A high-strength biodegradable material for cosmetic packaging bottles and its preparation method

PET copolyester was prepared by cocondensation of terephthalic acid diacid monomer and ethylene glycol, and then blended with polylactic acid. This solved the problems of poor biodegradability and compatibility of PET packaging materials, and achieved a cosmetic packaging material with high strength and high decomposition rate.

CN123107318APending Publication Date: 2026-11-17ZHEJIANG RONGYI PACKAGING TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611430600.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

PET packaging materials are difficult to biodegrade and have poor compatibility when compounded with polylactic acid, resulting in poor mechanical properties and biodegradability of the materials.

Method used

PET copolyester was prepared by replacing part of terephthalic acid with terephthalic acid lactate diacid monomer and co-polymerizing it with ethylene glycol. Then, it was blended with polylactic acid to form a high-strength biodegradable material.

Benefits of technology

It improves the tensile strength and elongation at break of the material, enhances its biodegradability, making it more environmentally friendly and suitable for cosmetic packaging bottles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention relates to the field of polyester materials technology, and discloses a high-strength biodegradable material for cosmetic packaging bottles and its preparation method. The high-strength biodegradable material of this invention comprises 65-85 parts by weight of PET copolyester and 15-35 parts by weight of polylactic acid, etc. The PET copolyester and polylactic acid are mixed evenly in a mixer, and then extruded and granulated using a twin-screw extruder to obtain the high-strength biodegradable material. The introduction of fatty lactic acid ester structural units into the PET copolyester endows it with excellent biodegradability. Combined with biodegradable polylactic acid, the material exhibits a higher biodegradability rate, is more environmentally friendly, and is suitable for packaging materials such as cosmetic packaging bottles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polyester materials technology, specifically to a high-strength biodegradable material for cosmetic packaging bottles and its preparation method. Background Technology

[0002] Polylactic acid (PLA) has advantages such as high mechanical strength, biodegradability, and being green, environmentally friendly, and non-toxic. It is widely used in packaging, films, and bioengineering. However, PLA is brittle and has poor toughness, making it difficult to manufacture packaging bottles and other materials on its own. Usually, PLA needs to be compounded with high-performance resins such as polyethylene terephthalate, nylon, and polyethylene to produce high-performance biodegradable materials.

[0003] Polyethylene terephthalate (PET) has high toughness, high strength, and strong high temperature resistance, making it important in packaging materials. However, PET is difficult to biodegrade, posing an environmental pollution problem. Usually, PET is compounded with biodegradable materials such as polylactic acid and polyvinyl alcohol, or functional monomers are added during the preparation process to make biodegradable PET copolyester. Summary of the Invention

[0004] This invention solves the problem of the difficulty in biodegrading PET packaging materials.

[0005] This invention provides a high-strength biodegradable material and its preparation method. The high-strength biodegradable material comprises 65-85 parts by weight of PET copolyester, 15-35 parts by weight of polylactic acid, and 0.1-0.2 parts by weight of antioxidant.

[0006] The preparation method of high-strength biodegradable materials includes: mixing PET copolyester, polylactic acid and antioxidant in a mixer, and then extruding and granulating the mixture through a twin-screw extruder to obtain high-strength biodegradable materials.

[0007] Furthermore, the temperature of sections 1-7 of the twin-screw extruder is 170-260℃, and the screw speed is 100-180 r / min.

[0008] Furthermore, the preparation method of PET copolyester is as follows: (1) Add lactic acid and triethylamine to tetrahydrofuran, stir, and then add terephthaloyl chloride; the molar ratio of lactic acid, triethylamine, and terephthaloyl chloride is (2-2.4):(4.2-4.6):1; stir the reaction at room temperature for 12-18 hours, filter, distill the filtrate under reduced pressure, dilute with water, stir, add hydrochloric acid to adjust the pH of the solution to 2-3, filter, wash the precipitate with ice water, dry, and obtain terephthalic lactate.

[0009] (2) Nitrogen gas is introduced into the reactor, and terephthalic acid, terephthalic acid lactate, ethylene glycol and tetrabutyl titanate are added in a molar ratio of (85-93):(7-15):(150-180):(0.09-0.12). The temperature of the top of the distillation column in the reactor is controlled at 98-102℃. The reactor is heated to 220-245℃ and kept at this temperature until no water is generated. The reactor is then heated to 260-270℃ and gradually evacuated to a vacuum of 50-100 Pa. The reaction is continued for 3-4 hours, nitrogen gas is introduced, and the reactor is cooled with water to obtain PET copolyester.

[0010] Furthermore, high-strength biodegradable materials are used in cosmetic packaging bottles.

[0011] The beneficial technical effects of this invention are as follows: Terephthalic acid lactate diacid monomer is used to replace part of the terephthalic acid in a copolymerization reaction with ethylene glycol to obtain a PET copolyester. This copolyester is then blended and extruded with polylactic acid to obtain a high-strength biodegradable material. The terephthalic acid lactate diacid monomer contains a benzene ring structure, which allows the PET copolymer to maintain good mechanical strength without affecting the material's mechanical properties. Furthermore, the introduction of lactate structural units into the main chain of the PET copolyester molecule gives the PET copolyester and polylactic acid good interfacial compatibility, resulting in higher tensile strength and elongation at break, and excellent mechanical properties.

[0012] This invention introduces fatty lactate structural units into PET copolyester, giving PET copolyester good biodegradability. When combined with biodegradable polylactic acid, the material has a higher biodegradability and is more environmentally friendly, making it suitable for packaging materials such as cosmetic bottles. Detailed Implementation

[0013] The present invention is illustrated below with reference to specific embodiments, but the present invention is not limited to these embodiments.

[0014] The following polylactic acid, model PLA, is NatureWorks 4032D from the USA.

[0015] Example 1: (1) Add 0.96 mol lactic acid (CAS No. 79-33-4) and 1.84 mol triethylamine to 80 mL tetrahydrofuran, stir, then add 0.4 mol terephthaloyl chloride, stir at room temperature for 12 h, filter, distill the filtrate under reduced pressure, dilute with water, stir, and add 3% hydrochloric acid dropwise to adjust the pH of the solution to 3, filter, wash the precipitate with ice water, dry, and obtain terephthalic acid lactate. The reaction formula is: .

[0016] (2) Nitrogen gas was introduced into the reactor, and 3.72 mol of terephthalic acid, 0.28 mol of terephthalic acid lactate, 6.4 mol of ethylene glycol and 4 mmol of tetrabutyl titanate were added. The temperature of the top of the distillation column in the reactor was controlled at 100°C. The reactor was heated to 230°C and kept at this temperature until no water was generated. The reactor was then heated to 260°C and gradually evacuated until the vacuum degree of the reactor was 80 Pa. The reaction was continued for 4 hours, nitrogen gas was introduced, and the reactor was cooled with water to obtain PET copolyester.

[0017] (3) Mix 850g of PET copolyester, 150g of polylactic acid and 1g of antioxidant 1076 in a mixer, and then extrude the mixture through a twin-screw extruder. The temperatures of sections 1-7 are 170℃, 210℃, 235℃, 250℃, 260℃, 260℃ and 250℃, and the screw speed is 180r / min. Granulate the mixture to obtain a high-strength biodegradable material.

[0018] Example 2: (1) Add 1 mol of lactic acid and 2.1 mol of triethylamine to 100 mL of tetrahydrofuran, stir, add 0.5 mol of terephthaloyl chloride, stir at room temperature for 18 h, filter, distill the filtrate under reduced pressure, add water to dilute, stir, add 3% hydrochloric acid dropwise to adjust the pH of the solution to 2, filter, wash the precipitate with ice water, dry, and obtain terephthalic lactate.

[0019] (2) Nitrogen gas was introduced into the reactor, and 3.64 mol of terephthalic acid, 0.36 mol of terephthalic acid lactate, 6 mol of ethylene glycol and 4 mmol of tetrabutyl titanate were added. The temperature of the top of the distillation column in the reactor was controlled at 100°C. The reactor was heated to 230°C and kept at this temperature until no water was generated. The reactor was heated to 265°C and gradually evacuated until the vacuum degree of the reactor was 100 Pa. The reaction was continued for 3 hours, nitrogen gas was introduced, and the reactor was cooled with water to obtain PET copolyester.

[0020] (3) Mix 800g of PET copolyester, 200g of polylactic acid and 1.5g of antioxidant 1076 in a mixer, and then extrude the mixture through a twin-screw extruder. The temperatures of sections 1-7 are 170℃, 210℃, 235℃, 250℃, 260℃, 260℃ and 250℃, and the screw speed is 180r / min. Granulate the mixture to obtain a high-strength biodegradable material.

[0021] Example 3: (1) Add 1.32 mol lactic acid and 2.64 mol triethylamine to 130 mL tetrahydrofuran, stir, add 0.6 mol terephthaloyl chloride, stir at room temperature for 18 h, filter, distill the filtrate under reduced pressure, add water to dilute, stir, add 3% hydrochloric acid dropwise to adjust the pH of the solution to 3, filter, wash the precipitate with ice water, dry, and obtain terephthalic lactate.

[0022] (2) Nitrogen gas was introduced into the reactor, and 3.56 mol of terephthalic acid, 0.44 mol of terephthalic acid lactate, 6.4 mol of ethylene glycol and 3.6 mmol of tetrabutyl titanate were added. The temperature of the top of the distillation column in the reactor was controlled at 100°C. The reactor was heated to 230°C and kept at this temperature until no water was generated. The reactor was heated to 270°C and gradually evacuated until the vacuum degree of the reactor was 80 Pa. The reaction was continued for 3 hours. Nitrogen gas was introduced and the reactor was cooled with water to obtain PET copolyester.

[0023] (3) Mix 750g of PET copolyester, 250g of polylactic acid and 1.5g of antioxidant 1076 in a mixer, and then extrude the mixture through a twin-screw extruder. The temperatures of sections 1-7 are 170℃, 210℃, 235℃, 250℃, 260℃, 260℃ and 250℃, and the screw speed is 150r / min. Granulate the mixture to obtain a high-strength biodegradable material.

[0024] Example 4: (1) Add 1.92 mol lactic acid and 3.68 mol triethylamine to 180 mL tetrahydrofuran, stir, add 0.8 mol terephthaloyl chloride, stir at room temperature for 12 h, filter, distill the filtrate under reduced pressure, add water to dilute, stir, add 3% hydrochloric acid dropwise to adjust the pH of the solution to 2, filter, wash the precipitate with ice water, dry, and obtain terephthalic lactate.

[0025] (2) Nitrogen gas was introduced into the reactor, and 3.48 mol of terephthalic acid, 0.52 mol of terephthalic acid lactate, 7.2 mol of ethylene glycol and 4.8 mmol of tetrabutyl titanate were added. The temperature of the top of the distillation column in the reactor was controlled at 100°C. The reactor was heated to 220°C and kept at this temperature until no water was generated. The reactor was heated to 270°C and gradually evacuated until the vacuum degree of the reactor was 50 Pa. The reaction was continued for 3 hours. Nitrogen gas was introduced and the reactor was cooled with water to obtain PET copolyester.

[0026] (3) Mix 700g of PET copolyester, 300g of polylactic acid and 2g of antioxidant 1076 in a mixer, and then extrude the mixture through a twin-screw extruder. The temperatures of sections 1-7 are 170℃, 210℃, 235℃, 250℃, 260℃, 260℃ and 250℃, and the screw speed is 150r / min. Granulate the mixture to obtain a high-strength biodegradable material.

[0027] Example 5: (1) Add 1.2 mol lactic acid and 2.52 mol triethylamine to 120 mL tetrahydrofuran, stir, add 0.6 mol terephthaloyl chloride, stir at room temperature for 18 h, filter, distill the filtrate under reduced pressure, add water to dilute, stir, add 3% hydrochloric acid dropwise to adjust the pH of the solution to 2, filter, wash the precipitate with ice water, dry, and obtain terephthalic lactate.

[0028] (2) Nitrogen gas was introduced into the reactor, and 2.55 mol of terephthalic acid, 0.45 mol of terephthalic acid lactate, 5.1 mol of ethylene glycol and 3 mmol of tetrabutyl titanate were added. The temperature of the top of the distillation column in the reactor was controlled at 100°C. The reactor was heated to 245°C and kept at this temperature until no water was generated. The reactor was heated to 265°C and gradually evacuated until the vacuum degree of the reactor was 100 Pa. The reaction was continued for 4 hours, nitrogen gas was introduced, and the reactor was cooled with water to obtain PET copolyester.

[0029] (3) Mix 650g of PET copolyester, 350g of polylactic acid and 2g of antioxidant 1076 in a mixer, and then extrude the mixture through a twin-screw extruder. The temperatures of sections 1-7 are 170℃, 210℃, 235℃, 250℃, 260℃, 260℃ and 250℃, and the screw speed is 100r / min. Granulate the mixture to obtain a high-strength biodegradable material.

[0030] Comparative Example 1: (1) Nitrogen gas was introduced into the reactor, and 4 mol of terephthalic acid, 6.4 mol of ethylene glycol and 4 mmol of tetrabutyl titanate were added. The temperature of the top of the distillation column in the reactor was controlled at 100°C. The reactor was heated to 230°C and kept at this temperature until no water was generated. The reactor was heated to 260°C and gradually evacuated until the vacuum degree of the reactor was 80 Pa. The reaction was continued for 4 hours, nitrogen gas was introduced, and the reactor was cooled with water to obtain PET polyester.

[0031] (2) Mix 850g of PET polyester, 150g of polylactic acid and 1g of antioxidant 1076 in a mixer, and then extrude the mixture through a twin-screw extruder. The temperatures of sections 1-7 are 170℃, 210℃, 235℃, 250℃, 260℃, 260℃ and 250℃, and the screw speed is 180r / min. Granulate the mixture to obtain a biodegradable material.

[0032] Comparative Example 2: (1) Nitrogen gas was introduced into the reactor, and 3.72 mol of terephthalic acid, 0.28 mol of terephthalic acid, 6.4 mol of ethylene glycol and 4 mmol of tetrabutyl titanate were added. The temperature of the top of the distillation column in the reactor was controlled at 100°C. The temperature was heated to 230°C and kept at that temperature until no water was generated. The temperature was then raised to 260°C and the reactor was gradually evacuated until the vacuum degree was 80 Pa. The reaction was continued for 4 hours, nitrogen gas was introduced, and the reactor was cooled with water to obtain PET copolyester.

[0033] (2) Mix 850g of PET copolyester, 150g of polylactic acid and 1g of antioxidant 1076 in a mixer, and then extrude the mixture through a twin-screw extruder. The temperatures of sections 1-7 are 170℃, 210℃, 235℃, 250℃, 260℃, 260℃ and 250℃, and the screw speed is 180r / min. Granulate the mixture to obtain a biodegradable material.

[0034] Comparative Example 3: (1) Nitrogen gas was introduced into the reactor, and 3.72 mol of terephthalic acid, 0.28 mol of adipic acid, 6.4 mol of ethylene glycol and 4 mmol of tetrabutyl titanate were added. The temperature of the top of the distillation column in the reactor was controlled at 100°C. The reactor was heated to 230°C and kept at this temperature until no water was generated. The reactor was heated to 260°C and gradually evacuated until the vacuum degree of the reactor was 80 Pa. The reaction was continued for 4 hours, nitrogen gas was introduced, and the reactor was cooled with water to obtain PET copolyester.

[0035] (2) Mix 850g of PET copolyester, 150g of polylactic acid and 1g of antioxidant 1076 in a mixer, and then extrude the mixture through a twin-screw extruder. The temperatures of sections 1-7 are 170℃, 210℃, 235℃, 250℃, 260℃, 260℃ and 250℃, and the screw speed is 180r / min. Granulate the mixture to obtain a biodegradable material.

[0036] The biodegradable material was injection molded into samples using an injection molding machine, with temperatures of 250℃, 260℃, and 265℃ for stages 1-3. Tensile properties were tested according to GB / T1040.1-2025. The 90-day biodegradation rate was tested according to GB / T 19277.1-2025.

[0037] Table 1 Performance Tests

[0038] The low tensile strength and elongation at break of the biodegradable material in Comparative Example 1 are mainly due to the poor compatibility between PET (polyethylene terephthalate) and polylactic acid, which affects the mechanical properties of the material. Furthermore, PET is difficult to biodegrade, resulting in a low biodegradability. In the preparation of PET in each embodiment, terephthalic acid lactate diacid monomer was added to replace part of the terephthalic acid in the cocondensation reaction. This monomer contains a benzene ring structure, which allows the PET copolymer to maintain good mechanical strength without affecting the material's mechanical properties. Additionally, lactate structural units are introduced into the main chain of the PET copolyester molecule. This process enables PET copolyester and polylactic acid to have good interfacial compatibility, resulting in higher tensile strength and elongation at break, and excellent mechanical properties. Simultaneously, the fatty lactic acid ester structural units endow PET copolyester with good biodegradability, thereby improving the material's biodegradability and making it more environmentally friendly.

[0039] Compared with Example 1, Comparative Example 2 used terephthalic acid to replace part of the terephthalic acid, and the prepared PET copolyesters did not contain lactate structural units. The PET copolyesters had poor compatibility with polylactic acid, resulting in lower tensile strength and elongation at break of the material, as well as lower biodegradability.

[0040] Comparative Example 3 used adipic acid without benzene rings to replace part of the terephthalic acid. The prepared PET copolyesters did not contain lactic acid ester structural units. The PET copolyesters had poor compatibility with polylactic acid, and the tensile strength of the materials was significantly lower than that of Example 1.

[0041] The above description is merely a preferred embodiment of the present invention and should not be considered as limiting the scope of the embodiments of the present invention. The present invention is also not limited to the above examples; all equivalent changes and improvements made by those skilled in the art within the scope of the present invention should fall within the patent coverage of the present invention.

Claims

1. A method for preparing a high-strength degradable material, characterized in that, The high-strength biodegradable material comprises 65-85 parts by weight of PET copolyester, 15-35 parts by weight of polylactic acid, and 0.1-0.2 parts by weight of antioxidant. The preparation method includes: mixing PET copolyester, polylactic acid, and antioxidant in a mixer, and then extruding and granulating the mixture through a twin-screw extruder to obtain a high-strength biodegradable material.

2. The method for preparing the high-strength biodegradable material according to claim 1, characterized in that, The temperature of sections 1-7 of the twin-screw extruder is 170-260℃, and the screw speed is 100-180 r / min.

3. The method for preparing the high-strength biodegradable material according to claim 1, characterized in that, The preparation method of the PET copolyester is as follows: nitrogen gas is introduced into the reaction vessel, terephthalic acid, terephthalic lactate, ethylene glycol, and tetrabutyl titanate are added, the temperature of the top of the distillation column in the reaction vessel is controlled at 98-102℃, heated to 220-245℃, and kept at this temperature until no water is generated. The temperature is then raised to 260-270℃, and the vacuum degree of the reaction vessel is gradually evacuated to 50-100Pa. The reaction is continued for 3-4 hours, nitrogen gas is introduced, and the mixture is cooled with water to obtain the PET copolyester.

4. The method for preparing the high-strength biodegradable material according to claim 1, characterized in that, The molar ratio of terephthalic acid, terephthalic acid lactate, ethylene glycol, and tetrabutyl titanate is (85-93):(7-15):(150-180):(0.09-0.12).

5. The method for preparing the high-strength biodegradable material according to claim 1, characterized in that, The method for preparing the terephthalic acid lactate is as follows: lactic acid and triethylamine are added to tetrahydrofuran, and after stirring, terephthaloyl chloride is added. The mixture is stirred at room temperature for 12-18 hours, filtered, and the filtrate is distilled under reduced pressure. Water is added to dilute the filtrate, and hydrochloric acid is added dropwise after stirring. The mixture is then filtered, and the precipitate is washed with ice water and dried to obtain terephthalic acid lactate.

6. The method for preparing the high-strength biodegradable material according to claim 5, characterized in that, The molar ratio of lactic acid, triethylamine, and terephthaloyl chloride is (2-2.4):(4.2-4.6):

1.

7. The method for preparing the high-strength biodegradable material according to claim 5, characterized in that, The pH is adjusted to 2-3 by adding hydrochloric acid.

8. A high-strength biodegradable material obtained by the preparation method according to any one of claims 1-7.

9. The application of the high-strength biodegradable material as described in claim 8 in cosmetic packaging bottles.