nitride, N,N-dimethylacetamide, hexafluorodianhydride, and porogen was 4.0:0. 4:60:3.6:0.10; Step 4: Coat the polyamic acid solution onto the mold, perform heat treatment, demold, and obtain a low-dielectric polyimide microporous film; The coating thickness of the polyamic acid solution is 200 μm; The heat treatment process conditions are: heat treatment at 80℃ for 2.5 h; heat treatment at 115℃ for 1.0 h; heat treatment at 175℃ for 1.0 h; heat treatment at 245℃ for 1.0 h; heat treatment at 300℃ for 1.0 h; The heating rate is 4℃ / min.

[0031] Example 3: A method for preparing a low-dielectric polyimide microporous film, comprising the following steps: (1) Preparation of aminated boron nitride: S1: Phenyboric acid, phenyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, p-toluenesulfonic acid, and anhydrous toluene were mixed and refluxed at 100°C for 6 hours. After the reaction, the mixture was recrystallized to obtain boron-containing siloxane. In S1, the molar ratio of phenylboric acid, phenyltrimethoxysilane, and γ-aminopropylmethyldiethoxysilane was 1:1.2:0.8. In S1, the ratio of phenylboric acid, p-toluenesulfonic acid, and anhydrous toluene was 2g:0.01g:50mL. S2: Hydroxylated boron nitride, boron-containing siloxane, and toluene were mixed at 1g:0.3mL:100mL and refluxed at 100°C for 8 hours under a nitrogen atmosphere. After the reaction, the mixture was filtered, washed, and dried at 50°C for 8 hours to obtain amino-containing boron nitride. (2) Preparation of low-dielectric polyimide microporous films: Step 1: 2,7-Dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, and tetrahydrofuran were mixed, and potassium carbonate aqueous solution and methyltrioctylammonium chloride were added under an argon atmosphere. The mixture was heated to 70°C and reacted for 20 h. After the reaction was completed, the mixture was extracted, rotary evaporated at 40°C for 40 min, and then purified to obtain the nitrated intermediate. In Step 1, 2,7-Dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, tetrahydrofuran, potassium carbonate aqueous solution, and... The ratio of methyltrioctylammonium chloride was 1g:2.1g:200mL:3.2g:0.06g; the concentration of potassium carbonate aqueous solution was 1.8mol / L; Step 2: The nitration intermediate and anhydrous ethanol were mixed and heated to 70℃ under an argon atmosphere. Palladium on carbon and hydrazine hydrate were added, and the mixture was refluxed at 70℃ for 20h. After the reaction was completed, the mixture was filtered, crystallized at 0℃ for 20h, and then vacuum dried at 60℃ for 20h to obtain the diamine monomer; In Step 2, the nitration intermediate... The ratio of the basicization intermediate, anhydrous ethanol, palladium on carbon, and hydrazine hydrate was 1 g: 250 mL: 0.025 g: 2 mL; Step 3: The diamine monomer, aminated boron nitride, and N,N-dimethylacetamide were mixed, stirred and dispersed, and then hexafluorodianhydride and porogen were added. The mixture was stirred in a water bath at 0 °C for 12 h to obtain a polyamic acid solution; In Step 3, the mass ratio of the diamine monomer, aminated boron nitride, N,N-dimethylacetamide, hexafluorodianhydride, and porogen was 3.4:0. 3:60:3.3:0.035; Step 4: Coat the polyamic acid solution onto the mold, perform heat treatment, demold, and obtain a low-dielectric polyimide microporous film; The coating thickness of the polyamic acid solution is 150μm; The heat treatment process conditions are: heat treatment at 75℃ for 2h; heat treatment at 110℃ for 0.8h; heat treatment at 170℃ for 0.8h; heat treatment at 240℃ for 0.8h; heat treatment at 290℃ for 0.8h; The heating rate is 3℃ / min.

[0032] Comparative Example 1: Compared with Example 1, the borosilicate was replaced with γ-aminopropylmethyldiethoxysilane, and the other conditions remained the same as in Example 1. Specifically: (1) Preparation of aminated boron nitride: Hydroxylated boron nitride, γ-aminopropylmethyldiethoxysilane and toluene were mixed at a ratio of 3g:0.9mL:100mL and refluxed at 110℃ for 12h under a nitrogen atmosphere. After the reaction was completed, the mixture was filtered, washed and dried at 60℃ for 12h to obtain aminolated boron nitride. (2) Preparation of low-dielectric polyimide microporous films: Step 1: 2,7-Dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, and tetrahydrofuran were mixed, and potassium carbonate aqueous solution and methyltrioctylammonium chloride were added under an argon atmosphere. The mixture was heated to 75°C and reacted for 24 hours. After the reaction was completed, the mixture was extracted, rotary evaporated at 50°C for 60 minutes, and then purified to obtain the nitrated intermediate. In Step 1, 2,7-Dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, tetrahydrofuran, potassium carbonate aqueous solution, and... The ratio of methyltrioctylammonium chloride was 3g:6.5g:200mL:10.3g:0.16g; the concentration of potassium carbonate aqueous solution was 2.2mol / L; Step 2: The nitration intermediate and anhydrous ethanol were mixed and heated to 80℃ under an argon atmosphere. Palladium on carbon and hydrazine hydrate were added, and the mixture was refluxed at 80℃ for 24h. After the reaction was completed, the mixture was filtered, crystallized at 4℃ for 24h, and then vacuum dried at 65℃ for 24h to obtain the diamine monomer; In Step 2, The ratio of nitration intermediate, anhydrous ethanol, palladium on carbon, and hydrazine hydrate was 2 g: 250 mL: 0.05 g: 4 mL; Step 3: The diamine monomer, aminated boron nitride, and N,N-dimethylacetamide were mixed, stirred, and dispersed. Then, hexafluorodianhydride and a porogen were added, and the mixture was stirred in a water bath at 20°C for 24 h to obtain a polyamic acid solution; In Step 3, the mass ratio of diamine monomer, aminated boron nitride, N,N-dimethylacetamide, hexafluorodianhydride, and porogen was 4.4:0. 5:60:3.9:0.20; Step 4: Coat the polyamic acid solution onto the mold, perform heat treatment, demold, and obtain a low-dielectric polyimide microporous film; The coating thickness of the polyamic acid solution is 250μm; The heat treatment process conditions are: heat treatment at 85℃ for 3h; heat treatment at 120℃ for 1.2h; heat treatment at 180℃ for 1.2h; heat treatment at 250℃ for 1.2h; heat treatment at 310℃ for 1.2h; The heating rate is 5℃ / min.

[0033] Comparative Example 2: Compared with Example 1, the diamine monomer was replaced with 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, and all other conditions remained the same as in Example 1. Specifically: (1) Preparation of aminated boron nitride: S1: Phenyboric acid, phenyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, p-toluenesulfonic acid, and anhydrous toluene were mixed and refluxed at 110°C for 8 hours. After the reaction, the mixture was recrystallized to obtain boron-containing siloxane. In S1, the molar ratio of phenylboric acid, phenyltrimethoxysilane, and γ-aminopropylmethyldiethoxysilane was 1:1.6:1.2. In S1, the ratio of phenylboric acid, p-toluenesulfonic acid, and anhydrous toluene was 5g:0.25g:50mL. S2: Hydroxylated boron nitride, boron-containing siloxane, and toluene were mixed at 3g:0.9mL:100mL and refluxed at 110°C for 12 hours under a nitrogen atmosphere. After the reaction, the mixture was filtered, washed, and dried at 60°C for 12 hours to obtain amino-containing boron nitride. (2) Preparation of low-dielectric polyimide microporous films: Step 1: Mix 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, aminated boron nitride, and N,N-dimethylacetamide, stir and disperse, then add hexafluorodianhydride and a porogen, and react in a water bath at 20°C for 24 hours to obtain a polyamic acid solution; In Step 3, the mass ratio of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, aminated boron nitride, N,N-dimethylacetamide, hexafluorodianhydride, and the porogen is 4.4:0. 5:60:3.9:0.20; Step 4: Coat the polyamic acid solution onto the mold, perform heat treatment, demold, and obtain a low-dielectric polyimide microporous film; The coating thickness of the polyamic acid solution is 250μm; The heat treatment process conditions are: heat treatment at 85℃ for 3h; heat treatment at 120℃ for 1.2h; heat treatment at 180℃ for 1.2h; heat treatment at 250℃ for 1.2h; heat treatment at 310℃ for 1.2h; The heating rate is 5℃ / min.

[0034] Comparative Example 3: Compared with Example 1, the diamine monomer was replaced with m-phenylenediamine, and all other conditions remained the same as in Example 1. Specifically: (1) Preparation of aminated boron nitride: S1: Phenyboric acid, phenyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, p-toluenesulfonic acid, and anhydrous toluene were mixed and refluxed at 110°C for 8 hours. After the reaction, the mixture was recrystallized to obtain boron-containing siloxane. In S1, the molar ratio of phenylboric acid, phenyltrimethoxysilane, and γ-aminopropylmethyldiethoxysilane was 1:1.6:1.2. In S1, the ratio of phenylboric acid, p-toluenesulfonic acid, and anhydrous toluene was 5g:0.25g:50mL. S2: Hydroxylated boron nitride, boron-containing siloxane, and toluene were mixed at 3g:0.9mL:100mL and refluxed at 110°C for 12 hours under a nitrogen atmosphere. After the reaction, the mixture was filtered, washed, and dried at 60°C for 12 hours to obtain amino-containing boron nitride. (2) Preparation of low-dielectric polyimide microporous films: Step 1: Mix m-phenylenediamine, aminated boron nitride, and N,N-dimethylacetamide, stir and disperse, then add hexafluorodianhydride and a pore-forming agent, and react in a water bath at 20°C for 24 hours to obtain a polyamic acid solution; In Step 3, the mass ratio of m-phenylenediamine, aminated boron nitride, N,N-dimethylacetamide, hexafluorodianhydride, and the pore-forming agent is 4.4:0.5:60:3.9:0.20; Step 4: Coat the polyamic acid solution onto a mold, perform heat treatment, and demold to obtain a low-dielectric polyimide microporous film; The coating thickness of the polyamic acid solution is 250 μm; The heat treatment conditions are: 85°C for 3 hours; 120°C for 1.2 hours; 180°C for 1.2 hours; 250°C for 1.2 hours; 310°C for 1.2 hours; The heating rate is 5°C / min.

[0035] Comparative Example 4: Compared with Example 1, no amino boron nitride was added, and all other conditions remained the same as in Example 1, specifically: Step 1: 2,7-Dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, and tetrahydrofuran were mixed, and potassium carbonate aqueous solution and methyltrioctylammonium chloride were added under an argon atmosphere. The mixture was heated to 75°C and reacted for 24 hours. After the reaction was completed, the mixture was extracted, rotary evaporated at 50°C for 60 minutes, and then purified to obtain the nitrated intermediate. In Step 1, 2,7-Dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, tetrahydrofuran, and potassium carbonate... The ratio of potassium aqueous solution to methyltrioctylammonium chloride was 3g:6.5g:200mL:10.3g:0.16g; the concentration of potassium carbonate aqueous solution was 2.2mol / L; Step 2: The nitration intermediate and anhydrous ethanol were mixed and heated to 80℃ under an argon atmosphere. Palladium on carbon and hydrazine hydrate were added, and the mixture was refluxed at 80℃ for 24h. After the reaction was completed, the mixture was filtered, refrigerated at 4℃ for 24h, and then vacuum dried at 65℃ for 24h to obtain the di- Amine monomer; in step 2, the ratio of nitration intermediate, anhydrous ethanol, palladium on carbon, and hydrazine hydrate is 2g:250mL:0.05g:4mL; in step 3, the diamine monomer and N,N-dimethylacetamide are mixed, stirred and dispersed, then hexafluorodianhydride and porogen are added, and the mixture is stirred in a water bath at 20°C for 24 hours to obtain a polyamic acid solution; in step 3, the mass ratio of diamine monomer, N,N-dimethylacetamide, hexafluorodianhydride, and porogen is 4.4:6. 0:3.9:0.20; Step 4: Coat the mold with polyamic acid solution, perform heat treatment, demold, and obtain a low dielectric polyimide microporous film; The coating thickness of the polyamic acid solution is 250μm; The heat treatment process conditions are: heat treatment at 85℃ for 3h; heat treatment at 120℃ for 1.2h; heat treatment at 180℃ for 1.2h; heat treatment at 250℃ for 1.2h; heat treatment at 310℃ for 1.2h; The heating rate is 5℃ / min.

[0036] Comparative Example 5: Compared with Example 1, the diamine monomer was replaced with m-phenylenediamine, and no amino boron nitride was added. All other conditions remained the same as in Example 1. Specifically: Step 1: Mix m-phenylenediamine, aminated boron nitride, and N,N-dimethylacetamide, stir and disperse, then add hexafluorodianhydride and a pore-forming agent, and react in a water bath at 20°C for 24 hours to obtain a polyamic acid solution; In Step 3, the mass ratio of m-phenylenediamine, N,N-dimethylacetamide, hexafluorodianhydride, and the pore-forming agent is 4.4:60:3.9:0.20; Step 4: Coat the polyamic acid solution onto a mold, perform heat treatment, and demold to obtain a low-dielectric polyimide microporous film; The coating thickness of the polyamic acid solution is 250 μm; The heat treatment conditions are: 85°C for 3 hours; 120°C for 1.2 hours; 180°C for 1.2 hours; 250°C for 1.2 hours; 310°C for 1.2 hours; The heating rate is 5°C / min.

[0037] Comparative Example 6: Compared with Example 1, no porogen was added, and all other conditions remained the same as in Example 1.

[0038] experiment: Dielectric properties: The dielectric constant and dielectric loss factor of low dielectric polyimide microporous films were tested in accordance with GB / T31838.6-2021 to characterize their dielectric properties. Mechanical properties: The tensile strength of low dielectric polyimide microporous films is used to characterize their mechanical properties, referring to GB / T1040.3-2006. Thermal stability: The obtained low-dielectric polyimide microporous film was made into a 5×5cm sample and tested for glass transition temperature by purging with nitrogen at 30~800℃ using a thermogravimetric analyzer at a heating rate of 10℃ / min. Micropore number measurement method: The porosity of polyimide microporous film samples was determined using a specific surface area distribution tester; Based on the data in the table above, the following conclusions can be drawn: Compared with Example 1, Comparative Example 1 replaced borosilicate with γ-aminopropylmethyldiethoxysilane. The dielectric constant and dielectric loss factor of the film increased, while the tensile strength decreased. This is because the polarizability of the BO bond is lower than that of the Si-O bond, which can reduce the dielectric constant of the film. The BO-Si hybrid interface can also play a stress buffering role, thereby improving the mechanical properties of the film. Compared with Example 1, Comparative Example 2 replaced the diamine monomer with 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl. The dielectric constant and dielectric loss factor of the film increased, the tensile strength decreased, and the glass transition temperature decreased. This is because the introduction of the fluorene ring into the main chain will disrupt the close packing of the molecular chains, increase the intermolecular gaps, and thus reduce the dielectric constant of the film. The fluorene ring also has good thermal stability. Compared with Example 1, Comparative Example 3 replaced the diamine monomer with m-phenylenediamine. The dielectric constant and dielectric loss factor of the film increased significantly, while the tensile strength decreased significantly. This is because m-phenylenediamine does not contain fluorine or fluorene rings, so its dielectric loss is higher. Compared with Example 1, Comparative Example 4 did not add aminated boron nitride. The dielectric constant and dielectric loss factor of the film increased significantly, the tensile strength decreased significantly, and the glass transition temperature decreased significantly. This is because boron nitride itself has intrinsic low dielectric properties, and the introduction of aminated boron nitride can both restrict the movement of molecular chain segments, thereby reducing the dielectric constant, and enhance and improve the mechanical properties of the film. Compared with Example 1, Comparative Example 5 replaced the diamine monomer with m-phenylenediamine and did not add aminated boron nitride, resulting in a significant decrease in all properties of the film. Compared with Example 1, Comparative Example 6 did not add a pore-forming agent, and no porosity was detected, which was close to 0. The dielectric constant and dielectric loss factor increased, indicating that the dielectric loss was high. As can be seen from the above, the preparation of aminated boron nitride and diamine monomers in this application can promote the improvement of the high temperature resistance and mechanical properties of the prepared film, while reducing the dielectric constant and dielectric loss of the film.

[0039] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.

Claims

1. A method for preparing a low-dielectric polyimide microporous film, characterized in that: Includes the following steps: Step 1: Mix 2,7-dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, and tetrahydrofuran. Add potassium carbonate aqueous solution and methyltrioctylammonium chloride under an argon atmosphere and heat to react to obtain the nitrated intermediate. Step 2: Mix the nitration intermediate and anhydrous ethanol, heat to 70-80°C under an argon atmosphere, add palladium on carbon and hydrazine hydrate, and reflux at a constant temperature to obtain the diamine monomer; Step 3: Mix the diamine monomer, aminated boron nitride, and N,N-dimethylacetamide, stir and disperse, then add hexafluorodianhydride and pore-forming agent, and react in a water bath to obtain a polyamic acid solution; Step 4: Coat the mold with polyamic acid solution, perform heat treatment, demold, and obtain a low dielectric polyimide microporous film.

2. The method for preparing a low-dielectric polyimide microporous film according to claim 1, characterized in that: The aminated boron nitride is prepared by the following process: S1: Mix phenylboronic acid, phenyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, p-toluenesulfonic acid and anhydrous toluene, and heat under reflux to react and obtain boron-containing siloxane; S2: Hydroxylated boron nitride, boron-containing siloxane and toluene are mixed and heated under a nitrogen atmosphere and refluxed to obtain aminolated boron nitride.

3. The method for preparing a low-dielectric polyimide microporous film according to claim 1, characterized in that: In step 1, the ratio of 2,7-dibromofluorene, (3-nitro-4-(trifluoromethoxy)phenyl)boronic acid, tetrahydrofuran, potassium carbonate aqueous solution and methyltrioctylammonium chloride is (1~3) g : (2.1~6.5) g : 200 mL : (3.2~10.3) g : (0.06~0.16) g.

4. The method for preparing a low-dielectric polyimide microporous film according to claim 1, characterized in that: In step 2, the ratio of nitration intermediate, anhydrous ethanol, palladium on carbon and hydrazine hydrate is (1~2) g: 250 mL: (0.025~0.05) g: (2~4) mL.

5. The method for preparing a low-dielectric polyimide microporous film according to claim 1, characterized in that: In step 3, the mass ratio of diamine monomer, amino boron nitride, N,N-dimethylacetamide, hexafluorodianhydride and porogen is (3.4~4.4):(0.3~0.5):60:(3.3~3.9):(0.035~0.20).

6. The method for preparing a low-dielectric polyimide microporous film according to claim 2, characterized in that: In S1, the molar ratio of phenylboronic acid, phenyltrimethoxysilane, and γ-aminopropylmethyldiethoxysilane is 1:(1.2~1.6):(0.8~1.2). In S1, the ratio of phenylboronic acid, p-toluenesulfonic acid and anhydrous toluene is (2~5) g : (0.01~0.25) g : 50 mL.

7. The method for preparing a low-dielectric polyimide microporous film according to claim 2, characterized in that: In S2, the ratio of hydroxylated boron nitride, borosilicate, and toluene is (1~3) g: (0.3~0.9) mL: 100 mL.

8. The method for preparing a low-dielectric polyimide microporous film according to claim 1, characterized in that: In step 3, the process conditions for the water bath stirring reaction are: temperature 0~20℃, time 12~24h.

9. The method for preparing a low-dielectric polyimide microporous film according to claim 1, characterized in that: In step 4, the heat treatment process conditions are as follows: heat treatment at 75~85℃ for 2~3h; heat treatment at 110~120℃ for 0.8~1.2h; heat treatment at 170~180℃ for 0.8~1.2h; heat treatment at 240~250℃ for 0.8~1.2h; heat treatment at 290~310℃ for 0.8~1.2h; and the heating rate is 3~5℃ / min.

10. A low-dielectric polyimide microporous film, characterized in that: The preparation method according to any one of claims 1 to 9 is used.

Citation Information

Patent Citations

  • A thermoplastic polyimide resin composite film with low dielectric properties and its preparation method

    CN113604045B