An inorganic composite filler-modified polypropylene wire and cable insulation material and its preparation method

By synergistically modifying polypropylene wire and cable insulation materials with potassium hexatitanate whiskers, cerium dioxide, magnesium oxide, and organic antioxidants, the aging problem of polypropylene wire and cable insulation materials under high temperature, oxygen, and ultraviolet radiation is solved, and the mechanical properties and electrical stability of the materials are improved. The materials are suitable for medium and low voltage power wires and cables and new energy vehicle wires and cables.

CN123107250APending Publication Date: 2026-11-17重庆科宝电缆股份有限公司 +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611530994.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polypropylene wire and cable insulation materials are prone to aging under high temperature, oxygen, ultraviolet radiation and alternating temperature conditions, resulting in molecular chain breakage, material embrittlement, mechanical property degradation, and easy accumulation of space charge, which affects the stability and lifespan of wires and cables. Modification with a single inorganic filler cannot simultaneously achieve both mechanical and insulation properties.

Method used

A ternary synergistic modification system of one-dimensional rigid framework and nanofunctional particles was constructed by using potassium hexatitanate whiskers, cerium dioxide, and magnesium oxide compounded with organic antioxidants for synergistic modification. Nanoparticles were loaded onto the whisker surface through in-situ precipitation combined with calcination process, thereby improving the material’s creep resistance, aging resistance and electrical stability.

Benefits of technology

It significantly improves the rigidity and creep resistance of polypropylene wires and cables, reduces the heat shrinkage rate, inhibits space charge accumulation, improves dielectric properties, and ensures the stability and safety of cables during long-term service.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses an inorganic composite filler-modified polypropylene wire and cable insulation material and its preparation method, which is made from the following raw materials in parts by weight: 85-94 parts of copolymer polypropylene, 5-11 parts of composite inorganic filler, 0.3-0.5 parts of organic composite antioxidant obtained by compounding pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] with tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 1:1-2:1, and 0.2-0.6 parts of processing aid. It overcomes the defects of existing polypropylene wire and cable insulation materials, such as poor creep resistance, high thermal shrinkage rate, insufficient thermo-oxidative aging performance, easy accumulation of space charge, prominent shortcomings in the modification performance of single inorganic filler, and easy agglomeration and deterioration of electrical performance in simple physical blending.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wire and cable technology, specifically to an inorganic composite filler-modified polypropylene wire and cable insulation material and its preparation method. Background Technology

[0002] Polypropylene (PP) possesses outstanding advantages such as low density, high insulation resistivity, excellent processability, chemical corrosion resistance, and halogen-free and low-smoke properties, making it an ideal insulating substrate for high-voltage, medium- and low-voltage power cables and cables, as well as for new energy vehicle cables. Compared to traditional polyvinyl chloride (PVC) and cross-linked polyethylene (XLPE) insulation materials, PP wire and cable insulation materials can be cross-link-free and recyclable, showing broad application prospects in the field of green and energy-saving wires and cables.

[0003] However, pure polypropylene matrix itself has obvious performance shortcomings: On the one hand, polypropylene molecular chains are highly flexible but lack rigidity, making them prone to molecular chain slippage and relaxation under long-term external forces. This results in poor creep resistance and high thermal shrinkage, leading to problems such as insulation layer deformation and loosening during long-term service of wires and cables, which seriously affect the operational stability and service life of the wires and cables. On the other hand, polypropylene is prone to thermo-oxidative aging and photo-aging under high temperature, oxygen, ultraviolet radiation, and alternating temperature conditions, causing molecular chain breakage and degradation, resulting in material embrittlement, mechanical property degradation, and decreased insulation resistance. At the same time, space charge accumulation is easily generated inside the polypropylene insulation, inducing local electric field distortion and causing insulation aging and breakdown, which greatly limits the large-scale application of polypropylene wires and cables in high-end outdoor and alternating conditions.

[0004] Currently, the industry mostly uses single inorganic fillers to modify polypropylene insulation materials, improving the mechanical and insulation properties of the material by adding rigid powders. However, single filler modification has significant performance limitations: rigid whisker fillers can only improve mechanical creep resistance, with limited effects on aging resistance and space charge suppression; rare earth oxides only possess excellent anti-aging and free radical scavenging capabilities, but offer weak improvements in material rigidity and dimensional stability; metal oxides can only optimize dielectric properties and construct charge traps, failing to provide mechanical reinforcement. Furthermore, existing modification processes often employ direct physical blending of powders, resulting in poor interfacial compatibility between inorganic fillers and the polypropylene matrix. The fillers are prone to agglomeration, which not only fails to achieve the modification effect but also creates interfacial defects and micropores within the matrix, deteriorating the material's mechanical and electrical insulation properties and hindering the overall performance improvement of modified polypropylene wire and cable insulation materials. Therefore, developing a multi-component synergistic modification method with uniform filler dispersion, excellent interfacial bonding, and simultaneously high strength creep resistance, low shrinkage, aging resistance, and low space charge accumulation in polypropylene wire and cable insulation materials is a key research focus and technical challenge for those skilled in the art. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide an inorganic composite filler-modified polypropylene wire and cable insulation material, and secondly, to provide its preparation method. This overcomes the deficiencies of existing polypropylene wire and cable insulation materials, such as poor creep resistance, high thermal shrinkage, insufficient thermo-oxidative aging performance, easy accumulation of space charge, significant shortcomings in the modification performance of single inorganic fillers, and easy agglomeration and deterioration of electrical properties in simple physical blending.

[0006] To achieve the aforementioned first objective, the present invention adopts the following technical solution: an inorganic composite filler synergistic modification polypropylene wire and cable insulation material, characterized in that it is made from the following raw materials in parts by weight: 85-94 parts copolymer polypropylene, 5-11 parts composite inorganic filler, 0.3-0.5 parts organic composite antioxidant obtained by compounding pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] with tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 1:1-2:1, and 0.2-0.6 parts processing aid;

[0007] The processing aid is one or both of stearic acid and polyethylene wax;

[0008] The composite inorganic filler was prepared according to the following method:

[0009] Potassium hexatitanate whiskers were added to deionized water to prepare a suspension with a solid content of 5%-6%. Cerium nitrate hexahydrate and magnesium nitrate hexahydrate were added at a mass ratio of 10:2-4:13-25. Polyethylene glycol 4000 (PEG-4000) was added at 2-3% of the total mass of cerium nitrate hexahydrate and magnesium nitrate hexahydrate, and the mixture was stirred to dissolve and disperse. Ammonium bicarbonate aqueous solution was slowly added dropwise to the suspension at 15℃-22℃, controlling the final pH to 9-11. After the addition was completed, the mixture was aged for 8-12 minutes (short aging time to avoid cerium and magnesium hydroxides forming independent particles and to ensure that the active components are loaded onto the surface of the potassium hexatitanate whiskers), and then immediately filtered under reduced pressure. The mixture was then subjected to pre-hydrocarbonation treatment. The ammonium citrate aqueous solution, adjusted to pH 8.8-9.2 and at 40℃-50℃, was used to slurry and wash the material. After stirring for 6-10 minutes, the mixture was filtered again. Then, the material was rinsed 2-3 times with deionized water at 40℃-55℃ and pH slightly adjusted to 8.5-9.0 using ammonium bicarbonate. The material was then dried. The solid was spread out and heated to 520℃-580℃ in air atmosphere, held for 40-70 minutes, and then cooled to room temperature in dry air to obtain a cerium dioxide and magnesium oxide in-situ supported potassium hexatitanate whisker composite inorganic filler. 2%-3% of the total mass of the composite inorganic filler was added as a silane coupling agent γ-(2,3-epoxypropoxy)propyltrimethoxysilane (KH-560), and the surface was modified by high-speed stirring using a dry method to obtain the composite inorganic filler.

[0010] In the above scheme: the melt flow rate of the copolymer polypropylene is 2-6 g / 10 min (230℃, 2.16 kg).

[0011] In the above scheme: the mass concentration of ammonium bicarbonate aqueous solution is 8%-10%, and the dropping rate is 0.8-1.2 mL / min.

[0012] In the above scheme, the mass concentration of ammonium citrate aqueous solution is 0.3%-0.5%.

[0013] In the above scheme, the temperature is increased to 520℃-580℃ at a heating rate of 3.0-3.5℃ / min.

[0014] In the above scheme, the mass ratio of potassium hexatitanate whiskers, cerium dioxide, and magnesium oxide in the composite inorganic filler is 12-18:0.8-2.4:2-6.

[0015] The second objective of this invention is achieved as follows: a method for preparing the inorganic composite filler synergistic modified polypropylene wire and cable insulation material, characterized by the following steps: accurately weighing copolymer polypropylene, composite inorganic filler, organic composite antioxidant and processing aid, and adding them together into a high-speed mixer, stirring and mixing at high speed for 5-8 minutes at room temperature to obtain a mixed premix; feeding the premix into a twin-screw extruder for melt extrusion granulation, with the extruder temperature set as follows: zone 1 180℃-190℃, zone 2 195℃-205℃, zone 3 210℃-220℃, die head temperature 215℃-225℃, and screw speed 220-260 r / min; the material undergoes melt blending, extrusion, water-cooled traction, pelletizing, and drying to obtain uniform modified polypropylene wire and cable insulation granules.

[0016] In the above method: dry in an oven at 60℃-80℃ for 2-4 hours.

[0017] Preparation method of inorganic composite filler synergistic modification of polypropylene wire and cable: The dried modified polypropylene wire and cable insulation granules are fed into the cable extrusion coating equipment, and the insulation layer is uniformly extruded on the conductor surface. The extrusion temperature is controlled at 210℃-225℃. After water cooling, shaping, traction and winding, high-strength, creep-resistant, aging-resistant and low space charge accumulation modified polypropylene wire and cable are finally obtained.

[0018] This invention employs a compound of potassium hexatitanate whiskers, cerium dioxide, and magnesium oxide, along with organic antioxidants, to leverage the complementary advantages of each filler component. While improving the rigidity and creep resistance of polypropylene insulation materials and reducing thermal shrinkage, it also inhibits the thermo-oxidative aging chain reaction and introduces deep traps in the matrix to suppress space charge accumulation, thereby obtaining a polypropylene wire and cable insulation material with balanced mechanical properties, dimensional stability, aging resistance, and dielectric properties.

[0019] This invention constructs a ternary synergistic modification system that combines a one-dimensional rigid framework with nano-functional particles. Through the synergistic effect of in-situ load composite structure and interface modification, it improves the comprehensive insulation performance of polypropylene wires and cables from multiple dimensions such as mechanical reinforcement, dimensional stability, aging resistance, and dielectric optimization.

[0020] Potassium hexatitanate whiskers, which exhibit excellent alkali resistance and thermal stability, are selected as a one-dimensional rigid support framework. They can form a uniformly interwoven network structure within the polypropylene matrix, effectively restricting the slippage and relaxation of polypropylene molecular chains under external forces and high-temperature conditions. This significantly improves the tensile strength, flexural modulus, and creep resistance of the material, reduces the thermal shrinkage rate of the insulation layer, and ensures the dimensional stability of the cable during long-term service. At the same time, potassium hexatitanate whiskers have excellent insulation properties and will not negatively affect the dielectric properties of the polypropylene matrix.

[0021] By uniformly loading nano-cerium dioxide and nano-magnesium oxide onto the surface of whiskers through in-situ precipitation combined with calcination, the problem of nanoparticle agglomeration is completely solved, replacing the traditional physical blending method. Nano-cerium dioxide possesses excellent UV absorption and free radical scavenging capabilities, effectively quenching active free radicals generated during the thermo-oxidative and photo-aging processes of polypropylene, blocking the aging chain reaction, and delaying material embrittlement. Nano-magnesium oxide introduces a large number of deep trap energy levels into the insulation system, effectively capturing and binding space charges, inhibiting charge migration and accumulation, alleviating electric field distortion, and significantly improving the electrical stability and withstand voltage performance of polypropylene insulation. Simultaneously, the addition of PEG-4000 as a steric hindrance dispersant effectively inhibits the growth of nanoparticles during calcination, ensuring that cerium dioxide and magnesium oxide maintain a uniform nanoscale dispersion. Through KH-560 dry surface modification, a compatible transition interface can be constructed between the inorganic filler and the polypropylene matrix, eliminating interfacial micropores and defects, improving the interfacial bonding force between the filler and the matrix, further improving filler dispersibility, and balancing the material's mechanical and insulation properties.

[0022] Composite antioxidants can form a synergistic anti-aging system of organic and inorganic composite fillers. The main antioxidant captures active free radicals, and the auxiliary antioxidant decomposes peroxides. Combined with the ultraviolet shielding and charge binding effects of inorganic fillers, it comprehensively improves the weather resistance and long-term service stability of polypropylene wire and cable insulation materials.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention uses alkali-resistant and heat-resistant potassium hexatitanate whiskers to construct a rigid interwoven network in the polypropylene matrix, which can effectively limit the slippage and relaxation of polypropylene molecular chains under high temperature and external force conditions, significantly improve the rigidity and creep resistance of the material, reduce the thermal shrinkage rate of the insulation material, solve the defects of traditional polypropylene insulation that is easy to deform and has poor dimensional stability, and effectively ensure the long-term service safety of wires and cables.

[0025] (2) The nano-cerium dioxide loaded on the surface of the whiskers can shield ultraviolet light and capture aging free radicals, forming multiple anti-aging barriers with organic composite antioxidants, inhibiting the thermal and photo-aging degradation of polypropylene; nano-magnesium oxide can introduce deep trap energy levels in the matrix, effectively binding space charge, alleviating electric field distortion, and greatly improving the voltage resistance stability and service life of the insulating material.

[0026] (3) The filler has excellent dispersibility and strong process adaptability and practicality. This invention solves the problem of nanoparticle agglomeration from the root by using in-situ precipitation and calcination process, and optimizes the interfacial compatibility between inorganic filler and polypropylene matrix by modifying with silane coupling agent, thus eliminating blending defects. The overall preparation process is simple and controllable, adaptable to existing wire and cable mass production equipment, and the raw materials are green, readily available and inexpensive, which has excellent industrial promotion value. Detailed Implementation

[0027] The present invention will be further described in detail below through specific embodiments: The copolymer polypropylene (Yanshan Petrochemical PP-R4220) has a melt flow rate of 4 g / 10 min (230℃, 2.16 kg).

[0028] Example 1

[0029] Potassium hexatitanate whiskers (needle-shaped) were added to deionized water to prepare a suspension with a potassium hexatitanate whisker content of 5.5%. Based on the calcination conversion coefficients of cerium nitrate hexahydrate and magnesium nitrate hexahydrate, the materials were weighed according to a mass ratio of potassium hexatitanate whiskers:cerium nitrate hexahydrate:magnesium nitrate hexahydrate of 10:3:19. PEG-4000, accounting for 3% of the total mass of cerium nitrate hexahydrate and magnesium nitrate hexahydrate, was added and stirred to dissolve and disperse. At a system temperature of 18℃, a 9% ammonium bicarbonate aqueous solution was added dropwise at a rate of 1.0 mL / min, controlling the final pH to 10. After the addition, the mixture was aged for 10 min (short aging time to avoid cerium and magnesium hydroxides forming independent particles and to ensure that the active components are loaded onto the surface of the potassium hexatitanate whiskers), and immediately filtered under reduced pressure. A 0.4% ammonium bicarbonate solution, pre-adjusted to pH 9 and maintained at 45℃, was then used. The ammonium citrate aqueous solution was used to slurry and wash the filter cake. After stirring for 8 minutes, the mixture was filtered again. Then, the filter cake was rinsed three times with deionized water at 45°C with ammonium bicarbonate to adjust the pH to 8.8, in order to remove ammonium nitrate and free cerium, magnesium, potassium and other impurity ions adsorbed on the surface of the filter cake. The filter cake was dried at 105°C. The solid was spread evenly in a crucible and heated to 550°C at 3.2°C / min in air atmosphere. The temperature was held for 55 minutes and then cooled to room temperature in dry air. A composite inorganic filler with a mass ratio of potassium hexatitanate whiskers, cerium dioxide and magnesium oxide of 15:1.56:3.8 was obtained. The cerium dioxide grain size in the filler was 15-45 nm and the magnesium oxide grain size was 20-50 nm. KH-560, accounting for 2% of the total mass of the composite inorganic filler, was added and the filter cake was dry-modified by high-speed stirring (3000 r / min) to obtain the composite modified filler.

[0030] Weigh the raw materials by weight as follows: 89 parts of copolymer polypropylene (melt flow rate of 4 g / 10 min (230℃, 2.16 kg)), 8 parts of the above-mentioned composite modified filler, 0.4 parts of organic composite antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 1.5:1), and a total of 0.5 parts of processing aids (0.2 parts of stearic acid and 0.3 parts of polyethylene wax).

[0031] All raw materials are fed into a high-speed mixer and mixed at room temperature for 6 minutes before being fed into a twin-screw extruder: zone 1 180℃-190℃, zone 2 195℃-205℃, zone 3 210℃-220℃, die head temperature 215℃-225℃, screw speed 220-260 r / min; melt extrusion, water cooling and traction pelletizing; the pellets are placed in a 70℃ oven to dry for 3 hours to remove trace amounts of moisture, obtaining polypropylene insulating pellets. The dried pellets are fed into a cable extrusion coating equipment at an extrusion temperature of 218℃ to extrude and coat the conductor with an insulation layer, followed by water cooling, shaping, traction, and winding to obtain modified polypropylene wires and cables.

[0032] Example 2

[0033] Potassium hexatitanate whiskers (needle-shaped) were added to deionized water to prepare a suspension with a potassium hexatitanate whisker content of 5%. Based on the calcination conversion coefficients of cerium nitrate hexahydrate and magnesium nitrate hexahydrate, the materials were weighed according to a mass ratio of potassium hexatitanate whiskers:cerium nitrate hexahydrate:magnesium nitrate hexahydrate of 10:2:13. PEG-4000, accounting for 2% of the total mass of cerium nitrate hexahydrate and magnesium nitrate hexahydrate, was added and stirred to dissolve and disperse. At a system temperature of 22℃, a 10% ammonium bicarbonate aqueous solution was added dropwise at a rate of 0.8 mL / min, controlling the final pH to 11. After the addition, the mixture was aged for 12 min (short aging time to avoid cerium and magnesium hydroxides forming independent particles and to ensure that the active components are loaded onto the surface of the potassium hexatitanate whiskers), and immediately filtered under reduced pressure. A 0.5% ammonium bicarbonate solution, pre-adjusted to pH 9.2 and maintained at 50℃, was then used. The mixture was slurried and washed with an ammonium citrate aqueous solution, stirred for 10 min, and then filtered again. It was then rinsed twice with deionized water at 55℃ and pH adjusted to 8.5 using ammonium bicarbonate to remove ammonium nitrate and free cerium, magnesium, and potassium impurities adsorbed on the filter cake surface. The mixture was dried at 105℃. The solid was spread evenly in a crucible and heated to 580℃ at 3.5℃ / min in air, held for 40 min, and then cooled to room temperature in dry air. This yielded a composite inorganic filler with a calcined product of potassium hexatitanate whiskers:cerium dioxide:magnesium oxide mass ratio of 12:0.8:2. The cerium dioxide grain size in the filler was 15-45 nm, and the magnesium oxide grain size was 20-50 nm. KH-560, accounting for 3% of the total mass of the composite inorganic filler, was added, and the mixture was dry-modified by high-speed stirring (3000 r / min) to obtain the composite modified filler.

[0034] Weigh the raw materials by weight as follows: 94 parts of copolymer polypropylene (melt flow rate of 4 g / 10 min (230℃, 2.16 kg)), 5 parts of the above-mentioned composite modified filler, 0.3 parts of organic composite antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 2:1), and a total of 0.2 parts of processing aids (0.1 parts of stearic acid and 0.1 parts of polyethylene wax).

[0035] All raw materials are fed into a high-speed mixer and mixed at room temperature for 8 minutes before being fed into a twin-screw extruder: zone 1 180℃-190℃, zone 2 195℃-205℃, zone 3 210℃-220℃, die head temperature 215℃-225℃, screw speed 220-260 r / min; melt extrusion, water cooling and traction pelletizing; the pellets are placed in an 80℃ oven to dry for 2.5 hours to remove trace amounts of moisture, obtaining polypropylene insulating pellets. The dried pellets are fed into a cable extrusion coating equipment at an extrusion temperature of 218℃ to extrude and coat the conductor with an insulation layer, followed by water cooling, shaping, traction, and winding to obtain modified polypropylene wires and cables.

[0036] Example 3

[0037] Potassium hexatitanate whiskers (needle-shaped) were added to deionized water to prepare a suspension with a potassium hexatitanate whisker content of 6%. Based on the calcination conversion coefficients of cerium nitrate hexahydrate and magnesium nitrate hexahydrate, the materials were weighed according to a mass ratio of potassium hexatitanate whiskers:cerium nitrate hexahydrate:magnesium nitrate hexahydrate of 10:4:25. PEG-4000, accounting for 3% of the total mass of cerium nitrate hexahydrate and magnesium nitrate hexahydrate, was added and stirred to dissolve and disperse. At a system temperature of 15℃, an 8% ammonium bicarbonate aqueous solution was added dropwise at a rate of 1.2 mL / min, controlling the final pH to 9. After the addition was completed, the mixture was aged for 12 min (short aging time to avoid cerium and magnesium hydroxides forming independent particles and to ensure that the active components are loaded onto the surface of the potassium hexatitanate whiskers), and immediately filtered under reduced pressure. A 0.5% ammonium bicarbonate solution, pre-adjusted to pH 8.8 and maintained at 50℃, was then used. The ammonium citrate aqueous solution was used for slurry washing, and after stirring for 10 min, it was filtered again. Then, it was rinsed three times with deionized water at 55℃ with ammonium bicarbonate to slightly adjust the pH to 9.0, in order to remove ammonium nitrate and free cerium, magnesium, potassium and other impurity ions adsorbed on the surface of the filter cake. The filter cake was dried at 105℃. The solid was spread evenly in a crucible and heated to 520℃ at 3.0℃ / min in air atmosphere, held at that temperature for 70 min, and then cooled to room temperature in dry air. A composite inorganic filler with a mass ratio of potassium hexatitanate whiskers:cerium dioxide:magnesium oxide of 18:2.4:6 was obtained. The cerium dioxide grain size in the filler was 15-45nm, and the magnesium oxide grain size was 20-50nm. KH-560, accounting for 3% of the total mass of the composite inorganic filler, was added and the filler was dry-modified by high-speed stirring (3000r / min) to obtain the composite modified filler.

[0038] Weigh the raw materials by weight as follows: 85 parts of copolymer polypropylene (melt flow rate of 4 g / 10 min (230℃, 2.16 kg)), 11 parts of the above-mentioned composite modified filler, 0.5 parts of organic composite antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 1:1), and a total of 0.6 parts of processing aids (0.4 parts of stearic acid and 0.2 parts of polyethylene wax).

[0039] All raw materials are fed into a high-speed mixer and mixed at room temperature for 8 minutes before being fed into a twin-screw extruder: zone 1 180℃-190℃, zone 2 195℃-205℃, zone 3 210℃-220℃, die head temperature 215℃-225℃, screw speed 220-260 r / min; melt extrusion, water cooling and traction pelletizing; the pellets are placed in a 60℃ oven to dry for 4 hours to remove trace amounts of moisture, obtaining polypropylene insulating pellets. The dried pellets are fed into a cable extrusion coating equipment at an extrusion temperature of 218℃ to extrude and coat the conductor with an insulation layer, followed by water cooling, shaping, traction, and winding to obtain modified polypropylene wires and cables.

[0040] Comparative Example 1 (Traditional physical blending process)

[0041] The rest is the same as in Example 1, except that the experimental conditions of the in-situ calcination loading process of Example 1 are used to prepare two inorganic fillers: nano-sized cerium dioxide powder and magnesium oxide. (The potassium hexatitanate whiskers are prepared according to the method of Example 1, first preparing a 5.5% suspension without adding cerium nitrate hexahydrate and magnesium nitrate hexahydrate, and then continuing with the subsequent steps. Cerium nitrate hexahydrate and magnesium nitrate hexahydrate are directly dissolved and dispersed in water, and then nano-sized cerium dioxide powder and nano-sized magnesium oxide are prepared according to the subsequent steps.) The prepared potassium hexatitanate whiskers:cerium dioxide:magnesium oxide are then physically mixed at a mass ratio of 15:1.56:3.8. 2% of the total filler mass of KH-560 is added for dry modification. The subsequent extrusion granulation and wire and cable manufacturing processes are exactly the same as in Example 1.

[0042] Comparative Example 2 (Traditional Physical Blending Process)

[0043] The rest is the same as in Example 1, except that: commercial potassium hexatitanate whiskers, nano-cerium dioxide, and nano-magnesium oxide powder are directly mixed by physical stirring at a mass ratio of 15:1.56:3.8; 2% by mass of KH-560 dry-process modification is added to obtain a physically blended composite filler. The polypropylene insulation formulation, the weight parts of each component, mixing, extrusion, granulation, and wire and cable preparation process are completely consistent with those in Example 1.

[0044] The polypropylene wire and cable insulation materials prepared in Examples 1-3 and Comparative Examples 1 and 2 were pressed into standard samples. The following standards were applied to each performance test: tensile / elongation at break GB / T1040.1-2018; creep GB / T11546.1-2008 (23℃, 2MPa, 100h); strength retention rate after 500h UV aging GB / T16422.3-2014; volume resistivity GB / T1410-2006.

[0045] Table 1 Comparison of performance test results of wire and cable insulation materials prepared in the examples and comparative examples.

[0046]

[0047] As can be seen from the test data in Table 1, the composite inorganic filler modified polypropylene insulation materials prepared by the in-situ loading method in Examples 1-3 have significantly better comprehensive performance than the samples prepared by physical blending in Comparative Examples 1 and 2.

[0048] Example 2 had the lowest filler content and the best elongation at break, but its creep resistance, thermal shrinkage, aging resistance, and space charge suppression performance were relatively weak. Example 3 had the highest filler content and the best tensile strength, creep resistance, UV aging resistance, and space charge suppression effect, but its elongation at break decreased. Example 1 had a filler content of 8 parts, and its various properties were balanced, resulting in excellent overall performance.

[0049] Comparative Example 1 involved the physical mixing of separately prepared single-component fillers, while Comparative Example 2 involved simple physical blending of commercially available powders. Although the filler ratios in both comparative examples remained consistent with Example 1, the lack of an in-situ loading structure resulted in significant agglomeration of nano-cerium dioxide and magnesium oxide, leading to interface defects and micropores within the matrix. Consequently, the tensile strength of the material decreased, creep strain and thermal shrinkage significantly increased, strength retention after UV aging decreased, volume resistivity decreased, and space charge accumulation was severe. This fully demonstrates that the in-situ precipitation-calcination loading process combined with silane coupling agent interface modification can effectively solve the filler agglomeration problem and achieve synergistic effects of the ternary components of potassium hexatitanate whiskers, nano-cerium dioxide, and nano-magnesium oxide.

[0050] This invention utilizes multiple mechanisms, including rigid skeleton reinforcement, free radical capture for anti-aging, and deep trap for binding space charge, to simultaneously address mechanical, dimensional stability, and electrical insulation properties. The resulting modified polypropylene insulation material is suitable for insulation layers of medium and low voltage power cables and cables of 35kV and below, as well as new energy vehicle cables.

[0051] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention, as long as they do not depart from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. An inorganic composite filler synergistically modified polypropylene wire and cable insulation material, characterized in that, It is made from the following raw materials in parts by weight: 85-94 parts of copolymer polypropylene, 5-11 parts of composite inorganic filler, 0.3-0.5 parts of organic composite antioxidant obtained by compounding pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] with tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 1:1-2:1, and 0.2-0.6 parts of processing aid; The processing aid is one or both of stearic acid and polyethylene wax; The composite inorganic filler was prepared according to the following method: Potassium hexatitanate whiskers were added to deionized water to prepare a suspension with a solid content of 5%-6%. Cerium nitrate hexahydrate and magnesium nitrate hexahydrate were added at a mass ratio of 10:2-4:13-25. Polyethylene glycol 4000 was added at 2-3% of the total mass of cerium nitrate hexahydrate and magnesium nitrate hexahydrate, and the mixture was stirred to dissolve and disperse. Ammonium bicarbonate aqueous solution was slowly added dropwise to the suspension at 15℃-22℃, controlling the final pH to 9-11. After the addition was complete, the mixture was aged for 8-12 minutes and immediately filtered under reduced pressure. The mixture was then washed with an ammonium citrate aqueous solution pre-adjusted to pH 8.8-9.2 with ammonium bicarbonate at 40℃-50℃, stirred for 6-10 minutes, and filtered again. Finally, the mixture was rinsed 2-3 times with deionized water at 40℃-55℃ with ammonium bicarbonate to finely adjust the pH to 8.5-9.0, and dried. The solid is spread out and heated to 520℃-580℃, held for 40-70 minutes, and then cooled to room temperature with dry air to obtain a composite inorganic filler with potassium hexatitanate whiskers supported in situ by cerium dioxide and magnesium oxide. 2%-3% of the total mass of the composite inorganic filler is added as a silane coupling agent γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and the surface is modified by dry stirring at high speed to obtain the composite inorganic filler.

2. The inorganic composite filler synergistically modified polypropylene wire and cable insulation material according to claim 1, characterized in that: The copolymer polypropylene melt flow rate is 2-6 g / 10 min at 230℃ and 2.16 kg conditions.

3. The inorganic composite filler synergistically modified polypropylene wire and cable insulation material according to claim 2, characterized in that: The mass concentration of the ammonium bicarbonate aqueous solution is 8%-10%, and the dropping rate is 0.8-1.2 mL / min.

4. The inorganic composite filler synergistically modified polypropylene wire and cable insulation material according to claim 3, characterized in that: The mass concentration of ammonium citrate aqueous solution is 0.3%-0.5%.

5. The inorganic composite filler synergistic modification polypropylene wire and cable insulation material according to claim 4, characterized in that: Heating rate is 3.0-3.5℃ / min to 520℃-580℃.

6. The inorganic composite filler synergistic modification polypropylene wire and cable insulation material according to claim 5, characterized in that: The mass ratio of potassium hexatitanate whiskers, cerium dioxide, and magnesium oxide in the composite inorganic filler is 12-18:0.8-2.4:2-6.

7. A method for preparing the inorganic composite filler synergistic modification polypropylene wire and cable insulation material according to any one of claims 1-6, characterized in that, Prepare the material according to the following steps: Accurately weigh the copolymer polypropylene, composite inorganic filler, organic composite antioxidant, and processing aids, and put them into a high-speed mixer. Mix them at high speed for 5-8 minutes at room temperature to obtain a mixed premix. Feed the premix into a twin-screw extruder for melt extrusion granulation. Set the temperatures of each section of the extruder as follows: Zone 1 180℃-190℃, Zone 2 195℃-205℃, Zone 3 210℃-220℃, die head temperature 215℃-225℃, and screw speed 220-260 r / min. After melt blending, extrusion, water cooling traction, pelletizing, and drying, obtain uniform modified polypropylene wire and cable insulation granules.

8. The preparation method of inorganic composite filler synergistic modification polypropylene wire and cable insulation material according to claim 7, characterized in that: Dry in an oven at 60℃-80℃ for 2-4 hours.