A double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material, its preparation method and application

By preparing a composite material of magnetic ellagic acid carbon nanofibers and spherical boron nitride, the problem of incompatibility between the insulation, thermal conductivity and microwave absorption properties of chip packaging materials was solved, and efficient chip packaging performance integration was achieved.

CN123107302APending Publication Date: 2026-11-17SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611266822.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing chip packaging materials have incompatibility issues in terms of insulation, thermal conductivity, and microwave absorption properties, resulting in severe interfacial thermal resistance and inadequate mechanical properties.

Method used

Magnetic ellagic acid carbon nanofibers were formed by reacting ellagic acid solution and nickel ion-containing solution in a mixed solvent. These nanofibers were then mixed with spherical boron nitride and epoxy resin under the influence of a magnetic field and gravity to prepare a double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material.

Benefits of technology

It integrates wave absorption, thermal conductivity and insulation properties, reduces interfacial thermal resistance, improves the overall performance of chip packaging, and has the advantages of simple process, high efficiency and good controllability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107302A_ABST
    Figure CN123107302A_ABST
Patent Text Reader

Abstract

This application relates to the field of microwave absorption and thermally conductive materials technology, and discloses a double-sided heterogeneous insulating thermally conductive-electromagnetic shielding composite material, its preparation method, and its application. The preparation method includes the following steps: adding ellagic acid solution and nickel ion-containing solution to a mixed solvent to prepare a reaction solution, stirring and reacting to obtain a suspension; centrifuging the suspension to collect the solid phase, washing, and drying to obtain a precursor; heat-treating the precursor in a nitrogen atmosphere to obtain magnetic ellagic acid carbon nanofibers; uniformly mixing the magnetic ellagic acid carbon nanofibers, spherical boron nitride, epoxy resin, and curing agent, and pressing and curing in a magnetic field to obtain the double-sided heterogeneous insulating thermally conductive-electromagnetic shielding composite material. This application, through the mixing of simple components and the effects of a magnetic field and gravity, can obtain a double-sided heterogeneous composite material with excellent microwave absorption, thermal conductivity, and insulation properties by curing at room temperature under a press. The process is simple, efficient, and highly controllable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of microwave absorption and thermal conductive materials technology, specifically to a double-sided heterogeneous insulating thermally conductive-electromagnetic shielding composite material, its preparation method, and its application. Background Technology

[0002] With the rapid development of communication technology, the electromagnetic environment in which radio frequency (RF) chips operate is becoming increasingly complex, and electromagnetic interference is becoming more and more serious. At the same time, as the electronic components of RF chips become increasingly dense, their heat dissipation problems are becoming more and more prominent.

[0003] Metal aluminum alloy shielding is a widely used shielding method on chips, achieving bidirectional electromagnetic isolation. This protects internal circuits from interference while preventing internal signals from interfering with external signals. However, the metal shielding primarily responds to electromagnetic waves through reflection, and these reflected waves can cause secondary interference to the internal circuits; this interference is becoming increasingly severe, especially with the large-scale upgrades of chips. Furthermore, to prevent short circuits in electronic components, an air layer separates the metal shielding from the circuitry, further complicating heat dissipation for the chip.

[0004] To address this issue, current research focuses on filling the space between the chip and the metal shield with heat-absorbing and absorbing materials to reduce the electromagnetic reflectivity of the metal while enhancing the chip's heat dissipation. However, most existing absorbing materials are conductive, which poses a risk of short circuits to the chip's electronic components. Therefore, most current research focuses on designing separate layers for heat conduction and absorbing materials. However, a distinct interface can lead to problems such as severe interfacial thermal resistance and incompatible mechanical properties.

[0005] Therefore, developing a new integrated, molded, double-layer wave-absorbing, thermally conductive, and insulating composite material is of great significance for chip packaging. Summary of the Invention

[0006] This application provides a double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material, its preparation method and application, aiming to solve the technical problem of incompatibility of insulation, thermal conductivity and wave absorption properties in existing chip packaging materials.

[0007] To achieve the above objectives, the present application adopts the following technical solution.

[0008] The first aspect of this application provides a method for preparing a double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material, comprising the following steps: S1, ellagic acid solution and nickel ion-containing solution are added to a mixed solvent to prepare a reaction solution, and the reaction is stirred to obtain a suspension; The suspension was centrifuged to collect the solid phase, which was then washed and dried to obtain the precursor. S2, the precursor is heat-treated in a nitrogen atmosphere to obtain magnetic ellagic acid carbon nanofibers. S3, the magnetic ellagic acid carbon nanofibers, spherical boron nitride, epoxy resin and curing agent are mixed evenly and then pressed and cured in a magnetic field to obtain a double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material.

[0009] Preferably, the mixed solvent comprises, by volume percentage, 0-62% methylpyrrolidone, 38-100% deionized water, and 0.051% ammonia. The ellagic acid solution is a methylpyrrolidone solution of ellagic acid with a concentration of 20 mg / mL; The nickel ion-containing solution is an aqueous solution of nickel chloride, with a nickel ion concentration of 60 mg / mL.

[0010] Preferably, the mass ratio of nickel ions to ellagic acid in the reaction solution is 10~35:90~65; The volume ratio of methylpyrrolidone to deionized water is 20~80:80~20.

[0011] More preferably, the reaction solution contains ellagic acid at a concentration of 3 mg / mL, nickel ions at a concentration of 0.4-1.6 mg / mL, and ammonia at a volume fraction of 0.044%.

[0012] Preferably, the reaction temperature in S1 is room temperature, and the reaction time is 6~24h; The heat treatment described in S2 specifically refers to: The temperature is increased to 900℃ at a rate of 2~5℃ / min and held for 1~3 hours; then it is cooled to room temperature at a rate of 2~5℃ / min.

[0013] Preferably, based on the total amount of magnetic ellagic acid carbon nanofibers, spherical boron nitride, epoxy resin, and curing agent, the amount of magnetic ellagic acid carbon nanofibers is 5-25 wt% of the total amount, the amount of spherical boron nitride is 10-50 wt% of the total amount, and the remainder is epoxy resin and curing agent. The mass ratio of the epoxy resin to the curing agent is 1~3:1; The curing agent is a low-viscosity epoxy resin curing agent.

[0014] Preferably, a magnetic field is formed by uniformly mixing magnetic ellagic acid carbon nanofibers, spherical boron nitride, epoxy resin and curing agent and placing them in a mold, and then placing a bar magnet on the mold.

[0015] Preferably, the pressing and curing temperature is room temperature, the pressure is 5~10 MPa, and the holding time is 5~12 h.

[0016] A second aspect of this application provides a double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material prepared by the above-described preparation method.

[0017] A third aspect of this application provides the application of the above-mentioned double-sided heterogeneous insulating thermally conductive-electromagnetic shielding composite material in chip packaging.

[0018] Compared with the prior art, the beneficial effects of this application are as follows: This application uses ellagic acid as a raw material and leverages the metal chelation properties of polyphenols to prepare a magnetoelectric composite absorbing filler. This filler is further mixed with spherical boron nitride and epoxy resin. Under the bidirectional influence of a magnetic field and gravity, the absorbing and thermally conductive fillers aggregate in different directions of the composite material, achieving an integration of absorption, thermal conductivity, and insulation properties. The double-sided heterogeneous insulating, thermally conductive, and electromagnetically shielding composite material of this application is integrally molded, with no obvious interface between the thermally conductive layer and the absorbing layer, effectively reducing interfacial thermal resistance and facilitating the packaging of radio frequency chips.

[0019] This application achieves a double-sided heterogeneous composite material with excellent wave absorption, thermal conductivity, and insulation properties by mixing simple components and applying magnetic and gravitational fields, and then curing it at room temperature under a press. It has the advantages of simple process, high efficiency, and good controllability. Attached Figure Description

[0020] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 Scanning electron microscope image of magnetic ellagic acid nanofiber precursor; Figure 2 Scanning electron microscope image of magnetic ellagic acid carbon nanofibers; Figure 3 The graph shows the test results of magnetic metal content in magnetic ellagic acid carbon nanofibers. Figure 4 The graph shows the test results of the microwave absorption performance of the double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material. Figure 5 The resistivity test results are shown in the figure for the double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material. Figure 6 The figure shows the test results of the in-plane thermal conductivity of the double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material. Figure 7 The figure shows the vertical thermal conductivity test results of the double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material. Detailed Implementation

[0022] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.

[0023] In the following description of this embodiment, the terms "including", "comprising", "having", and "containing" are all open-ended terms, meaning that they include but are not limited to.

[0024] In the following description of this embodiment, the term "and / or" is used to describe the association relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, B existing alone, and A and B existing simultaneously. A and B can be singular or plural. The character " / " generally indicates that the preceding and following related objects have an "or" relationship.

[0025] In the following description of this embodiment, the term "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0026] The terminology used in the embodiments of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of this application. The singular forms "a" and "the" as used in the embodiments of this application and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise.

[0027] Those skilled in the art should understand that, in the following description of the embodiments of this application, the sequence of numbers does not imply the order of execution. Some or all steps may be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.

[0028] Those skilled in the art will understand that the numerical ranges in the embodiments of this application should be understood as each intermediate value between the upper and lower limits of the specifically disclosed range. Each smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this application. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0029] Unless otherwise stated, the technical / scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains. While this application describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this application. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0030] This application provides a method for preparing a double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material. Magnetic ellagic acid is used as a microwave absorbing filler, and spherical boron nitride is used as a thermally conductive filler. Under the combined action of a magnetic field and a gravitational field, the thermally conductive filler and the microwave absorbing filler are aggregated in different directions to obtain the double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material. Specifically, the method includes the following steps: S1, add ellagic acid solution and nickel ion-containing solution to a mixed solvent to prepare a reaction solution, and stir at room temperature for 6-24 hours to obtain a suspension; The suspension was centrifuged to collect the solid phase, which was then washed and dried to obtain the precursor. Specifically, methylpyrrolidone and deionized water are mixed and ultrasonicated for 5-15 minutes. Then, ammonia is added at room temperature and stirred for 3-5 minutes to obtain a homogeneous and transparent mixed solvent. The mixed solvent, by volume percentage, comprises 0-62% methylpyrrolidone, 38-100% deionized water, and 0.051% ammonia.

[0031] In this application, the ellagic acid solution is a methylpyrrolidone solution of ellagic acid with a concentration of 20 mg / mL, which is a brown, transparent, and homogeneous solution.

[0032] The nickel ion-containing solution is an aqueous solution of nickel chloride with a nickel ion concentration of 60 mg / mL. It is a green, transparent, and homogeneous solution.

[0033] Specifically, ellagic acid solution and nickel ion-containing solution are added to a mixed solvent to prepare a reaction solution; the mixture is stirred at a constant speed at room temperature for 6-24 hours to obtain a homogeneous and stable dark green suspension. The suspension is centrifuged at 14000 r / min for 5-10 min and then washed 2-4 times with deionized water to obtain the magnetic ellagic acid nanofiber precursor.

[0034] In this application, the mass ratio of nickel ions to ellagic acid in the reaction solution is 10~35:90~65, preferably 28.23:71.77; the volume ratio of methylpyrrolidone to deionized water is 20~80:80~20, preferably 60:40. Specifically, the concentration of ellagic acid in the reaction solution is 3 mg / mL; the concentration of nickel ions is 0.4~1.6 mg / mL, preferably 1.18 mg / mL; and the volume fraction of ammonia in the reaction solution is 0.044%.

[0035] In this application, under the influence of ammonia, polyphenols form more quinone structures, which exhibit a stronger delocalized π-electron effect and tend to form ordered π-π stacking structures. This long-range ordered structure is beneficial for the dissipation of electromagnetic waves. Meanwhile, the metal ion coordinating groups of ellagic acid are located outside the molecular ring, and the doping of metal ions does not disrupt the long-range ordered structure of ellagic acid fibers.

[0036] S2, the precursor is heat-treated in a nitrogen atmosphere to obtain magnetic ellagic acid carbon nanofibers; the heat treatment specifically involves: In a nitrogen atmosphere, the precursor is heated to 900°C at a heating rate of 2-5°C / min and held at that temperature for 1-3 hours; then cooled to room temperature at a cooling rate of 2-5°C / min.

[0037] Further heat treatment leads to the formation of more graphite phase structures, oxygen vacancies, and electron holes in ellagic acid nanofibers. Simultaneously, their long-range ordered π-π packing structure is well preserved after heat treatment, which enhances the material's dielectric loss capability. Furthermore, during heat treatment, carbon reduces magnetic metal ions in situ at high temperatures, forming magnetic metal particles. These magnetic metal particles are confined within the one-dimensional nanofibers and exhibit magnetic coupling under an electromagnetic field, resulting in strong magnetic loss performance. Therefore, after heat treatment, magnetic ellagic acid carbon nanofibers possess strong dielectric and magnetic loss properties, effectively dissipating electromagnetic waves.

[0038] S3, the magnetic ellagic acid carbon nanofibers, spherical boron nitride, epoxy resin and curing agent are mixed evenly and then pressed and cured in a magnetic field to obtain a double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material.

[0039] In this application, based on the total amount of magnetic ellagic acid carbon nanofibers, spherical boron nitride, epoxy resin, and curing agent, the amount of magnetic ellagic acid carbon nanofibers is 5-25 wt% of the total amount, the amount of spherical boron nitride is 10-50 wt% of the total amount, and the remainder is epoxy resin and curing agent; wherein, the mass ratio of epoxy resin to curing agent is 1-3:1.

[0040] In this application, the spherical boron nitride is granulated boron nitride with a particle size of 25 micrometers. In the embodiments of this application, Brofos-BN type boron nitride from Bonavis Nanotechnology Co., Ltd. is selected.

[0041] The curing agent is a low-viscosity epoxy resin curing agent. In this embodiment, the CEH500 epoxy resin curing agent from Guangzhou Metallographic Instrument Equipment Co., Ltd. is selected.

[0042] In this application, magnetic ellagic acid carbon nanofibers, spherical boron nitride, epoxy resin, and curing agent are mixed evenly and placed in a mold. A bar magnet is then placed on top of the mold to create a magnetic field. The mold is made of a non-magnetic material, preferably polytetrafluoroethylene (PTFE).

[0043] In this application, the pressing and curing temperature is room temperature, the pressure is 5~10 MPa, and the holding time is 5~12 h.

[0044] This application achieves the aggregation of microwave absorbing fillers and thermally conductive fillers in different directions of the composite material through simple component mixing and the bidirectional action of magnetic and gravitational fields, thus integrating microwave absorption, thermal conductivity and insulation properties. The double-sided heterogeneous composite material with excellent microwave absorption, thermal conductivity and insulation properties can be obtained by room temperature curing under a press. It has the advantages of simple process, high efficiency and good controllability.

[0045] The double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material of this application is integrally molded, with no obvious interface between the thermally conductive layer and the wave-absorbing layer, which can effectively reduce the interface thermal resistance. It exhibits excellent wave absorption, thermal conductivity, and insulation properties, with a reflection loss value reaching -53dB, and an internal thermal conductivity of 8.3W / (m²) on the boron nitride enriched side. K), the vertical thermal conductivity can reach 7.4 W / (m). K); The resistivity of one side of the boron nitride enrichment can reach 4×10⁻⁶. ^ 14 Ω cm, which can be used for chip packaging.

[0046] The present application will be further described below through specific embodiments.

[0047] Example 1 This embodiment provides a method for preparing magnetic ellagic acid carbon nanofibers, including the following steps: S1, Methylpyrrolidone, deionized water and ammonia are mixed, ultrasonicated for 10 min and stirred for 3 min to obtain a mixed solvent; wherein the volume fraction of methylpyrrolidone is 53.8%, the volume fraction of deionized water is 46.2% and the volume fraction of ammonia is 0.051%.

[0048] Ellagic acid powder was added to methylpyrrolidone solvent and sonicated for 5 minutes to prepare an ellagic acid solution with a concentration of 20 mg / mL.

[0049] Add nickel chloride crystals to deionized water and sonicate for 5 minutes to prepare a nickel chloride solution with a nickel ion concentration of 60 mg / mL.

[0050] S2, ellagic acid solution and nickel chloride solution are added to a mixed solvent to prepare a reaction liquid; wherein, the concentration of ellagic acid in the reaction liquid is 3 mg / mL, the concentration of nickel ions is 1.18 mg / mL, and the volume fraction of ammonia is 0.044%; at this time, the volume fractions of methylpyrrolidone and deionized water in the reaction liquid are 60% and 40%, respectively, and nickel ions account for 28.23% of the total mass of nickel ions and ellagic acid in the reaction liquid, while ellagic acid accounts for 71.77% of the total mass of nickel ions and ellagic acid.

[0051] The reaction solution was stirred at 500 rpm at room temperature to obtain a suspension; the suspension was centrifuged at 14000 r / min for 5 min to collect the solid phase, washed three times with deionized water, and freeze-dried to obtain magnetic ellagic acid nanofiber precursor, wherein the freeze-drying conditions were a vacuum degree of less than 40 Pa and a cold trap temperature of less than -50 °C. S4. The precursor was placed in a tube furnace under a nitrogen atmosphere and heated to 900°C at a heating rate of 5°C / min, and held at that temperature for 2 hours. Then it was cooled to room temperature at a cooling rate of 5°C / min to obtain magnetic ellagic acid carbon nanofibers.

[0052] Examples 1-1 to 1-9 The preparation methods of Examples 1-1 to 1-9 are the same as those of Example 1. The difference between Examples 1 and Example 1 is that the process parameters are different, as shown in Table 1.

[0053] Table 1. Process parameters for Examples 1-1 to 1-9

[0054] Example 2 This embodiment provides a method for preparing a double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material, including the following steps: 0.2g of the magnetic ellagic acid carbon nanofibers prepared in Example 1, 0.5g of spherical boron nitride, 0.2g of epoxy resin, and 0.1g of epoxy resin curing agent (model CEH500) were mixed evenly and filled into a mold. A bar magnet was placed above the mold, and a pressure of 7.5MPa was applied under a press. The mixture was cured at room temperature for 8 hours to obtain a double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material. It is a circular disc with a diameter of 12mm and a thickness of 1mm.

[0055] Examples 2-1 to 2-8 Examples 2-1 to 2-8 are prepared in the same way as Example 2, except that the process parameters are different, as shown in Table 2.

[0056] Table 2 Process parameters for Examples 2-1 to 2-8

[0057] The magnetic ellagic acid nanofiber precursor, magnetic ellagic acid carbon nanofiber, and double-sided heterogeneous insulating thermally conductive-electromagnetic shielding composite material prepared in this application were characterized as follows: 1. Microscopic morphological characterization The magnetic ellagic acid nanofiber precursor obtained in step S2 of Example 1 was subjected to microscopic morphology testing, and its scanning electron microscope image is shown below. Figure 1 As shown. From Figure 1 It can be seen that it has a good nanofiber morphology.

[0058] Scanning electron microscope image of the magnetic ellagic acid carbon nanofibers prepared in Example 1 is shown below. Figure 2 As shown. From Figure 2 It can be seen that the magnetic ellagic acid carbon nanofibers obtained after heat treatment of the precursor still maintain good nanofiber morphology.

[0059] 2. Performance Characterization The magnetic ellagic acid carbon nanofibers prepared in Examples 1, 1-1 to 1-3 were characterized for their magnetic metal content, and the results are as follows: Figure 3 As shown. From Figure 3 It can be seen that as the amount of nickel ions added increases, the metal loading of magnetic carbon nanofibers first increases and then decreases. When the mass fractions of nickel ions and ellagic acid in the reaction solution are 28.23% and 71.77% respectively, the magnetic metal loading in magnetic ellagic acid carbon nanofibers is the highest.

[0060] The properties of the double-sided heterogeneous insulating thermally conductive-electromagnetic shielding composite materials prepared in Examples 2, 2-1 to 2-8 were characterized as follows: 2.1 Absorption Performance Test The microwave absorption of the double-sided heterogeneous insulating thermally conductive-electromagnetic shielding composite materials prepared in Examples 2 and 2-1 to 2-4 was tested using a vector network analyzer. Specifically, the composite material was processed into a coaxial ring with an outer diameter of 7 mm, an inner diameter of 3.02 mm, and a thickness of 2 mm. The microwave absorption efficiency of the material was tested using the coaxial method, and the results are as follows: Figure 4 As shown.

[0061] from Figure 4It is known that the double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material of this application has good microwave absorption performance. Moreover, as the mass fraction of magnetic ellagic acid carbon nanofiber increases, the microwave absorption efficiency of the composite material first increases and then decreases (the sample thickness is 2 mm when calculating the reflection loss value). Among them, the microwave absorption performance is the best when the content of magnetic ellagic acid carbon nanofiber microwave absorbing filler is 20 wt%, and its reflection loss value can reach -53 dB.

[0062] 2.2 Resistivity Test The resistivity of the double-sided heterogeneous insulating thermally conductive-electromagnetic shielding composite materials prepared in Examples 2 and 2-1 to 2-4 was measured using an ultra-high resistivity microcurrent tester. The test surface was the side enriched with boron nitride. The results are as follows: Figure 5 As shown. From Figure 5 It can be seen that as the amount of magnetic ellagic acid carbon nanofibers added increases, their surface resistivity gradually decreases, and overall, they meet the requirements for chip packaging. When the mass fraction of ellagic acid carbon nanofibers is greater than 20%, their resistivity decreases significantly, reaching a minimum of 4 × 10⁻⁶. 14 Ω cm.

[0063] 2.3 Thermal conductivity test The in-plane thermal conductivity and vertical thermal conductivity of the double-sided heterogeneous insulating thermally conductive-electromagnetic shielding composite materials prepared in Examples 2, 2-5 to 2-8 were tested. When testing the in-plane thermal conductivity, the test surface was the one enriched in boron nitride. The test results are as follows: Figure 6 and Figure 7 As shown. From Figure 6 , Figure 7 It can be seen that the above-mentioned double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite materials all have good thermal conductivity. With the increase of the amount of spherical boron nitride added, both the in-plane thermal conductivity and the vertical thermal conductivity increase. When the mass fraction of spherical boron nitride is 50%, it exhibits the best thermal conductivity, with the highest in-plane thermal conductivity reaching 8.3 W / (m²). The vertical thermal conductivity can reach up to 7.4 W / (m²). K).

[0064] In this application, the double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material prepared in Example 2 has the best overall performance.

[0065] Although this application has been described in detail in this specification with general descriptions and specific embodiments, some modifications or improvements can be made to it, which will be obvious to those skilled in the art. Therefore, such modifications or improvements made without departing from the spirit of this application are all within the scope of protection claimed in this application.

Claims

1. A method for preparing a double-sided hetero-insulating thermally-conductive and electromagnetic-shielding composite material, characterized in that, Includes the following steps: S1, ellagic acid solution and nickel ion-containing solution are added to a mixed solvent to prepare a reaction solution, and the reaction is stirred to obtain a suspension; The suspension was centrifuged to collect the solid phase, which was then washed and dried to obtain the precursor. S2, the precursor is heat-treated in a nitrogen atmosphere to obtain magnetic ellagic acid carbon nanofibers. S3, the magnetic ellagic acid carbon nanofibers, spherical boron nitride, epoxy resin and curing agent are mixed evenly and then pressed and cured in a magnetic field to obtain a double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material.

2. The preparation method according to claim 1, characterized in that, The mixed solvent, by volume percentage, comprises 0-62% methylpyrrolidone, 38-100% deionized water, and 0.051% ammonia. The ellagic acid solution is a methylpyrrolidone solution of ellagic acid with a concentration of 20 mg / mL; The nickel ion-containing solution is an aqueous solution of nickel chloride, with a nickel ion concentration of 60 mg / mL.

3. The preparation method according to claim 1, characterized in that, The mass ratio of nickel ions to ellagic acid in the reaction solution is 10~35:90~65; The volume ratio of methylpyrrolidone to deionized water is 20~80:80~20.

4. The preparation method according to claim 3, characterized in that, The reaction solution contains ellagic acid at a concentration of 3 mg / mL, nickel ions at a concentration of 0.4–1.6 mg / mL, and ammonia at a volume fraction of 0.044%.

5. The preparation method according to claim 1, characterized in that, The reaction described in S1 is carried out at room temperature for 6 to 24 hours. The heat treatment described in S2 specifically refers to: The temperature is increased to 900℃ at a rate of 2~5℃ / min and held for 1~3 hours; then it is cooled to room temperature at a rate of 2~5℃ / min.

6. The preparation method according to claim 1, characterized in that, The amount of magnetic ellagic acid carbon nanofibers, spherical boron nitride, epoxy resin and curing agent is 5-25 wt% of the total amount, the amount of spherical boron nitride is 10-50 wt% of the total amount, and the remainder is epoxy resin and curing agent. The mass ratio of the epoxy resin to the curing agent is 1~3:1; The curing agent is a low-viscosity epoxy resin curing agent.

7. The preparation method according to claim 1, characterized in that, A magnetic field is formed by uniformly mixing magnetic ellagic acid carbon nanofibers, spherical boron nitride, epoxy resin and curing agent and placing them in a mold, and then placing a bar magnet on top of the mold.

8. The preparation method according to claim 1, characterized in that, The pressing and curing temperature is room temperature, the pressure is 5~10 MPa, and the holding time is 5~12 hours.

9. The double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material prepared by the preparation method according to any one of claims 1-8.

10. The application of the double-sided heterogeneous insulating thermally conductive electromagnetic shielding composite material as described in claim 9 in chip packaging.