An ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material and its preparation method

By adding low-dielectric nanofillers and compatibilizers to syndiotactic polystyrene materials and combining them with twin-screw extrusion technology, ultra-low dielectric loss glass fiber reinforced composite materials were prepared, solving the problem of insufficient dielectric properties and improving the mechanical and dielectric properties of the materials, making them suitable for high-frequency signal transmission.

CN123107260APending Publication Date: 2026-11-17CHAMBROAD CHEM IND RES INST CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611453468.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing syndiotactic polystyrene materials have shortcomings in dielectric properties, failing to fully realize their advantages in high-frequency signal transmission, and their mechanical properties need further improvement.

Method used

By adding low-dielectric nanofillers, compatibilizers, and toughening agents, and combining them with twin-screw extrusion technology, ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite materials are prepared, which enhance the compatibility and dielectric properties of the materials and reduce dielectric loss.

Benefits of technology

The material achieves low dielectric constant and low dielectric loss, improves mechanical properties and heat resistance, and is suitable for high-frequency electronic components and communication equipment, solving the compatibility problem between enhancement and low loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention provides an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material and its preparation method, comprising the following raw materials by mass fraction: syndiotactic polystyrene resin: 60~98.9%; compatibilizer: 0.1~5%; coupling agent: 0.1~2%; antioxidant: 0.1~1%; lubricant: 0.1~0.5%; toughening agent: 0.1~5%; glass fiber: 0.1~30%; low dielectric nanofiller: 0.05-0.2%; the toughening agent includes one or more of methyl methacrylate-butadiene-styrene copolymer, acrylate core-shell rubber, acrylonitrile-styrene-acrylate copolymer, and silicone-modified acrylate polymer. This invention compensates for the mechanical shortcomings of syndiotactic polystyrene through glass fiber reinforcement, optimizes its heat resistance, and simultaneously retains and enhances its extremely low dielectric loss characteristics, solving the compatibility problem between "reinforcement" and "low loss".
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer materials technology, and particularly relates to an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material and its preparation method. Background Technology

[0002] Syndiotactic polystyrene (SPS) is a crystalline polymer material produced by the polymerization of styrene monomers using a metallocene catalyst. Its unique crystalline structure and comprehensive properties make it important in the industrial field. First synthesized in 1985 and industrialized in 1997, SPS shows great promise in high-frequency signal transmission applications such as communication antennas, oscillators, and radar.

[0003] Syndiotactic polystyrene (SPS) materials are widely used in electrical / electronic, automotive, optical, and precision instrument industries due to their low density, excellent electrical properties, good hydrolytic stability, excellent heat resistance, solvent resistance, and dimensional stability. However, further modification is still needed to better improve their material properties and applications. Chinese patent CN108976629B describes a high thermal conductivity halogen-free flame-retardant SPS material and its preparation method, showcasing the excellent heat resistance of modified SPS materials, but it does not mention dielectric properties and does not demonstrate its advantages in the field of information transmission. Summary of the Invention

[0004] The purpose of this invention is to provide an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material and its preparation method. The ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material of this invention has excellent mechanical properties and heat resistance, and at the same time has the advantages of low dielectric constant and low dielectric loss, taking into account both reinforcement and low loss. It is suitable for high-frequency electronic components and communication equipment with low signal loss and high reliability.

[0005] This invention provides an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material, comprising the following raw materials by mass fraction: Syndiotactic polystyrene resin: 60~98.9% Compatibilizer: 0.1~5% Coupling agent: 0.1~2% Antioxidant: 0.1~1% Lubricant: 0.1~0.5% Toughening agent: 0.1~5% Glass fiber: 0.1~30% Low dielectric nanofiller dispersion: 0.5~2% The toughening agent includes one or more of the following: methyl methacrylate-butadiene-styrene copolymer, acrylate core-shell rubber, acrylonitrile-styrene-acrylate copolymer, and silicone-modified acrylate polymer.

[0006] Preferably, the syndiotactic polystyrene has a number-average molecular weight of 10W to 13W and a degree of polymerization of 3000 to 5000.

[0007] Preferably, the compatibilizer includes one or more of PPO-grafted maleic anhydride polymer, SEBS-grafted maleic anhydride polymer, and SPS-grafted maleic anhydride polymer.

[0008] Preferably, the glass fiber is a long glass fiber or a chopped glass fiber with a diameter of 10~13µm; The length of the long glass fiber is 5~25mm, and the length of the chopped glass fiber is 3~6mm.

[0009] Preferably, the low-dielectric nanofiller dispersion comprises low-dielectric nanofiller and solvent, wherein the low-dielectric nanofiller comprises one or more of porous nano-silica, nano-boron nitride, hollow silica, and nano-PTFE powder. The solid content of the low-dielectric nanofiller dispersion is 1-20%.

[0010] Preferably, the coupling agent is one or more of γ-methacryloyloxypropyltrimethoxysilane, methacryloyloxysilane, vinyltrimethoxysilane, vinyltri(β-methoxyethoxy)silane, vinyltriethoxysilane, and vinyltriisopropoxysilane. The antioxidants include one or more of the following: anti-thermal oxidative aging agents and anti-photoaging agents; The anti-thermal-oxidative aging agent includes one or more of the following: 2,6-di-tert-butyl-4-methylphenol, 2,2'-methylenebis(4-methyl-6-tert-butyl)phenol, tris(2,4-di-tert-butylphenyl) phosphite, triphenyl phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, trinonylphenyl phosphite, and dilaurate thiodipropionate. The anti-photoaging agent includes one or more of 2,4-dihydroxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, phenyl benzoate, 2-(2ˊ-hydroxy-5ˊ-methylphenyl)benzotriazole, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, and poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-S-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]]hexamethylene[(2,2,6,6-tetramethyl-4-piperidinyl)imino]; The lubricant includes one or more of N,N′-bis(ethylene)-stearic acid amide, stearamide, pentaerythritol stearate, silicone powder, talc, paraffin wax, polyethylene wax, polypropylene wax, and siloxane.

[0011] This invention provides a method for preparing ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material as described above, comprising the following steps: A) Mix the low-dielectric nanofiller and part of the coupling agent in an alcohol solvent to obtain a low-dielectric nanodispersion. B) Syndiotactic polystyrene resin, compatibilizer, antioxidant, lubricant, toughening agent, low dielectric nano-dispersion, glass fiber and remaining coupling agent are extruded and granulated using a twin-screw extruder, and then dried to obtain an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material.

[0012] Preferably, the mass ratio of the low dielectric nanofiller to the coupling agent in step A) is (8~12):1.

[0013] Preferably, in step B), the temperature zones of the twin-screw extruder from the main feed port to the die are set sequentially as follows: Zone 1: 195~205℃, Zone 2: 245~255℃, Zone 3: 265~275℃, Zone 4: 285~295℃, Zone 5: 295~305℃, Zone 6: 295~305℃, Zone 7: 285~295℃, Zone 8: 285~295℃, Zone 9: 285~295℃, Zone 10: 285~295℃, Zone 11: 295~305℃; The twin-screw extruder operates at a speed of 300-400 rpm.

[0014] Preferably, the drying temperature in step B) is 100~150℃ and the drying time is 3~5 hours.

[0015] This invention provides an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material, comprising the following raw materials by mass fraction: syndiotactic polystyrene resin: 60~98.9%; compatibilizer: 0.1~5%; coupling agent: 0.1~2%; antioxidant: 0.1~1%; lubricant: 0.1~0.5%; toughening agent: 0.1~5%; glass fiber: 0.1~30%; low dielectric nanofiller: 0.05-0.2%. The toughening agent includes one or more of methyl methacrylate-butadiene-styrene copolymer, acrylate core-shell rubber, acrylonitrile-styrene-acrylate copolymer, and silicone-modified acrylate polymer. This invention enhances the compatibility between syndiotactic polystyrene and glass fiber through the synergistic effect of the toughening agent and compatibilizer. The compatibilizer forms chemical bonds at the interface between the two phases, reducing inherent porosity during molding and suppressing Maxwell-Wagner interface polarization. The toughening elastomer disperses and absorbs stress, suppressing interface debonding and the formation of new micro-defects under thermal and external force. The two-phase combination stabilizes the microstructure, effectively reducing dielectric loss and dielectric constant temperature drift, promoting crystal nucleation, improving the mechanical and heat resistance properties of syndiotactic polystyrene, and enhancing the long-term stability of the composite material's dielectric properties. The addition of a low-dielectric nanofiller dispersion further reduces dielectric loss, and the modification process is simple and convenient. The syndiotactic polystyrene material prepared by this invention combines ultra-low signal loss with high strength and high heat resistance. Glass fiber reinforcement compensates for the mechanical shortcomings of syndiotactic polystyrene, optimizes its heat resistance, and simultaneously retains and enhances its extremely low dielectric loss characteristics. This solves the compatibility problem between "reinforcement" and "low loss," and is of great significance for improving the quality of syndiotactic polystyrene and promoting the development of industries in high-frequency applications. Detailed Implementation

[0016] This invention provides an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material, comprising the following raw materials by mass fraction: Syndiotactic polystyrene resin: 60~98.9% Compatibilizer: 0.1~5% Coupling agent: 0.1~2% Antioxidant: 0.1~1% Lubricant: 0.1~0.5% Toughening agent: 0.1~5% Glass fiber: 0.1~30% Low dielectric nanofiller dispersion: 0.5~2% The toughening agent includes one or more of the following: methyl methacrylate-butadiene-styrene copolymer, acrylate core-shell rubber, acrylonitrile-styrene-acrylate powder, and silicone-acrylate.

[0017] In this invention, the number average molecular weight of syndiotactic polystyrene is preferably 10W~13W, and the degree of polymerization is preferably 3000~5000; the mass fraction of syndiotactic polystyrene in the composite material is preferably 60~76.1%, such as 60%, 61%, 62%, 62.6%, 65%, 68%, 70%, 72%, 75%, 76.1%, or any of the above values ​​as the upper or lower limit.

[0018] In this invention, the compatibilizer preferably includes one or more of PPO-grafted maleic anhydride polymer (polyether-grafted maleic anhydride polymer), SEBS-grafted maleic anhydride polymer (styrene-ethylene-butadiene-styrene block copolymer grafted maleic anhydride), and SPS-grafted maleic anhydride polymer (syndiotactic polystyrene grafted maleic anhydride polymer); the mass fraction of the compatibilizer is preferably 0.1-5%, more preferably 1-4%, such as 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or any of the above values ​​as the upper or lower limit.

[0019] In this invention, the coupling agent preferably includes one or more of γ-methacryloxypropyltrimethoxysilane, methacryloxysilane, vinyltrimethoxysilane, vinyltri(β-methoxyethoxy)silane, vinyltriethoxysilane, and vinyltriisopropoxysilane; the mass fraction of the coupling agent is preferably 0.1-2%, more preferably 0.5-1.5%, such as 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, or any of the above values ​​as the upper or lower limit.

[0020] In this invention, the antioxidant preferably includes one or more of the anti-thermal oxidative aging agent and the anti-photoaging agent.

[0021] The anti-thermal-oxidative aging agent includes one or more of the following: 2,6-di-tert-butyl-4-methylphenol, 2,2'-methylenebis(4-methyl-6-tert-butyl)phenol, tris(2,4-di-tert-butylphenyl) phosphite, triphenyl phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, trinonylphenyl phosphite, and dilaurate thiodipropionate.

[0022] The anti-photoaging agent includes one or more of 2,4-dihydroxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, phenyl benzoate, 2-(2ˊ-hydroxy-5ˊ-methylphenyl)benzotriazole, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, and poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-S-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]]hexamethylene[(2,2,6,6-tetramethyl-4-piperidinyl)imino].

[0023] In this invention, the mass fraction of the antioxidant is preferably 0.1-1%, more preferably 0.2-0.8%, such as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, or any of the above values ​​as the upper or lower limit.

[0024] In this invention, the lubricant preferably includes one or more of N,N′-bis(ethylene)-stearamide (TAF), stearamide, pentaerythritol stearate, silicone powder, talc, paraffin wax, polyethylene wax, polypropylene wax, and siloxane; the mass fraction of the lubricant is preferably 0.1-0.5%, more preferably 0.2-0.4%, such as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, or any of the above values ​​as the upper or lower limit.

[0025] In this invention, the toughening agent preferably includes one or more of methyl methacrylate-butadiene-styrene copolymer, acrylate core-shell rubber (ACR), acrylonitrile-styrene-acrylate copolymer (ASA), and silicone-modified acrylate polymer. In this invention, the acrylate core-shell rubber (ACR) refers to core / shell structured particles composed of cross-linked n-butyl acrylate polymer as the core and methacrylate polymer as the shell. The mass fraction of the toughening agent is preferably 0.1-5%, more preferably 1-4%, such as 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or any of the above values ​​as the upper or lower limit.

[0026] In this invention, the glass fiber preferably comprises long glass fibers or chopped glass fibers with a diameter of 10-13 µm; the length of the long glass fibers is 5-25 mm, more preferably 10-20 mm, and the length of the chopped glass fibers is 3-6 mm, more preferably 4-5 mm. The mass fraction of the glass fiber is preferably 0.1-30%, more preferably 15-30%, such as 0.1%, 1%, 5%, 10%, 15%, 17%, 20%, 25%, 30%, or any of the above values ​​as the upper or lower limit.

[0027] In this invention, the low-dielectric nanofiller dispersion comprises a low-dielectric nanofiller and a solvent. The low-dielectric nanofiller preferably comprises one or more of porous nano-silica, nano-boron nitride, hollow silica, and nano-PTFE powder. The particle size of the low-dielectric nanofiller is preferably 10-50 nm. The solvent is preferably an alcohol solvent, such as anhydrous ethanol. The mass fraction of the low-dielectric nanofiller dispersion is preferably 0.5-2%, more preferably 1-1.5%, such as 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, or any of the above values ​​as the upper or lower limit.

[0028] Specifically, in some embodiments of the present invention, the low-dielectric nanofiller dispersion further includes a portion of a coupling agent, the type of which is consistent with the coupling agents described above. The solid content of the low-dielectric nanofiller dispersion is preferably 1-20%, more preferably 5-15%, such as 1%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 18%, 20%, or any of the above figures as the upper or lower limit.

[0029] This invention also provides a method for preparing the ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material described above, comprising the following steps: A) Mix the low-dielectric nanofiller and part of the coupling agent in an alcohol solvent to obtain a low-dielectric nanodispersion. B) Syndiotactic polystyrene resin, compatibilizer, antioxidant, lubricant, toughening agent, low dielectric nano-dispersion, glass fiber and remaining coupling agent are extruded and granulated using a twin-screw extruder, and then dried to obtain an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material.

[0030] In this invention, the types and amounts of the low-dielectric nanofiller, coupling agent, syndiotactic polystyrene resin, compatibilizer, antioxidant, lubricant, toughening agent and glass fiber are the same as those described above, and will not be repeated here.

[0031] In this invention, the low-dielectric nanofiller and a portion of the coupling agent are first mixed in an alcohol solvent and then dispersed by ultrasonication to obtain a low-dielectric nanodispersion.

[0032] In this invention, the mass ratio of the low dielectric nanofiller to the coupling agent is preferably (8~12):1, more preferably (9~11):1, such as 8:1, 8.5:1, 9:1, 9.5:1, 10:1, 10.5:1, 11:1, 11.5:1, 12:1, or any of the above values ​​as the upper or lower limit range.

[0033] In this invention, the alcohol solvent is preferably an anhydrous alcohol solvent, such as anhydrous ethanol.

[0034] In this invention, the ultrasonic dispersion time is preferably 10-40 min, more preferably 20-30 min. This invention does not impose any special restrictions on the frequency of the ultrasonic waves, as long as the aggregation of the low-dielectric nanofiller is prevented and a uniformly dispersed low-dielectric nanodispersion is obtained.

[0035] In this invention, the solid content of the low dielectric nano-dispersion is preferably 1-20%, more preferably 5-15%, such as 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or any of the above values ​​as the upper or lower limit.

[0036] After obtaining the low-dielectric nano-dispersion, the present invention mixes syndiotactic polystyrene resin, compatibilizer, antioxidant, lubricant, toughening agent and remaining coupling agent evenly and feeds them into a twin-screw extruder through the main feed port. Glass fiber is added from the side feed port. The low-dielectric nano-filler dispersion is added into the twin-screw extruder through a liquid pump for extrusion granulation.

[0037] In this invention, the temperature zones of the twin-screw extruder from the main feed port to the die are set sequentially as follows: Zone 1: 195~205℃, Zone 2: 245~255℃, Zone 3: 265~275℃, Zone 4: 285~295℃, Zone 5: 295~305℃, Zone 6: 295~305℃, Zone 7: 285~295℃, Zone 8: 285~295℃, Zone 9: 285~295℃, Zone 10: 285~295℃, Zone 11: 295~305℃.

[0038] Preferably, the temperature zones of the twin-screw extruder from the main feed port to the die are set sequentially as follows: Zone 1: 200℃, Zone 2: 250℃, Zone 3: 270℃, Zone 4: 290℃, Zone 5: 300℃, Zone 6: 300℃, Zone 7: 290℃, Zone 8: 290℃, Zone 9: 290℃, Zone 10: 290℃, and Zone 11: 300℃.

[0039] In this invention, the rotational speed of the twin-screw extruder is preferably 300~400 rpm, more preferably 350~400 rpm; the main feed is 11~13 Hz, the upper stage feed is 3~5 Hz, the lower stage feed is 11 Hz, and the mass flow rate of the liquid pump is preferably 3 kg / h~12 kg / h, more preferably 5 kg / h~10 kg / h.

[0040] After extrusion granulation, the present invention cools and dries the extruded composite material particles to obtain an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material.

[0041] In this invention, the drying temperature is preferably 100~150℃, more preferably 110~140℃, such as 100℃, 110℃, 120℃, 130℃, 140℃, 150℃, or any of the above values ​​as the upper or lower limit; the drying time is preferably 3~5 hours.

[0042] This invention provides an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material, primarily used in high-frequency, high-speed signal transmission scenarios, such as high-frequency connectors, 5G RF components, IC slots, and SMT carriers. Its lightweight and low water absorption characteristics allow for wider applications compared to PA, PBT, and LCP, and it shows great promise in fields such as high-frequency antenna supports for Wi-Fi 7 wireless routers, lightweight RF insulation components for satellite communications, and high-frequency insulation frameworks inside photovoltaic inverters.

[0043] This invention provides an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material, comprising the following raw materials by mass fraction: syndiotactic polystyrene resin: 60~98.9%; compatibilizer: 0.1~5%; coupling agent: 0.1~2%; antioxidant: 0.1~1%; lubricant: 0.1~0.5%; toughening agent: 0.1~5%; glass fiber: 0.1~30%; low dielectric nanofiller: 0.05-0.2%. The toughening agent includes one or more of methyl methacrylate-butadiene-styrene copolymer, acrylate core-shell rubber, acrylonitrile-styrene-acrylate copolymer, and silicone-modified acrylate polymer. The compatibilizer forms chemical bonds at the interface between the two phases, reducing inherent porosity during molding and suppressing Maxwell-Wagner interface polarization; the toughening elastomer disperses and absorbs stress, suppressing interfacial debonding and the formation of new micro-defects under thermal and external force. The two-phase combination stabilizes the microstructure, effectively reducing dielectric loss and dielectric constant temperature drift, promoting crystal nucleation, improving the mechanical and heat resistance properties of syndiotactic polystyrene, and enhancing the long-term stability of the composite material's dielectric properties. The addition of a low-dielectric nanofiller dispersion further reduces dielectric loss, and the modification process is simple and convenient. The syndiotactic polystyrene material prepared by this invention combines ultra-low signal loss with high strength and high heat resistance. Glass fiber reinforcement compensates for the mechanical shortcomings of syndiotactic polystyrene, optimizes its heat resistance, and simultaneously retains and enhances its extremely low dielectric loss characteristics. This solves the compatibility problem between "reinforcement" and "low loss," and is of great significance for improving the quality of syndiotactic polystyrene and promoting the development of industries in high-frequency applications.

[0044] To further illustrate the present invention, the following detailed description of an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material and its preparation method provided by the present invention is provided in conjunction with embodiments, but it should not be construed as limiting the scope of protection of the present invention.

[0045] Example 1

[0046] It contains the following ingredients by weight: Syndiotactic polystyrene resin 130ZC 76.1% 1% low dielectric nanofiller dispersion Compatibilizer PPO-g-MAH 3% Coupling agent KH-550 0.5% Antioxidant 0.2% 0.2% silicone lubricant Toughening agent ASA 2% Taishan chopped glass fiber 17% The low dielectric nanofiller dispersion is an anhydrous ethanol dispersion of porous nano silica with a solid content of 10%; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1.

[0047] Syndiotactic polystyrene resin, compatibilizer, coupling agent, antioxidant, lubricant and toughening agent are mixed evenly and fed into a twin-screw extruder through the main feed port. Short-cut glass fiber and low dielectric nanofiller dispersion are added from the side feed port and fed into the twin-screw extruder through a liquid pump for extrusion granulation. The glass fiber reinforced syndiotactic polystyrene composite material after extrusion in step (1) is cooled and dried at a temperature of 120°C for 3 hours. The set temperatures of the twin-screw extruder from the main feed port to the die head are 200℃, 250℃, 270℃, 290℃, 300℃, 300℃, 290℃, 290℃, 290℃, 290℃, and 300℃ respectively.

[0048] The twin-screw extruder operates at 350 rpm, with the main feed at 13 Hz, the upper side feed at 3 Hz, the lower side feed at 11 Hz, and the liquid pump set at 9 kg / h.

[0049] Example 2

[0050] It contains the following ingredients by weight: Syndiotactic polystyrene resin 130ZC 76.1% 1% low dielectric nanofiller dispersion Compatibilizer PPO-g-MAH 2% Coupling agent KH-550 0.5% Antioxidant 0.2% 0.2% silicone lubricant Toughening agent ASA 3% Taishan chopped glass fiber 17% The low dielectric nanofiller dispersion is an anhydrous ethanol dispersion of porous nano silica with a solid content of 10%; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1.

[0051] Glass fiber reinforced syndiotactic polystyrene material was prepared using the same method as in Example 1.

[0052] Example 3

[0053] It contains the following ingredients by weight: Syndiotactic polystyrene resin 130ZC 76.1% 1% low dielectric nanofiller dispersion Compatibilizer PPO-g-MAH 3% Coupling agent KH-550 0.5% Antioxidant 0.2% 0.2% silicone lubricant Toughening agent ACR 2% Taishan chopped glass fiber 17% The low dielectric nanofiller dispersion is an anhydrous ethanol dispersion of porous nano silica with a solid content of 10%; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1.

[0054] Glass fiber reinforced syndiotactic polystyrene material was prepared using the same method as in Example 1.

[0055] Example 4

[0056] It contains the following ingredients by weight: Syndiotactic polystyrene resin 130ZC 62.6% 1% low dielectric nanofiller dispersion Compatibilizer PPO-g-MAH 3% Coupling agent KH-550 1% Antioxidant 0.2% 0.2% silicone lubricant Toughening agent ASA 2% Taishan chopped glass fiber 30% The low dielectric nanofiller dispersion is an anhydrous ethanol dispersion of porous nano silica with a solid content of 10%; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1.

[0057] Glass fiber reinforced syndiotactic polystyrene material was prepared using the same method as in Example 1, with the extruder parameters changed to main machine speed of 350 rpm, main feed 11 Hz, upper side feed 5 Hz, lower side feed 11 Hz, and liquid pump set to 9 kg / h.

[0058] Example 5

[0059] It contains the following ingredients by weight: Syndiotactic polystyrene resin 130ZC 62.6% 1% low dielectric nanofiller dispersion Compatibilizer PPO-g-MAH 2% Coupling agent KH-550 1% Antioxidant 0.2% 0.2% silicone lubricant Toughening agent ASA 3% Taishan chopped glass fiber 30% The low dielectric nanofiller dispersion is an anhydrous ethanol dispersion of porous nano silica with a solid content of 10%; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1.

[0060] Glass fiber reinforced syndiotactic polystyrene material was prepared using the same method as in Example 4.

[0061] Example 6

[0062] It contains the following ingredients by weight: Syndiotactic polystyrene resin 130ZC 62.6% 1% low dielectric nanofiller dispersion Compatibilizer PPO-g-MAH 3% Coupling agent KH-550 1% Antioxidant 0.2% 0.2% silicone lubricant Toughening agent ACR 2% Taishan chopped glass fiber 30% The low dielectric nanofiller dispersion is an anhydrous ethanol dispersion of porous nano silica with a solid content of 10%; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1.

[0063] Glass fiber reinforced syndiotactic polystyrene material was prepared using the same method as in Example 4.

[0064] Comparative Example 1

[0065] It contains the following ingredients by weight: 130ZC 79.1% PPO-g-MAH 3% KH-550 0.5% 1010 : 168 = 1 : 1 0.2% Silicone powder 0.2% Taishan chopped glass fiber 17% Syndiotactic polystyrene resin 130ZC, compatibilizer PPO-g-MAH, coupling agent KH-550, antioxidant (1010:168 mass ratio of 1:1), and lubricant silicone powder are mixed evenly and fed into a twin-screw extruder through the main feed port. Short-cut glass fiber and low-dielectric nanofiller dispersion are added from the side feed port and fed into the twin-screw extruder through a liquid pump for extrusion granulation. The glass fiber reinforced syndiotactic polystyrene composite material after extrusion in step (1) is cooled and dried at a temperature of 120°C for 3 hours. The twin-screw extruder is set to temperatures of 200℃, 250℃, 270℃, 290℃, 300℃, 300℃, 290℃, 290℃, 290℃, 290℃, and 300℃.

[0066] The twin-screw extruder operates at a speed of 350 rpm, with the main feed at 13 Hz, the upper side feed at 3 Hz, and the lower side feed at 11 Hz.

[0067] Comparative Example 2

[0068] It contains the following ingredients by weight: 130ZC 81.1% 1% low dielectric nanofiller dispersion KH-550 0.5% 1010 : 168 = 1 : 1 0.2% Silicone powder 0.2% Taishan chopped glass fiber 17% Glass fiber reinforced syndiotactic polystyrene material was prepared using the same method as Comparative Example 1.

[0069] Comparative Example 3

[0070] It contains the following ingredients by weight: 130ZC 80.1% KH-550 0.5% 1010 : 168 = 1 : 1 0.2% Silicone powder 0.2% ASA 2% Taishan chopped glass fiber 17% Glass fiber reinforced syndiotactic polystyrene material was prepared using the same method as Comparative Example 1.

[0071] Comparative Example 4

[0072] It contains the following ingredients by weight: 130ZC 66.1% PPO-g-MAH 3% KH-550 0.5% 1010 : 168 = 1 : 1 0.2% Silicone powder 0.2% Taishan chopped glass fiber 30% Glass fiber reinforced syndiotactic polystyrene material was prepared using the same method as Comparative Example 1. The difference was that the twin-screw extruder operated at 350 rpm, with a main feed rate of 11 Hz, an upper-stage side feed rate of 5 Hz, and a lower-stage side feed rate of 11 Hz.

[0073] Comparative Example 5

[0074] It contains the following ingredients by weight: 130ZC 68.1% 1% low dielectric nanofiller dispersion KH-550 0.5% 1010 : 168 = 1 : 1 0.2% Silicone powder 0.2% Taishan chopped glass fiber 30% Glass fiber reinforced syndiotactic polystyrene material was prepared using the same method as Comparative Example 4.

[0075] Comparative Example 6

[0076] It contains the following ingredients by weight: 130ZC 67.1% KH-550 0.5% 1010 : 168 = 1 : 1 0.2% Silicone powder 0.2% ASA 2% Taishan chopped glass fiber 30% Glass fiber reinforced syndiotactic polystyrene material was prepared using the same method as Comparative Example 4.

[0077] Comparative Example 7

[0078] It contains the following ingredients by weight: 130ZC 62.6% 1% low dielectric nanofiller dispersion PPO-g-MAH 3% KH-550 1% 1010 : 168 = 1 : 1 0.2% Silicone powder 0.2% PSU 2% Taishan chopped glass fiber 30% Glass fiber reinforced syndiotactic polystyrene material was prepared using the same method as Comparative Example 4.

[0079] Comparative Example 8

[0080] It contains the following ingredients by weight: 130ZC 62.6% 1% low dielectric nanofiller dispersion POE-g-MAH 3% KH-550 1% 1010 : 168 = 1 : 1 0.2% Silicone powder 0.2% ASA 2% Taishan chopped glass fiber 30% Glass fiber reinforced syndiotactic polystyrene material was prepared using the same method as Comparative Example 4.

[0081] Table 1 shows the performance test results of the composite materials prepared in the examples and comparative examples.

[0082] Table 1 Performance test results of the composite materials in the examples and comparative examples

[0083] In summary, the differences between the examples and comparative examples show that the glass fiber reinforced syndiotactic polystyrene resin provided by this invention has excellent mechanical and heat resistance properties, while also possessing the advantages of low dielectric constant and low dielectric loss. It balances reinforcement and low loss, making it suitable for high-frequency electronic components and communication equipment with low signal loss and high reliability. While maintaining excellent high-frequency performance, it has advantages over LCP in terms of lightweight and cost, and has good application prospects.

[0084] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. An ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material, comprising the following raw materials by mass fraction: Syndiotactic polystyrene resin: 60~98.9% Compatibilizer: 0.1~5% Coupling agent: 0.1~2% Antioxidant: 0.1~1% Lubricant: 0.1~0.5% Toughening agent: 0.1~5% Fiberglass: 0.1~30% Low dielectric nanofiller dispersion: 0.5~2% The toughening agent includes one or more of the following: methyl methacrylate-butadiene-styrene copolymer, acrylate core-shell rubber, acrylonitrile-styrene-acrylate copolymer, and silicone-modified acrylate polymer.

2. The ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material according to claim 1, characterized in that, The syndiotactic polystyrene has a number average molecular weight of 10W~13W and a degree of polymerization of 3000~5000.

3. The ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material according to claim 1, characterized in that, The compatibilizer includes one or more of PPO-grafted maleic anhydride polymer, SEBS-grafted maleic anhydride polymer, and SPS-grafted maleic anhydride polymer.

4. The ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material according to claim 1, characterized in that, The glass fiber is a long glass fiber or a short-cut glass fiber with a diameter of 10~13µm; The length of the long glass fiber is 5~25mm, and the length of the chopped glass fiber is 3~6mm.

5. The ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material according to claim 1, characterized in that, The low-dielectric nanofiller dispersion comprises low-dielectric nanofiller and solvent, wherein the low-dielectric nanofiller comprises one or more of porous nano-silica, nano-boron nitride, hollow silica, and nano-PTFE powder. The solid content of the low-dielectric nanofiller dispersion is 1-20%.

6. The ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material according to claim 1, characterized in that, The coupling agent is one or more of γ-methacryloyloxypropyltrimethoxysilane, methacryloyloxysilane, vinyltrimethoxysilane, vinyltri(β-methoxyethoxy)silane, vinyltriethoxysilane, and vinyltriisopropoxysilane. The antioxidants include one or more of the following: anti-thermal oxidative aging agents and anti-photoaging agents; The anti-thermal-oxidative aging agent includes one or more of the following: 2,6-di-tert-butyl-4-methylphenol, 2,2'-methylenebis(4-methyl-6-tert-butyl)phenol, tris(2,4-di-tert-butylphenyl) phosphite, triphenyl phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, trinonylphenyl phosphite, and dilaurate thiodipropionate. The anti-photoaging agent includes one or more of 2,4-dihydroxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, phenyl benzoate, 2-(2ˊ-hydroxy-5ˊ-methylphenyl)benzotriazole, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, and poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-S-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]]hexamethylene[(2,2,6,6-tetramethyl-4-piperidinyl)imino]; The lubricant includes one or more of N,N′-bis(ethylene)-stearic acid amide, stearamide, pentaerythritol stearate, silicone powder, talc, paraffin wax, polyethylene wax, polypropylene wax, and siloxane.

7. A method for preparing the ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material as described in claim 1, comprising the following steps: A) Mix the low-dielectric nanofiller and part of the coupling agent in an alcohol solvent to obtain a low-dielectric nanodispersion. B) Syndiotactic polystyrene resin, compatibilizer, antioxidant, lubricant, toughening agent, low dielectric nano-dispersion, glass fiber and remaining coupling agent are extruded and granulated using a twin-screw extruder, and then dried to obtain an ultra-low dielectric loss glass fiber reinforced syndiotactic polystyrene composite material.

8. The preparation method according to claim 7, characterized in that, The mass ratio of the low dielectric nanofiller to part of the coupling agent in step A) is (8~12):

1.

9. The preparation method according to claim 8, characterized in that, In step B), the temperature zones of the twin-screw extruder from the main feed port to the die head are set sequentially as follows: Zone 1: 195~205℃, Zone 2: 245~255℃, Zone 3: 265~275℃, Zone 4: 285~295℃, Zone 5: 295~305℃, Zone 6: 295~305℃, Zone 7: 285~295℃, Zone 8: 285~295℃, Zone 9: 285~295℃, Zone 10: 285~295℃, Zone 11: 295~305℃; The twin-screw extruder operates at a speed of 300-400 rpm.

10. The preparation method according to claim 8, characterized in that, The drying temperature in step B) is 100~150℃, and the drying time is 3~5 hours.

Citation Information

Patent Citations

  • High thermal conductivity halogen-free flame-retardant syndiotactic polystyrene composite materials and their preparation methods

    CN108976629B