A green and environmentally friendly material and preparation method for cosmetic packaging bottles

By preparing a blend of lactate copolymers with polyethylene and polylactic acid, the problems of low strength and poor biodegradability of polyethylene packaging materials were solved, resulting in a high-performance, green, and environmentally friendly material suitable for cosmetic packaging bottles.

CN123107212APending Publication Date: 2026-11-17ZHEJIANG RONGYI PACKAGING TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611305239.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Polyethylene packaging materials have low strength, are difficult to biodegrade, and have poor compatibility with polylactic acid, which affects the mechanical properties of composite materials.

Method used

By preparing a lactate copolymer and blending it with polyethylene and polylactic acid, a green and environmentally friendly material is formed. The main chain structure of the lactate copolymer is used to improve the compatibility between the two. The preparation method includes mixing in a mixer and extruding and granulating in a twin-screw extruder.

Benefits of technology

It significantly improves the compatibility of polyethylene and polylactic acid, enhances the tensile strength, elongation at break and flexural strength of the material, and also has excellent biodegradability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to the field of packaging bottle materials technology, and discloses a green and environmentally friendly material for cosmetic packaging bottles and its preparation method. The green and environmentally friendly material for cosmetic packaging bottles of this invention comprises 60-80 parts by weight of polyethylene resin, 20-40 parts by weight of polylactic acid, and 2-5 parts by weight of lactate copolymer, etc. The polyethylene resin, polylactic acid, and lactate copolymer are mixed evenly in a mixer, and then extruded and granulated in a twin-screw extruder to obtain the green and environmentally friendly material. Polyethylene and polylactic acid have good compatibility, and the material has high tensile strength, flexural strength, and other properties. Furthermore, polylactic acid has excellent biodegradability, and the main chain of the lactate copolymer also contains a large number of degradable ester groups. Blending with polyethylene can improve the biodegradability of the material, making it green and environmentally friendly, and applicable to packaging materials such as cosmetic packaging bottles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of packaging bottle material technology, specifically to a green and environmentally friendly material and preparation method for cosmetic packaging bottles. Background Technology

[0002] Polyethylene mainly includes homopolymer polyethylene and α-olefin ethylene copolymer, which have advantages such as low cost, light weight, high toughness, and strong impact resistance, and are widely used in packaging materials, agricultural films, and wires and cables. However, polyethylene has low mechanical strength and is a non-renewable petroleum-based polymer that is difficult to biodegrade. Excessive use can lead to energy crises and environmental pollution.

[0003] In recent years, the development of green, renewable, and biodegradable materials has been a research hotspot. Polylactic acid (PLA) is widely used in packaging, biomedicine, and textiles due to its abundant raw material sources, simple preparation methods, high mechanical strength, and excellent biodegradability. However, PLA has poor toughness. Combining high-strength PLA with high-toughness polyethylene can combine the advantages of both to create high-performance composite materials. However, the mismatch in molecular polarity and large difference in solubility parameters between polyethylene and PLA leads to poor compatibility, which affects the mechanical strength and other properties of the composite material. Summary of the Invention

[0004] This invention solves the problems of low strength and poor biodegradability of polyethylene packaging materials.

[0005] This invention provides a method for preparing a green and environmentally friendly material, the material comprising 60-80 parts by weight of polyethylene resin, 20-40 parts by weight of polylactic acid, 2-5 parts by weight of lactate copolymer, and 0.2-0.4 parts by weight of antioxidant.

[0006] The preparation method of green and environmentally friendly materials includes: mixing polyethylene resin, polylactic acid, lactate copolymer and antioxidant in a mixer, and then extruding and granulating in a twin-screw extruder to obtain green and environmentally friendly materials.

[0007] Furthermore, the temperature of sections 1-7 of the twin-screw extruder is 140-190℃.

[0008] Furthermore, the preparation method of the lactate copolymer includes: Lactic acid was added to methanol, and the catalyst 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) was added dropwise in an ice-water bath. The mixture was stirred at room temperature for 30-40 min, and methanol was removed by vacuum distillation. N,N-dimethylformamide was added, followed by the dropwise addition of a dibromine compound. The molar ratio of lactic acid, 1,8-diazabicyclo[5.4.0]undec-7-ene, and the dibromine compound was (2.2-2.4):(2.2-2.4):1. The mixture was stirred for 24-30 h, and ethyl acetate and water were added. The mixture was shaken, allowed to stand, and allowed to separate into layers. The organic layer of ethyl acetate was collected and washed successively with dilute hydrochloric acid, sodium bicarbonate aqueous solution, and water. Anhydrous magnesium sulfate was added to the organic layer, and the mixture was stirred and filtered. The filtrate was distilled under vacuum and dried to obtain the lactate diol monomer. The reaction formula is: .

[0009] Triethylamine (TEA), lactate diol monomer, and diacyl chloride monomer were added to ethyl acetate in a molar ratio of (2-2.1):(1-1.04):1. The mixture was stirred at room temperature for 12-18 hours. After filtration, the precipitate was added to water, stirred, washed with water and ethanol, and dried to obtain the lactate copolymer. The reaction formula is as follows: .

[0010] Furthermore, the dibromo compound is 1,10-dibromodecane, 1,12-dibromododecane, 1,14-dibromotetradecane, or 1,16-dibromohexadecane.

[0011] Furthermore, the diacyl chloride monomer is malonyl chloride, succinic chloride, glutaryl chloride, or adipyl chloride.

[0012] Furthermore, environmentally friendly materials are being used in cosmetic packaging bottles.

[0013] The beneficial technical effects of this invention are as follows: by polymerizing lactate diol monomers with diacyl chloride monomers to obtain lactate copolymers, and then blending them with polyethylene and polylactic acid to obtain green and environmentally friendly materials, the main chain of the lactate copolymer contains long carbon chains similar to the polyethylene molecular chain and lactate structural units similar to polylactic acid, which allows the lactate copolymer to compatibilize polyethylene and polylactic acid, significantly improving their compatibility and giving the material better mechanical properties, exhibiting higher tensile strength, elongation at break and flexural strength.

[0014] The polylactic acid of this invention has excellent biodegradability, and the main chain of the lactic acid ester copolymer also contains a large number of degradable ester groups. When blended with polyethylene, it can improve the biodegradability of the material, making it green and environmentally friendly. It can be applied to packaging materials such as cosmetic packaging bottles. Detailed Implementation

[0015] The present invention will now be described in detail with reference to the embodiments.

[0016] The following polyethylene resin grades are: Yanshan Petrochemical LDPE 1I2A-1, Ningbo Xinfei Plastics Co., Ltd.; and polylactic acid (PLA), NatureWorks 4032D (USA).

[0017] Example 1: (1) Add 2.4 mmol of lactic acid to 0.5 mL of methanol, add 2.4 mmol of 1,8-diazabicyclo[5.4.0]undec-7-ene dropwise in an ice-water bath, stir at room temperature for 30 min, remove methanol by vacuum distillation, add 0.5 mL of N,N-dimethylformamide, add 1 mmol of 1,12-dibromododecane dropwise, stir and react for 24 h, add ethyl acetate and water, shake, let stand and separate into layers, collect the organic layer of ethyl acetate, wash successively with 4% dilute hydrochloric acid, saturated sodium bicarbonate aqueous solution and water, add anhydrous magnesium sulfate to the organic layer, stir and filter, distill under vacuum and dry to obtain lactate diol monomer.

[0018] (2) Add 2 mmol of triethylamine, 1 mmol of lactate diol monomer and 1 mmol of succinyl chloride to 4 mL of ethyl acetate. Stir at room temperature for 12 h. After filtration, add the precipitate to water, stir, wash the precipitate with water and ethanol, and dry to obtain the lactate copolymer.

[0019] (3) Mix 800g of polyethylene resin, 200g of polylactic acid, 20g of lactic acid ester copolymer and 4g of antioxidant 1076 in a mixer, and then extrude and granulate in a twin-screw extruder. The temperatures of stages 1-7 are 140℃, 160℃, 175℃, 185℃, 190℃, 190℃ and 185℃, respectively, to obtain green and environmentally friendly materials.

[0020] Example 2: (1) Add 2.4 mmol of lactic acid to 0.5 mL of methanol, add 2.4 mmol of 1,8-diazabicyclo[5.4.0]undec-7-ene dropwise in an ice-water bath, stir at room temperature for 30 min, remove methanol by vacuum distillation, add 0.5 mL of N,N-dimethylformamide, add 1 mmol of 1,10-dibromodecane dropwise, stir for 30 h, add ethyl acetate and water, shake, let stand to separate the layers, collect the organic layer of ethyl acetate, wash successively with 4% dilute hydrochloric acid, saturated sodium bicarbonate aqueous solution, and water, add anhydrous magnesium sulfate to the organic layer, stir and filter, distill under vacuum and dry to obtain lactate diol monomer.

[0021] (2) Add 2.1 mmol of triethylamine, 1 mmol of lactate diol monomer and 1 mmol of succinyl chloride to 4 mL of ethyl acetate. Stir at room temperature for 12 h. After filtration, add the precipitate to water, stir, wash the precipitate with water and ethanol, and dry to obtain the lactate copolymer.

[0022] (3) Mix 750g of polyethylene resin, 250g of polylactic acid, 30g of lactic acid ester copolymer and 4g of antioxidant 1076 in a mixer, and then extrude and granulate in a twin-screw extruder. The temperatures of stages 1-7 are 140℃, 160℃, 175℃, 185℃, 190℃, 190℃ and 185℃, respectively, to obtain green and environmentally friendly materials.

[0023] Example 3: (1) Add 2.2 mmol of lactic acid to 0.5 mL of methanol, add 2.2 mmol of 1,8-diazabicyclo[5.4.0]undec-7-ene dropwise in an ice-water bath, stir at room temperature for 30 min, remove methanol by vacuum distillation, add 0.5 mL of N,N-dimethylformamide, add 1 mmol of 1,12-dibromododecane dropwise, stir for 30 h, add ethyl acetate and water, shake, let stand to separate the layers, collect the organic layer of ethyl acetate, wash successively with 4% dilute hydrochloric acid, saturated sodium bicarbonate aqueous solution, and water, add anhydrous magnesium sulfate to the organic layer, stir and filter, distill under vacuum and dry to obtain lactate diol monomer.

[0024] (2) Add 2.1 mmol of triethylamine, 1 mmol of lactate diol monomer and 1 mmol of succinyl chloride to 4 mL of ethyl acetate. Stir at room temperature for 12 h. After filtration, add the precipitate to water, stir, wash the precipitate with water and ethanol, and dry to obtain the lactate copolymer.

[0025] (3) Mix 700g of polyethylene resin, 300g of polylactic acid, 40g of lactic acid ester copolymer and 3g of antioxidant 1076 in a mixer, and then extrude and granulate in a twin-screw extruder. The temperatures of sections 1-7 are 140℃, 160℃, 175℃, 185℃, 190℃, 190℃ and 185℃, respectively, to obtain green and environmentally friendly materials.

[0026] Example 4: (1) Add 2.4 mmol of lactic acid to 0.5 mL of methanol, add 2.4 mmol of 1,8-diazabicyclo[5.4.0]undec-7-ene dropwise in an ice-water bath, stir at room temperature for 40 min, remove methanol by vacuum distillation, add 0.5 mL of N,N-dimethylformamide, add 1 mmol of 1,10-dibromodecane dropwise, stir and react for 24 h, add ethyl acetate and water, shake, stand and separate into layers, collect the organic layer of ethyl acetate, wash successively with 4% dilute hydrochloric acid, saturated sodium bicarbonate aqueous solution and water, add anhydrous magnesium sulfate to the organic layer, stir and filter, distill under vacuum and dry to obtain lactate diol monomer.

[0027] (2) Add 2 mmol of triethylamine, 1 mmol of lactate diol monomer and 1 mmol of succinyl chloride to 4 mL of ethyl acetate. Stir at room temperature for 18 h. After filtration, add the precipitate to water, stir, wash the precipitate with water and ethanol, and dry to obtain the lactate copolymer.

[0028] (3) Mix 600g of polyethylene resin, 400g of polylactic acid, 50g of lactic acid ester copolymer and 2g of antioxidant 1076 in a mixer, and then extrude and granulate in a twin-screw extruder. The temperatures of sections 1-7 are 140℃, 160℃, 175℃, 185℃, 190℃, 190℃ and 185℃, respectively, to obtain green and environmentally friendly materials.

[0029] Comparative Example 1: (1) Mix 800g of polyethylene resin, 200g of polylactic acid and 4g of antioxidant 1076 in a mixer, and then extrude and granulate in a twin-screw extruder. The temperatures of sections 1-7 are 140℃, 160℃, 175℃, 185℃, 190℃, 190℃ and 185℃, respectively, to obtain green and environmentally friendly materials.

[0030] Comparative Example 2: (1) Add 2 mmol of triethylamine, 1 mmol of 1,4-butanediol and 1 mmol of succinyl chloride to 4 mL of ethyl acetate. Stir the mixture at room temperature for 12 h. After filtration, add the precipitate to water, stir, wash the precipitate with water and ethanol, and dry to obtain the copolymer.

[0031] (2) Mix 800g of polyethylene resin, 200g of polylactic acid, 20g of copolymer and 4g of antioxidant 1076 in a mixer, and then extrude and granulate in a twin-screw extruder. The temperatures of sections 1-7 are 140℃, 160℃, 175℃, 185℃, 190℃, 190℃ and 185℃, respectively, to obtain green and environmentally friendly materials.

[0032] Comparative Example 3: (1) Add 2 mmol of triethylamine, 1 mmol of 1,12-dodecanediol (CAS No. 5675-51-4) and 1 mmol of succinyl chloride to 4 mL of ethyl acetate. Stir at room temperature for 12 h. After filtration, add the precipitate to water, stir, wash the precipitate with water and ethanol, and dry to obtain the copolymer.

[0033] (2) Mix 800g of polyethylene resin, 200g of polylactic acid, 20g of copolymer and 4g of antioxidant 1076 in a mixer, and then extrude and granulate in a twin-screw extruder. The temperatures of sections 1-7 are 140℃, 160℃, 175℃, 185℃, 190℃, 190℃ and 185℃, respectively, to obtain green and environmentally friendly materials.

[0034] The biodegradable material was hot-pressed using a flat vulcanizing apparatus at 190℃, 10MPa, and 5min to prepare test specimens. Tensile properties were tested according to GB / T 1040.1-2025. Flexural strength was tested according to GB / T 9341-2008.

[0035] Table 1 Performance Tests

[0036] The poor compatibility between polyethylene and polylactic acid in Comparative Example 1 resulted in lower tensile strength, elongation at break, and flexural strength, leading to poor mechanical properties. Each Example 1 incorporated a lactic acid ester copolymer, whose main chain contained long carbon chains similar to those of polyethylene and lactic acid ester structural units similar to those of polylactic acid. This allows the lactate copolymer to compatibilize polyethylene and polylactic acid, significantly improving their compatibility and giving the material better mechanical properties, exhibiting higher tensile strength, elongation at break, and flexural strength.

[0037] Compared with Example 1, the copolymers of Comparative Example 2 and Comparative Example 3 do not contain lactate structural units, resulting in poor compatibilization of polyethylene and polylactic acid, leading to poor compatibility between polyethylene and polylactic acid, and lower tensile strength, elongation at break, and flexural strength than in Example 1.

[0038] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements can be made without departing from the principle of the present invention, and these improvements should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing a green and environmentally friendly material, characterized in that, The environmentally friendly materials used in the cosmetic packaging bottles include 60-80 parts by weight of polyethylene resin, 20-40 parts by weight of polylactic acid, 2-5 parts by weight of lactic acid ester copolymer, and 0.2-0.4 parts by weight of antioxidant. The preparation method includes: mixing polyethylene resin, polylactic acid, lactate copolymer, and antioxidant in a mixer, and then extruding and granulating the mixture in a twin-screw extruder to obtain a green and environmentally friendly material.

2. The method for preparing green and environmentally friendly materials according to claim 1, characterized in that, The temperature of sections 1-7 of the twin-screw extruder is 140-190℃.

3. The method for preparing green and environmentally friendly materials according to claim 1, characterized in that, The preparation method of the lactate copolymer includes: adding triethylamine, lactate diol monomer, and diacyl chloride monomer to ethyl acetate, stirring and reacting at room temperature for 12-18 hours, filtering and adding the precipitate to water, stirring, washing the precipitate with water and ethanol, and drying to obtain the lactate copolymer.

4. The method for preparing green and environmentally friendly materials according to claim 3, characterized in that, The molar ratio of triethylamine, lactate diol monomer, and diacyl chloride monomer is (2-2.1):(1-1.04):

1.

5. The method for preparing green and environmentally friendly materials according to claim 4, characterized in that, The diacyl chloride monomer is malonyl chloride, succinic chloride, glutaryl chloride, or adipyl chloride.

6. The method for preparing green and environmentally friendly materials according to claim 4, characterized in that, The preparation method of the lactate diol monomer includes: adding lactic acid to methanol, adding 1,8-diazabicyclo[5.4.0]undec-7-ene dropwise in an ice-water bath, stirring at room temperature for 30-40 min, removing methanol by vacuum distillation, adding N,N-dimethylformamide, adding dibromo compound dropwise, stirring and reacting for 24-30 h, adding ethyl acetate and water, shaking, allowing to stand and separate into layers, collecting the ethyl acetate organic layer, washing it successively with dilute hydrochloric acid, sodium bicarbonate aqueous solution, and water, adding anhydrous magnesium sulfate to the organic layer, stirring and filtering, distilling the filtrate under vacuum, and drying to obtain the lactate diol monomer.

7. The method for preparing green and environmentally friendly materials according to claim 6, characterized in that, The molar ratio of the lactic acid, 1,8-diazabicyclo[5.4.0]undec-7-ene, and dibromo compound is (2.2-2.4):(2.2-2.4):

1.

8. The method for preparing green and environmentally friendly materials according to claim 7, characterized in that, The dibromo compound is 1,10-dibromodecane, 1,12-dibromododecane, 1,14-dibromotetradecane, or 1,16-dibromohexadecane.

9. A green and environmentally friendly material obtained by the preparation method according to any one of claims 1-8.

10. The application of the green and environmentally friendly material as described in claim 9 in cosmetic packaging bottles.