A calcium carbonate / polyolefin elastomer composite material modified with octadecyl surfactant and its preparation method
By modifying calcium carbonate with octadecyl surfactant and combining it with polyolefin elastomer, a flexible organic interface layer was constructed, which solved the problem of poor compatibility between calcium carbonate and polyolefin elastomer and improved the water resistance and mechanical properties of the composite material.
Patent Information
- Application Number
- CN202611574613.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-17
AI Technical Summary
In the prior art, calcium carbonate has poor compatibility with polyolefin elastomers, resulting in insufficient mechanical properties and hydrophobic properties of the composite material, which limits its application, especially in humid environments.
Calcium carbonate was surface modified with octadecyl surfactant to construct a flexible organic interface layer, which enhanced the interfacial anchoring force and compatibility. The long-chain physical entanglement improved the filler dispersion and interfacial compatibility.
It significantly improves the water resistance, moisture resistance and mechanical properties of composite materials, provides excellent application prospects, and avoids performance degradation caused by excessive filler.
Smart Images

Figure CN123107224A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer composite materials technology, specifically relating to a calcium carbonate / polyolefin elastomer composite material modified with octadecyl surfactant and its preparation method. Background Technology
[0002] To improve the mechanical and hydrophobic properties of polyolefin elastomer (POE) composites, inorganic fillers (such as calcium carbonate and silica) are typically added to the POE matrix, and inorganic filler / POE composites are prepared through physical blending. Calcium carbonate (CaCO3) is one of the most commonly used fillers due to its wide availability, low price, non-toxicity, and good thermal stability. However, during the preparation of inorganic filler / POE composites, the significant differences in surface chemistry between CaCO3 and POE lead to poor compatibility. CaCO3 tends to agglomerate in the POE matrix, resulting in weak interfacial bonding. This often causes the mechanical properties of the composite, especially tensile strength and impact toughness, to decrease rather than improve.
[0003] To improve the compatibility between the inorganic filler CaCO3 and the polymer matrix POE, existing technologies typically employ coupling agents or surfactants to modify the surface of the inorganic filler CaCO3. While this can improve its compatibility with the polymer matrix to some extent, it still has some shortcomings: conventional short-chain surfactants (e.g., short-chain organic acids or short-chain silanes with carbon chain lengths of 2–8 carbon atoms) can introduce organic groups, but due to their short chain segments, they cannot effectively entangle and interact with the polymer molecular chains, resulting in limited interfacial modification effects. Furthermore, when calcium carbonate modified with conventional short-chain surfactants or coupling agents is combined with POE, the improvement in the surface hydrophobicity of the resulting CaCO3 / POE composite material is limited, leading to poor water resistance and moisture resistance, which restricts its application in humid environments or outdoors.
[0004] In view of this, the present invention is proposed. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides a calcium carbonate / polyolefin elastomer (POE) composite material modified with octadecyl surfactant and its preparation method. This application modifies CaCO3 with octadecyl surfactant to construct a flexible organic interface layer on the CaCO3 surface. This not only reduces the interfacial energy between CaCO3 and POE but also enhances the interfacial anchoring force between CaCO3 and POE through long-chain physical entanglement. This synergistically improves filler dispersibility and interfacial compatibility between CaCO3 and POE, thereby enhancing the mechanical properties and water and moisture resistance of the composite material.
[0006] One objective of this invention is to provide a method for preparing a calcium carbonate / polyolefin elastomer (POE) composite material modified with octadecyl surfactant, comprising the following steps: CaCO3 and octadecyl surfactant were dispersed in ethanol for surface modification. After the reaction was completed, the mixture was separated from its solid state and dried to obtain octadecyl surfactant-modified CaCO3. Octadecyl surfactant-modified CaCO3 was melt-blended with POE elastomer and then extruded to obtain octadecyl surfactant-modified CaCO3 / POE composite material.
[0007] The octadecyl surfactant-modified CaCO3 accounts for 3-5% of the total mass of the octadecyl surfactant-modified CaCO3 / POE composite material.
[0008] Furthermore, the molar ratio of CaCO3 to octadecyl surfactant is 24:1 to 36:1.
[0009] Furthermore, the octadecyl surfactant is selected from one or more of octadecyltriethoxysilane and octadecyl phosphoric acid.
[0010] Furthermore, the specific process of modifying CaCO3 with the octadecyl surfactant is as follows: First, CaCO3 is dispersed in ethanol to wet the CaCO3 particles, resulting in a CaCO3 dispersion. Then, an ethanol solution of the octadecyl surfactant is added dropwise to the CaCO3 dispersion to carry out a surface modification reaction. After the reaction is completed, the CaCO3 is obtained by solid-liquid separation, ethanol washing, drying, and pulverization.
[0011] Furthermore, the reaction temperature of the surface modification reaction is 50~70℃, the reaction time is 60~180min, and the stirring speed is 500~1000r / min.
[0012] Furthermore, the melt blending is carried out using a twin-screw extruder, and the parameters for melt blending using the twin-screw extruder are as follows: zone 1 temperature is 60~70℃, zone 2 temperature is 80~90℃, zone 3 temperature is 120~130℃, pressure is 0.4~0.6MPa, rotation speed is 10~50r / min, and cycle time is 10~30min.
[0013] The second objective of this invention is to provide a calcium carbonate / polyolefin elastomer (POE) composite material modified with octadecyl surfactant obtained by the above preparation method.
[0014] Furthermore, the calcium carbonate / polyolefin elastomer (POE) composite material based on octadecyl surfactant modification comprises, by weight, the following components: 90-99 parts of polyolefin elastomer and 1-10 parts of octadecyl surfactant modified CaCO3.
[0015] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention uses octadecyl surfactant to modify the surface of CaCO3. The long-chain structure of octadecyl surfactant can form a thick and flexible organic interface layer on the surface of CaCO3. On the one hand, it adjusts the surface solubility parameter of the filler and reduces the interfacial energy between CaCO3 and POE. On the other hand, it enhances the interfacial anchoring force through the full physical entanglement of the octadecyl long chain with the molecular chain of polyolefin elastomer (POE). The synergistic effect of the two effectively improves the interfacial compatibility between CaCO3 and POE and the dispersibility of the filler. At the same time, the octadecyl long chain gives the material surface excellent hydrophobic properties, which significantly improves the water resistance and moisture resistance of the composite material. In addition, by controlling the mass fraction of octadecyl surfactant-modified CaCO3 in the composite material to be 3%~5%, the interfacial modification and hydrophobic enhancement effects are guaranteed, and the mechanical properties of the composite material are avoided due to excessive filler. This effectively overcomes the defects of insufficient interfacial modification and insufficient hydrophobic properties in the prior art, and obtains a CaCO3 / POE composite material with excellent comprehensive performance, which has good application prospects.
[0016] (2) According to the present invention, when the amount of CaCO3 modified by octadecyltriethoxysilane accounts for 5% of the total mass of the CaCO3 / POE composite material modified by octadecyl surfactant, the composite material has the highest tensile strength and the strongest hydrophobicity. This specific amount provides a precise and reliable process window for industrial production, avoiding resource waste and unstable performance of composite materials. Attached Figure Description
[0017] Figure 1 This is a scanning electron microscope image of the octadecyltriethoxysilane-modified calcium carbonate / polyolefin elastomer composite material obtained in Example 1 of the present invention.
[0018] Figure 2 This is a scanning electron microscope image of the calcium carbonate / polyolefin elastomer composite material obtained in Comparative Example 2 of the present invention.
[0019] Figure 3 This is a scanning electron microscope image of the octanoic acid modified calcium carbonate / polyolefin elastomer composite material obtained in Comparative Example 3 of the present invention. Detailed Implementation
[0020] To enable those skilled in the art to better understand and implement the technical solutions of the present invention, the present invention will be further described below in conjunction with specific embodiments and accompanying drawings.
[0021] Unless otherwise specified, all reagents used in this invention are commercially available, and all methods used are conventional techniques in the art.
[0022] Example 1 A method for preparing a calcium carbonate / polyolefin elastomer (POE) composite material modified with octadecyl surfactant includes the following steps: (1) CaCO3 was placed in a vacuum drying oven and dried at 120°C for 2 hours. The dried CaCO3 and octadecyltriethoxysilane were dispersed in ethanol at a molar ratio of 36:1 and stirred evenly at 60°C to obtain CaCO3 ethanol dispersion and octadecyltriethoxysilane ethanol solution, respectively. (2) Add the ethanol solution of octadecyltriethoxysilane dropwise to the ethanol dispersion of CaCO3, and stir the reaction at 800 r / min for 120 min. After the reaction is completed, the reaction product is filtered, washed with ethanol, dried and pulverized to obtain octadecyltriethoxysilane modified CaCO3. (3) 95 parts by weight of polyolefin elastomer and 5 parts by weight of octadecyltriethoxysilane-modified CaCO3 were placed in a vacuum drying oven and dried for 2 hours. The dried POE elastomer and octadecyltriethoxysilane-modified CaCO3 were then added to a twin-screw extruder for melt blending and extrusion to obtain octadecyltriethoxysilane-modified CaCO3. 3 / POE composite material; wherein, during melt blending, the barrel temperature of the twin-screw extruder is 65℃ in zone one, 85℃ in zone two, and 125℃ in zone three, the main extruder speed is 50r / min, the feed speed is 40r / min, the cycle time is 10min, and the vacuum degree of the vacuum section is 0.4MPa.
[0023] Example 2 A method for preparing a calcium carbonate / polyolefin elastomer (POE) composite material modified with octadecyl surfactant includes the following steps: (1) CaCO3 was placed in a vacuum drying oven and dried at 100°C for 2 hours. The dried CaCO3 and octadecyl phosphoric acid were dispersed in ethanol at a molar ratio of 30:1 and stirred evenly at 55°C to obtain CaCO3 ethanol dispersion and octadecyl phosphoric acid ethanol solution respectively. (2) Add the ethanol solution of octadecyl phosphoric acid dropwise to the ethanol dispersion of CaCO3, and stir the reaction at 500 r / min for 60 min. After the reaction is completed, the reaction product is filtered, washed with ethanol, dried and pulverized to obtain octadecyl phosphoric acid modified CaCO3. (3) 95 parts by weight of polyolefin elastomer and 5 parts by weight of octadecyl phosphate modified CaCO3 were placed in a vacuum drying oven and dried for 2 hours. The dried POE elastomer and octadecyl phosphate modified CaCO3 were added to a twin-screw extruder for melt blending and extrusion to obtain octadecyl phosphate modified CaCO3 / POE composite material. During melt blending, the barrel temperature of the twin-screw extruder was 65℃ in zone 1, 85℃ in zone 2, and 125℃ in zone 3. The main machine speed was 50 r / min, the feed speed was 40 r / min, the cycle time was 10 min, and the vacuum degree of the vacuum section was 0.5 MPa.
[0024] Example 3 A method for preparing a calcium carbonate / polyolefin elastomer (POE) composite material modified with octadecyl surfactant includes the following steps: (1) CaCO3 was placed in a vacuum drying oven and dried at 120°C for 2 hours. The dried CaCO3 and octadecyltriethoxysilane were dispersed in ethanol at a molar ratio of 24:1 and stirred evenly at 50°C to obtain ethanol dispersion of CaCO3 and ethanol solution of octadecyltriethoxysilane, respectively. (2) Add the ethanol solution of octadecyltriethoxysilane dropwise to the ethanol dispersion of CaCO3, and stir the reaction at 1000 r / min for 180 min. After the reaction is completed, the reaction product is filtered, washed with ethanol, dried and pulverized to obtain octadecyltriethoxysilane modified CaCO3. (3) 97 parts by weight of polyolefin elastomer and 3 parts by weight of octadecyltriethoxysilane modified CaCO3 were placed in a vacuum drying oven and dried for 2 hours. The dried POE elastomer and octadecyltriethoxysilane modified CaCO3 were added to a twin-screw extruder for melt blending and extrusion to obtain octadecyltriethoxysilane modified CaCO3 / POE composite material. During melt blending, the barrel temperature of the twin-screw extruder was 65℃ in zone 1, 85℃ in zone 2, and 125℃ in zone 3. The main engine speed was 50 r / min, the feed speed was 40 r / min, the cycle time was 10 min, and the vacuum degree of the vacuum section was 0.6 MPa.
[0025] Comparative Example 1 A method for preparing POE material includes the following steps: 100 parts by weight of polyolefin elastomer were placed in a vacuum drying oven and dried for 2 hours. The dried POE elastomer was then added to a twin-screw extruder for melting and extrusion to obtain POE material. During melting, the barrel temperature of the twin-screw extruder was 65℃ in zone 1, 85℃ in zone 2, and 125℃ in zone 3. The main extruder speed was 50 r / min, the feed speed was 40 r / min, the cycle time was 10 min, and the vacuum degree in the vacuum section was 0.4 MPa.
[0026] Comparative Example 2 A method for preparing a CaCO3 / POE composite material includes the following steps: 95 parts by weight of polyolefin elastomer and 5 parts by weight of CaCO3 were placed in a vacuum drying oven and dried for 2 hours. The dried POE elastomer and CaCO3 were then added to a twin-screw extruder for melt blending and extrusion to obtain a CaCO3 / POE composite material. During melt blending, the barrel temperature of the twin-screw extruder was 65℃ in zone 1, 85℃ in zone 2, and 125℃ in zone 3. The main extruder speed was 50 r / min, the feed speed was 40 r / min, the cycle time was 10 min, and the vacuum degree in the vacuum section was 0.5 MPa.
[0027] Comparative Example 3 A method for preparing a CaCO3 / POE composite material based on n-octanoic acid modification includes the following steps: (1) Place CaCO3 in a vacuum drying oven and dry at 120℃ for 2h. Disperse the dried CaCO3 and n-octanoic acid in ethanol at a molar ratio of 28:1 and stir evenly at 55℃ to obtain CaCO3 ethanol dispersion and n-octanoic acid ethanol solution respectively. (2) Add the ethanol solution of octanoic acid dropwise to the ethanol dispersion of CaCO3, stir at 600 r / min for 100 min, and after the reaction is completed, filter, wash with ethanol, dry and pulverize the reaction product to obtain octanoic acid modified CaCO3. (3) 95 parts by weight of polyolefin elastomer and 5 parts by weight of n-octanoic acid modified CaCO3 were placed in a vacuum drying oven and dried for 2 hours. The dried POE elastomer and n-octanoic acid modified CaCO3 were added to a twin-screw extruder for melt blending and extrusion to obtain n-octanoic acid modified CaCO3 / POE composite material. During melt blending, the barrel temperature of the twin-screw extruder was 65℃ in zone 1, 85℃ in zone 2, and 125℃ in zone 3. The main machine speed was 50 r / min, the feed speed was 40 r / min, the cycle time was 10 min, and the vacuum degree of the vacuum section was 0.6 MPa.
[0028] Comparative Example 4 A method for preparing a calcium carbonate / polyolefin elastomer (POE) composite material modified with octadecyl surfactant includes the following steps: (1) CaCO3 was placed in a vacuum drying oven and dried at 120°C for 2 hours. The dried CaCO3 and octadecyltriethoxysilane were dispersed in ethanol at a molar ratio of 24:1 and stirred evenly at 50°C to obtain ethanol dispersion of CaCO3 and ethanol solution of octadecyltriethoxysilane, respectively. (2) Add the ethanol solution of octadecyltriethoxysilane dropwise to the ethanol dispersion of CaCO3, and stir the reaction at 1000 r / min for 180 min. After the reaction is completed, the reaction product is filtered, washed with ethanol, dried and pulverized to obtain octadecyltriethoxysilane modified CaCO3. (3) 99 parts by weight of polyolefin elastomer and 1 part by weight of octadecyltriethoxysilane modified CaCO3 were placed in a vacuum drying oven and dried for 2 hours. The dried POE elastomer and octadecyltriethoxysilane modified CaCO3 were added to a twin-screw extruder for melt blending and extrusion to obtain octadecyltriethoxysilane modified CaCO3 / POE composite material. During melt blending, the barrel temperature of the twin-screw extruder was 65℃ in zone 1, 85℃ in zone 2, and 125℃ in zone 3. The main engine speed was 50 r / min, the feed speed was 40 r / min, the cycle time was 10 min, and the vacuum degree of the vacuum section was 0.6 MPa.
[0029] Comparative Example 5 A method for preparing a calcium carbonate / polyolefin elastomer (POE) composite material modified with octadecyl surfactant includes the following steps: (1) CaCO3 was placed in a vacuum drying oven and dried at 120°C for 2 hours. The dried CaCO3 and octadecyltriethoxysilane were dispersed in ethanol at a molar ratio of 24:1 and stirred evenly at 50°C to obtain ethanol dispersion of CaCO3 and ethanol solution of octadecyltriethoxysilane, respectively. (2) Add the ethanol solution of octadecyltriethoxysilane dropwise to the ethanol dispersion of CaCO3, and stir the reaction at 1000 r / min for 180 min. After the reaction is completed, the reaction product is filtered, washed with ethanol, dried and pulverized to obtain octadecyltriethoxysilane modified CaCO3. (3) 92 parts by weight of polyolefin elastomer and 8 parts by weight of octadecyltriethoxysilane modified CaCO3 were placed in a vacuum drying oven and dried for 2 hours. The dried POE elastomer and octadecyltriethoxysilane modified CaCO3 were added to a twin-screw extruder for melt blending and extrusion to obtain octadecyltriethoxysilane modified CaCO3 / POE composite material. During melt blending, the barrel temperature of the twin-screw extruder was 65℃ in zone 1, 85℃ in zone 2, and 125℃ in zone 3. The main engine speed was 50 r / min, the feed speed was 40 r / min, the cycle time was 10 min, and the vacuum degree of the vacuum section was 0.6 MPa.
[0030] The CaCO3 / POE composite materials obtained in Examples 1-2 and Comparative Examples 1-5 were subjected to a pressure of 15 MPa, a temperature of 130 °C, and a holding time of 20 min. The resulting materials were then used to prepare 5b-type dumbbell-shaped tensile specimens with a thickness of 1 mm using a flat vulcanizing machine. The tensile strength of these specimens was tested according to GB / T 1040-2006, and the water contact angle was measured using a contact angle measuring instrument. The specific test results are shown in Table 1.
[0031] Table 1. Test results of tensile strength and water contact angle of CaCO3 / POE composite materials prepared in Examples 1-2 and Comparative Examples 1-5 As shown in Table 1, the CaCO3 / POE composite materials modified with octadecyl surfactants prepared in Examples 1-2 of this invention exhibit significantly improved tensile strength compared to the pure POE material prepared in Comparative Example 1, and are superior to the octanoic acid-modified CaCO3 / POE composite material prepared in Comparative Example 3. Comparative Example 2 uses a mixture of pure CaCO3 and POE to form a CaCO3 / POE composite material. Because pure CaCO3 lacks groups that can effectively interact with the POE molecular chains, the tensile properties of the composite material decrease. Comparative Example 3 uses octanoic acid-modified CaCO3. Due to the short carbon chain of octanoic acid, it is difficult to form physical entanglement with the POE molecular chains, resulting in poor hydrophobicity of the composite material. This leads to phase separation during processing, thus affecting the interfacial compatibility of the composite material. Compared with Comparative Examples 4 and 5, in Examples 1 and 3 of this invention, when the content of octadecyl surfactant-modified CaCO3 (1%) in the composite material was low in Comparative Example 4, the modified CaCO3 could not fully exert its stress dispersion effect, resulting in limited improvement in the tensile properties of the octadecyl surfactant-modified CaCO3 / POE composite material. When the content of octadecyl surfactant-modified CaCO3 (1%) in the composite material increased to 3%~5%, a large number of modified CaCO3 particles were uniformly dispersed in the system, thereby significantly improving the tensile properties of the CaCO3 / POE composite material (39%~45%). Further increasing the proportion of octadecyl surfactant-modified CaCO3 in the composite material (8%) would cause CaCO3 to agglomerate in the CaCO3 / POE composite material, thereby reducing the tensile properties of the CaCO3 / POE composite material.
[0032] The composite materials obtained in Example 1 and Comparative Examples 2-3 were characterized by SEM. Figure 2 As can be seen, the CaCO3 / POE composite material exhibits significant phase separation after melt blending, indicating poor compatibility between CaCO3 and POE. This is primarily due to the weak interaction between the hydrophilic groups on the surface of calcium carbonate and the hydrophobic segments of POE. Figure 1 It can be seen that the surface of the octadecyltriethoxysilane-modified CaCO3 / POE composite material is relatively smooth, and the interface between the CaCO3 particles and the POE matrix is blurred, indicating high interfacial compatibility. This is mainly because the longer octadecyl segments on the surface of the modified CaCO3 particles are exposed, allowing for significant interaction with the POE segments. Figure 3 It can be seen that the CaCO3 particles in the octanoic acid-modified CaCO3 / POE composite material have a clear boundary with the POE matrix, indicating that the octanoic acid-modified CaCO3 and POE have poor compatibility. The main reason is that the carbon chain of octanoic acid is relatively short, making it difficult to form physical entanglement with the POE molecular chain, thus leading to phase separation.
[0033] It should be noted that when numerical ranges are involved in this invention, it should be understood that both endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as in the embodiments, preferred embodiments are described in this invention to avoid redundancy. Although preferred embodiments of this invention have been described, those skilled in the art, once they understand the inventive concept of this invention, can make other changes and modifications to these embodiments, and all such changes and modifications fall within the scope of this invention.
[0034] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from the spirit and scope of the invention. If such modifications and variations fall within the scope of equivalents of this invention, then this invention is also intended to include these modifications and variations.
Claims
1. A method for preparing a calcium carbonate / polyolefin elastomer composite material modified with octadecyl surfactant, characterized in that, Includes the following steps: CaCO3 and octadecyl surfactant were dispersed in ethanol for surface modification. After the reaction was completed, the mixture was separated from its solid state and dried to obtain octadecyl surfactant-modified CaCO3. Octadecyl surfactant-modified CaCO3 was melt-blended with polyolefin elastomer and extruded to obtain an octadecyl surfactant-modified CaCO3 / polyolefin elastomer composite material; The octadecyl surfactant-modified CaCO3 accounts for 3-5% of the total mass of the octadecyl surfactant-modified CaCO3 / polyolefin elastomer composite material.
2. The method for preparing the calcium carbonate / polyolefin elastomer composite material modified with octadecyl surfactant according to claim 1, characterized in that, The molar ratio of CaCO3 to octadecyl surfactant is 24:1 to 36:
1.
3. The method for preparing the calcium carbonate / polyolefin elastomer composite material modified with octadecyl surfactant according to claim 1, characterized in that, The octadecyl surfactant is selected from one or more of octadecyltriethoxysilane and octadecyl phosphoric acid.
4. The method for preparing the calcium carbonate / polyolefin elastomer composite material modified with octadecyl surfactant according to claim 1, characterized in that, The specific process of modifying CaCO3 with octadecyl surfactant is as follows: First, CaCO3 is dispersed in ethanol to wet the CaCO3 particles and obtain a CaCO3 dispersion. Then, an ethanol solution of octadecyl surfactant is added dropwise to the CaCO3 dispersion to carry out a surface modification reaction. After the reaction is completed, the CaCO3 is obtained by solid-liquid separation, ethanol washing, drying, and pulverization.
5. The method for preparing the calcium carbonate / polyolefin elastomer composite material modified with octadecyl surfactant according to claim 4, characterized in that, The surface modification reaction is carried out at a temperature of 50-70℃, for a reaction time of 60-180 min, and at a stirring speed of 500-1000 r / min.
6. The method for preparing the calcium carbonate / polyolefin elastomer composite material modified with octadecyl surfactant according to claim 1, characterized in that, The melt blending is carried out using a twin-screw extruder. The parameters for melt blending using the twin-screw extruder are as follows: zone 1 temperature is 60~70℃, zone 2 temperature is 80~90℃, zone 3 temperature is 120~130℃, pressure is 0.4~0.6MPa, rotation speed is 10~50r / min, and cycle time is 10~30min.
7. A calcium carbonate / polyolefin elastomer composite material based on octadecyl surfactant modification prepared by the preparation method according to any one of claims 1 to 6.
8. The calcium carbonate / polyolefin elastomer composite material modified with octadecyl surfactant according to claim 7, characterized in that, The calcium carbonate / polyolefin elastomer composite material based on octadecyl surfactant modification comprises, by weight, the following components: 90-99 parts of polyolefin elastomer and 1-10 parts of octadecyl surfactant-modified CaCO3.