A thermally conductive composite material, a method for preparing the thermally conductive composite material, a copper-clad laminate, and a printed circuit board.

By combining a modified boron nitride precursor with epoxy resin, a continuous thermal conductivity pathway is constructed, which solves the problems of increased viscosity and loss of flexibility caused by high boron nitride filling in the epoxy resin matrix. This achieves both efficient heat conduction and insulation, making it suitable for high-density printed circuit boards.

CN123107301APending Publication Date: 2026-11-17SHENNAN CIRCUITS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611184439.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-05
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, the introduction of high boron nitride content into the epoxy resin matrix leads to problems such as increased viscosity, processing difficulties, and loss of flexibility, which affects its application in high-density, high-power printed circuit boards.

Method used

A modified boron nitride precursor is used. By grafting hydroxyl modification groups onto the surface of boron nitride to form a band-like structure, and then combining it with epoxy resin, a continuous thermally conductive pathway is constructed, reducing the filler content to improve thermal conductivity and enhancing interfacial compatibility.

Benefits of technology

It significantly improves thermal conductivity at low filler content, avoids viscosity increase and loss of flexibility, ensures insulation and processing performance, is suitable for heat conduction in high-density printed circuit boards, reduces chip junction temperature, and improves the stability and lifespan of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107301A_ABST
    Figure CN123107301A_ABST
Patent Text Reader

Abstract

This invention provides a thermally conductive composite material, a method for preparing the thermally conductive composite material, a copper-clad laminate, and a printed circuit board. The composite material includes resin and filler, the filler including modified boron nitride. The modified boron nitride comprises a boron nitride precursor and hydroxyl-modified groups. The boron nitride precursor has a ribbon-like structure, and the hydroxyl-modified groups are grafted onto the surface of the boron nitride precursor. The thermally conductive composite material provided by this invention constructs a continuous thermally conductive pathway through the ribbon-like structure of the boron nitride precursor. Its ribbon-like shape makes it easier for the precursors to overlap and form a through-type thermally conductive network, achieving improved thermal conductivity with a lower filler content. The surface-grafted hydroxyl-modified groups enhance the interfacial compatibility and interaction between boron nitride and the resin, reducing interfacial thermal resistance. Furthermore, the low filler content avoids problems such as a sharp increase in composite material viscosity and loss of flexibility. Thus, while ensuring insulation and processing performance, it effectively resolves the contradiction between insufficient thermal conductivity of epoxy resin-based materials and the negative impact of high filler content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electronic packaging materials technology, and in particular to a thermally conductive composite material, a method for preparing the thermally conductive composite material, a copper-clad laminate, and a printed circuit board. Background Technology

[0002] Epoxy resin is the primary matrix material for manufacturing copper clad laminates (CCL) for printed circuit boards (PCBs) and electronic encapsulation potting compounds due to its excellent adhesion, mechanical strength, electrical insulation, chemical corrosion resistance, and mature processing technology. However, the extremely low intrinsic thermal conductivity of epoxy resin (approximately 0.2 W / (m·K)) severely limits its application in high-density, high-power PCBs.

[0003] In existing technologies, the thermal conductivity of epoxy resin is often improved by introducing high thermal conductivity fillers. Among them, boron nitride (BN) is considered an ideal insulating and thermally conductive filler due to its excellent electrical insulation (low dielectric constant and high volume resistivity) and good thermal conductivity. However, spherical or plate-shaped boron nitride fillers are difficult to form effective thermal conduction pathways in epoxy resin matrices, requiring a very high filler content (usually >30 vol%) to significantly improve thermal conductivity. High filler content of boron nitride leads to a sharp increase in viscosity, processing difficulties, loss of flexibility, increased internal stress, and increased cost of the resulting thermally conductive composite material. Summary of the Invention

[0004] To address the problems of drastically increased viscosity, processing difficulties, and loss of flexibility caused by the introduction of excessive boron nitride into resin materials during the fabrication of printed circuit boards in the prior art, this paper provides a thermally conductive composite material, a method for preparing the thermally conductive composite material, a copper-clad laminate, and a printed circuit board.

[0005] The technical solution adopted by the present invention to solve the above-mentioned technical problems is as follows: On one hand, the present invention provides a thermally conductive composite material, comprising a resin and a filler, wherein the filler comprises modified boron nitride, the modified boron nitride comprising a boron nitride precursor and hydroxyl-modifying groups, the boron nitride precursor having a band-like structure, and the hydroxyl-modifying groups being grafted onto the surface of the boron nitride precursor.

[0006] Optionally, the banded structure of the boron nitride precursor has a width of 0.5-5 μm, a length of 10-100 μm, and a thickness of 50-300 nm.

[0007] Optionally, in the thermally conductive composite material, the resin has a mass percentage content of 90%-96%.

[0008] Optionally, in the thermally conductive composite material, the modified boron nitride has a mass percentage content of 4%-8%.

[0009] Optionally, the resin is an epoxy resin, including one or more of bisphenol A type epoxy resin and brominated epoxy resin.

[0010] Optionally, the preparation method of the above-mentioned thermally conductive composite material includes the following operations: Boron source, nitrogen source and catalyst, under high temperature catalytic conditions, form boron nitride precursor; The boron nitride precursor was placed in a strong acid solution and refluxed. After washing with water and drying, the modified boron nitride with hydroxyl-modified groups was obtained. Modified boron nitride and resin were added to a diluent and dispersed to obtain a thermally conductive composite material.

[0011] Optionally, the boron source includes one or more of boric acid and boron oxide; and / or, Nitrogen sources include one or more of ammonia and urea; and / or, The catalyst comprises one or more of magnesium oxides and iron oxides; and / or, Strong acid solutions include one or more of concentrated nitric acid and concentrated sulfuric acid.

[0012] Optionally, during the reflux treatment, the reflux temperature is 60-120℃ and the reflux time is 2-12h.

[0013] On the other hand, the present invention provides a copper-clad laminate, comprising a copper layer and a thermally conductive layer, wherein the thermally conductive layer is obtained by curing the aforementioned thermally conductive composite material, or by curing the thermally conductive composite material prepared by the aforementioned thermally conductive composite material preparation method. The thermally conductive layer is placed on the surface of the copper layer.

[0014] On the other hand, the present invention provides a printed circuit board including the copper-clad laminate.

[0015] The beneficial effects of this application are as follows: The thermally conductive composite material provided in this application features a continuous thermally conductive pathway constructed through a boron nitride precursor with a strip-like structure. Compared to spherical or sheet-like boron nitride, its strip-like shape makes it easier for them to overlap and form a through-type thermally conductive network, achieving a significant improvement in thermal conductivity with a lower filler content. Simultaneously, the hydroxyl-modified groups grafted onto the surface enhance the interfacial compatibility and interaction between boron nitride and the resin matrix, reducing interfacial thermal resistance and further optimizing the efficiency of the thermal conductive path. Furthermore, the low filler content avoids problems such as a sharp increase in composite material viscosity and loss of flexibility. Thus, while ensuring insulation and processing performance, it effectively resolves the contradiction between insufficient thermal conductivity of epoxy resin-based materials and the negative impact of high filler content. Consequently, when the thermally conductive composite material provided in this application is used in printed circuit boards, it can quickly and effectively conduct and disperse the heat of the printed circuit board, effectively reducing the chip junction temperature and the hot spot temperature of the printed circuit board, thereby improving the operational stability and lifespan of electronic devices. Attached Figure Description

[0016] Figure 1 This invention provides a thermally conductive composite material, a method for preparing the thermally conductive composite material, and a process for preparing copper-clad laminates and printed circuit boards. Detailed Implementation

[0017] To make the technical problems solved, the technical solutions, and the beneficial effects of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0018] The present invention provides a thermally conductive composite material comprising a resin and a filler, wherein the filler comprises modified boron nitride, the modified boron nitride comprising a boron nitride precursor and hydroxyl-modifying groups, the boron nitride precursor having a band-like structure, and the hydroxyl-modifying groups being grafted onto the surface of the boron nitride precursor.

[0019] Specifically, in the thermally conductive composite material provided in this application, the boron nitride precursor (HBNR) with a strip structure constructs a continuous thermally conductive path. Its strip shape is easier to overlap with each other to form a through-type thermally conductive network compared to spherical or sheet-like shapes, which can significantly improve thermal conductivity with a lower filler content. At the same time, the hydroxyl-modified groups grafted on the surface can enhance the interfacial compatibility and interaction between boron nitride and the resin matrix, reduce interfacial thermal resistance, further optimize the efficiency of the thermal conductive path, and the low filler content can avoid problems such as a sharp increase in the viscosity of the composite material and loss of flexibility. Thus, while ensuring insulation and processing performance, it effectively solves the contradiction between the insufficient thermal conductivity of epoxy resin (EP) based materials and the negative impact of high filler content. Furthermore, when the thermally conductive composite material provided in this application is used in printed circuit boards, it can quickly and effectively conduct and disperse the heat of the printed circuit board, effectively reduce the chip junction temperature and the hot spot temperature of the printed circuit board, and improve the operating stability and life of electronic devices.

[0020] In some embodiments, the banded structure of the boron nitride precursor has a width of 0.5-5 μm, a length of 10-100 μm, and a thickness of 50-300 nm.

[0021] Specifically, the boron nitride precursor contains a strip-shaped structure with a width of 0.5-5 μm, a length of 10-100 μm, and a thickness of 50-300 nm. The width and length within the above range facilitate the contact between the strip-shaped structures to form a continuous thermally conductive network, thereby improving the thermal conductivity. The thickness of 50-300 nm can reduce the amount of filler per unit volume, while increasing the contact area with the resin matrix. Combined with hydroxyl modification, this further improves the interfacial compatibility, thus achieving the construction of an efficient thermally conductive pathway with a lower filler content. This balances the mechanical properties and processing fluidity of the composite material, avoiding the performance degradation caused by high filler content.

[0022] Furthermore, the width of the banded structure of the boron nitride precursor can be 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm or 5 μm; The length of the band-like structure of the boron nitride precursor can be 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm; The thickness of the band structure of the boron nitride precursor can be 50nm, 80nm, 100nm, 120nm, 150nm, 170nm, 200nm, 230nm, 260nm or 300nm.

[0023] In some embodiments, the resin in the thermally conductive composite material has a mass percentage content of 90%-96%.

[0024] Specifically, when the mass percentage of the resin is in the range of 90%-96%, it can ensure the continuity of the resin as a matrix and the good coating of the filler, ensuring that the composite material has basic mechanical properties and processing fluidity. It can also provide suitable filling space for the strip-modified boron nitride, so that it can form a continuous thermally conductive network through efficient overlapping at a low dosage. This avoids problems such as excessive interruption of the thermal conductive path due to excessive resin content, or increased material brittleness and molding difficulties due to excessive resin content, thereby achieving a balance between thermal conductivity and overall performance.

[0025] In some embodiments, the modified boron nitride in the thermally conductive composite material has a mass percentage content of 4%-8%.

[0026] Specifically, the modified boron nitride content of 4%-8% in the thermally conductive composite material of this application can effectively avoid problems such as a sharp increase in the viscosity of the composite material and processing difficulties. At the same time, the boron nitride precursor band structure in the modified boron nitride enables it to form a continuous thermally conductive network through efficient overlapping at a low content (4%-8%). Combined with the enhanced interfacial compatibility due to hydroxyl modification, it can significantly improve thermal conductivity while ensuring material flexibility, reducing internal stress and cost, and achieving a balance between thermal conductivity and processing performance.

[0027] In some embodiments, the resin is an epoxy resin, including one or more of bisphenol A type epoxy resin and brominated epoxy resin.

[0028] Specifically, when one or more of bisphenol A epoxy resin and brominated epoxy resin are selected as the matrix resin, bisphenol A epoxy resin has good adhesion and mechanical strength, providing a stable matrix framework for the composite material; brominated epoxy resin, while possessing adhesion, can also impart excellent flame retardant properties to the material, meeting the fire safety requirements of electronic devices; the combination or use of the two can form a good interfacial bond with strip-modified boron nitride, ensuring the effectiveness of the thermal conductive network, and enabling the composite material to maintain high insulation and chemical corrosion resistance while adapting to the multiple performance requirements of printed circuit boards and electronic packaging, achieving a balance between function and reliability.

[0029] In some embodiments, the method for preparing the above-mentioned thermally conductive composite material includes the following operations: Boron source, nitrogen source and catalyst, under high temperature catalytic conditions, form boron nitride precursor; The boron nitride precursor was placed in a strong acid solution and refluxed. After washing with water and drying, the modified boron nitride with hydroxyl-modified groups was obtained. Modified boron nitride and resin were added to a diluent and dispersed to obtain a thermally conductive composite material.

[0030] Specifically, in the above preparation method, under high-temperature catalytic conditions, boron and nitrogen sources react with the catalyst to generate a banded boron nitride precursor, and its microstructure is directionally controlled to optimize the thermal conductivity network construction capability; strong acid reflux treatment promotes the grafting of hydroxyl-modified groups onto the surface of boron nitride, and enhances the interfacial compatibility with the resin matrix through chemical modification, thereby reducing the interfacial thermal resistance; the modified boron nitride and resin are dispersed in a diluent to prepare a composite slurry, and the viscosity of the system can be controlled by the diluent, promoting uniform dispersion of fillers, avoiding agglomeration, and ensuring the continuity of the thermal conductivity pathway.

[0031] Furthermore, under high-temperature catalytic conditions, the boron and nitrogen sources undergo a directional chemical reaction under the action of the catalyst. Specifically, the metal oxide catalyst (such as magnesium oxide and iron oxide) serves as a nucleation site in the reaction system. The anisotropy of its surface energy leads to differences in the growth rate of different crystal planes. First, the catalyst preferentially adsorbs on the side of the boron nitride crystal nucleus (non-c-axis direction), which increases the growth barrier in this direction and thus inhibits the lateral expansion of the crystal. At the same time, the c-axis direction (axial direction) maintains a high growth rate. Driven by the sufficient atomic migration energy provided by the high temperature of 1000-1400℃, active boron / nitrogen atoms are continuously deposited on the axial growth front, which promotes the continuous extension of the crystal along the axial direction, and finally forms a ribbon structure with a width of submicron to several micrometers, a length of tens to hundreds of micrometers, and a thickness of nanometers.

[0032] The aforementioned directional growth mechanism is synergistically regulated by the type of catalyst, reaction temperature, and feed rate. Changing any of these factors may result in the failure of the banded structure to form or morphological degradation.

[0033] Specifically, the boron nitride precursor can be prepared by chemical vapor deposition or a template method. In some embodiments, the boron source includes one or more of boric acid and boron oxide; and / or, Nitrogen sources include one or more of ammonia and urea; and / or, The catalyst comprises one or more of magnesium oxides and iron oxides; and / or, Strong acid solutions include one or more of concentrated nitric acid and concentrated sulfuric acid.

[0034] In high-temperature catalysis, the catalytic temperature is 1000-1400℃.

[0035] Specifically, boric acid / boron oxide is selected as the boron source because its molten or gaseous molecules readily react with the nitrogen source at high temperatures, and the hydroxyl or oxygen bridge bonds contained in its structure can help regulate the growth direction of boron nitride crystals. Ammonia / urea is selected as the nitrogen source because the former participates in the reaction in a gaseous state at high temperatures and has good diffusion uniformity, while the latter decomposes to produce nitrogen-containing active groups, and the reaction is mild and controllable. Both can provide sufficient nitrogen atoms to form the boron nitride framework. That is, the high temperature environment of 1000-1400℃ provides sufficient migration energy for the active atoms produced by the decomposition of the boron and nitrogen sources, enabling them to overcome the potential barrier and reach the catalyst-induced preferential growth sites, maintaining the continuous extension of the banded structure. If the temperature is below 1000℃ (such as 800℃), the atomic migration energy is insufficient, and directional growth cannot be maintained, resulting in irregular granular or short fragments of the product. When ammonia is used as a nitrogen source, its flow rate and partial pressure affect the concentration of active nitrogen atoms in the reaction system. An excessively high feed rate, for example, a flow rate higher than 400 mL / min, may lead to an excessively high concentration of active nitrogen atoms in the reaction system, resulting in the simultaneous growth of multiple nuclei and the formation of sheet-like aggregates. A moderate feed rate (e.g., 50-400 mL / min) is conducive to the continuous growth of single ribbon-like structures. On the other hand, an excessively low feed rate (e.g., below 50 mL / min) will result in insufficient concentration of active nitrogen atoms, limited nitrogen source supply, a significant reduction in the growth rate of boron nitride, difficulty in maintaining the continuous directional growth of ribbon-like structures, and a tendency to form short fragments or irregular granular products. Magnesium oxide / iron oxide can act as a catalyst, and its metal ions can be adsorbed on the surface of boron nitride crystal nuclei during the reaction. By changing the surface energy of different crystal planes, the crystal can be preferentially grown along the c-axis, promoting the formation of a banded structure (forming a one-dimensional extended banded morphology). Furthermore, if no catalyst is used or other catalysts (such as Al2O3, ZnO, etc.) are used, boron nitride tends to grow uniformly along the basal plane, forming a plate-like or granular structure, rather than forming the band-like structure described in this application.

[0036] The strong oxidizing properties and acidic environment of concentrated nitric acid / concentrated sulfuric acid can etch the surface of boron nitride during reflux treatment, generating hydroxyl functional groups, while removing amorphous impurities and improving the uniformity of surface modification. The synergistic effect of each component ensures the high efficiency of the preparation of banded boron nitride precursor and the controllability of grafting of modified groups.

[0037] In some embodiments, the reflux temperature is 60-120°C and the reflux time is 2-12 hours.

[0038] Specifically, a temperature range of 60-120℃ can ensure that the strong acid solution has sufficient oxidative etching ability to promote the hydroxylation reaction on the surface of boron nitride, while avoiding the destruction of the boron nitride crystal structure due to excessive temperature. Controlling the reflux time helps ensure the sufficiency and uniformity of hydroxyl-modified group grafting. A reflux treatment time of 2-12 hours can achieve precise control of the surface hydroxylation degree while ensuring the integrity of the boron nitride band structure. This enhances the interfacial bonding force with the resin matrix and avoids filler agglomeration caused by excessive modification.

[0039] Reference Figure 1 In another embodiment of the present invention, a copper-clad laminate is provided, comprising a copper layer and a thermally conductive layer, wherein the thermally conductive layer is obtained by curing the aforementioned thermally conductive composite material, or by curing the thermally conductive composite material prepared by the aforementioned thermally conductive composite material preparation method. The thermally conductive layer is placed on the surface of the copper layer.

[0040] The specific operations include: Reinforcing materials such as fiberglass cloth are impregnated into thermally conductive composite materials, the adhesive content is controlled, and the material is semi-cured in an oven to produce a thermally conductive prepreg. Multiple sheets of prepreg are laminated with copper foil and pressed together under high temperature and high pressure to produce a thermally conductive epoxy fiberglass copper clad laminate (CCL) for PCB manufacturing. The composite thermally conductive material contains a curing agent, which includes one or more of methyltetrahydrophthalic anhydride or dicyandiamide.

[0041] Specifically, the copper-clad laminate is obtained by curing the thermally conductive composite material to form a thermally conductive layer and attaching it to the surface of the copper layer. The efficient thermally conductive network constructed by the strip-shaped modified boron nitride in the thermally conductive layer can quickly dissipate the heat generated by the copper layer (circuit wiring area), make up for the defect of insufficient intrinsic thermal conductivity of epoxy resin, and meet the heat dissipation requirements of high-density PCBs. It should be noted that boron nitride itself has excellent insulating properties, and the volume resistivity of composite materials prepared using modified boron nitride can be maintained at 10 Ω·cm. 14 With a strength of Ω·cm or higher, it can meet the insulation requirements of dielectric materials for high-frequency and high-speed PCBs.

[0042] The cured thermally conductive composite material forms a good interface bond with the copper layer, which not only retains the adhesion, electrical insulation and processability of the epoxy resin matrix, but also avoids the sharp increase in viscosity and deterioration of mechanical properties of the traditional high-filler system by modifying the filler with low filler content. At the same time, the presence of the thermally conductive layer can uniformly disperse the thermal stress of the copper layer, improve the reliability of the copper clad laminate, and is suitable for heat dissipation and packaging scenarios of high-power electronic devices, achieving a synergistic improvement in thermal conductivity, electrical performance and mechanical performance.

[0043] In another embodiment of the present invention, a printed circuit board is provided, including the copper-clad laminate.

[0044] Specifically, when the printed circuit board uses the copper-clad laminate provided in this application, the high-efficiency heat dissipation capability of the thermal conductive layer in the copper-clad laminate can effectively solve the problem of heat accumulation during the operation of high-density circuit wiring and high-power devices. The continuous thermal conductive network constructed by the strip-modified boron nitride in the thermal conductive layer can quickly dissipate the heat generated by the copper layer circuit, avoiding device failure caused by local overheating. At the same time, the excellent electrical insulation, mechanical strength and processability of the epoxy resin matrix retained by the copper-clad laminate ensure that the circuit board has good heat dissipation performance while meeting the requirements of electrical connection reliability and processing molding. It is suitable for high-frequency and high-speed electronic scenarios with high heat dissipation requirements, such as 5G communication and new energy vehicles, and achieves synergistic optimization of heat dissipation efficiency and circuit performance.

[0045] The present invention will be further illustrated by the following examples.

[0046] Table 1 Example 1 This embodiment illustrates the preparation method of the thermally conductive composite material and the copper-clad laminate disclosed in this invention, and includes the following steps: Preparation of thermally conductive composite materials Boric acid, ammonia, and magnesium oxide undergo a catalytic reaction at 1000°C under a protective atmosphere (Ar) to form a boron nitride precursor. The boron nitride precursor has a width of 0.5 μm, a length of 10 μm, and a thickness of 50 nm. The boron nitride precursor was placed in a concentrated nitric acid solution and refluxed at 60°C for 2 hours. After washing with water and drying, the modified boron nitride with hydroxyl-modified groups was obtained. 5% modified boron nitride, 93% resin, and 2% curing agent were added to acetone diluent and dispersed to obtain a thermally conductive composite material. Preparation of copper-clad laminates 1080 type electronic-grade glass fiber cloth was impregnated with a thermally conductive composite material. The content of the thermally conductive composite material was controlled at 50±2% by using a doctor blade. The impregnated glass fiber cloth was baked in an oven at 160℃ for 5 minutes to obtain a semi-cured (B-stage) thermally conductive prepreg. Eight sheets of prepreg were laminated with two sheets of 18μm electrolytic copper foil (copper layer) and placed in a vacuum hot press at 180℃ and 15kg / cm². 2 After being kept under pressure for 2 hours and then cooled, a high thermal conductivity epoxy fiberglass copper-clad laminate is obtained.

[0047] Example 2-12 2-12 are used to illustrate the preparation method of the thermally conductive composite material and the copper-clad laminate disclosed in this invention, including most of the operations in Example 1, the difference being: In Examples 2-12, the types of nitrogen source, boron source, catalyst, catalytic reaction temperature (°C), resin content (%), modified boron nitride content (%), as well as the width of the banded structure of the boron nitride precursor, the length of the boron nitride precursor, and the thickness of the boron nitride precursor are set according to the parameters in Table 1. Comparative Example 1 This comparative example is used to illustrate the preparation method of the thermally conductive composite material and the copper-clad laminate disclosed in this invention, including most of the operations in Example 1, the difference being: No catalyst is added when preparing the boron nitride precursor: Boric acid and ammonia were subjected to a catalytic reaction at 1000℃ under a protective atmosphere (Ar).

[0048] In this comparative example, no catalytic reaction was carried out, so boron nitride tended to grow uniformly along the basal plane, forming a plate-like or granular structure, rather than forming the band-like structure described in this application.

[0049] Comparative Example 2 This comparative example is used to illustrate the preparation method of the thermally conductive composite material and the copper-clad laminate disclosed in this invention, including most of the operations in Example 1, the difference being: When preparing boron nitride precursors, the catalytic temperature is below 1000℃: Boric acid, ammonia, and magnesium oxide undergo a catalytic reaction at 800°C under a protective atmosphere (Ar).

[0050] In this comparative example, the catalytic temperature was much lower than the range specified in this application, the atomic migration energy was insufficient, and directional growth could not be maintained. The resulting product was irregularly granular or short fragmented, and the ribbon-like structure described in this application could not be obtained.

[0051] Comparative Example 3 This comparative example is used to illustrate the preparation method of the thermally conductive composite material and the copper-clad laminate disclosed in this invention, including most of the operations in Example 1, the difference being: In composite materials, boron nitride is typically in the form of sheet-like boron nitride.

[0052] Comparative Example 4 This comparative example is used to illustrate the preparation method of the thermally conductive composite material and the copper-clad laminate disclosed in this invention, including most of the operations in Example 1, the difference being: In composite materials, boron nitride is typically spherical.

[0053] Comparative Example 5 This comparative example is used to illustrate the preparation method of the thermally conductive composite material and the copper-clad laminate disclosed in this invention, including most of the operations in Example 1, the difference being: When preparing the boron nitride precursor, the ammonia feed rate is lower than the range specified in this application, making it impossible to form a banded structure. Boric acid, ammonia, and magnesium oxide were catalytically reacted at 1000 °C under a protective atmosphere (Ar), with the ammonia feed rate being 30 mL / min.

[0054] Performance testing The following performance tests were performed on Examples 1-12 and Comparative Examples 1-5 prepared above: (1) Thermal conductivity test: The laser flare method (LFA) was used, referring to the ASTM E1461 standard. The test sample was a circular piece with a diameter of 12.7 mm and a thickness of 2 mm. The test temperature was 25℃. Each sample was tested 3 times and the average value was taken. (2) Volume resistivity test: Refer to GB / T 1410-2006, use a high resistivity meter at 500V DC, test temperature 23±2℃, relative humidity 50±5%; (3) Bending strength test: Refer to GB / T 9341-2008, adopt the three-point bending method, span 64mm, loading rate 2mm / min; (4) Glass transition temperature (Tg) test: Differential scanning calorimetry (DSC) was used, referring to GB / T 19466.2-2004, with a heating rate of 10℃ / min and a nitrogen atmosphere; (5) Dielectric constant and dielectric loss test: Refer to GB / T 1409-2006, use an impedance analyzer, and test frequency 1MHz.

[0055] The test results are entered into Table 2.

[0056] Table 2 As can be seen from the test results in Table 2, the boron nitride precursors of Examples 1-12 obtained by the preparation method of the present invention have a continuous ribbon structure. Their thermal conductivity, volume resistivity, flexural strength and glass transition temperature are all better than those of the comparative examples. This indicates that the ribbon boron nitride formed at the catalytic reaction temperature and ammonia feeding rate can synergistically improve the thermal conductivity, insulation, mechanical and heat resistance properties of the obtained thermally conductive composite material.

[0057] Comparing the test results of Examples 1-12 and Comparative Examples 1-5, it can be seen that each comparative example failed to form a continuous ribbon structure due to reasons such as no catalytic reaction (Comparative Example 1), low catalytic temperature (Comparative Example 2), use of traditional sheet-like or spherical boron nitride (Comparative Examples 3 and 4), and excessively low ammonia feeding rate (Comparative Example 5). Consequently, their thermal conductivity, volume resistivity, flexural strength, and Tg all decreased to varying degrees compared with the examples. Among them, Comparative Example 5 showed a particularly significant performance decline due to excessively low feeding rate, insufficient active nitrogen, and incomplete ribbon structure.

[0058] In other words, the thermally conductive composite material provided in this application constructs a continuous thermally conductive path through a boron nitride precursor with a strip-shaped structure. Compared with spherical or sheet-shaped boron nitride, its strip-shaped morphology makes it easier for them to overlap and form a through-type thermally conductive network, which can significantly improve thermal conductivity with a lower filler content. At the same time, the hydroxyl-modified groups grafted on the surface can enhance the interfacial compatibility and interaction between boron nitride and the resin matrix, reduce interfacial thermal resistance, further optimize the efficiency of the thermal conductive path, and the low filler content can avoid problems such as a sharp increase in the viscosity of the composite material and loss of flexibility. Thus, while ensuring insulation and processing performance, it effectively solves the contradiction between the insufficient thermal conductivity of epoxy resin-based materials and the negative impact of high filler content. Furthermore, when the thermally conductive composite material provided in this application is used in printed circuit boards, it can quickly and effectively conduct and disperse the heat of the printed circuit board, effectively reduce the chip junction temperature and the hot spot temperature of the printed circuit board, and improve the operating stability and life of electronic devices.

[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A thermally conductive composite material, characterized in that, The invention includes a resin and a filler, wherein the filler includes modified boron nitride, the modified boron nitride comprising a boron nitride precursor and hydroxyl-modifying groups, the boron nitride precursor having a band-like structure, and the hydroxyl-modifying groups being grafted onto the surface of the boron nitride precursor.

2. The thermally conductive composite material according to claim 1, characterized in that, The banded structure of the boron nitride precursor has a width of 0.5-5 μm, a length of 10-100 μm, and a thickness of 50-300 nm.

3. The thermally conductive composite material according to claim 1, characterized in that, In the thermally conductive composite material, the resin has a mass percentage content of 90%-96%.

4. The thermally conductive composite material according to claim 1, characterized in that, In the thermally conductive composite material, the modified boron nitride has a mass percentage content of 4%-8%.

5. The thermally conductive composite material according to claim 1, characterized in that, The resin is an epoxy resin, including one or more of bisphenol A type epoxy resin and brominated epoxy resin.

6. The method for preparing the thermally conductive composite material according to any one of claims 1-5, characterized in that, Includes the following operations: Boron source, nitrogen source and catalyst, under high temperature catalytic conditions, form boron nitride precursor; The boron nitride precursor was placed in a strong acid solution and refluxed. After washing with water and drying, the modified boron nitride with hydroxyl-modified groups was obtained. Modified boron nitride and resin were added to a diluent and dispersed to obtain a thermally conductive composite material.

7. The method for preparing the thermally conductive composite material according to claim 6, characterized in that, Boron sources include one or more of boric acid and boron oxide; and / or, Nitrogen sources include one or more of ammonia and urea; and / or, The catalyst comprises one or more of magnesium oxides and iron oxides; and / or, Strong acid solutions include one or more of concentrated nitric acid and concentrated sulfuric acid.

8. The method for preparing the thermally conductive composite material according to claim 6, characterized in that, During reflux treatment, the reflux temperature is 60-120℃ and the reflux time is 2-12h.

9. A copper-clad laminate, characterized in that, It includes a copper layer and a thermally conductive layer, wherein the thermally conductive layer is obtained by curing the thermally conductive composite material according to any one of claims 1-5, or the thermally conductive composite material prepared by the method of preparing the thermally conductive composite material according to any one of claims 6-8. The thermally conductive layer is placed on the surface of the copper layer.

10. A printed circuit board, characterized in that, Including the copper-clad laminate as described in claim 9.