A polyphenylene ether composite dielectric adhesive solution, its preparation method, and copper-clad laminate.

By combining modified inorganic fillers with polyphenylene ether resin and other components, and using dry premixing and wet mixing methods, the problem of agglomeration of high dielectric ceramic fillers in polyphenylene ether resin was solved, achieving high dielectric constant, low dielectric loss and high copper foil peel strength in high frequency copper clad laminates.

CN123107311APending Publication Date: 2026-11-17ZHEJIANG FORESTRY UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611370326.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, when polyphenylene ether resin is used as a high-dielectric ceramic filler in high-frequency copper-clad laminates, it is easy to form agglomerates, which leads to interface defects and reduced bonding strength, making it difficult to achieve high dielectric constant, low dielectric loss and high copper foil peel strength.

Method used

A polyphenylene ether composite medium was prepared by combining modified inorganic fillers with components such as polyphenylene ether resin, phenolic resin, and epoxy resin through dry premixing and wet mixing methods. This improved the interfacial compatibility between the ceramic filler and the resin, and the dispersibility was enhanced by surface treatment with a silane coupling agent.

Benefits of technology

This invention achieves copper-clad laminates with high dielectric constant, low dielectric loss and high copper foil peel strength, while also having good thermal stability and reducing ceramic filler agglomeration and interface defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This application relates to the technical field of copper-clad laminate materials, specifically disclosing a polyphenylene ether composite dielectric adhesive, its preparation method, and a copper-clad laminate. The polyphenylene ether composite dielectric adhesive comprises the following components in parts by weight: 8-12 parts polyphenylene ether resin, 16-24 parts epoxy resin, 8-12 parts phenolic resin, 55-65 parts modified inorganic filler, 0.6-1.0 parts curing agent, 0.02-0.05 parts curing accelerator, and 12-18 parts organic solvent; the modified inorganic filler is a high-dielectric ceramic filler surface-treated with a silane coupling agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the technical field of copper clad laminate materials, and in particular to a polyphenylene ether composite dielectric adhesive solution, its preparation method, and copper clad laminate. Background Technology

[0002] Copper clad laminates (CCLs) are essential materials in printed circuit boards, antenna modules, and high-frequency electronic devices. Their dielectric properties, thermal stability, and the bonding strength between the copper foil and the dielectric layer directly affect the signal transmission performance, dimensional stability, and long-term reliability of electronic devices. As AI computing devices, intelligent systems for new energy vehicles, automotive millimeter-wave radar, and high-frequency communication equipment continue to develop towards higher frequencies, higher integration, and miniaturization, higher requirements are being placed on the dielectric constant, dielectric loss, and interface bonding performance of CCLs.

[0003] Polyphenylene ether resin (PPE) is widely used as a dielectric material in high-frequency copper-clad laminates due to its low dielectric loss and good heat resistance. However, PPE itself has a relatively low dielectric constant. When used in antennas and other high-frequency devices requiring higher dielectric constants, high-dielectric ceramic fillers are typically added to PPE to increase the dielectric constant of the composite dielectric layer and reduce the size of the antenna and corresponding high-frequency devices. As the content of high-dielectric ceramic fillers increases, the contact probability between ceramic particles increases, making it easier for agglomerates to form in the resin matrix. This leads to insufficient wetting and coating of the ceramic filler by the resin, and the formation of interfacial defects such as micropores and gaps at the filler / resin interface.

[0004] Furthermore, while increasing the content of high-dielectric ceramic fillers is beneficial for improving the dielectric constant of composite materials, high inorganic filler content reduces the proportion of the continuous resin phase and easily leads to localized stress concentrations in the ceramic particle agglomeration areas. When the copper-clad laminate is subjected to hot pressing, high-temperature thermal stress, or thermal cycling, the aforementioned interface defects are prone to further expansion, resulting in a decrease in the bonding strength between the copper foil and the composite dielectric layer.

[0005] Therefore, there is an urgent need to develop a polyphenylene ether composite dielectric adhesive that enables high-content, high-dielectric ceramic fillers to be uniformly dispersed in the polyphenylene ether composite resin matrix and form a stable filler / resin interface. This would improve the dielectric constant of the copper clad laminate while reducing dielectric loss and interface stress concentration caused by ceramic filler agglomeration and interface defects, thus achieving a balance of higher dielectric constant, lower dielectric loss, and higher copper foil peel strength. Summary of the Invention

[0006] In order to achieve a copper-clad laminate with a high dielectric constant, low dielectric loss, and high copper foil peel strength, this application provides a polyphenylene ether composite dielectric adhesive, its preparation method, and a copper-clad laminate.

[0007] In the first aspect, the polyphenylene ether composite medium adhesive provided in this application adopts the following technical solution: A polyphenylene ether composite dielectric adhesive, wherein the raw materials of the polyphenylene ether composite dielectric adhesive include the following components in parts by weight: 8-12 parts of polyphenylene ether resin, 16-24 parts of epoxy resin, 8-12 parts of phenolic resin, 55-65 parts of modified inorganic filler, 0.6-1.0 parts of curing agent, 0.02-0.05 parts of curing accelerator, and 12-18 parts of organic solvent; wherein the modified inorganic filler is a high-dielectric ceramic filler surface-treated with a silane coupling agent.

[0008] By adopting the above technical solutions, polyphenylene ether resin has low dielectric loss, epoxy resin can improve the adhesion and curing performance of the system, and phenolic resin is beneficial to improving the heat resistance and structural stability of the cured network. High dielectric ceramic filler can improve the dielectric constant of the composite medium, and surface treatment with silane coupling agent can improve the interfacial compatibility between ceramic filler and organic resin. The above resin system and modified inorganic filler work together to improve the dielectric constant while reducing filler agglomeration and interfacial defects, thereby achieving both low dielectric loss and high peel strength.

[0009] In one specific implementation, the method for preparing the modified inorganic filler includes the following steps: The high dielectric ceramic filler was vacuum dried; anhydrous ethanol and deionized water were mixed evenly, and the pH was adjusted to 4.5-5.0 with glacial acetic acid. Silane coupling agent was added and stirred to obtain a silane coupling agent hydrolysate. The dried high-dielectric ceramic filler was added to the silane coupling agent hydrolysate and dispersed. The temperature was then raised to 60°C and the mixture was stirred to react. After the reaction was completed, the mixture was cooled to room temperature, filtered, and washed. The washed filter cake was then vacuum dried, heat-treated, cooled, and pulverized to obtain the modified inorganic filler.

[0010] In one specific implementation, the weight ratio of the silane coupling agent to the high-dielectric ceramic filler is (1.6-2.0):100.

[0011] By adopting the above technical solution, the weight ratio of silane coupling agent to high dielectric ceramic filler is controlled at (1.6~2.0):100, which is beneficial to form a more continuous and appropriate amount of coupling layer on the surface of ceramic filler. This can take into account both the surface coverage and dispersion stability of ceramic filler, thereby further improving the interfacial compatibility between filler and resin matrix.

[0012] In one specific embodiment, the curing agent comprises one or both of dicyandiamide and 4,4'-diaminodiphenyl sulfone; the curing accelerator comprises 2-ethyl-4-methylimidazole.

[0013] In one specific embodiment, the organic solvent includes one or more of acetone, N,N-dimethylformamide, and propylene glycol methyl ether.

[0014] In one specific implementation, the raw materials of the polyphenylene ether composite medium liquid further include 2 to 6 parts by weight of bismaleimide resin and 1 to 4 parts by weight of reactive low molecular weight polyphenylene ether oligomer.

[0015] By adopting the above technical solution, the reactive low molecular weight polyphenylene ether oligomer and polyphenylene ether resin have good structural compatibility. Its low polarity is beneficial to improving the dielectric properties of the polyphenylene ether composite resin system and can improve the compatibility between different resin components. The bismaleimide resin has high heat resistance rigidity, which is beneficial to improving the heat resistance stability of the resin system. The two work together to enable the composite resin system to have good heat resistance while maintaining low dielectric loss.

[0016] In one specific implementation, the raw materials of the polyphenylene ether composite medium solution further include 0.3 to 1.0 parts by weight of titanate coupling agent and 0.2 to 0.8 parts by weight of non-aqueous ceramic polymeric dispersant.

[0017] By adopting the above technical solutions, titanate coupling agents can further improve the wettability and interfacial affinity between high-dielectric ceramic fillers and resin matrices, while non-aqueous ceramic polymeric dispersants can inhibit secondary agglomeration of particles through adsorption on the surface of ceramic particles and steric hindrance generated by polymeric chain segments. The two, together with silane coupling agents, form a synergistic interfacial regulation effect, thereby improving the dispersion stability of high-content ceramic fillers in the resin system, reducing interfacial micropores and local stress concentration, and further balancing dielectric properties and peel strength.

[0018] Secondly, this application provides a method for preparing a polyphenylene ether composite medium adhesive, which adopts the following technical solution: A method for preparing a polyphenylene ether composite medium adhesive includes the following steps: Dry premixing: The modified inorganic filler, polyphenylene ether resin and phenolic resin are dry premixed and ball-milled to obtain premixed composite powder; Wet mixing: The premixed composite powder is wet mixed with epoxy resin, curing agent, curing accelerator and organic solvent to obtain polyphenylene ether composite medium adhesive.

[0019] By adopting the above technical solution, the modified inorganic filler is first dry-premixed and ball-milled with polyphenylene ether resin and phenolic resin. This allows the mechanical shearing action to break up the ceramic filler agglomerates and pre-distribute the resin components around the ceramic particles. Subsequently, epoxy resin, curing agent, curing accelerator and organic solvent are added for wet mixing, which further completes the wetting, dispersion and homogenization of the premixed composite powder. The dry premixing and wet mixing work together to reduce the secondary agglomeration and interface defects of the high dielectric ceramic filler, while avoiding the curing system from being subjected to high-energy ball milling for a long time, thus taking into account the filler dispersibility, the stability of the adhesive and the subsequent curing performance.

[0020] Thirdly, the copper-clad laminate provided in this application adopts the following technical solution: A copper-clad laminate includes a copper foil and a polyphenylene ether composite dielectric layer stacked with the copper foil, wherein the polyphenylene ether composite dielectric layer is formed by curing the polyphenylene ether composite dielectric adhesive.

[0021] By adopting the above technical solution, the polyphenylene ether composite dielectric adhesive is cured to form a polyphenylene ether composite dielectric layer, and a laminated structure is formed with copper foil. The high dielectric ceramic filler in the composite dielectric layer provides a high dielectric constant, the polyphenylene ether composite resin system is conducive to maintaining a low dielectric loss, and the relatively stable interfacial bonding between the modified inorganic filler and the resin can reduce internal defects and thermal stress concentration, so that the obtained copper clad laminate has a high dielectric constant, low dielectric loss, high copper foil peel strength and good heat resistance stability.

[0022] In summary, this application includes at least one of the following beneficial technical effects: In this application, polyphenylene ether resin exhibits low dielectric loss, epoxy resin enhances the adhesion and curing properties of the system, and phenolic resin improves the heat resistance and structural stability of the cured network. High-dielectric ceramic filler increases the dielectric constant of the composite medium, and surface treatment with a silane coupling agent improves the interfacial compatibility between the ceramic filler and the organic resin. The above resin system, in combination with the modified inorganic filler, increases the dielectric constant while reducing filler agglomeration and interfacial defects, thus achieving both low dielectric loss and high peel strength. The method in this application first involves dry premixing and ball milling the modified inorganic filler with polyphenylene ether resin and phenolic resin. This utilizes mechanical shearing to break up the ceramic filler agglomerates and pre-distributes the resin components around the ceramic particles. Subsequently, epoxy resin, curing agent, curing accelerator, and organic solvent are added for wet mixing, which further wets, disperses, and homogenizes the premixed composite powder. The dry premixing and wet mixing work synergistically to reduce secondary agglomeration and interface defects of the high-dielectric ceramic filler, while avoiding prolonged exposure of the curing system to high-energy ball milling, thus balancing filler dispersibility, adhesive stability, and subsequent curing performance. In this application, polyphenylene ether composite dielectric adhesive is cured to form a polyphenylene ether composite dielectric layer, which is then laminated with copper foil. The high dielectric ceramic filler in the composite dielectric layer provides a high dielectric constant, the polyphenylene ether composite resin system helps to maintain a low dielectric loss, and the relatively stable interfacial bonding between the modified inorganic filler and the resin can reduce internal defects and thermal stress concentration, so that the resulting copper clad laminate has a high dielectric constant, low dielectric loss, high copper foil peel strength, and good heat resistance stability. Attached Figure Description

[0023] Figure 1 This is an optical microscope image of the filler dispersion in Application Example 1; Figure 2 For comparison, see the optical microscope images of the filler dispersion in Application Example 1; Figure 3 The graph shows the effect of different ceramic powder to resin mass ratios on the dielectric properties of copper clad laminates. Detailed Implementation

[0024] The present application will be further described in detail below with reference to the embodiments.

[0025] All raw materials used in the examples are commercially available. The polyphenylene ether resin is high-frequency, high-speed communication polyphenylene ether resin produced by Huaibei Oasis New Materials Co., Ltd.; the epoxy resin is E-51 type bisphenol A epoxy resin from Shanghai Maclean Biochemical Technology Co., Ltd.; the phenolic resin is electronic-grade linear phenol-formaldehyde resin produced by Shandong Shengquan Chemical Co., Ltd.; the high-dielectric ceramic filler is barium titanate-based high-dielectric ceramic powder produced by Huaxing Electronics Technology Co., Ltd.; the bismaleimide resin is diphenylmethane type bismaleimide resin; the reactive low molecular weight polyphenylene ether oligomer is SABICNORYL™ SA9000; the titanate coupling agent is isopropyltris(dioctylpyrophosphate) titanate, model NDZ-201; and the non-aqueous ceramic polymeric dispersant is Lubrizol Solsperse™ AC7550. Preparation Example

[0026] Preparation Example 1 Preparation Example 1 provides a method for preparing a modified inorganic filler, comprising the following steps: The high-dielectric ceramic filler was placed in a vacuum drying oven and dried at 110℃ for 3 hours, then cooled to room temperature for later use. Anhydrous ethanol and deionized water were mixed evenly, and the pH was adjusted to 4.7 with glacial acetic acid. A silane coupling agent was added, and the mixture was stirred and hydrolyzed for 30 min at 30℃ and 300 r / min to obtain a silane coupling agent hydrolysate. The silane coupling agent was γ-aminopropyltriethoxysilane, and the weight ratio of anhydrous ethanol, deionized water, and silane coupling agent was 90:10:1.6. The weight ratio of silane coupling agent to high dielectric ceramic filler was 1.8:100. The dried high-dielectric ceramic filler was added to the silane coupling agent hydrolysate and dispersed at 1000 r / min for 30 min. Then, the temperature was raised to 60℃ and the reaction was continued to be stirred at 500 r / min for 2 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the resulting filter cake was washed twice with anhydrous ethanol. The washed filter cake was placed in a vacuum drying oven at 85℃ for 6 h and then heat-treated at 110℃ for 1 h. After cooling and pulverizing, the modified inorganic filler was obtained.

[0027] Preparation Example 2 The difference between Preparation Example 2 and Preparation Example 1 is that the silane coupling agent is γ-aminopropyltriethoxysilane, and the weight ratio of anhydrous ethanol, deionized water, and silane coupling agent is 90:10:1.8; the weight ratio of silane coupling agent to high dielectric ceramic filler is 1.6:100; the remaining steps are the same as those in Preparation Example 1.

[0028] Preparation Example 3 The difference between Preparation Example 3 and Preparation Example 1 is that the silane coupling agent is γ-aminopropyltriethoxysilane, and the weight ratio of anhydrous ethanol, deionized water, and silane coupling agent is 90:10:2.0; the weight ratio of silane coupling agent to high dielectric ceramic filler is 2.0:100; the remaining steps are the same as those in Preparation Example 1. Example

[0029] Example 1 Example 1 provides a method for preparing a polyphenylene ether composite medium adhesive, comprising the following steps: Dry premixing: 60g of the modified inorganic filler, 10g of polyphenylene ether resin and 10g of phenolic resin from Preparation Example 1 were dry premixed and ball-milled. The ball milling was carried out using a high-energy planetary ball mill at a speed of 500 rpm for 3 hours. The ball-to-material ratio was 3:1 and the target powder particle size was 10μm, thus obtaining the premixed composite powder. Wet mixing: The premixed composite powder is wet-mixed twice with 20g epoxy resin, 0.78g curing agent, and 0.03g curing accelerator in 15g organic solvent using mechanical stirring at 350rpm for 15h to obtain polyphenylene ether composite medium solution; wherein the curing agent is dicyandiamide; the curing accelerator is 2-ethyl-4-methylimidazole; and the organic solvent is acetone.

[0030] Example 2 Example 2 provides a method for preparing a polyphenylene ether composite medium adhesive, comprising the following steps: Dry premixing: 55g of the modified inorganic filler, 8g of polyphenylene ether resin and 8g of phenolic resin from Preparation Example 1 were dry premixed and ball-milled. The ball milling was carried out using a high-energy planetary ball mill at a speed of 500 rpm for 3 hours. The ball-to-material ratio was 3:1 and the target powder particle size was 10 μm, thus obtaining the premixed composite powder. Wet mixing: The premixed composite powder is wet-mixed twice with 16g epoxy resin, 0.6g curing agent, and 0.02g curing accelerator in 12g organic solvent using mechanical stirring at 350rpm for 15h to obtain polyphenylene ether composite medium solution; wherein the curing agent is dicyandiamide; the curing accelerator is 2-ethyl-4-methylimidazole; and the organic solvent is acetone.

[0031] Example 3 Example 3 provides a method for preparing a polyphenylene ether composite medium adhesive, comprising the following steps: Dry premixing: 65g of the modified inorganic filler, 12g of polyphenylene ether resin and 12g of phenolic resin from Preparation Example 1 were dry premixed and ball-milled. The ball milling was carried out using a high-energy planetary ball mill at a speed of 500 rpm for 3 hours. The ball-to-material ratio was 3:1 and the target powder particle size was 10μm, thus obtaining the premixed composite powder. Wet mixing: The premixed composite powder is wet-mixed twice with 24g epoxy resin, 1.0g curing agent, and 0.05g curing accelerator in 18g organic solvent using mechanical stirring at 350rpm for 15h to obtain polyphenylene ether composite medium adhesive; wherein the curing agent is dicyandiamide; the curing accelerator is 2-ethyl-4-methylimidazole; and the organic solvent is acetone.

[0032] Example 4 The difference between Example 4 and Example 1 is that the dry premixing method was used: 60g of the modified inorganic filler from Example 2, 10g of polyphenylene ether resin and 10g of phenolic resin were dry premixed and ball-milled. The ball milling was carried out using a high-energy planetary ball mill at a speed of 500 rpm for 3 hours, with a ball-to-material ratio of 3:1 and a target powder particle size of 10μm, to obtain the premixed composite powder; the remaining steps were the same as in Example 1.

[0033] Example 5 The difference between Example 5 and Example 1 is that the dry premixing method is used: 60g of the modified inorganic filler, 10g of polyphenylene ether resin and 10g of phenolic resin from Example 3 are dry premixed and ball-milled. The ball milling is carried out using a high-energy planetary ball mill at a speed of 500 rpm for 3 hours. The ball-to-material ratio is 3:1 and the target powder particle size is 10μm, thus obtaining the premixed composite powder. The remaining steps are the same as in Example 1.

[0034] Example 6 Example 6 provides a method for preparing a polyphenylene ether composite medium adhesive, comprising the following steps: Dry premixing: 60g of the modified inorganic filler, 10g of polyphenylene ether resin, 10g of phenolic resin, and 2.5g of reactive low molecular weight polyphenylene ether oligomer from Preparation Example 2 were dry premixed and then ball-milled. The ball milling was performed using a high-energy planetary ball mill at a speed of 500 rpm for 3 hours. The ball-to-material ratio was 3:1, and the target powder particle size was 10μm, resulting in premixed composite powder. Wet mixing: The premixed composite powder is wet-mixed twice with 20g epoxy resin, 4g bismaleimide resin, 0.78g curing agent, and 0.03g curing accelerator in 15g organic solvent using mechanical stirring at 350rpm for 15h to obtain polyphenylene ether composite medium solution; wherein the curing agent is dicyandiamide; the curing accelerator is 2-ethyl-4-methylimidazole; and the organic solvent is acetone.

[0035] Example 7 The difference between Example 7 and Example 4 is that the dry premixing method is used: 60g of the modified inorganic filler, 10g of polyphenylene ether resin, 10g of phenolic resin, and 2.5g of reactive low molecular weight polyphenylene ether oligomer from Preparation Example 2 are dry premixed and then ball-milled. The ball milling is performed using a high-energy planetary ball mill at a speed of 500 rpm for 3 hours, with a ball-to-material ratio of 3:1 and a target powder particle size of 10μm, to obtain a premixed composite powder; the remaining steps are the same as in Example 4.

[0036] Example 8 The difference between Example 8 and Example 4 is that the wet mixing method is used: the premixed composite powder is wet mixed twice with 20g of epoxy resin, 4g of bismaleimide resin, 0.78g of curing agent, and 0.03g of curing accelerator in 15g of organic solvent, and mechanical stirring is used at a speed of 350rpm for 15h to obtain polyphenylene ether composite medium adhesive; the remaining steps are the same as in Example 4.

[0037] Example 9 The difference between Example 9 and Example 6 is that the wet mixing method is as follows: the premixed composite powder is wet-mixed twice with 20g of epoxy resin, 4g of bismaleimide resin, 0.78g of curing agent, 0.03g of curing accelerator, 0.6g of titanate coupling agent and 0.5g of non-aqueous ceramic polymeric dispersant in 15g of organic solvent, using mechanical stirring at 350rpm for 15h to obtain polyphenylene ether composite medium solution; the remaining steps are the same as in Example 6.

[0038] Example 10 The difference between Example 10 and Example 6 is that the wet mixing method is used: the premixed composite powder is wet mixed twice with 20g of epoxy resin, 4g of bismaleimide resin, 0.78g of curing agent, 0.03g of curing accelerator, and 0.6g of titanate coupling agent in 15g of organic solvent, using mechanical stirring at 350rpm for 15h to obtain polyphenylene ether composite medium solution; the remaining steps are the same as in Example 6.

[0039] Example 11 The difference between Example 11 and Example 6 is that the wet mixing method is as follows: the premixed composite powder is wet-mixed twice with 20g of epoxy resin, 4g of bismaleimide resin, 0.78g of curing agent, 0.03g of curing accelerator, and 0.5g of non-aqueous ceramic polymeric dispersant in 15g of organic solvent. The mixture is mechanically stirred at 350rpm for 15h to obtain a polyphenylene ether composite medium solution. The remaining steps are the same as in Example 6. Comparative Example

[0040] Comparative Example 1 Comparative Example 1 provides a method for preparing a polyphenylene ether composite medium adhesive, comprising the following steps: 40g of polyphenylene ether resin and 60g of high dielectric ceramic filler were blended to obtain a composite material; then 0.78g of curing agent, 0.03g of curing accelerator and 15g of toluene were added and mixed evenly to obtain a polyphenylene ether composite medium adhesive.

[0041] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that phenolic resin was not added, and the amount of epoxy resin was adjusted from 20g to 30g; the remaining steps were the same as in Example 1.

[0042] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that polyphenylene ether resin was not added, and the amount of epoxy resin was adjusted from 20g to 30g; the remaining steps were the same as in Example 1.

[0043] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that the modified inorganic filler was replaced by an equal weight of a high-dielectric ceramic filler that was not surface-treated with silane coupling agent; the remaining steps were the same as in Example 1. Application examples

[0044] Application Example 1 Application Example 1 provides a method for preparing a copper-clad laminate, comprising the following steps: Prepreg preparation: 7628 electronic grade glass fiber cloth was used to impregnate the polyphenylene ether composite medium adhesive from Example 1, so that the polyphenylene ether composite medium adhesive was uniformly attached to and wetted the glass fiber cloth; the impregnated glass fiber cloth was baked at a temperature of 165°C, a linear velocity of 6 m / min, a gel time of 120 seconds, and the resin flow rate was controlled at 18% to obtain a prepreg. Lamination: Eight prepreg sheets were stacked, and 18μm low-roughness electrolytic copper foils were applied to both sides of the stacked prepreg sheets. Gradient hot pressing was then performed. First, pre-pressing was conducted at 130℃ and 120psi for 15 minutes. Then, the temperature was increased to 150℃ and the pressure to 135psi, and hot pressing was performed for 10 minutes. Next, the temperature was increased to 200℃ and the pressure to 150psi, and hot pressing was performed for 15 minutes. Finally, the temperature was increased to 220℃ and the pressure to 180psi, and hot pressing was maintained at this temperature for 1 hour. The polyphenylene ether composite dielectric adhesive is fully cured; then, under pressure, a gradient cooling process is performed, holding at 180℃ and 150psi for 15 min, at 150℃ and 135psi for 30 min, and at 120℃ and 120psi for 30 min. After cooling to room temperature, the pressure is released to obtain a copper-clad laminate. The obtained copper-clad laminate includes copper foils on both sides and a polyphenylene ether composite dielectric layer disposed between the two copper foils. The thickness of the polyphenylene ether composite dielectric layer is 1.5 mm.

[0045] Application Example 2 The difference between Application Example 2 and Application Example 1 is that the polyphenylene ether composite medium solution in Application Example 2 is used for impregnation and then baked; the remaining steps are the same as in Application Example 1.

[0046] Application Example 3 The difference between Application Example 3 and Application Example 1 is that the polyphenylene ether composite medium solution in Application Example 3 is impregnated and then baked; the remaining steps are the same as in Application Example 1.

[0047] Application Example 4 The difference between Application Example 4 and Application Example 1 is that the polyphenylene ether composite medium solution in Application Example 4 is impregnated and then baked; the remaining steps are the same as in Application Example 1.

[0048] Application Example 5 The difference between Application Example 5 and Application Example 1 is that the polyphenylene ether composite medium solution in Application Example 5 is impregnated and then baked; the remaining steps are the same as in Application Example 1.

[0049] Application Example 6 The difference between Application Example 6 and Application Example 1 is that the polyphenylene ether composite medium solution in Application Example 6 is used for impregnation and then baked; the remaining steps are the same as in Application Example 1.

[0050] Application Example 7 The difference between Application Example 7 and Application Example 1 is that the polyphenylene ether composite medium solution in Application Example 7 is impregnated and then baked; the remaining steps are the same as in Application Example 1.

[0051] Application Example 8 The difference between Application Example 8 and Application Example 1 is that the polyphenylene ether composite medium solution in Application Example 8 is impregnated and then baked; the remaining steps are the same as in Application Example 1.

[0052] Application Example 9 The difference between Application Example 9 and Application Example 1 is that the polyphenylene ether composite medium solution in Application Example 9 is impregnated and then baked; the remaining steps are the same as in Application Example 1.

[0053] Application Example 10 The difference between Application Example 10 and Application Example 1 is that the polyphenylene ether composite medium solution in Application Example 10 is impregnated and then baked; the remaining steps are the same as in Application Example 1.

[0054] Application Example 11 The difference between Application Example 11 and Application Example 1 is that the polyphenylene ether composite medium solution in Application Example 11 is impregnated and then baked; the remaining steps are the same as in Application Example 1. Comparative Application Examples

[0055] Comparative Application Example 1 The difference between Comparative Example 1 and Application Example 2 is that the polyphenylene ether composite medium solution in Comparative Example 1 is impregnated and then baked; the remaining steps are the same as in Application Example 1.

[0056] Comparative Application Example 2 The difference between Application Example 2 and Application Example 1 is that the polyphenylene ether composite medium solution in Comparative Example 2 is impregnated and then baked; the remaining steps are the same as in Application Example 1.

[0057] Comparative Application Example 3 The difference between Application Example 3 and Application Example 1 is that the polyphenylene ether composite medium solution in Comparative Example 3 is impregnated and then baked; the remaining steps are the same as in Application Example 1.

[0058] Comparative Application Example 4 The difference between Application Example 4 and Application Example 1 is that the polyphenylene ether composite medium solution in Comparative Example 4 is impregnated and then baked; the remaining steps are the same as in Application Example 1. Performance testing experiment

[0059] Dielectric constant: Tested according to the method specified in 8.5 of GB / T 4722-2017 "Test Methods for Rigid Copper Clad Laminates for Printed Circuits". Copper foil in the test area was removed from the copper-clad laminates prepared in Application Examples 1-11 and Comparative Application Examples 1-4 to obtain dielectric test samples. The parallel plate method was used for testing at a frequency of 1 MHz. At least three valid samples from each group were tested in parallel, and the average value of the test results was taken as the dielectric constant Dk of that group of copper-clad laminates.

[0060] Loss: Tested according to the method specified in 8.5 of GB / T 4722-2017. Remove the copper foil from the test area of ​​the copper-clad laminate, and use the parallel plate method to determine the dielectric loss tangent Df of the sample at a test frequency of 1MHz; take no less than 3 valid samples for parallel testing in each group, and take the average value of the test results.

[0061] Peel strength: The test was conducted according to the acceptance peel strength test method specified in 7.2.1 of GB / T 4722-2017. Each group of copper-clad laminates was cut into samples. A copper foil peel strip with a width of 3.0±0.1 mm was formed on the copper foil surface by etching. One end of the copper foil peel strip was pre-peeled and fixed in the universal testing machine fixture, maintaining a peel direction of approximately 90° between the copper foil and the substrate. Peeling was performed at a speed of 50 mm / min, and the average peel load during the stable peeling stage was recorded. The peel strength was calculated as the ratio of the stable peel load to the width of the copper foil peel strip, in N / mm. At least 5 valid samples were tested in each group, and the average value was taken.

[0062] Thermal stress: Tested according to the thermal delamination time test method specified in 6.11 of GB / T 4722-2017. A thermomechanical analyzer was used to test the copper-clad laminate in the Z-axis direction. The sample was heated to 288℃ and then held at that temperature. The time from the start of the holding period at 288℃ to the occurrence of delamination was recorded, denoted as T288, in minutes. The larger the T288, the stronger the copper-clad laminate's resistance to delamination under high-temperature conditions.

[0063] Tg: The test was performed according to the differential scanning calorimetry method specified in 6.7.1 of GB / T 4722-2017. After removing the copper foil from the copper-clad laminate, a dielectric layer sample was taken and placed in a differential scanning calorimeter. The test was conducted under nitrogen protection conditions. The test temperature range was 30–250℃, and the heating rate was 10℃ / min. The glass transition temperature Tg was determined based on the region where the baseline of the DSC curve showed a step change. At least three parallel tests were performed for each group, and the average value was taken.

[0064] Table 1 Performance test results of copper clad laminate

[0065] Combining Application Example 1 with Comparative Application Examples 1-4, Comparative Application Example 1, which uses direct blending of polyphenylene ether with unmodified high-dielectric ceramic filler, exhibits a dielectric loss of 0.0125, a peel strength of only 0.91 N / mm, and a T288 thermal delamination time of only 26 min. This indicates that when the content of high-dielectric ceramic filler is high, simple blending is insufficient to simultaneously achieve filler dispersion and interfacial bonding performance. Comparative Application Example 2, without the addition of phenolic resin, shows a reduction in Tg and T288 thermal delamination time to 136℃ and 41 min, respectively, indicating that phenolic resin is beneficial for improving the heat resistance and structural stability of the composite resin cured network. Comparative Application Example 3, without the addition of polyphenylene ether resin, shows an increased dielectric loss to 0.0132, significantly higher than Application Example 1. Although its peel strength remains at a certain level, the low-loss performance is significantly reduced, indicating that polyphenylene ether resin plays an important role in constructing a low-polarity resin continuous phase and reducing the dielectric loss of the composite media system. In contrast to Application Example 4, when the modified inorganic filler was replaced with a high-dielectric ceramic filler without silane coupling agent surface treatment, the peel strength decreased to 1.07 N / mm, the dielectric loss increased to 0.0111, and the T288 thermal delamination time decreased to 34 min. This indicates that the untreated ceramic filler has poor interfacial compatibility with the organic resin, which easily leads to particle agglomeration and filler-resin interface defects.

[0066] In conjunction with Application Examples 1-3, within the component dosage range specified in this application, the dielectric constant of the obtained copper-clad laminate remains above 25, the dielectric loss tangent remains at a low level, and it also exhibits good peel strength, T288 thermal delamination time, and glass transition temperature. Specifically, in Application Example 2, the proportion of high-dielectric ceramic filler relative to the resin component is relatively high, increasing the dielectric constant to 26.2, but the dielectric loss slightly increases and the peel strength decreases. In Application Example 3, the proportion of the resin component is relatively increased, resulting in a slight decrease in the dielectric constant, while peel strength and heat resistance are improved.

[0067] Based on Application Examples 1, 4, and 5, it can be seen that when preparing modified inorganic fillers, controlling the weight ratio of silane coupling agent to high dielectric ceramic filler to be (1.6-2.0):100 results in modified inorganic fillers with better performance.

[0068] Combining Application Examples 4 and 6-8, it can be seen that in Application Example 7, after adding reactive low molecular weight polyphenylene ether oligomer to the base system, the dielectric loss decreased from 0.0074 to 0.0066, while the peel strength and heat resistance also improved. This indicates that the reactive low molecular weight polyphenylene ether oligomer has good structural compatibility with polyphenylene ether resin, which can improve the compatibility between resin phases and the low loss performance of the system. In Application Example 8, after adding bismaleimide resin, the Tg increased from 151℃ to 163℃, and the T288 thermal delamination time increased from 68min to 81min. This indicates that bismaleimide resin has high heat resistance rigidity, which is beneficial to improving the heat resistance stability of the composite resin system. In Application Example 6, after simultaneously adding reactive low molecular weight polyphenylene ether oligomer and bismaleimide resin, the dielectric loss was further reduced to 0.0061, the Tg increased to 166℃, and the T288 thermal delamination time was extended to 85min. The overall performance was better than that of Application Examples 7 and 8, which added only one component. This demonstrates that the synergistic effect of the two enables the polyphenylene ether composite media system to achieve both low media loss and good heat resistance.

[0069] Combining Application Examples 6 and 9-11, Application Example 10, which only added titanate coupling agent, and Application Example 11, which only added non-aqueous ceramic polymeric dispersant, showed improvements in dielectric loss, peel strength, and T288 thermal delamination time. In Application Example 9, which simultaneously added titanate coupling agent and non-aqueous ceramic polymeric dispersant, the dielectric loss was further reduced to 0.0052, the peel strength increased to 1.78 N / mm, and the T288 thermal delamination time reached 101 min. This indicates that titanate coupling agent can improve the wettability and interfacial affinity of high-dielectric ceramic fillers to organic resin systems, while non-aqueous ceramic polymeric dispersant can inhibit secondary agglomeration of ceramic particles through particle surface adsorption and steric hindrance. The two, combined with silane-modified interfaces, form a synergistic effect in terms of interfacial wetting, particle dispersion, and interfacial bonding, further reducing agglomeration and interfacial defects in highly filled ceramic systems.

[0070] Combination Figure 1 and Figure 2 In Application Example 1, the high-dielectric ceramic filler was relatively uniformly distributed in the resin matrix, with no obvious large-size agglomerations observed. In contrast, in the corresponding Application Example 1, larger particle agglomeration areas were observed, and the uniformity of filler distribution was relatively poor in some areas. These results indicate that the present application, through surface modification of the high-dielectric ceramic filler with a silane coupling agent and further employing a staged dispersion method—dry premixing and ball milling of modified inorganic filler, polyphenylene ether resin, and phenolic resin, followed by wet mixing with epoxy resin and the curing system—can effectively break down the initial agglomerates of the high-dielectric ceramic filler. Furthermore, the pre-wetting and pre-coating effect of the resin on the ceramic particles inhibits their secondary agglomeration during subsequent wet mixing and curing processes, thereby improving the uniformity of filler dispersion in the resin matrix.

[0071] Combination Figure 3 As the weight ratio of high-dielectric ceramic filler to resin gradually increases from 50:50 to 70:30, the dielectric constant of the resulting composite dielectric material gradually increases, but the dielectric loss also tends to increase. Specifically, when the weight ratio of high-dielectric ceramic filler to resin is 60:40, the dielectric constant reaches 25.8, while the dielectric loss tangent remains at 0.008. Further increasing the proportion of high-dielectric ceramic filler can further improve the dielectric constant, but the dielectric loss increases significantly. Conversely, decreasing the proportion of high-dielectric ceramic filler can reduce the dielectric loss, but the dielectric constant decreases significantly. Therefore, a weight ratio of high-dielectric ceramic filler to resin of approximately 60:40 achieves a better balance between a higher dielectric constant and a lower dielectric loss.

[0072] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A polyphenylene ether composite medium adhesive, characterized in that: The raw materials of the polyphenylene ether composite medium adhesive include the following components in parts by weight: 8-12 parts of polyphenylene ether resin, 16-24 parts of epoxy resin, 8-12 parts of phenolic resin, 55-65 parts of modified inorganic filler, 0.6-1.0 parts of curing agent, 0.02-0.05 parts of curing accelerator, and 12-18 parts of organic solvent; the modified inorganic filler is a high-dielectric ceramic filler surface-treated with silane coupling agent.

2. The polyphenylene ether composite medium adhesive according to claim 1, characterized in that: The preparation method of the modified inorganic filler includes the following steps: The high dielectric ceramic filler was vacuum dried; anhydrous ethanol and deionized water were mixed evenly, and the pH was adjusted to 4.5-5.0 with glacial acetic acid. Silane coupling agent was added and stirred to obtain a silane coupling agent hydrolysate. The dried high-dielectric ceramic filler was added to the silane coupling agent hydrolysate and dispersed. The temperature was then raised to 60°C and the mixture was stirred to react. After the reaction was completed, the mixture was cooled to room temperature, filtered, and washed. The washed filter cake was then vacuum dried, heat-treated, cooled, and pulverized to obtain the modified inorganic filler.

3. The polyphenylene ether composite medium adhesive according to claim 2, characterized in that: The weight ratio of the silane coupling agent to the high-dielectric ceramic filler is (1.6-2.0):

100.

4. The polyphenylene ether composite medium adhesive according to claim 1, characterized in that: The curing agent includes one or both of dicyandiamide and 4,4'-diaminodiphenyl sulfone; the curing accelerator includes 2-ethyl-4-methylimidazole.

5. The polyphenylene ether composite medium adhesive according to claim 1, characterized in that: The organic solvent includes one or more of acetone, N,N-dimethylformamide, and propylene glycol methyl ether.

6. The polyphenylene ether composite medium adhesive according to claim 1, characterized in that: The raw materials of the polyphenylene ether composite medium also include 2 to 6 parts by weight of bismaleimide resin and 1 to 4 parts by weight of reactive low molecular weight polyphenylene ether oligomer.

7. The polyphenylene ether composite medium adhesive according to claim 1, characterized in that: The raw materials of the polyphenylene ether composite medium also include 0.3 to 1.0 parts by weight of titanate coupling agent and 0.2 to 0.8 parts by weight of non-aqueous ceramic polymer dispersant.

8. A method for preparing a polyphenylene ether composite medium adhesive as described in any one of claims 1-7, characterized in that: Includes the following steps: Dry premixing: The modified inorganic filler, polyphenylene ether resin and phenolic resin are dry premixed and ball-milled to obtain premixed composite powder; Wet mixing: The premixed composite powder is wet mixed with epoxy resin, curing agent, curing accelerator and organic solvent to obtain polyphenylene ether composite medium adhesive.

9. A copper-clad laminate, characterized in that: It includes a copper foil and a polyphenylene ether composite medium layer stacked with the copper foil, wherein the polyphenylene ether composite medium layer is formed by curing the polyphenylene ether composite medium adhesive according to any one of claims 1 to 7.