A storage-stable acrylic epoxy resin for PCB via plugging and its preparation method
By dual-blocking of imidazole activity through covalent and ionic bonds, and combining imidazole carboxylate polyurethane prepolymer with anhydride curing agent, a dual curing mode of UV pre-curing and thermal curing deep crosslinking is formed, which solves the problem of insufficient storage stability of epoxy acrylate resin and achieves ultra-long storage period and high performance PCB via plugging process applicability.
Patent Information
- Application Number
- CN202611286604.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing epoxy acrylate resins have insufficient storage stability during storage. Existing modification schemes are cumbersome to operate, have complex processes, or cannot achieve a dual curing mode of UV pre-curing and thermal curing, which cannot meet the high aspect ratio hole filling requirements of PCB plugging process.
By doubly blocking the activity of imidazole through covalent and ionic bonds, and combining imidazole carboxylate polyurethane prepolymer with anhydride curing agent, a dual curing mode of UV pre-curing and thermal curing deep crosslinking is formed. The crosslinking network is formed by imidazole thermocatalyzing anhydride-epoxy ring-opening polymerization and isocyanate group reaction.
It achieves an ultra-long room temperature storage period, simplifies the preparation process, avoids resin collapse and shrinkage stress, improves crack resistance and heat resistance, is suitable for PCB via plugging process, and is compatible with existing production processes.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of resin technology and relates to a storage-stable acrylic epoxy resin for PCB via plugging and its preparation method. Background Technology
[0002] Epoxy acrylate resins combine the excellent adhesion and chemical resistance of epoxy resins with the rapid crosslinking properties of acrylates through photocuring / thermal curing, making them widely used in PCB via-filling inks, coatings, adhesives, and 3D printing. However, epoxy acrylate resins often face the problem of insufficient storage stability during storage.
[0003] To improve storage stability, existing technologies have explored various technical approaches:
[0004] Two-component packaging: The epoxy resin and curing agent are stored separately and mixed before use. While this method can extend the shelf life, it increases the complexity of the process, can lead to inconsistent mixing ratios, and the usable time after mixing is still limited.
[0005] Microencapsulation with physical isolation: The active curing agent is encapsulated inside a polymer shell, physically isolated from the resin matrix at room temperature. Upon heating, the shell ruptures, releasing the curing agent. For example, patent CN114773577B discloses a method for preparing a self-assembled microcapsule epoxy resin latent curing agent, which involves a three-step reaction of addition of a double-bonded silane coupling agent to imidazole, salt formation, and hydrolytic polymerization of siloxane to obtain microcapsules.
[0006] Imidazole chemical modification: By modifying imidazole, its active sites are blocked. For example, the article "Preparation and Performance Study of Long-Storage Flame-Retardant Epoxy / Imidazole Latent System" systematically studied the activity of blocking the nitrogen atom at the 3 position in 2-phenylimidazolium and 2-ethyl-4-methylimidazolium by 2-carboxyethylphenylphosphine acid (HPP), and synthesized latent phosphorus-containing imidazole curing agents PHI-HPP and EMI-HPP. The single-component system composed of epoxy resin E51 achieved a room temperature storage period of 91 days and 84 days, respectively, and a gel time of less than 6 minutes at 150℃, while also having a UL-94 V-0 flame retardant rating. In addition, the article "Synthesis and Properties of an Imidazole Urea-Coordination Dual-Dynamic Cross-Linked Latent Accelerator and Its Recyclable One-Component Epoxy Resin. Macromolecules, 2025, 58 (17)" uses imidazole urea bonds to bind with Zn 2+Coordination bonds construct a dual dynamic cross-linking network, firmly anchoring imidazole in the three-dimensional network, enabling the single-component epoxy system to have a room temperature storage period of over 90 days and a curing degree of 84% within 45 minutes at 120°C.
[0007] The aforementioned technical approaches all improve the storage stability of epoxy acrylate resins to some extent, but each still has its limitations. Two-component dispensing is cumbersome and has a short usable time after mixing; microencapsulation can achieve a longer shelf life, but the preparation process is complex, and shell residue may affect the electrical properties of the cured product; while imidazole chemical modification can block imidazole activity at the molecular level, existing reports mostly focus on a single locking mechanism or a single curing mode, and there is no systematic design that integrates dual locking of covalent and ionic bonds, the introduction of UV-curable double bonds, and in-situ toughening of polyurethane prepolymers into the same molecular system. Existing modified imidazole products do not incorporate UV curing functionality into their molecular design, making it impossible to achieve a dual curing mode of UV pre-curing and deep cross-linking through thermosetting, which is precisely the key requirement for filling high aspect ratio holes in PCB via plugging processes.
[0008] Therefore, developing an acrylic epoxy resin for PCB via plugging that has an ultra-long room temperature storage period, UV / thermal dual curing capability, simple preparation process, and does not require microencapsulation has significant industrial value and application prospects. Summary of the Invention
[0009] The purpose of this invention is to provide a storage-stable acrylic epoxy resin for PCB via plugging and its preparation method. It achieves long-term storage at room temperature by dual blocking of imidazole activity through covalent and ionic bonds, and utilizes double bonds to achieve UV pre-curing and shaping. At the same time, it achieves dual curing by forming a double crosslinking network through imidazole thermocatalytic anhydride-epoxy ring-opening polymerization and the reaction of residual isocyanate groups with hydroxyl groups in the system, thereby achieving dual curing of UV pre-curing and thermo-curing deep crosslinking.
[0010] The objective of this invention can be achieved through the following technical solutions:
[0011] In a first aspect, the present invention provides a storage-stable acrylic epoxy resin for plugging PCB vias, comprising, by weight, the following components:
[0012] The resin component comprises 20-30 parts of acrylic-modified epoxy resin and 40-60 parts of epoxy resin; the acrylic-modified epoxy resin is an epoxy resin containing acrylate double bonds in its molecular chain, preferably bisphenol A type epoxy diacrylate; the epoxy resin is bisphenol A type epoxy resin or bisphenol F type epoxy resin.
[0013] The curing system comprises 5-10 parts of imidazole carboxylate polyurethane prepolymer and 5-10 parts of acid anhydride curing agent;
[0014] The preparation method of the imidazole carboxylate polyurethane prepolymer includes the following steps:
[0015] (a) Isoethyl methacrylate (IEM) is reacted with imidazole at a molar ratio of 1:1.1-1.2 at 40-60°C for 2-4 hours to generate 1-imidazolium carbonylamino-2-ethyl methacrylate; in this reaction, the isocyanate group on the IEM molecule undergoes a nucleophilic addition reaction with the NH at the 1-position of the imidazole ring to form an imidazole-terminated product containing a urea bond, while the methacrylate double bond is retained on the molecule;
[0016] (b) The product of step (a) is reacted with dimethylolpropionic acid (DMPA) at a molar ratio of 1:1 at 50-60°C for 6-12 hours to form a salt. The nitrogen atom at the 3 position of the imidazole ring forms an imidazole-carboxylate ion pair with the carboxyl group of DMPA, thereby blocking the catalytic activity of imidazole.
[0017] (c) The salt-forming product from step (b) is reacted with the diisocyanate-polyethylene glycol prepolymer at 60-80°C for 3-5 hours. The two hydroxyl groups of DMPA react with the isocyanate groups of the diisocyanate, thereby embedding the salt-forming product into the polyurethane backbone.
[0018] The anhydride curing agent is selected from at least one of methylhexahydrophthalic anhydride and methyltetrahydrophthalic anhydride.
[0019] 15-40 parts of inorganic filler, wherein the inorganic filler is silica surface-modified with an epoxy silane coupling agent, and the epoxy silane coupling agent is γ-glycidoxypropyltrimethoxysilane (KH-560).
[0020] 3-5 parts of reactive diluent, wherein the reactive diluent is a compound containing at least two acrylate double bonds, selected from at least one of tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, and trimethylolpropane triacrylate.
[0021] 1-3 parts of photoinitiator, wherein the photoinitiator is selected from at least one of 2-hydroxy-2-methyl-1-phenylpropanone (photoinitiator 1173), 1-hydroxycyclohexylphenyl ketone (photoinitiator 184), and 2,4,6-trimethylbenzoyl diphenylphosphine oxide (TPO).
[0022] 1-2 parts of additives, wherein the additives include at least one of silicone leveling agents and silicone defoamers.
[0023] The solvent is 10-15 parts, and the solvent includes propylene glycol methyl ether acetate.
[0024] In this invention, the imidazole carboxylate chain-extended polyurethane prepolymer simultaneously performs multiple functions: Firstly, the imidazole activity is dually locked by the urea bond (covalent bond) formed by the reaction of IEM with imidazole and the carboxylate formed by DMPA with the nitrogen atom at the 3-position of the imidazole ring, thereby causing it to lose its ability to catalyze the epoxy-anhydride reaction at room temperature and improving storage stability.
[0025] Secondly, the methacrylate double bonds retained on the IEM molecule can participate in UV free radical polymerization under the action of photoinitiators and be grafted during the pre-curing of the plugging resin.
[0026] Third, when heated, it releases imidazole, which catalyzes the ring-opening polymerization reaction between the acid anhydride and the epoxy group to form an epoxy-acid anhydride thermal crosslinking network. This provides the main crosslinking structure for the pore-sealing resin, giving the cured product a high glass transition temperature, excellent heat resistance, and mechanical strength.
[0027] Fourth, the end isocyanates of the polyurethane main chain of the prepolymer and the isocyanates of the IEM react with a large number of hydroxyl groups generated in situ by the ring-opening reaction of epoxy-anhydride under heating conditions to form a polyurethane crosslinking network, thereby achieving in-situ toughening of the cured product and enhancing the chemical connection between resins.
[0028] Secondly, the present invention also provides a method for preparing a storage-stable acrylic epoxy resin for PCB via plugging, comprising the following steps:
[0029] (1) Add acrylic modified epoxy resin, epoxy resin, reactive diluent, additives and solvent to a dispersion vessel according to the formula, stir evenly to obtain resin premix;
[0030] (2) Add imidazole carboxylate chain-extended polyurethane prepolymer, acid anhydride curing agent, photoinitiator and inorganic filler to the resin premix and stir until uniform;
[0031] (3) Grind the mixture from step (2) 2-3 times using a three-roll mill until the fineness is ≤15μm;
[0032] (4) Transfer the ground material to a vacuum degassing machine and degas it to no bubbles at a vacuum of -0.095MPa to obtain a stable acrylic epoxy resin for PCB via plugging.
[0033] The beneficial effects of this invention are as follows:
[0034] (1) In this invention, an imidazole-urea bond is formed by the reaction of isocyanate ethyl methacrylate with imidazole. At the same time, the carboxyl group of dimethylolpropionic acid forms a salt with the nitrogen atom at the 3-position of the imidazole ring, thus constructing a dual active blockade, which effectively inhibits the catalytic activity of imidazole at room temperature, so that the composition can be stored stably at room temperature for ≥3 months without the need for low-temperature refrigeration, which greatly extends the storage period and reduces storage and transportation costs.
[0035] (2) This invention embeds the IEM-imidazolium-DMPA salt product into the polyurethane backbone. The double bonds of methacrylate retained on the IEM molecule are used to achieve double bond grafting during UV pre-curing under the action of photoinitiator. At the same time, after heating, the imidazolium gradually releases to catalyze the ring-opening polymerization of acid anhydride and epoxy groups, achieving deep cross-linking through thermo-curing. This forms a dual curing mode of UV pre-curing shaping and deep cross-linking through thermo-curing, which effectively avoids the problems of resin collapse and large shrinkage stress when filling high aspect ratio holes in PCB plugging process. Meanwhile, the isocyanate groups remaining in the prepolymer react with the hydroxyl groups generated in situ by the epoxy-acid anhydride ring-opening reaction to form a polyurethane cross-linking network, achieving in-situ toughening of the cured product. While maintaining high Tg (≥150℃), it improves crack resistance. Moreover, the preparation process is simple, does not require microencapsulation, and is compatible with existing PCB ink production processes and equipment. Detailed Implementation
[0036] To further illustrate the technical means and effects of the present invention in achieving the intended purpose, the following detailed description of the specific implementation methods, structures, features and effects of the present invention, in conjunction with preferred embodiments, is provided below.
[0037] Example 1
[0038] A method for preparing a storage-stable acrylic epoxy resin for PCB via plugging includes the following steps:
[0039] Weigh each component according to the following parts by weight:
[0040] Bisphenol A type epoxy diacrylate (RJ313): 25 parts
[0041] Bisphenol A type epoxy resin (E51, epoxy equivalent 210-230 g / eq): 50 parts
[0042] Imidazole carboxylate polyurethane prepolymer: 8 parts
[0043] Methylhexahydrophthalic anhydride (MHHPA): 8 parts
[0044] KH-560 modified spherical silica: 25 parts
[0045] Tripropylene glycol diacrylate (TPGDA): 4 parts
[0046] Photoinitiator 1173: 3 parts
[0047] Organosilicon leveling agent (BYK-333): 0.5 parts
[0048] Silicone defoamer (BYK-019): 0.5 parts
[0049] Propylene glycol methyl ether acetate (PMA): 10 parts
[0050] Preparation method:
[0051] Bisphenol A type epoxy diacrylate, bisphenol A type epoxy resin, tripropylene glycol diacrylate, BYK-333, BYK-019, and propylene glycol methyl ether acetate were added to a dispersion vessel and stirred at 500 rpm for 30 minutes at 50°C to obtain a resin premix. Imidazole carboxylate chain-extended polyurethane prepolymer, methyl hexahydrophthalic anhydride, photoinitiator 1173, and KH-560 modified spherical silica were added to the resin premix, and the mixture was stirred at 600 rpm for 50 minutes at 40°C. The mixture was then ground using a three-roll mill to a fineness ≤15 μm. The ground material was transferred to a vacuum degassing machine and degassed under a vacuum of -0.095 MPa until no bubbles were present, yielding a storage-stable acrylic epoxy resin for PCB via plugging.
[0052] The preparation of imidazole carboxylate polyurethane prepolymer:
[0053] 7.5 g of imidazole was dissolved in a mixed solvent of 20 g dimethylformamide and 20 g xylene to obtain an imidazole solution. 15 g of isocyanate methacrylate was added dropwise to the imidazole solution, and the reaction was carried out at 60 °C for 2 hours. The reaction was monitored by TLC to determine the end of the reaction, yielding a solution of 1-imidazolium carbonylamino-2-ethyl methacrylate. Infrared spectroscopy analysis was performed at 1645-1679 cm⁻¹. -1 An absorption peak for the stretching vibration of C=O in the urea bond appears at the location.
[0054] The above solution was mixed with 13g of dimethylolpropionic acid (DMPA) at 60°C and reacted to form a salt for 8 hours. 14g of isophorone diisocyanate (IPDI) and 8g of polyethylene glycol 400 (PEG400) were prepolymerized at 70°C for 2 hours to obtain an NCO-terminated prepolymer. The above salt-forming product was added to the prepolymer and reacted at 70°C for 4 hours to obtain an imidazole carboxylate polyurethane prepolymer.
[0055] The preparation of modified silica includes:
[0056] Silica was placed in a high-speed mixer, and an ethanol-water solution of γ-glycidoxypropyltrimethoxysilane (KH-560) (KH-560 to ethanol-water mass ratio of 1:5, ethanol:water = 3:1) was sprayed in, accounting for 9% of the weight of silica. The mixture was then stirred at high speed at 90°C for 4 hours to obtain spherical silica modified with KH-560.
[0057] Example 2
[0058] A method for preparing a storage-stable acrylic epoxy resin for PCB via plugging includes the following steps:
[0059] Weigh each component according to the following parts by weight:
[0060] Bisphenol A type epoxy diacrylate (RJ313): 25 parts
[0061] Bisphenol A type epoxy resin (E51, epoxy equivalent 210-230 g / eq): 50 parts
[0062] Imidazole carboxylate polyurethane prepolymer: 8 parts
[0063] Methyltetrahydrophthalic anhydride: 8 parts
[0064] KH-560 modified spherical silica: 15 parts
[0065] Tripropylene glycol diacrylate (TPGDA): 4 parts
[0066] Photoinitiator 1173: 3 parts
[0067] Organosilicon leveling agent (BYK-333): 0.5 parts
[0068] Silicone defoamer (BYK-019): 0.5 parts
[0069] Propylene glycol methyl ether acetate (PMA): 15 parts
[0070] Preparation method:
[0071] Bisphenol A type epoxy diacrylate, bisphenol A type epoxy resin, tripropylene glycol diacrylate, BYK-333, BYK-019, and propylene glycol methyl ether acetate were added to a dispersion vessel and stirred at 500 rpm for 30 minutes at 50°C to obtain a resin premix. Imidazole carboxylate polyurethane prepolymer, methyltetrahydrophthalic anhydride, photoinitiator 1173, and KH-560 modified spherical silica were added to the resin premix, and the mixture was stirred at 600 rpm for 60 minutes at 40°C. The mixture was then ground using a three-roll mill to a fineness ≤15 μm. The ground material was transferred to a vacuum degassing machine and degassed until no bubbles were present under a vacuum of -0.095 MPa to obtain a storage-stable acrylic epoxy resin for PCB via plugging.
[0072] Example 3
[0073] A method for preparing a storage-stable acrylic epoxy resin for PCB via plugging includes the following steps:
[0074] Weigh each component according to the following parts by weight:
[0075] Bisphenol A type epoxy diacrylate (RJ313): 30 parts
[0076] Bisphenol F type epoxy resin (epoxy equivalent 160-180g / eq): 60 parts
[0077] Imidazole carboxylate polyurethane prepolymer: 10 parts
[0078] Methylhexahydrophthalic anhydride (MHHPA): 10 parts
[0079] KH-560 modified spherical silica: 40 parts
[0080] 1,6-Hexanediol diacrylate (HDDA): 4 parts
[0081] Photoinitiator 184: 2 parts
[0082] Organosilicon leveling agent (BYK-333): 1.0 part
[0083] Organosilicon defoamer (BYK-019): 1.0 part
[0084] Propylene glycol methyl ether acetate (PMA): 10 parts
[0085] Preparation method:
[0086] Bisphenol A type epoxy diacrylate, bisphenol F type epoxy resin, 1,6-hexanediol diacrylate, BYK-333, BYK-019, and propylene glycol methyl ether acetate were added to a dispersion vessel and stirred at 500 rpm for 40 minutes at 60°C to obtain a resin premix. Imidazole carboxylate polyurethane prepolymer, methyl hexahydrophthalic anhydride, photoinitiator 184, and KH-560 modified spherical silica were added to the resin premix, and the mixture was stirred at 600 rpm for 50 minutes at 40°C. The mixture was then ground using a three-roll mill to a fineness ≤15 μm. The ground material was transferred to a vacuum degassing machine and degassed until no bubbles were present under a vacuum of -0.095 MPa to obtain a storage-stable acrylic epoxy resin for PCB via plugging.
[0087] Example 4
[0088] A method for preparing a storage-stable acrylic epoxy resin for PCB via plugging includes the following steps:
[0089] Weigh each component according to the following parts by weight:
[0090] Bisphenol A type epoxy diacrylate (RJ313): 20 parts
[0091] Bisphenol A type epoxy resin (E51, epoxy equivalent 210-230 g / eq): 40 parts
[0092] Imidazole carboxylate polyurethane prepolymer: 5 parts
[0093] Methylhexahydrophthalic anhydride (MHHPA): 5 parts
[0094] KH-560 modified spherical silica: 20 parts
[0095] Trimethylolpropane triacrylate (TMPTA): 5 parts
[0096] Photoinitiator TPO: 1 part
[0097] Organosilicon leveling agent (BYK-333): 0.5 parts
[0098] Silicone defoamer (BYK-019): 0.5 parts
[0099] Propylene glycol methyl ether acetate (PMA): 10 parts
[0100] Preparation method:
[0101] Bisphenol A type epoxy diacrylate, bisphenol A type epoxy resin, trimethylolpropane triacrylate, BYK-333, BYK-019, and propylene glycol methyl ether acetate were added to a dispersion vessel and stirred at 500 rpm for 30 minutes at 50°C to obtain a resin premix. Imidazole carboxylate polyurethane prepolymer, methyl hexahydrophthalic anhydride, photoinitiator TPO, and KH-560 modified spherical silica were added to the resin premix, and the mixture was stirred at 600 rpm for 50 minutes at 40°C. The mixture was then ground using a three-roll mill to a fineness ≤15 μm. The ground material was transferred to a vacuum degassing machine and degassed under a vacuum of -0.095 MPa until no bubbles were present, yielding a storage-stable acrylic epoxy resin for PCB via plugging.
[0102] Example 5
[0103] A method for preparing a storage-stable acrylic epoxy resin for PCB via plugging includes the following steps:
[0104] Weigh each component according to the following parts by weight:
[0105] Bisphenol A type epoxy diacrylate (RJ313): 25 parts
[0106] Bisphenol A type epoxy resin (E51, epoxy equivalent 210-230 g / eq): 50 parts
[0107] Imidazole carboxylate polyurethane prepolymer: 8 parts
[0108] Methylhexahydrophthalic anhydride (MHHPA): 8 parts
[0109] KH-560 modified spherical silica: 25 parts
[0110] Tripropylene glycol diacrylate (TPGDA): 3 parts
[0111] Photoinitiator 1173: 3 parts
[0112] Organosilicon leveling agent (BYK-333): 0.5 parts
[0113] Silicone defoamer (BYK-019): 0.5 parts
[0114] Propylene glycol methyl ether acetate (PMA): 10 parts
[0115] Preparation method:
[0116] Bisphenol A type epoxy diacrylate, bisphenol A type epoxy resin, tripropylene glycol diacrylate, BYK-333, BYK-019, and propylene glycol methyl ether acetate were added to a dispersion vessel and stirred at 500 rpm for 30 minutes at 50°C to obtain a resin premix. Imidazole carboxylate polyurethane prepolymer, methyl hexahydrophthalic anhydride, photoinitiator 1173, and KH-560 modified spherical silica were added to the resin premix, and the mixture was stirred at 600 rpm for 50 minutes at 40°C. The mixture was then ground using a three-roll mill to a fineness ≤15 μm. The ground material was transferred to a vacuum degassing machine and degassed under a vacuum of -0.095 MPa until no bubbles were present, yielding a storage-stable acrylic epoxy resin for PCB via plugging.
[0117] Comparative Example 1
[0118] Compared to Example 1, the difference lies in the use of 2-ethyl-4-methylimidazolium instead of the imidazolium carboxylate polyurethane prepolymer. This means the imidazolium is neither locked by carboxylate salt formation nor modified by chain extension of the polyurethane prepolymer. The room temperature storage period is approximately 7 days, indicating that the dual locking of imidazolium activity by urea bonds and carboxylate is key to achieving the long storage period in the imidazolium carboxylate polyurethane prepolymer.
[0119] Comparative Example 2
[0120] Compared to Example 1, the difference lies in that the salt formation step with dimethylolpropionic acid was omitted in the prepolymer preparation; the imidazole was only locked by the urea bond of the IEM, without being locked by the carboxylate ionic bond. The storage period at room temperature was approximately 30 days, indicating that the carboxylate formed by DMPA salt formation has a secondary locking effect on the imidazole activity.
[0121] Comparative Example 3
[0122] Compared to Example 1, the difference lies in the fact that the photoinitiator was omitted in the preparation method, and UV pre-curing was not performed; only thermal curing was performed. After thermal curing, a depression of approximately 8-12 μm appeared on the surface of the plugged hole, indicating that the methacrylate double bonds introduced by IEM achieved UV pre-curing and shaping under the action of the photoinitiator, which is indispensable for preventing resin collapse.
[0123] Comparative Example 4
[0124] Compared to Example 1, the difference lies in that the polyurethane chain extension step (c) is omitted in the prepolymer preparation, and the IEM-imidazolium-DMPA salt-forming product is not incorporated into the polyurethane backbone, but is used directly as an accelerator in the form of a small salt molecule. The room temperature storage period is still ≥3 months (double locking is still effective), but the flexural strength decreases by about 25% after curing, and microcracks appear in the 288℃ heat resistance, indicating that the in-situ toughening function of the polyurethane backbone is lost.
[0125] Comparative Example 5
[0126] Compared to Example 1, the difference lies in that the DMPA salt formation and polyurethane chain extension steps were omitted in the prepolymer preparation, and the IEM-imidazolium product was used directly as an accelerator. The storage period at room temperature was approximately 14 days, and the cured Tg was approximately 140°C. Significant cracking occurred at 288°C, indicating that the dual locking and the polyurethane backbone make irreplaceable contributions to both the storage period and the post-cured performance.
[0127] Performance testing:
[0128] 1. Storage period at room temperature
[0129] Following ASTM D2196, the pore-filling resin compositions prepared in the examples and comparative examples were sealed in brown bottles and stored in a constant temperature and humidity chamber at 25°C. Rotational viscosity was measured periodically. The time required for the viscosity to increase to 150% of the initial viscosity was recorded.
[0130] 2. The surface of the plug hole is concave.
[0131] The pore-filling resin composition was screen-printed into the through-holes of an FR-4 test plate with a pore size of 0.2 mm and a plate thickness of 1.0 mm, and then pre-cured by UV exposure (365 nm, exposure dose 500 mJ / cm). 2 Then, heat-cur at 130℃ for 45 minutes. The height difference between the plugged hole surface and the substrate surface was measured using an optical profilometer.
[0132] 3. Glass transition temperature (Tg) and coefficient of thermal expansion (CTE)
[0133] According to GB / T 36800.2-2018 standard, after the pore-filling resin composition is cured according to the curing process, samples of appropriate size are cut to determine the glass transition temperature and coefficient of thermal expansion.
[0134] 4. Heat resistance
[0135] Referring to the IPC-TM-650 2.6.8 standard, the via-filling resin composition was filled into the PCB vias and cured according to the curing process. The test sample was then floated in a 288°C solder bath.
[0136] 5. Bending strength
[0137] According to GB / T 9341-2008 standard, after the pore-filling resin composition is cured according to the curing process, a standard bending test strip (80mm×10mm×4mm) is prepared. A three-point bending test is performed using a universal testing machine, the maximum bending force is recorded, and the bending strength is calculated.
[0138]
[0139] The room temperature storage period of Examples 1-5 is ≥3 months. The room temperature storage period of Comparative Examples 1 and 2 is too short (7 days and 30 days), and the samples have gelled before curing, so the performance test after curing cannot be completed. Comparative Example 3 has increased surface depression of the plug hole due to lack of UV pre-curing, but other properties are basically the same as those of Example 1. The flexural strength of Comparative Example 4 decreased by 25%, and microcracks appeared in the heat resistance at 288℃. All properties of Comparative Example 5 are inferior to those of Example 1.
[0140] This invention achieves a viscosity increase of no more than 50% of the initial viscosity after storage at room temperature for ≥3 months, eliminating the need for low-temperature refrigeration, significantly extending the shelf life and reducing storage and transportation costs. Simultaneously, by embedding the IEM-imidazole-DMPA salt product as a chain extender into the polyurethane backbone, and utilizing the methacrylate double bonds retained on the IEM molecule under the action of a photoinitiator to achieve UV pre-curing and shaping, the imidazole gradually releases upon heating, catalyzing the ring-opening polymerization of the anhydride and epoxy groups to achieve thermosetting deep crosslinking. This forms a dual curing mode of UV pre-curing and thermosetting deep crosslinking, avoiding the problems of resin collapse and high shrinkage stress during high aspect ratio hole filling in PCB via plugging processes. Furthermore, the residual isocyanate groups in the prepolymer react with the large number of hydroxyl groups generated in situ by the epoxy-anhydride ring-opening reaction to form a polyurethane crosslinking network, achieving in-situ toughening of the cured product. While maintaining a high Tg (≥150℃), it improves crack resistance. Moreover, the preparation process is simple, requires no microencapsulation, and is highly compatible with existing PCB ink production processes and equipment, making it suitable for industrial production.
[0141] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A storage-stable acryl-epoxy resin for PCB jack, characterized by, Based on parts by weight, it comprises the following components: The resin component comprises 20-30 parts of acrylic-modified epoxy resin and 40-60 parts of epoxy resin; The curing system comprises 5-10 parts of imidazole carboxylate polyurethane prepolymer and 5-10 parts of acid anhydride curing agent; 15-40 parts of inorganic filler; 3-5 parts reactive diluent; 1-3 parts of photoinitiator; 1-2 parts of auxiliary agent; Solvent 10-15 parts; The preparation method of the imidazole carboxylate chain-extended polyurethane prepolymer includes: (a) Isoethyl methacrylate reacts with imidazole at 40-60°C to produce 1-imidazolium carbonylamino-2-ethyl methacrylate; (b) The product of step (a) reacts with dimethylolpropionic acid to form a salt at 50-60°C; (c) The salt formation product of step (b) reacts with the diisocyanate-polyethylene glycol prepolymer at 60-80°C.
2. The acryl-epoxy resin for a PCB jack according to claim 1, characterized by, The 1-imidazolium carbonylamino-2-ethyl methacrylate was prepared by reacting isocyanate ethyl methacrylate with imidazolium in a molar ratio of 1:1.1-1.2 at 60°C for 2 hours.
3. The acrylic epoxy resin for PCB via plugging according to claim 1, characterized in that, The 1-imidazolium carbonylamino-2-ethyl methacrylate reacts with dimethylolpropionic acid at a molar ratio of 1:1 at 50-60°C for 6-12 hours to form a salt.
4. The acryl-epoxy resin for a PCB jack hole according to claim 1, characterized by, The diisocyanate is selected from at least one of isophorone diisocyanate and hexamethylene diisocyanate.
5. The acryl-epoxy resin for a PCB jack according to claim 1, characterized by, The anhydride curing agent is selected from at least one of methylhexahydrophthalic anhydride and methyltetrahydrophthalic anhydride.
6. The acryl-epoxy resin for a PCB jack according to claim 1, characterized by, The reactive diluent is selected from at least one of tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, and trimethylolpropane triacrylate.
7. The acryl-epoxy resin for a PCB jack according to claim 1, characterized by, The photoinitiator is selected from at least one of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenyl ketone, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.
8. The acrylic epoxy resin for PCB via plugging according to claim 1, characterized in that, The inorganic filler is spherical silica surface-modified with an epoxy silane coupling agent.
9. The acrylic epoxy resin for PCB via plugging according to claim 1, characterized in that, The additives include at least one of silicone leveling agents and silicone defoamers.
10. A method for preparing a storage-stable acrylic epoxy resin for PCB via plugging as described in any one of claims 1-9, characterized in that, Includes the following steps: The resin, imidazole carboxylate polyurethane prepolymer, acid anhydride curing agent, photoinitiator, inorganic filler, reactive diluent, additives and solvent are mixed and ground with a three-roll mill until the fineness is ≤15μm. After vacuum degassing, the acrylic epoxy resin for PCB via plugging is obtained.