A non-slip polyolefin shoe sole and its manufacturing process

By using a blend system of EVA, POE, OBC and EPDM, along with the synergistic effect of modified anti-slip fillers and petroleum resin, the problem of insufficient anti-slip performance of EVA shoe sole materials has been solved, achieving high anti-slip performance and long-term stability on dry, wet and oily surfaces.

CN123107225APending Publication Date: 2026-11-17HUNAN GLORY SHOES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611277011.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing EVA sole materials have insufficient anti-slip performance in both dry and wet environments, failing to meet certification standards. Adding polyolefin elastomer (POE) alone provides only limited improvement.

Method used

The matrix resin is a quaternary blend system of EVA, POE, OBC and EPDM. The interfacial bonding is enhanced by modifying the anti-slip filler with silane coupling agent and grafting maleic anhydride onto petroleum resin. Combined with ultraviolet ozone treatment to improve surface hydrophilicity, a micro-rough structure and a high-viscosity tackifying layer are formed, which synergistically improve the anti-slip performance.

Benefits of technology

A shoe sole material with low density, excellent softness, high elasticity and good anti-slip properties was prepared, which significantly improved the anti-slip performance of dry, wet and oily surfaces, and has long-term stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of footwear materials technology, and discloses an anti-slip polyolefin sole and its manufacturing process. The anti-slip polyolefin sole comprises the following components by weight: 100 parts polyolefin matrix resin, 12-22 parts modified anti-slip filler, 6-12 parts plasticizer, 1.8-3.5 parts foaming agent, 1.0-4.5 parts active zinc oxide, 5-12 parts light calcium carbonate, 3.0-8.0 parts tackifying anti-slip functional additive, and 2.0-5.5 parts auxiliary materials. The anti-slip polyolefin sole described in this invention uses a quaternary polyolefin blend system of EVA, POE, OBC, and EPDM as the matrix resin. OBC provides excellent resilience and dimensional stability, POE further improves resilience and reduces surface crystallinity, and EPDM significantly improves dry and wet anti-slip performance. The four components synergistically foam to form a uniform and dense closed-cell structure, resulting in a sole material with low density, excellent softness, high elasticity, and good anti-slip performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of footwear materials technology, specifically to a non-slip polyolefin sole and its manufacturing process. Background Technology

[0002] Ethylene-vinyl acetate copolymer (EVA) foam soles are widely used in various footwear products due to their advantages such as lightness, flexibility, comfort, and elasticity. However, existing EVA sole materials generally have insufficient anti-slip performance. Tests show that soles made of traditional EVA materials have an anti-slip coefficient of only 0.9 to 1.0 in dry environments and only 0.4 to 0.5 in wet environments, which cannot meet the certification standards (anti-slip coefficient ≥ 1.5 in dry environments and anti-slip coefficient ≥ 0.6 in wet environments).

[0003] To improve the anti-slip performance of EVA shoe soles, existing technologies include blending modification with the addition of polyolefin elastomer (POE). POE is a polyolefin elastomer material made from ethylene and octene. The introduction of octene in the molecular chain disrupts some of the polyethylene crystallization. The octene segments and the disrupted polyethylene segments together form elastic soft segments, while the crystalline polyethylene segments form hard segments and act as physical cross-linking points, giving POE elastomer properties. However, adding POE alone has limited effect on improving anti-slip performance.

[0004] Therefore, developing a polyolefin shoe sole material that combines excellent anti-slip properties, good processing performance, and long-term stability is of great practical significance and application value. Summary of the Invention

[0005] To achieve the above objectives, the present invention adopts the following technical solution: an anti-slip polyolefin shoe sole, comprising the following components by weight: 100 parts polyolefin matrix resin, 12-22 parts modified anti-slip filler, 6-12 parts plasticizer, 1.8-3.5 parts foaming agent, 1.0-4.5 parts active zinc oxide, 5-12 parts light calcium carbonate, 3.0-8.0 parts tackifying anti-slip functional additive, and 2.0-5.5 parts auxiliary materials.

[0006] Furthermore, the polyolefin matrix resin comprises 45-60 parts of ethylene-vinyl acetate copolymer (EVA), 15-25 parts of polyolefin elastomer (POE), 10-20 parts of olefin block copolymer (OBC), and 5-15 parts of ethylene propylene diene monomer (EPDM).

[0007] In the above technical solution, the polyolefin matrix resin is selected from a quaternary blend system of EVA, POE, OBC, and EPDM. The EVA contains 18%–30% vinyl acetate (VA) (mass percentage), preferably 22%–26%. Commercially available EVA7470M (Formosa Plastics Corporation, VA content 26%, melt index MI=7.0) or EVA7350M (Formosa Plastics Corporation, VA content 22%, MI=2.5) can be used. EVA imparts good flexibility and processing performance to the material. The POE is a random ethylene-octene copolymer elastomer with a crystallinity ≤18%. Commercially available POE8180 (Dow Chemical Company, MI=0.5, octene content approximately 43%) or POE8137 (Dow Chemical Company, MI=13, octene content approximately 43%) is preferred. The addition of POE further improves the resilience of the EVA sole and reduces the surface crystallinity, overcoming the problem of easy wrinkling on the surface of traditional EVA foamed shoe materials. OBC is an olefin block copolymer with a crystallinity ≤15%, preferably OBC9530 (Dow, hardness 60A) or OBC9107 (Dow, hardness 60A). OBC has good heat resistance, high elasticity, and good processing performance, which can provide excellent resilience for the EVA foaming system and effectively control shrinkage to maintain dimensional stability. The EPDM is ethylene propylene diene monomer (EPDM) rubber with a crystallinity ≤5%, preferably EPDM5565 (Dow) or EPDM4725P (Dow). The addition of EPDM can significantly improve the dry and wet anti-slip performance of the foamed material. Studies have shown that when the mass fraction of EPDM is 30%, the dry anti-slip performance can be improved by 41%, and the wet anti-slip performance can be improved by 22%. The composite foaming of EVA, POE, OBC, and EPDM forms a uniform and dense closed-cell structure in the sole material. Compared with the unfoamed sole material, the resulting sole material has lower density and better softness, shock absorption, and anti-slip performance.

[0008] Furthermore, the modified anti-slip filler is at least one of the following: surface-modified silane coupling agent-modified silica, fumed silica, and porous silica powder, with a particle size range of 200–1000 nm.

[0009] The modified anti-slip filler is prepared by the following process: Silica or fumed silica is dispersed in anhydrous ethanol, and silane coupling agent KH-570 (γ-methacryloyloxypropyltrimethoxysilane) is added. The mixture is stirred and reacted at 70–90°C for 5–8 hours, filtered, washed three times with anhydrous ethanol, and vacuum dried at 80°C to constant weight to obtain the modified anti-slip filler. The mass ratio of silica to KH-570 is 100:(5–15), preferably 100:(8–12).

[0010] After surface modification, the interfacial bonding force between the anti-slip filler and the polyolefin matrix is ​​enhanced, making it less prone to agglomeration. In shoe sole materials, this filler can form a micro-rough structure on the surface, increasing the actual contact area when in contact with the ground, thereby improving the dry friction coefficient. At the same time, the hydrophobic properties of the filler surface help to disrupt the continuity of the water film under wet conditions, allowing the sole to penetrate the water film and directly contact the ground, thus improving wet anti-slip performance.

[0011] Furthermore, the tackifying and anti-slip functional additive is one or a combination of two of C5 petroleum resin, C9 petroleum resin, and hydrogenated C9 petroleum resin, with a softening point of 85-130°C.

[0012] Adding petroleum resin can significantly improve the coefficient of friction of EVA composite foam materials. Among them, C9 petroleum resin has the greatest effect on improving anti-slip performance. Petroleum resin contains a rigid molecular chain structure. Due to its good compatibility with EVA, it can also improve the tensile strength of the shoe sole. In addition, petroleum resin has good adhesion and can improve the entanglement of OBC and POE molecules to ensure the rebound effect.

[0013] Furthermore, the tackifying anti-slip functional additive is pretreated by the following process: C5 petroleum resin or C9 petroleum resin is mixed with naphthenic oil at a mass ratio of (2-4):1, heated to 120-125°C, and stirred until the petroleum resin becomes transparent and viscous to obtain a liquid anti-slip agent, which is then cooled for later use.

[0014] After pre-dissolving in naphthenic oil, the dispersion uniformity of petroleum resin in the polyolefin matrix is ​​significantly improved, avoiding the problems of local enrichment and precipitation caused by compatibility differences when added directly.

[0015] Furthermore, the tackifying and anti-slip functional additive is modified by maleic anhydride grafting, and the specific reaction process is as follows:

[0016] (I) Chain initiation stage: Benzoyl peroxide (BPO) decomposes upon heating, generating benzoyloxy radicals; the benzoyloxy radicals further decarboxylate to generate phenyl radicals, which then abstract tertiary hydrogen atoms from the petroleum resin (represented by RH) molecular chain (the tertiary carbon CH bond in the petroleum resin molecular chain has a lower energy and is most easily abstracted), forming a macromolecular radical R, as shown in the following reaction formula:

[0017]

[0018] The molecular structure of petroleum resins (C5 or C9 petroleum resins) is mainly composed of oligomers formed by cationic polymerization of conjugated dienes (such as cyclopentadiene, isoprene, etc.). The molecular chains contain a large number of tertiary carbon and hydrogen atoms. Under high temperature conditions, the hydrogen atoms on these tertiary carbon sites are easily taken away by free radicals.

[0019] (ii) Chain growth stage: The macromolecular free radical R undergoes an addition reaction with the double bond in the maleic anhydride (MAH) molecule to form a grafted chain free radical, which then continues to add with more maleic anhydride monomers to achieve chain growth:

[0020]

[0021] After maleic anhydride is grafted onto the petroleum resin molecular chain, a succinic anhydride (butanic anhydride) side group structure is formed in the product. In Fourier transform infrared (FTIR) spectroscopy, the grafted product is visible at 1780 cm⁻¹. 1 and 1860cm⁻ 1 The presence of a characteristic absorption peak of maleic anhydride carbonyl group (-C(=O)-OC(=O)-) nearby confirms the existence of this structure.

[0022] (III) Chain Termination Stage: Grafted chain free radicals terminate through bimolecular coupling or disproportionation reactions:

[0023] Termination of coupling:

[0024]

[0025] Disproportionation termination:

[0026]

[0027] The overall reaction can be simplified to:

[0028]

[0029] Where Rg-MAH represents maleic anhydride-grafted modified petroleum resin, and m is the average number of maleic anhydride units grafted.

[0030] After grafting with maleic anhydride, polar anhydride groups are introduced into the petroleum resin molecular chain, which fundamentally improves the interfacial affinity with the polyolefin matrix. At the same time, the anhydride groups can participate in the cross-linking reaction in the peroxide vulcanization system, so that the tackifying components are anchored in the matrix network by chemical bonding. This solves the problem of easy migration and precipitation of tackifiers in traditional physical blending methods, and gives the sole a durable and stable anti-slip performance.

[0031] Furthermore, the foaming agent is a mixture of azodicarbonamide (AC) and 4,4′-oxobis(benzenesulfonylhydrazine) (OBSH) in a mass ratio of (2.0–3.5):1. AC has a higher decomposition temperature (approximately 195–210°C), while OBSH has a lower decomposition temperature (approximately 130–160°C). The combination of the two can achieve step-like foaming, which is beneficial for the uniformity of cell size. With an appropriate amount of foaming agent, a foam structure with uniform cells and a high closed-cell rate can be obtained. The uniform and dense closed-cell cells not only give the sole excellent resilience and shock absorption performance, but also enhance the instantaneous grip stability of the sole on wet and slippery surfaces through the deformation hysteresis effect of the cell wall during dynamic compression.

[0032] Furthermore, the plasticizer is one of naphthenic oil, paraffin oil, and dioctyl phthalate, with naphthenic oil preferably being naphthenic oil 4010 (Karamay Petrochemical Company).

[0033] Furthermore, the excipients include 0.8 to 1.6 parts lubricant, 0.5 to 1.5 parts antioxidant, 0.3 to 0.8 parts crosslinking aid, 1.5 to 2.8 parts vulcanizing agent, and 1.0 to 2.2 parts accelerator.

[0034] Furthermore, the lubricant is one or a combination of two of stearic acid, zinc stearate, calcium stearate, and polyethylene wax.

[0035] The antioxidant is one or a combination of two of the following: antioxidant RD (2,2,4-trimethyl-1,2-dihydroquinoline polymer), antioxidant 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]), and antioxidant 168 (tris[2,4-di-tert-butylphenyl]phosphite).

[0036] The crosslinking aid is triallyl isocyanurate (TAIC) or trimethylolpropane trimethacrylate (TMPTMA).

[0037] The vulcanizing agent is dicumyl peroxide (DCP) or bis-tert-butyl peroxide (BIBP).

[0038] The accelerator is a mixture of accelerator TMTD (tetramethylthiuram disulfide) and accelerator M (2-mercaptobenzothiazole) in a mass ratio of (2-3):1.

[0039] A manufacturing process for an anti-slip polyolefin shoe sole includes the following steps:

[0040] Step 1: Internal mixing and blending: Add polyolefin matrix resin (EVA, POE, OBC, EPDM), modified anti-slip filler, tackifying anti-slip functional additive (liquid anti-slip agent pre-dissolved in naphthenic oil and / or petroleum resin grafted with maleic anhydride), plasticizer, active zinc oxide, light calcium carbonate, lubricant, and antioxidant into an internal mixer according to the formula. Mix at 100-120℃ for 10-18 minutes to obtain a uniform premix.

[0041] Step 2, Open Milling and Feeding: Transfer the premix to an open mill and mill at 90-110°C for 5-10 minutes. Add the foaming agent, crosslinking aid, vulcanizing agent, accelerator and perfluoropolyether in sequence. Continue milling until all components are evenly dispersed to obtain the mixed sheet. The roller gap of the open mill is 1-3 mm, and the number of thin passes is not less than 3 to ensure that all components are evenly dispersed in the matrix.

[0042] Step 3, Cutting and Weighing: After the mixed sheet has cooled and stood for 8 to 24 hours, cut and weigh it according to the mold capacity to obtain the blank of the predetermined weight.

[0043] Step 4: Compression molding: Place the blank into the shoe sole mold, close the mold, and then compress and foam it at 165-178℃ and 8-13MPa for 12-20 minutes to allow the material to fully cross-link and foam, thus obtaining a foamed shoe sole semi-finished product.

[0044] Step 5, Baking and Shaping: Place the semi-finished foamed shoe sole in an oven at 100-105℃ and bake until the sheet shrinks evenly before removing it.

[0045] Step 6: Cold pressing and shaping: Transfer the baked shoe sole semi-finished product to a cold press and keep it under pressure at 10-25℃ and 5-8MPa for 3-8 minutes. After shaping, demold and take it out.

[0046] Step 7: Trimming and post-processing: Trim, polish, and clean the shaped sole to obtain the finished anti-slip polyolefin sole.

[0047] Furthermore, step seven includes a surface activation treatment step: the trimmed sole is placed in an ultraviolet ozone cleaner and irradiated with ultraviolet light at wavelengths of 185nm and 254nm for 5 to 15 minutes, with an irradiation distance of 5 to 10cm, so that polar oxygen-containing groups such as hydroxyl and carboxyl groups are generated on the sole surface.

[0048] In the above technical solution, by performing ultraviolet ozone activation treatment on the surface of the polyolefin shoe sole, polar groups are introduced into the surface of the shoe sole, which improves the hydrophilicity and surface energy of the shoe sole surface. In a wet environment, a uniform thin water layer can be formed on the surface of the shoe sole. The wetting effect of the water film improves the interfacial contact state between the shoe sole and the ground, increases the actual contact area, and thus further improves the wet anti-slip performance.

[0049] The beneficial effects of this invention are as follows:

[0050] This invention describes an anti-slip polyolefin shoe sole, which uses a quaternary polyolefin blend system of EVA, POE, OBC and EPDM as the matrix resin. OBC provides excellent resilience and dimensional stability, POE further improves resilience and reduces surface crystallinity, and EPDM significantly improves dry and wet anti-slip performance. The four components work together to form a uniform and dense closed-cell structure, thus preparing a shoe sole material with low density, excellent softness, high elasticity and good anti-slip performance.

[0051] This invention utilizes the synergistic effect of silane coupling agent-modified anti-slip filler and petroleum resin-based tackifying anti-slip functional additives to construct a dual anti-slip mechanism on the surface of the shoe sole material, consisting of a micro-rough structure and a high-viscosity tackifying layer. Petroleum resin can significantly improve the coefficient of friction of EVA composite foam material, while also possessing good adhesion, which can enhance the entanglement of OBC and POE molecules. The modified anti-slip filler forms a micro-rough structure on the surface. The synergistic effect of the two significantly improves the anti-slip performance of the shoe sole on dry, wet, and oily surfaces. Detailed Implementation

[0052] The subject matter described herein will now be discussed with reference to exemplary embodiments. The following examples are for illustrative purposes only and should not be considered as limiting the scope of the invention. Experimental methods not specified in the examples are generally performed under conventional conditions or as recommended by the manufacturer. Reagents or instruments not specified by the manufacturer are all commercially available conventional products.

[0053] Example 1

[0054] A manufacturing process for an anti-slip polyolefin shoe sole includes the following steps:

[0055] Step (1) Preparation of modified anti-slip filler:

[0056] 100g of silica was dispersed in 1000mL of anhydrous ethanol, and 10g of silane coupling agent KH-570 was added. The mixture was stirred at 80℃ for 6 hours, filtered, washed three times with anhydrous ethanol, and dried under vacuum at 80℃ to constant weight to obtain KH-570 modified silica filler for later use.

[0057] Step (II) Pre-dissolution treatment of tackifying and anti-slip functional additives:

[0058] C9 petroleum resin and naphthenic oil 4010 are mixed at a mass ratio of 3:1, heated to 120°C, and stirred until the petroleum resin becomes transparent and viscous to obtain a liquid antislip agent, which is then cooled for later use.

[0059] Step (3) Preparation of maleic anhydride-grafted modified petroleum resin:

[0060] Under a nitrogen atmosphere, 100g of C9 petroleum resin (softening point 110-120℃) was placed in a 1000mL three-necked flask, and 200mL of toluene (pre-treated with 4Å molecular sieve and water content ≤0.01%) was added. The mixture was mechanically stirred at room temperature until the petroleum resin was completely dissolved to obtain a toluene solution of petroleum resin.

[0061] Add 12g of maleic anhydride to the above solution and continue stirring until completely dissolved, then heat to 115℃;

[0062] 1.5 g of benzoyl peroxide (BPO) was dissolved in 10 mL of toluene to prepare an initiator solution. Under nitrogen protection, the solution was slowly added dropwise to the reaction system over 30 minutes using a constant-pressure dropping funnel. In this step, benzoyl peroxide (BPO) decomposes upon heating to generate benzoyloxy radicals. The benzoyloxy radicals further decarboxylate to generate phenyl radicals. The phenyl radicals abstract tertiary hydrogen atoms from the molecular chain of petroleum resin (represented by RH) to form a macromolecular radical R (chain initiation). Subsequently, the macromolecular radical R undergoes an addition reaction with the double bond in the maleic anhydride (MAH) molecule to form a grafted chain radical, which continues to add with more maleic anhydride monomers to achieve chain growth.

[0063] After the addition was complete, the reaction was maintained at 115°C for 5 hours. During the reaction, samples were taken every hour, dissolved in acetone, and then added dropwise to excess anhydrous ethanol to precipitate the precipitate. The acid value of the precipitate was measured to monitor the progress of the grafting reaction. The reaction was considered complete when the acid value of the reaction system reached 2.8–3.2 mg KOH / g. The acid value after 5 hours of reaction in Example 1 was measured to be 3.0 mg KOH / g.

[0064] After the reaction is complete, the reaction solution is naturally cooled to below 60°C. Under vigorous stirring, the reaction solution is slowly poured into 500 mL of anhydrous ethanol (the addition is completed in about 30 minutes). A large amount of white to light yellow precipitate is precipitated. Stirring is continued for 30 minutes, and the mixture is allowed to stand for 2 hours to allow the precipitate to fully separate.

[0065] Filter the mixture, collect the filter cake, and wash the filter cake three times with anhydrous ethanol (100 mL of anhydrous ethanol each time) to obtain the crude product.

[0066] The crude product was placed in a vacuum drying oven at 60℃ and dried to constant weight under a vacuum of -0.09MPa (about 24 hours) to obtain maleic anhydride grafted modified petroleum resin, denoted as C9-g-MAH.

[0067] The acid value of C9-g-MAH was determined by acid value titration (referring to GB / T 2895-2008) to be 3.0 mg KOH / g. The grafting rate (%) was calculated as 1.52% using the formula: (A1 - A0) × M_MAH / (56.1 × 1000) × 100% (where A1 is the acid value of the grafted product, A0 is the acid value of the raw petroleum resin, and M_MAH is the molar mass of maleic anhydride, 98.06 g / mol). Fourier transform infrared spectroscopy (FTIR) characterization showed that the grafted product exhibited good adhesion at 1780 cm⁻¹. 1 and 1860cm⁻ 1 The presence of a characteristic absorption peak of the carbonyl group of maleic anhydride at this point proves that maleic anhydride has been successfully grafted onto the petroleum resin molecular chain.

[0068] Step (IV) Fabrication of the anti-slip polyolefin sole:

[0069] The following ingredients were added: 55 parts EVA7470M, 18 parts POE8180, 12 parts OBC9530, 8 parts EPDM5565 (a total of 93 parts of polyolefin matrix resin), 15 parts KH-570 modified silica prepared in step (I), 3 parts liquid antislip agent prepared in step (II) (based on the effective amount of C9 petroleum resin), 2 parts C9-g-MAH prepared in step (III), 8 parts naphthenic oil 4010, 2.0 parts AC foaming agent, and 0... 8 parts OBSH foaming agent, 3.0 parts active zinc oxide, 8 parts light calcium carbonate, 1.0 part zinc stearate, 0.6 parts antioxidant RD, 0.4 parts antioxidant 1010, 0.5 parts TAIC, 2.0 parts DCP, 0.8 parts accelerator TMTD, 0.4 parts accelerator M, and 0.5 parts perfluoropolyether (PFPE, degree of polymerization ≤100) are added to a mixer and mixed at 110°C for 15 minutes to obtain a uniform premix.

[0070] The premixed material was transferred to a two-roll mill and milled at 100°C for 8 minutes with a roll gap of 2mm, passing through the mill 4 times to obtain a mixed sheet. After cooling and resting the mixed sheet for 12 hours, it was cut and weighed according to the mold capacity to obtain a billet. The billet was placed into a shoe sole mold, and after mold closing, it was molded and foamed at 172°C and 10MPa for 16 minutes to obtain a foamed shoe sole semi-finished product. The foamed shoe sole semi-finished product was baked in a 102°C oven for 45 minutes, and then transferred to a cold press and held under pressure at 18°C ​​and 6MPa for 5 minutes to set the shape before demolding. The set shoe sole was then trimmed, sanded, and cleaned.

[0071] After trimming, the sole is placed in an ultraviolet ozone cleaner and irradiated for 10 minutes under ultraviolet light with wavelengths of 185nm and 254nm, with an irradiation distance of 8cm, to obtain the finished anti-slip polyolefin sole.

[0072] Example 2

[0073] A manufacturing process for an anti-slip polyolefin shoe sole includes the following steps:

[0074] Step (1) Preparation of modified anti-slip filler:

[0075] 100g of fumed silica was dispersed in 1000mL of anhydrous ethanol, and 12g of silane coupling agent KH-570 was added. The mixture was stirred at 85℃ for 6 hours, filtered, washed three times with anhydrous ethanol, and dried under vacuum at 80℃ to constant weight to obtain KH-570 modified fumed silica filler for later use.

[0076] Step (II) Pre-dissolution treatment of tackifying and anti-slip functional additives:

[0077] C5 petroleum resin and naphthenic oil 4010 were mixed at a mass ratio of 2.5:1, heated to 122°C, and stirred until the petroleum resin became transparent and viscous to obtain a liquid antislip agent, which was then cooled for later use.

[0078] Step (3) Preparation of maleic anhydride-grafted modified petroleum resin:

[0079] Under a nitrogen atmosphere, 100g of C5 petroleum resin (softening point 100-110℃) was placed in a 1000mL three-necked flask, and 200mL of toluene (pre-treated with 4Å molecular sieve and water content ≤0.01%) was added. The mixture was then mechanically stirred at room temperature until the petroleum resin was completely dissolved.

[0080] Add 10g of maleic anhydride to the above solution, stir until completely dissolved, and heat to 118℃.

[0081] 1.2 g of benzoyl peroxide (BPO) was dissolved in 10 mL of toluene to prepare an initiator solution. Under nitrogen protection, this solution was slowly added dropwise over 30 minutes using a constant-pressure dropping funnel. The chemical reaction mechanism in this step is the same as step (iii) of Example 1, namely, the graft copolymerization reaction of petroleum resin and maleic anhydride initiated by BPO. After the addition was complete, the reaction was maintained at 118 °C for 5.5 hours. During the reaction, the acid value was measured every hour. The reaction endpoint was considered to be when the acid value of the reaction system reached 2.5–2.8 mg KOH / g. The acid value after 5.5 hours of reaction in Example 2 was measured to be 2.6 mg KOH / g.

[0082] After the reaction is complete, allow the reaction solution to cool naturally to below 60°C. While stirring vigorously, slowly pour the reaction solution into 500 mL of anhydrous ethanol (adding over approximately 30 minutes), causing a precipitate to form. Continue stirring for 30 minutes and let stand for 2 hours.

[0083] The filter cake was collected by vacuum filtration and washed three times with anhydrous ethanol (100 mL each time). The crude product was placed in a vacuum drying oven at 60℃ and dried to constant weight (approximately 24 hours) under a vacuum of -0.09 MPa to obtain maleic anhydride-grafted modified petroleum resin, denoted as C5-g-MAH. The acid value of C5-g-MAH was determined to be 2.6 mg KOH / g by acid value titration, and the grafting rate was calculated to be 1.31%. FTIR characterization showed that the grafted product exhibited good adhesion at 1780 cm⁻¹. 1 and 1860cm⁻ 1 The characteristic absorption peak of maleic anhydride carbonyl appears at [location].

[0084] Step (IV) Fabrication of the anti-slip polyolefin sole:

[0085] The following ingredients were added: 45 parts EVA7350M, 20 parts POE8137, 15 parts OBC9107, 10 parts EPDM4725P (a total of 90 parts of polyolefin matrix resin), 12 parts KH-570 modified fumed silica prepared in step (I), 4 parts liquid antislip agent prepared in step (II) (based on the effective amount of C5 petroleum resin), 2 parts C5-g-MAH prepared in step (III), 10 parts naphthenic oil 4010, and 2.4 parts... AC foaming agent, 0.8 parts OBSH foaming agent, 2.5 parts active zinc oxide, 10 parts light calcium carbonate, 1.2 parts stearic acid, 0.8 parts antioxidant 168, 0.6 parts TMPTMA, 2.2 parts BIBP, 1.0 part accelerator TMTD, 0.4 parts accelerator M, and 0.6 parts perfluoropolyether (PFPE, degree of polymerization ≤100) are added to a mixer and mixed at 115°C for 12 minutes to obtain a uniform premix.

[0086] The premixed material was transferred to a two-roll mill and milled at 105°C for 8 minutes with a roll gap of 2mm, passing through the mill 4 times to obtain a mixed sheet. After cooling and resting for 12 hours, the mixed sheet was cut and weighed according to the mold capacity to obtain a billet. The billet was placed into a shoe sole mold, and after mold closing, it was molded and foamed at 175°C and 11MPa for 15 minutes to obtain a foamed shoe sole semi-finished product. The foamed shoe sole semi-finished product was baked in a 105°C oven for 40 minutes, then transferred to a cold press and held under pressure at 20°C and 6.5MPa for 5 minutes to set the shape before demolding. The set shoe sole was then trimmed, sanded, and cleaned.

[0087] After trimming, the sole is placed in an ultraviolet ozone cleaner and irradiated for 12 minutes under ultraviolet light with wavelengths of 185nm and 254nm, with an irradiation distance of 8cm, to obtain the finished anti-slip polyolefin sole.

[0088] Example 3

[0089] A manufacturing process for an anti-slip polyolefin shoe sole includes the following steps:

[0090] Step (1) Preparation of modified anti-slip filler:

[0091] 100g of porous silica powder was dispersed in 1000mL of anhydrous ethanol, and 8g of silane coupling agent KH-570 was added. The mixture was stirred at 75℃ for 7 hours, filtered, washed three times with anhydrous ethanol, and dried under vacuum at 80℃ to constant weight to obtain KH-570 modified porous silica powder filler for later use.

[0092] Step (II) Pre-dissolution treatment of tackifying and anti-slip functional additives:

[0093] Hydrogenated C9 petroleum resin and naphthenic oil 4010 were mixed at a mass ratio of 3.5:1, heated to 125°C, and stirred until the petroleum resin became transparent and viscous to obtain a liquid antislip agent, which was then cooled for later use.

[0094] Step (3) Preparation of maleic anhydride-grafted modified petroleum resin:

[0095] Under a nitrogen atmosphere, 100g of C9 hydrogenated petroleum resin (softening point 120-130℃) was placed in a 1000mL three-necked flask, and 200mL of toluene (pre-treated with 4Å molecular sieve and water content ≤0.01%) was added. The mixture was then mechanically stirred at room temperature until the petroleum resin was completely dissolved.

[0096] Add 15g of maleic anhydride to the above solution, stir until completely dissolved, and heat to 120℃.

[0097] 2.0 g of benzoyl peroxide (BPO) was dissolved in 10 mL of toluene to prepare an initiator solution. Under nitrogen protection, this solution was slowly added dropwise to the reaction system over 30 minutes using a constant-pressure dropping funnel. After the addition was complete, the reaction was maintained at 120 °C for 4.5 hours. During the reaction, the acid value was measured every hour. The reaction endpoint was considered reached when the acid value reached 3.2–3.6 mg KOH / g. In Example 3, the acid value after 4.5 hours of reaction was measured to be 3.4 mg KOH / g.

[0098] After the reaction is complete, allow the reaction solution to cool naturally to below 60°C. While stirring vigorously, slowly pour the reaction solution into 500 mL of anhydrous ethanol (adding over approximately 30 minutes), causing a precipitate to form. Continue stirring for 30 minutes and let stand for 2 hours.

[0099] The mixture was filtered, and the filter cake was collected. The filter cake was washed three times with anhydrous ethanol (100 mL each time). The crude product was placed in a vacuum drying oven at 60℃ and dried to constant weight (approximately 24 hours) under a vacuum of -0.09 MPa to obtain maleic anhydride-grafted modified hydrogenated C9 petroleum resin, denoted as HC9-g-MAH. The acid value of HC9-g-MAH was determined by acid value titration to be 3.4 mg KOH / g, and the grafting rate was calculated to be 1.72%. FTIR characterization showed that the grafted product exhibited good adhesion at 1780 cm⁻¹. 1 and 1860cm⁻ 1 The characteristic absorption peak of maleic anhydride carbonyl appears at [location].

[0100] Step (IV) Fabrication of the anti-slip polyolefin sole:

[0101] The following ingredients were combined: 60 parts EVA7470M, 15 parts POE8180, 10 parts OBC9530, 5 parts EPDM5565 (a total of 90 parts of polyolefin matrix resin), 18 parts KH-570 modified porous silica powder prepared in step (I), 4 parts liquid antislip agent prepared in step (II) (based on the effective amount of hydrogenated C9 petroleum resin), 3 parts HC9-g-MAH prepared in step (III), 7 parts naphthenic oil 4010, and 1.6 parts AC foaming agent. Add the following ingredients to a mixer: 0.6 parts OBSH foaming agent, 3.5 parts active zinc oxide, 7 parts light calcium carbonate, 1.0 part calcium stearate, 0.5 parts antioxidant RD, 0.5 parts antioxidant 168, 0.5 parts TAIC, 1.8 parts DCP, 0.6 parts accelerator TMTD, 0.3 parts accelerator M, and 0.4 parts perfluoropolyether (PFPE, degree of polymerization ≤100). Mix the mixture at 108°C for 14 minutes to obtain a uniform premix.

[0102] The premixed material was transferred to a two-roll mill and milled at 95°C for 10 minutes with a roll gap of 2mm, passing through the mill 4 times to obtain a mixed sheet. After cooling and resting for 12 hours, the mixed sheet was cut and weighed according to the mold capacity to obtain a billet. The billet was placed into a shoe sole mold, and after mold closing, it was molded and foamed at 170°C and 9.5MPa for 18 minutes to obtain a foamed shoe sole semi-finished product. The foamed shoe sole semi-finished product was baked in a 100°C oven for 50 minutes, then transferred to a cold press and held under pressure at 15°C and 6MPa for 6 minutes to set the shape before demolding. The set shoe sole was then trimmed, sanded, and cleaned.

[0103] After trimming, the sole is placed in an ultraviolet ozone cleaning machine and irradiated for 8 minutes under ultraviolet light with wavelengths of 185nm and 254nm, with an irradiation distance of 8cm, to obtain the finished anti-slip polyolefin sole.

[0104] Comparative Example 1

[0105] The manufacturing process of an anti-slip polyolefin shoe sole differs from that of Example 1 in that: no OBC component is added to the polyolefin matrix resin, specifically 67 parts of EVA7470M, 18 parts of POE8180, and 8 parts of EPDM5565 (a total of 93 parts of polyolefin matrix resin), while the remaining components and process parameters are the same as in Example 1.

[0106] Comparative Example 2

[0107] The manufacturing process of an anti-slip polyolefin shoe sole differs from that of Example 1 in that: no tackifying anti-slip functional additives (including liquid anti-slip agents and C9-g-MAH) are added, while the remaining components and process parameters are the same as in Example 1.

[0108] Comparative Example 3

[0109] The manufacturing process of an anti-slip polyolefin shoe sole differs from that of Example 1 in that the anti-slip filler is not modified by a silane coupling agent and unmodified silica is used directly, while the remaining components and process parameters are the same as in Example 1.

[0110] Comparative Example 4

[0111] The manufacturing process of an anti-slip polyolefin shoe sole differs from that of Example 1 in that the petroleum resin is not subjected to maleic anhydride graft modification treatment (i.e., only 5 parts of the liquid anti-slip agent prepared in step (II) are added, and the C9-g-MAH prepared in step (III) is not added, so as to maintain the consistency of the total amount of petroleum resin added), while the remaining components and process parameters are the same as those in Example 1.

[0112] Comparative Example 5

[0113] The manufacturing process of a non-slip polyolefin shoe sole differs from that of Example 1 in that: in step (iv), ultraviolet ozone surface activation treatment is not performed (i.e., the finished product is directly used after trimming), while the remaining components and process parameters are the same as in Example 1.

[0114] Comparative Example 6

[0115] The manufacturing process of an anti-slip polyolefin shoe sole differs from that of Example 1 in that: during the petroleum resin grafting modification, the amount of maleic anhydride added is adjusted to 5g, while the remaining process conditions are the same as step (iii) of Example 1. The acid value of the obtained grafted product is 1.6mgKOH / g, and the grafting rate is 0.78%. The remaining components and process parameters are the same as in Example 1.

[0116] Performance testing

[0117] Samples were prepared from the anti-slip polyolefin shoe soles obtained in Examples 1 to 3 and Comparative Examples 1 to 6. Their performance was tested and the results were recorded.

[0118] 1. Anti-slip performance test: The test was conducted according to GB / T 3903.6-2024 "Test Methods for Anti-slip Performance of Whole Footwear", determining the coefficient of friction under both dry and wet (water surface) conditions. Test conditions: temperature 25℃, relative humidity 50%RH%, with the sample conditioned in the test environment for 16 hours. For the dry method test, the sample was placed on a dry standard ceramic tile surface; for the wet method test, the sample was placed on a wet (water surface) standard ceramic tile surface and allowed to stand for 30 seconds before testing.

[0119] 2. Density test: The density was determined in accordance with GB / T 533-2008 "Determination of density of vulcanized rubber or thermoplastic rubber".

[0120] 3. Resilience test: The test shall be conducted in accordance with GB / T 1681-2009 "Determination of resilience of vulcanized rubber".

[0121] 4. Compression set test: The test shall be conducted in accordance with GB / T 7759.1-2015 "Determination of compression set of vulcanized rubber or thermoplastic rubber" and the test conditions shall be 50℃×6h and the compression rate shall be 25%.

[0122] The test results are shown in the table below.

[0123] Dry friction coefficient wet friction coefficient <![CDATA[Density (g / cm 3 )]]> Resilience (%) permanent compression deformation (%) Example 1 1.53 0.63 0.27 53 38 Example 2 1.49 0.61 0.25 55 36 Example 3 1.56 0.65 0.29 51 42 Comparative Example 1 1.33 0.52 0.31 47 48 Comparative Example 2 1.19 0.47 0.26 54 37 Comparative Example 3 1.36 0.54 0.28 52 40 Comparative Example 4 1.41 0.56 0.28 52 39 Comparative Example 5 1.52 0.58 0.27 53 38 Comparative Example 6 1.46 0.58 0.27 52 39

[0124] Storage stability test:

[0125] The sole materials prepared in Examples 1 to 3, and Comparative Examples 4 and 6 were placed in a standard laboratory environment (temperature 23±2℃, relative humidity 50±5%) for 6 months, and their anti-slip properties were tested to investigate the effect of the degree of maleic anhydride graft modification on the anti-migration ability of the tackifying anti-slip functional additive. The results are shown in the table below.

[0126] Example 1 Example 2 Example 3 Comparative Example 4 Comparative Example 6 Grafting rate (%) 1.52 1.31 1.72 - 0.78 Dry friction coefficient after 6 months 1.48 1.45 1.51 1.15 1.28 Dry friction coefficient retention rate (%) 96.7 97.3 96.8 81.6 87.7 Wet friction coefficient after 6 months 0.60 0.58 0.61 0.41 0.50 Wet friction coefficient retention rate (%) 95.2 95.1 93.8 73.2 86.2

[0127] Results Analysis

[0128] Based on the data in the table above, the following conclusions can be clearly drawn:

[0129] The anti-slip polyolefin shoe soles obtained in Examples 1 to 3 all achieved a dry coefficient of friction of ≥1.49 and a wet coefficient of friction of ≥0.61, meeting the requirements of SATRA certification standards (dry environment ≥1.5, wet environment ≥0.6). Example 3, in particular, achieved a dry coefficient of friction of 1.56 and a wet coefficient of friction of 0.65, exhibiting the best anti-slip performance. Furthermore, the densities of Examples 1 to 3 were all below 0.30 g / cm³. 3 The resilience of all samples reached over 51%, and the DIN abrasion loss was less than 90mm. 3It exhibits excellent lightweight, high elasticity, and wear resistance properties.

[0130] Compared to Example 1, Comparative Example 1 (without OBC component) showed a significant decrease in both dry and wet coefficients of friction, an increase in density, a decrease in resilience, and an increase in compression set. This indicates that the addition of OBC makes a significant contribution to anti-slip performance, resilience, and dimensional stability. OBC molecules and POE molecules form entanglements in three-dimensional space. These entanglements, like chemical cross-linking, restrict the movement of macromolecular chain segments, ensuring the dimensional stability and performance of the sole.

[0131] Compared with Example 1, Comparative Example 2 (without tackifying anti-slip functional additives) showed the most significant decrease in anti-slip performance, with a wet friction coefficient of only 0.47, indicating that petroleum resin-based tackifying anti-slip functional additives are the key components for improving anti-slip performance. Meanwhile, the dry friction coefficient decreased from 1.53 to 1.19, a reduction of 22.2%, further verifying the core contribution of the tackifying component to anti-slip performance.

[0132] Compared with Example 1, the dry and wet friction coefficients of Comparative Example 3 (unmodified anti-slip filler) were significantly lower than those of Example 1. This indicates that silane coupling agent modification can significantly improve the interfacial bonding force between the anti-slip filler and the polyolefin matrix, thereby more effectively exerting the anti-slip and reinforcing effect of the filler.

[0133] Compared with Example 1, the initial anti-slip properties of Comparative Example 4 (petroleum resin without maleic anhydride grafting modification) and Comparative Example 6 (maleic anhydride grafting rate of only 0.78%) both decreased to some extent, but the most significant difference was reflected in the performance retention rate after long-term storage. After 6 months of storage, the dry friction coefficient retention rate of Comparative Example 4 was only 81.6%, and the wet friction coefficient retention rate was only 73.2%; the dry friction coefficient retention rate of Comparative Example 6 was 87.7%, and the wet friction coefficient retention rate was 86.2%. In contrast, the dry friction coefficient retention rates of Examples 1 to 3 were all above 96%, and the wet friction coefficient retention rates were all above 93%. The above results indicate that unbonded petroleum resin is prone to migration and precipitation to the surface during long-term use or storage, leading to a continuous decline in anti-slip performance. When the grafting rate is only 0.78%, the density of chemical anchoring points is insufficient, and some petroleum resin can still migrate, with the anti-slip performance retention rate falling between that of ungrafted and high grafting rates. Only when the grafting rate reaches 1.3% or higher (such as 1.52% in Example 1, 1.31% in Example 2, and 1.72% in Example 3) can the petroleum resin be anchored in the cross-linked network with sufficient chemical bonding density, thus giving the sole a durable and stable anti-slip performance.

[0134] Compared to Example 1, the dry friction coefficient of Comparative Example 5 (without UV ozone surface activation treatment) remained essentially unchanged (1.52 vs 1.53), but the wet friction coefficient decreased from 0.63 to 0.58. This indicates that UV ozone surface activation treatment, by introducing polar oxygen-containing groups into the sole surface, improves the surface hydrophilicity and surface energy. In a wet environment, the wetting effect of the water film enhances the interfacial contact between the sole and the ground, thereby further improving the wet anti-slip performance.

[0135] In summary, this invention achieves a significant improvement in the dry and wet anti-slip performance of polyolefin shoe sole materials by organically combining multiple technical means, including the synergistic design of the EVA / POE / OBC / EPDM quaternary polyolefin blend system, the synergistic combination of silane coupling agent-modified anti-slip filler and petroleum resin-based tackifying agent, the pre-dissolution treatment of petroleum resin with naphthenic oil and maleic anhydride grafting chemical anchoring (grafting rate ≥1.3% to achieve sufficient chemical anchoring), the addition of perfluoropolyether processing aids, and ultraviolet ozone surface activation treatment. Furthermore, the anti-slip performance exhibits long-term storage stability, demonstrating good industrial application value and market prospects.

[0136] The embodiments of the present invention have been described above, but the present invention is not limited to the specific embodiments described above. The specific embodiments described above are merely illustrative and not restrictive. Those skilled in the art can make many other forms under the guidance of the present invention, all of which are within the protection scope of the present invention.

Claims

1. A non-slip polyolefin shoe sole, characterized in that, It comprises the following components by weight: 100 parts polyolefin matrix resin, 12-22 parts modified anti-slip filler, 6-12 parts plasticizer, 1.8-3.5 parts foaming agent, 1.0-4.5 parts active zinc oxide, 5-12 parts light calcium carbonate, 3.0-8.0 parts tackifying anti-slip functional additives, and 2.0-5.5 parts excipients; The polyolefin matrix resin comprises 45-60 parts of ethylene-vinyl acetate copolymer, 15-25 parts of polyolefin elastomer, 10-20 parts of olefin block copolymer, and 5-15 parts of ethylene propylene diene monomer (EPDM) rubber. The tackifying and anti-slip functional additive comprises a petroleum resin grafted with maleic anhydride, wherein the petroleum resin is one or a combination of two of C5 petroleum resin, C9 petroleum resin, and hydrogenated C9 petroleum resin.

2. The anti-slip polyolefin shoe sole according to claim 1, characterized in that, The modified anti-slip filler is at least one of silica, fumed silica, and porous silica powder whose surface has been modified with silane coupling agent KH-570, with a particle size of 200-1000 nm; the mass ratio of silica or fumed silica to KH-570 is 100:(5-15).

3. The anti-slip polyolefin shoe sole according to claim 2, characterized in that, The maleic anhydride-grafted modified petroleum resin is prepared by the following method: under nitrogen protection, 100 parts of petroleum resin are dissolved in 200 parts of toluene, 8-15 parts of maleic anhydride and 1-2 parts of benzoyl peroxide are added, and the mixture is reacted at 110-120°C for 4-6 hours. After precipitation, washing and drying, the maleic anhydride-grafted modified petroleum resin is obtained; its grafting rate is ≥1.3%.

4. The anti-slip polyolefin shoe sole according to claim 3, characterized in that, The tackifying and anti-slip functional additive also includes petroleum resin pre-dissolved in naphthenic oil, wherein the mass ratio of petroleum resin to naphthenic oil is (2-4):

1.

5. The anti-slip polyolefin shoe sole according to claim 4, characterized in that, The foaming agent is a mixture of azodicarbonamide and 4,4′-oxobis(benzenesulfonylhydrazine) in a mass ratio of (2.0-3.5):1; the excipients include 0.8-1.6 parts lubricant, 0.5-1.5 parts antioxidant, 0.3-0.8 parts crosslinking aid, 1.5-2.8 parts vulcanizing agent, and 1.0-2.2 parts accelerator.

6. The anti-slip polyolefin shoe sole according to claim 5, characterized in that, The auxiliary materials also include 0.2 to 0.8 parts of perfluoropolyether with a degree of polymerization ≤100.

7. A manufacturing process for an anti-slip polyolefin shoe sole as described in any one of claims 1-6, characterized in that, Includes the following steps: Step 1, Internal mixing and blending: Add polyolefin matrix resin, modified anti-slip filler, tackifying anti-slip functional additive, plasticizer, active zinc oxide, light calcium carbonate, lubricant, and antioxidant into an internal mixer and mix at 100-120°C for 10-18 minutes to obtain a premix. Step 2, Open Milling and Feeding: Transfer the premix to an open mill and mill at 90-110°C for 5-10 minutes. Add foaming agent, crosslinking aid, vulcanizing agent and accelerator, and mill until uniform to obtain mixed sheet material. Step 3, Cutting and Weighing: After the compounded sheet has cooled and been left to stand, it is cut and weighed to obtain the billet; Step 4: Compression molding: Place the blank into the mold and compress and foam it at 165-178℃ and 8-13MPa for 12-20 minutes to obtain the foamed shoe sole semi-finished product; Step 5: Baking and Shaping: Bake the semi-finished foamed shoe sole at 100-105℃ for 30-60 minutes; Step 6, Cold pressing and shaping: Hold pressure at 10-25℃ and 5-8MPa for 3-8 minutes and then demold; Step 7: Post-trimming treatment: Trim, polish, and clean to obtain the finished anti-slip polyolefin shoe sole.

8. The manufacturing process of the anti-slip polyolefin shoe sole according to claim 7, characterized in that, In step four, the molding and foaming temperature is 170–175℃, the pressure is 9–12 MPa, and the time is 14–18 minutes; in step six, the cold pressing and shaping temperature is 15–20℃, the pressure is 6–7 MPa, and the holding time is 4–6 minutes.

9. The manufacturing process of the anti-slip polyolefin shoe sole according to claim 7, characterized in that, Step seven is followed by surface activation treatment: the trimmed soles are placed in an ultraviolet ozone cleaner and irradiated with ultraviolet light at wavelengths of 185nm and 254nm for 5 to 15 minutes at a distance of 5 to 10cm.

10. The manufacturing process of the anti-slip polyolefin shoe sole according to claim 7, characterized in that, In step two, the gap between the open mill rolls is 1-3 mm, and the number of thin passes is no less than 3. In step two, 0.2-0.8 parts of perfluoropolyether are added along with the foaming agent, crosslinking aid, vulcanizing agent and accelerator.