A high-performance PVB encapsulation interlayer adapted for N-type photovoltaic cells and its preparation method
By using high and low residual hydroxyl PVB resins and composite anhydride compatibilizers, the problems of high haze, yellowing, PID effect and interface debonding of N-type photovoltaic cell encapsulation materials have been solved, achieving a high-performance encapsulation interlayer that meets the long-term stability and reliability requirements of N-type photovoltaic cells.
Patent Information
- Application Number
- CN202611348309.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-17
AI Technical Summary
N-type photovoltaic cells have stringent requirements for encapsulation materials. Existing encapsulation layers suffer from high haze, yellowing, poor weather resistance, PID effects, and interface debonding caused by plasticizer migration, making it difficult to meet the optical stability and long-term reliability requirements for a 25-year lifespan.
The composite material is made by combining high residual hydroxyl PVB resin with low residual hydroxyl PVB resin, and adding anhydride compatibilizer, plasticizer, anti-PID additive, anti-photoaging agent and silane coupling agent. Through in-situ esterification reaction and chemical bonding to form molecular bridges, the bonding strength, flexibility and anti-PID performance of the interlayer are improved.
It achieves ultra-low haze, excellent weather resistance, strong anti-PID capability, and long-term stable interface adhesion performance, significantly improving the encapsulation effect of N-type photovoltaic cells and meeting the encapsulation requirements of TOPCon, HJT, IBC, and other categories.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and in particular to a high-performance PVB encapsulation interlayer adapted to N-type photovoltaic cells and its preparation method. Background Technology
[0002] N-type photovoltaic cells, represented by TOPCon, HJT, and IBC, possess significant advantages such as high conversion efficiency, low light-induced degradation, excellent temperature coefficient, and good low-light response. However, N-type cells place far more stringent requirements on encapsulation materials than traditional P-type cells. Currently, N-type cell encapsulation faces four major challenges: Firstly, the high haze of the encapsulation interlayer itself will significantly reduce the light-receiving efficiency of the battery, while N-type batteries require extremely low haze encapsulation materials with a haze of less than 0.5%. Secondly, during long-term outdoor aging, the existing encapsulation interlayer is prone to yellowing and haze recurrence, making it difficult to meet the optical stability requirements for a 25-year service life. Third, N-type batteries are more sensitive to the migration of alkali metal ions such as sodium ions, and are prone to potential-induced degradation (PID) under high pressure, high temperature and high humidity conditions, resulting in a sharp drop in battery efficiency. Fourth, traditional plasticizers are prone to migration, causing delamination between the interlayer and the cell or glass interface, generating bubbles, which seriously affects the long-term reliability of the module.
[0003] Therefore, it is necessary to develop encapsulation sandwich materials with low haze, high weather resistance, PID resistance, and interface stability to better meet the needs of N-type photovoltaic cells. Summary of the Invention
[0004] Based on the above background technology, this invention provides a high-performance PVB encapsulation interlayer adapted to N-type photovoltaic cells and its preparation method. This invention uses a composite of high-residual-hydroxyl PVB resin and low-residual-hydroxyl PVB resin as the matrix material, simultaneously achieving high adhesion strength between the interlayer and the glass or solar cell, as well as excellent flexibility of the film itself. Simultaneously, a composite anhydride compatibilizer is added. During processing, the anhydride groups of the two anhydride components can undergo in-situ esterification grafting reactions with the residual hydroxyl groups on the high- and low-hydroxyl PVB molecular chains, forming molecular bridges between the two phase molecular chains. This significantly reduces the interfacial tension between the two phases, solving the incompatibility problem between high- and low-hydroxyl PVB resins and achieving uniform compatibility between the two phases. Furthermore, this invention rationally combines plasticizers, anti-PID additives, composite anti-photoaging agents, and silane coupling agents, working synergistically to produce a PVB encapsulation interlayer that possesses ultra-low haze, excellent weather resistance and anti-photoaging performance, strong anti-PID capability, and long-term stable interfacial adhesion performance, meeting the stringent encapsulation requirements of various N-type photovoltaic cells such as TOPCon, HJT, and IBC.
[0005] The technical solution of the present invention: A high-performance PVB encapsulation interlayer adapted for N-type photovoltaic cells, wherein the raw materials for its preparation are composed of the following by weight percentage: First PVB resin 40-60 wt%; Secondary PVB resin 25-45 wt%; Composite anhydride compatibilizer 0.5–3 wt%; Plasticizer 12-20 wt%; Anti-PID additive 0.1–0.5 wt%; Anti-photoaging agent 0.2–0.8 wt%; Silane coupling agent 0.05–0.2 wt%; in: The first PVB resin has a residual hydroxyl content of 18-22 wt%, a residual acetate content of ≤2 wt%, a number-average molecular weight (Mn) of 70,000-150,000, and a molecular weight distribution index (PDI) of 1.8-2.8. The second PVB resin has a residual hydroxyl content of 8-12 wt%, a residual acetate content of ≤2 wt%, a number-average molecular weight (Mn) of 50,000-120,000, and a molecular weight distribution index (PDI) of 1.8-2.8. The composite anhydride compatibilizer is composed of hexahydrophthalic anhydride and 2-octen-1-ylsuccinic anhydride in a mass ratio of (1-3):1; The anti-PID additive is composed of C8-C18 alkyl sulfonate lithium and nano silica in a mass ratio of 1:(2-5).
[0006] Preferably, the amount of the composite anhydride compatibilizer is 1.0 to 2.5 wt%.
[0007] Preferably, the composite anhydride compatibilizer is composed of hexahydrophthalic anhydride and 2-octen-1-ylsuccinic anhydride in a mass ratio of 2:1.
[0008] Furthermore, the plasticizer is composed of triethylene glycol di(2-ethylhexanoate) and diethylene glycol dibenzoate in a mass ratio of (4-6):1.
[0009] Preferably, the plasticizer is composed of triethylene glycol di(2-ethylhexanoate) and diethylene glycol dibenzoate in a mass ratio of 5:1.
[0010] Furthermore, the anti-photoaging agent is composed of a hindered amine light stabilizer and an ultraviolet absorber in a mass ratio of 1:(1-2).
[0011] Furthermore, the difference in residual hydroxyl content between the first PVB resin and the second PVB resin is ≥8wt%.
[0012] Preferably, the difference in residual hydroxyl content between the first PVB resin and the second PVB resin is 9 to 12 wt%.
[0013] More preferably, the difference in residual hydroxyl content between the first PVB resin and the second PVB resin is 10 wt%.
[0014] Furthermore, the particle size of the nano-silica is 20–50 nm.
[0015] Furthermore, the silane coupling agent is selected as γ-aminopropyltriethoxysilane.
[0016] Based on the same inventive concept, this invention also provides a method for preparing a high-performance PVB encapsulation interlayer adapted to N-type photovoltaic cells, characterized by comprising the following steps: ①Premixed After measuring each component, they are mixed evenly to obtain a premixed material; Specifically, each component is added to a high-speed mixer and stirred at 200–400 r / min for 10–15 min at room temperature to ensure that the components are fully and evenly mixed. ②Mel-reactive extrusion A twin-screw extruder is used to melt-blend and extrude the premixed materials into a melt. In this step, during the melt blending and extrusion of the premixed material using a twin-screw extruder, the anhydride groups in the composite anhydride compatibilizer undergo an in-situ esterification reaction with the hydroxyl groups on the PVB resin, thereby achieving reactive compatibilization. In this step, the twin-screw extruder is divided into a feeding zone, a plasticizing zone, a homogenizing zone, a metering zone, and a die head zone along the material conveying direction. The heating temperatures of each zone are controlled as follows: feeding zone 160-170℃, plasticizing zone 175-185℃, homogenizing zone 185-190℃, metering zone 180-188℃, and die head zone 175-185℃. ③ Cooling and pressing The melt extruded in step ② is introduced into a three-roll calender for rapid cooling and pressing.
[0017] Specifically, the temperature of the upper roll of the calender is controlled at 25–35℃, the temperature of the middle roll is controlled at 30–40℃, and the temperature of the lower roll is controlled at 25–35℃. The calender roll speed is 2–8 m / min, the pressing line pressure is 2.0–5.0 kN / m, and the roll gap adjustment range is 0.25–0.55 mm. The thickness of the film preform prepared in this step is 0.3–0.5 mm, and the thickness tolerance does not exceed ±0.02 mm. ④ Rolling up and cutting The thin-film preform, which has been naturally cooled to room temperature, is traction-driven, inspected for defects online, and then wound up. Finally, it is cut according to the design dimensions of the photovoltaic module to obtain the finished product.
[0018] Furthermore, in step ③, the melt is rapidly cooled and pressed into shape using a cooling roller at 25–40°C.
[0019] Based on the same inventive concept, the present invention also provides an N-type photovoltaic cell module, comprising a high-performance PVB encapsulation interlayer adapted to N-type photovoltaic cells.
[0020] Furthermore, the photovoltaic cell module is a single-glass photovoltaic cell module or a double-glass photovoltaic cell module.
[0021] The beneficial effects achieved by this invention are as follows: This invention uses a blend of high residual hydroxyl PVB resin and low residual hydroxyl PVB resin as the matrix material, which can simultaneously achieve high bonding strength between the interlayer and the glass or battery cell and excellent flexibility of the film itself: the high residual hydroxyl PVB resin provides a high density of hydroxyl groups that form strong hydrogen bonds with the surface of the glass or battery cell, ensuring high initial bonding strength between the interlayer and the glass or battery cell, while the low residual hydroxyl PVB resin imparts good flexibility, impact resistance and sound insulation properties to the interlayer, and regulates the overall melt flowability; This invention also incorporates a composite anhydride compatibilizer. During processing, the anhydride groups of the two anhydride components can undergo in-situ esterification grafting reactions with the residual hydroxyl groups on the high- and low-hydroxyl PVB molecular chains, forming molecular bridges between the two phase molecular chains. This significantly reduces the interfacial tension between the two phases, solving the incompatibility problem between high- and low-hydroxyl PVB resins and achieving uniform compatibilization between the two phases. Furthermore, hexahydrophthalic anhydride provides a rigid framework, while the long alkyl chain of 2-octene-1-ylsuccinic anhydride provides flexible compatibilization. Both components synergistically compatibilize the high- and low-residual hydroxyl PVB resins, eliminating the phase separation problem between high- and low-hydroxyl PVB, reducing film haze at its source, achieving a stable haze of 0.5% and a transmittance >89%, which can significantly improve the photoelectric power generation efficiency of N-type batteries.
[0022] The present invention utilizes a rationally compounded plasticizer, anti-PID additive, composite anti-photoaging agent, and silane coupling agent to achieve a synergistic effect, resulting in a PVB encapsulation interlayer that possesses ultra-low haze, excellent weather resistance and anti-photoaging performance, strong anti-PID capability, and long-term stable interfacial adhesion performance. This allows it to meet the stringent encapsulation requirements of various N-type photovoltaic cells, including TOPCon, HJT, and IBC. Among them, triethylene glycol di(2-ethylhexanoate) (3GEH) is used as the main plasticizer, which can provide the system with good processing fluidity and flexibility; diethylene glycol dibenzoate, due to its higher molecular weight and stronger interaction with PVB molecules, can effectively "anchor" plasticizer molecules, significantly reduce their migration rate in high temperature and high humidity environments, thereby avoiding interface debonding and bubble problems caused by plasticizer precipitation after long-term aging.
[0023] Lithium alkyl sulfonate, an anti-PID additive, can release lithium ions and undergo ion exchange reactions with sodium ions migrating from the glass, thereby blocking the path of sodium ions migrating to the battery surface. Due to its high specific surface area, nano-silica can physically adsorb sodium ions and other mobile ions. The synergy of the two can significantly suppress the PID effect and control the PID efficiency degradation rate of N-type photovoltaic modules to below 1.0%.
[0024] The hindered amine light stabilizer in the composite anti-photoaging agent can capture free radicals generated during photo-oxidative degradation and inhibit the oxidative degradation of polymer chains; the ultraviolet absorber can effectively absorb harmful ultraviolet rays in the 300 to 400 nm wavelength band and convert them into heat energy for dissipation. The two work synergistically to give the encapsulation interlayer excellent anti-ultraviolet aging ability and anti-yellowing performance.
[0025] The ethoxy group at one end of the silane coupling agent can react with the silanol group on the glass surface to form a chemical bond, while the aminopropyl group at the other end can form a hydrogen bond or react with the PVB molecular chain, thereby establishing a chemical bridge between the PVB and glass interface and between the PVB and the cell electrode interface, significantly enhancing the interfacial adhesion stability after damp heat aging. Detailed Implementation
[0026] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0027] Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods; the experiments used in the following embodiments... Unless otherwise specified, all materials were purchased from commercial channels.
[0028] The performance testing results of the PVB encapsulation interlayers prepared in the following embodiments and comparative examples are shown below.
[0029] Haze and transmittance were tested using a haze meter according to ASTM D1003-Program B (Light Source C) for single-layer sandwich samples. Bond strength shall conform to GB / T 2790-1995: The T-peel strength was tested after laminating the PVB encapsulation interlayer with 3.2mm thick tempered glass. Anti-PID performance according to IEC 62804 standard: N-type monocrystalline double glass module (60 cells) with PVB encapsulation sandwich layer is placed in an environment of 85℃ and 85%RH, and a -1000V bias voltage is applied to the negative electrode of the module for 96 hours to test the maximum power degradation rate of the module. UV aging performance was tested according to IEC 61215 standard: PVB encapsulated interlayer samples were subjected to 3000 hours of UV aging (wavelength 300-400nm, irradiance 60W / m²), and the haze increase and yellowing index ΔYI were tested after aging. Damp heat aging performance: The PVB encapsulation interlayer was placed in a constant temperature and humidity chamber at 85℃ and 85%RH for 1000 hours. The plasticizer migration rate was determined by weighing method, and the bond strength retention rate was tested.
[0030] The first PVB resin used in the following examples has a residual hydroxyl content of 20 wt%, a residual acetate content of 1.5 wt%, a number average molecular weight of 100,000, and a PDI of 2.0. The second PVB resin has a residual hydroxyl content of 10 wt%, a residual acetate content of 1.2 wt%, a number average molecular weight of 85,000, and a PDI of 2.0. The hindered amine light stabilizer is HALS-944 (light stabilizer 944). The ultraviolet absorber is UV-327.
[0031] The silane coupling agent is KH-550.
[0032] Triethylene glycol di(2-ethylhexanoate) (3GEH) CAS No. 94-28-0.
[0033] Diethylene glycol dibenzoate CAS No. 120-55-8.
[0034] Lithium dodecyl sulfonate, CAS number 2044-56-6.
[0035] The silica used is fumed silica.
[0036] Example 1: A high-performance PVB encapsulation interlayer adapted for N-type photovoltaic cells, the raw materials used in its preparation are as follows (by weight percentage): First, 50 wt% PVB resin; The second PVB resin was 35.5 wt%; 1.5 wt% of composite anhydride compatibilizer (mass ratio of hexahydrophthalic anhydride to 2-octen-1-ylsuccinic anhydride is 2:1); Plasticizer 12.2wt% (3GEH to diethylene glycol dibenzoate mass ratio of 5:1); Anti-PID additive 0.3wt% (mass ratio of lithium dodecyl sulfonate to nano silica (average particle size 30nm) is 1:3); Anti-photoaging agent 0.4wt% (HALS-944 to UV-327 mass ratio is 1:1); Silane coupling agent 0.1 wt%; Its preparation includes the following steps: ①Premixed After measuring each component, add each component to a high-speed mixer and stir at 400 r / min for 12 minutes at room temperature to ensure that each component is fully mixed and homogeneous, thus obtaining a premixed material. ②Mel-reactive extrusion A twin-screw extruder was used to melt-blend and extrude the premixed materials. The temperatures of each zone of the twin-screw extruder along the material conveying direction were as follows: feeding zone 165℃, melting zone 175℃, reaction blending zone 188℃, venting zone 185℃, metering zone 180℃, and die head zone 175℃. The screw speed was 250 r / min. ③ Cooling and pressing The melt extruded in step ② is introduced into a calendering and cooling unit. The temperature of the cooling roller is 30℃, the temperature of the rubber pressure roller is 35℃, the roller speed is 4 m / min, the pressing line pressure is 3.0 kN / m, and the roller gap is adjusted to 0.32 mm. After rapid cooling and pressing, a film preform (i.e., the PVB encapsulation interlayer) is obtained, with a measured thickness of 0.36 mm.
[0037] Example 2: A high-performance PVB encapsulation interlayer adapted for N-type photovoltaic cells, the raw materials for which are prepared by weight percentage are as follows: First, PVB resin 45 wt%; Secondary PVB resin 40wt%; 2 wt% of composite anhydride compatibilizer (the mass ratio of hexahydrophthalic anhydride to 2-octen-1-ylsuccinic anhydride is 1:1); Plasticizer 12wt% (3GEH to diethylene glycol dibenzoate mass ratio of 4:1); Anti-PID additive 0.4wt% (mass ratio of lithium dodecyl sulfonate to nano-silica with a particle size of 30nm is 1:4); Anti-photoaging agent 0.5wt% (HALS-944 to UV-327 mass ratio is 1:1.5); Silane coupling agent 0.1 wt%; Everything else is the same as in Example 1.
[0038] Example 3: A high-performance PVB encapsulation interlayer adapted for N-type photovoltaic cells, the raw materials for which are prepared by weight percentage are as follows: First, PVB resin 55 wt%; 30 wt% of the second PVB resin; 1 wt% of composite anhydride compatibilizer (the mass ratio of hexahydrophthalic anhydride to 2-octen-1-ylsuccinic anhydride is 3:1); Plasticizer 13.2wt% (3GEH to diethylene glycol dibenzoate mass ratio of 6:1); Anti-PID additive 0.4wt% (mass ratio of lithium dodecyl sulfonate to nano-silica with a particle size of 30nm is 1:2); Anti-photoaging agent 0.3wt% (HALS-944 to UV-327 mass ratio is 1:1.2); Silane coupling agent 0.1 wt%; Everything else is the same as in Example 1.
[0039] Example 4: A high-performance PVB encapsulation interlayer adapted for N-type photovoltaic cells, the raw materials for which are prepared by weight percentage are as follows: First PVB resin 40wt%; 45 wt% of the second PVB resin; 2.5 wt% of composite anhydride compatibilizer (mass ratio of hexahydrophthalic anhydride to 2-octen-1-ylsuccinic anhydride is 2:1); Plasticizer 11.4wt% (3GEH to diethylene glycol dibenzoate mass ratio of 5:1); Anti-PID additive 0.4wt% (mass ratio of lithium dodecyl sulfonate to nano-silica with a particle size of 30nm is 1:5); Anti-photoaging agent 0.6wt% (HALS-944 to UV-327 mass ratio is 1:2); Silane coupling agent 0.1 wt%; Everything else is the same as in Example 1.
[0040] Example 5: A high-performance PVB encapsulation interlayer adapted for N-type photovoltaic cells, the raw materials for which are prepared by weight percentage are as follows: First, PVB resin 60 wt%; Second PVB resin 26wt%; 0.8 wt% of composite anhydride compatibilizer (mass ratio of hexahydrophthalic anhydride to 2-octen-1-ylsuccinic anhydride is 3:1); Plasticizer 12.7wt% (3GEH to diethylene glycol dibenzoate mass ratio of 6:1); Anti-PID additive 0.15wt% (mass ratio of lithium dodecyl sulfonate to nano-silica with a particle size of 30nm is 1:4); Anti-photoaging agent 0.25wt% (HALS-944 to UV-327 mass ratio is 1:1); Silane coupling agent 0.1 wt%; Everything else is the same as in Example 1.
[0041] Comparative Example 1 The PVB encapsulation interlayer, by weight percentage, is composed of the following components: First, PVB resin 51 wt%; Second PVB resin 36wt%; Plasticizer 12.2 wt% (the mass ratio of triethylene glycol di(2-ethylhexanoate) to diethylene glycol dibenzoate is 5:1); Anti-PID additive 0.3wt% (mass ratio of lithium dodecyl sulfonate to nano-silica with a particle size of 30nm is 1:3); Anti-photoaging agent 0.4wt% (the mass ratio of hindered amine light stabilizer HALS-944 to ultraviolet absorber UV-327 is 1:1); 0.1 wt% silane coupling agent (γ-aminopropyltriethoxysilane, KH-550); The remaining components and preparation methods are the same as in Example 1.
[0042] Comparative Example 2: PVB encapsulation interlayer, by weight percentage, is composed of the following components: First, 50 wt% PVB resin; The second PVB resin was 35.5 wt%; Hexahydrophthalic anhydride 1.5 wt%; Plasticizer 12.2 wt% (the mass ratio of triethylene glycol di(2-ethylhexanoate) to diethylene glycol dibenzoate is 5:1); Anti-PID additive 0.3wt% (mass ratio of lithium dodecyl sulfonate to nano-silica with a particle size of 30nm is 1:3); Anti-photoaging agent 0.4wt% (the mass ratio of hindered amine light stabilizer HALS-944 to ultraviolet absorber UV-327 is 1:1); 0.1 wt% silane coupling agent (γ-aminopropyltriethoxysilane, KH-550); The remaining components and preparation methods are the same as in Example 1.
[0043] Comparative Example 3: PVB encapsulation interlayer, by weight percentage, is composed of the following components: First, 50 wt% PVB resin; The second PVB resin was 35.5 wt%; 1.5 wt% 2-Octen-1-ylsuccinic anhydride; Plasticizer 12.2 wt% (the mass ratio of triethylene glycol di(2-ethylhexanoate) to diethylene glycol dibenzoate is 5:1); Anti-PID additive 0.3wt% (mass ratio of lithium dodecyl sulfonate to nano-silica with a particle size of 30nm is 1:3); Anti-photoaging agent 0.4wt% (the mass ratio of hindered amine light stabilizer HALS-944 to ultraviolet absorber UV-327 is 1:1); 0.1 wt% silane coupling agent (γ-aminopropyltriethoxysilane, KH-550); The remaining components and preparation methods are the same as in Example 1.
[0044] Comparative Example 4 The PVB encapsulation interlayer, by weight percentage, is composed of the following components: First, 50 wt% PVB resin; The second PVB resin was 35.8 wt%; 1.5 wt% of composite anhydride compatibilizer (mass ratio of hexahydrophthalic anhydride to 2-octen-1-ylsuccinic anhydride is 2:1); Plasticizer 12.2 wt% (the mass ratio of triethylene glycol di(2-ethylhexanoate) to diethylene glycol dibenzoate is 5:1); Anti-photoaging agent 0.4wt% (the mass ratio of hindered amine light stabilizer HALS-944 to ultraviolet absorber UV-327 is 1:1); 0.1 wt% silane coupling agent (γ-aminopropyltriethoxysilane, KH-550); The remaining components and preparation methods are the same as in Example 1.
[0045] Comparative Example 5: The PVB encapsulation interlayer, by weight percentage, is composed of the following components: First, 50 wt% PVB resin; The second PVB resin was 35.5 wt%; 1.5 wt% of composite anhydride compatibilizer (mass ratio of hexahydrophthalic anhydride to 2-octen-1-ylsuccinic anhydride is 2:1); Plasticizer 12.2wt% (3GEH to diethylene glycol dibenzoate mass ratio of 5:1); Lithium dodecyl sulfonate 0.3 wt%; Anti-photoaging agent 0.4wt% (HALS-944 to UV-327 mass ratio is 1:1); 0.1 wt% silane coupling agent.
[0046] Comparative Example 6: PVB encapsulation interlayer, by weight percentage, is composed of the following components: First, 50 wt% PVB resin; The second PVB resin was 35.5 wt%; 1.5 wt% of composite anhydride compatibilizer (mass ratio of hexahydrophthalic anhydride to 2-octen-1-ylsuccinic anhydride is 2:1); Plasticizer 12.2wt% (3GEH to diethylene glycol dibenzoate mass ratio of 5:1); Nano-silica (average particle size 30nm) 0.3wt% Anti-photoaging agent 0.4wt% (HALS-944 to UV-327 mass ratio is 1:1); 0.1 wt% silane coupling agent.
[0047] The performance test results of the PVB encapsulation interlayers prepared in the examples and comparative examples are shown in Table 1.
[0048] Table 1: Performance test results of PVB encapsulation interlayers in the examples and comparative examples
[0049] The data in the table are the average values obtained after testing 5 replicate samples.
[0050] N-type photovoltaic PVB industry qualification standards (haze < 0.5%, transmittance > 89%, PID efficiency degradation rate ≤ 1%, UV aging ΔYI yellowing index < 2, damp heat aging plasticizer migration rate < 1.5%).
[0051] As shown in the table above, the overall performance of the PVB encapsulation interlayer in each group of embodiments is superior to that of any comparative example, and its performance meets the requirements of high-end N-type photovoltaic encapsulation materials. Furthermore, the performance of each group of embodiments is superior to that of each comparative example group. Comparing Comparative Example 1 (which omits the compatibilizer) with Example 1, Comparative Example 1 showed significantly increased haze, PID efficiency decay rate, UV aging haze increase, and damp heat aging plasticizer migration rate, but significantly decreased adhesive strength and overall performance. Analysis suggests that the lack of compatibilizer led to poor compatibility between the high residual hydroxyl PVB resin and the low residual hydroxyl PVB resin, resulting in phase separation. Microphase scattering caused a surge in haze, and interface defects caused simultaneous deterioration of adhesion and weather resistance. Comparative Examples 2 and 3, which used a single compatibilizer, were compared with Example 1. Their overall performance was significantly inferior to that of Example 1. This shows that compared to hexahydrophthalic anhydride and 2-octen-1-ylsuccinic anhydride alone, both have a synergistic effect on improving the overall performance of the PVB encapsulation interlayer. Analysis shows that hexahydrophthalic anhydride provides a rigid framework to inhibit photo-oxidative yellowing, while 2-octen-1-ylsuccinic anhydride provides a flexible chain to improve the two-phase dispersion. The performance improvement is limited when used alone, but the synergistic effect of the two in combination significantly improves the overall performance. Comparing Comparative Example 4, which lacks the anti-PID additive, with Example 1, its PID efficiency decay rate is significantly increased, indicating a significant decrease in anti-PID performance. Comparing Comparative Examples 5 and 6, which use a single anti-PID component, with Example 1, their anti-PID performance is inferior to Example 1. This shows that lithium alkyl sulfonate and nano-silica have a synergistic effect in improving the anti-PID performance of the PVB encapsulation interlayer. Furthermore, the anti-PID performance of Comparative Example 6 is better than that of Comparative Example 5. Analysis shows that lithium alkyl sulfonate actively blocks the sodium ion migration path through lithium-sodium ion exchange, which is more effective than the simple physical adsorption of nano-silica. However, when lithium alkyl sulfonate is used alone, the exchanged sodium ions lack adsorption and fixation sites and may still partially migrate to the battery surface, resulting in a decay rate of 3.8%. Combining the chemical blocking of lithium alkyl sulfonate with the high specific surface area physical adsorption of nano-silica, the synergistic effect of both can stably control the PID decay rate below 1.0%, fully meeting the stringent encapsulation requirements of N-type photovoltaic cells.
[0052] The present invention and its embodiments have been described above. This description is not restrictive, and the embodiments shown are only one of the embodiments of the present invention. The actual structure is not limited to this. In conclusion, if those skilled in the art are inspired by this description and design similar structures and embodiments without departing from the spirit of the present invention, they should all fall within the protection scope of the present invention.
Claims
1. A high-performance PVB encapsulation interlayer adapted to N-type photovoltaic cells, characterized in that, By weight percentage, its preparation raw materials consist of the following: First PVB resin 40-60 wt%; Secondary PVB resin 25-45 wt%; Composite anhydride compatibilizer 0.5–3 wt%; Plasticizer 12-20 wt%; Anti-PID additive 0.1–0.5 wt%; Anti-photoaging agent 0.2–0.8 wt%; Silane coupling agent 0.05–0.2 wt%; in: The first PVB resin has a residual hydroxyl content of 18-22 wt%, a residual acetate content of ≤2 wt%, and a number-average molecular weight Mn of 70,000-150,000. The second PVB resin has a residual hydroxyl content of 8-12 wt%, a residual acetate content of ≤2 wt%, and a number-average molecular weight Mn of 50,000-120,000. The composite anhydride compatibilizer is composed of hexahydrophthalic anhydride and 2-octen-1-ylsuccinic anhydride in a mass ratio of (1-3):1; The anti-PID additive is composed of C8-C18 alkyl sulfonate lithium and nano silica in a mass ratio of 1:(2-5).
2. The high-performance PVB encapsulation interlayer adapted for N-type photovoltaic cells according to claim 1, characterized in that, The plasticizer is composed of triethylene glycol di(2-ethylhexanoate) and diethylene glycol dibenzoate in a mass ratio of (4-6):
1.
3. The high-performance PVB encapsulation interlayer adapted for N-type photovoltaic cells according to claim 1, characterized in that, The anti-photoaging agent is composed of hindered amine light stabilizer and ultraviolet absorber in a mass ratio of 1:(1-2).
4. The high-performance PVB encapsulation interlayer adapted for N-type photovoltaic cells according to claim 1, characterized in that, The difference in residual hydroxyl content between the first PVB resin and the second PVB resin is ≥8wt%.
5. The high-performance PVB encapsulation interlayer adapted for N-type photovoltaic cells according to claim 1, characterized in that, The particle size of the nano-silica is 20–50 nm.
6. The high-performance PVB encapsulation interlayer adapted for N-type photovoltaic cells according to claim 1, characterized in that, The silane coupling agent is selected from γ-aminopropyltriethoxysilane.
7. A method for preparing a high-performance PVB encapsulation interlayer adapted to N-type photovoltaic cells according to any one of claims 1 to 6, characterized in that, Includes the following steps: ①Premixed After measuring each component, they are mixed evenly to obtain a premixed material; ②Mel-reactive extrusion A twin-screw extruder is used to melt-blend and extrude the premixed materials into a melt. ③ Cooling and pressing The melt extruded in step ② is rapidly cooled and pressed into shape to obtain a film preform.
8. The method for preparing a high-performance PVB encapsulation interlayer adapted to N-type photovoltaic cells according to claim 7, characterized in that, Step ③ The melt is rapidly cooled and pressed into shape using a cooling roller at 25-40℃.
9. An N-type photovoltaic cell module, characterized in that, It includes a high-performance PVB encapsulation interlayer adapted to N-type photovoltaic cells as described in any one of claims 1 to 6.
10. An N-type photovoltaic cell module according to claim 9, characterized in that, The photovoltaic cell module is a single-glass photovoltaic cell module or a double-glass photovoltaic cell module.