Preparation method of hydrolysis-resistant and low-temperature-resistant polyester polyols

By introducing long carbon-chain hydrophobic side chains into polyester polyols and using a stepwise esterification process to passivate terminal carboxyl groups with polymeric polycarbodiimide, the problems of hydrolysis resistance and low-temperature resistance of polyester polyols were solved, and the performance stability of the material under low temperature and humid heat conditions was improved.

CN123107322APending Publication Date: 2026-11-17SHANDONG INOV POLYURETHANE
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202611610005.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot simultaneously improve the hydrolysis resistance and low-temperature resistance of polyester polyols. Traditional methods have limited effectiveness in improving hydrolysis resistance or low-temperature performance and suffer from problems such as gelation and uneven dispersion.

Method used

By introducing long carbon-chain hydrophobic side chains into the polyester main chain through a stepwise esterification process, and combining it with medium- and low-temperature end-group passivation technology, polymeric polycarbodiimide is used to capture residual end carboxyl groups, forming a hydrolysis-resistant and low-temperature-resistant polyester polyol.

Benefits of technology

It improves the flexibility and hydrolysis resistance of polyester polyols in low-temperature environments, and the material exhibits low mechanical property degradation under humid and hot conditions, making it suitable for frozen packaging and extremely cold working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of polyurethane raw material synthesis technology, specifically a method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyols. The method includes: pre-esterifying an aliphatic trifunctional polyol with a long-chain aliphatic monobasic acid to obtain a long-chain hydrophobic side-chain modified alcohol intermediate; adding a branched diol and an aliphatic diacid to the intermediate, followed by esterification and gradient negative compression polymerization to obtain the polyester polyol; cooling after polycondensation to the target temperature, adding a polymerizable polycarbodiimide, and maintaining the temperature with stirring to obtain the final product. This invention utilizes the synergistic effect of the physical shielding effect of the long-chain hydrophobic side chain and the chemical removal effect of the terminal carboxyl groups of the polycarbodiimide to simultaneously improve the hydrolysis resistance and low-temperature resistance of the polyester polyol. The process is stable and suitable for applications such as cold chain packaging and high-temperature sterilization soft packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polyurethane raw material synthesis technology, specifically to a method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyols. Background Technology

[0002] Polyester polyols are important raw materials for the preparation of polyurethane adhesives, elastomers, and coating materials. However, the ester bonds in the polyester molecular chain are prone to hydrolytic breakage under humid and hot conditions, and the carboxyl groups produced by hydrolysis can further catalyze the hydrolysis of ester bonds, leading to a continuous decline in the mechanical properties of the products. Meanwhile, traditional linear aliphatic polyester polyols have regular molecular structures and high crystallinity, resulting in reduced molecular chain mobility at low temperatures, making the materials prone to brittleness and adhesion failure. Therefore, how to simultaneously improve the hydrolysis resistance and low-temperature resistance of polyester polyols is a technical problem of ongoing concern in this field.

[0003] To improve hydrolysis resistance, existing technologies often employ the addition of carbodiimide compounds. For example, Chinese patent application CN105940053A, published on September 14, 2016, discloses a polyester resin composition containing a polyester resin and a carbodiimide compound. The carbodiimide groups capture the carboxyl groups in the polyester, inhibiting the autocatalytic hydrolysis reaction. This technical solution mainly targets the polyester resin composition and has limited improvement on the low-temperature performance of the polyester polyol itself. Chinese patent application CN104804698A, published on July 29, 2015, discloses a two-component composite adhesive for solar backsheets, wherein after esterification and polycondensation of the polyester polyol, the esterification vessel is cooled to 110°C before adding polycarbodiimide. This document discloses the operation of adding polycarbodiimide after cooling following polycondensation, but it does not address the introduction of long-chain hydrophobic side chains, and the selection of the subsequent temperature window is not optimized for a specific polyester structure.

[0004] In improving low-temperature performance, existing technologies often reduce crystallinity by introducing long-chain side chains or branched structures. Chinese patent application CN114634616A, published on June 17, 2022, discloses a modified polyester polyol whose main chain structure contains at least one ether bond and at least one side chain near the ester end. The side chain is selected from saturated or unsaturated hydrocarbon groups with 1-5 carbon atoms, utilizing the steric hindrance of the side chain to improve hydrolysis resistance. However, the short carbon number of the side chain in this document limits its improvement effect on hydrophobic shielding and low-temperature toughness. European patent application EP0201100B1, published on November 12, 1986, discloses a polyester containing side chains, using a monocarboxylic acid ester of trimethylolpropane as one of the starting materials. The monocarboxylic acid can have 4-18 carbon atoms. However, this document aims at general polyester modification and does not address the synergistic improvement of hydrolysis resistance and low-temperature resistance in polyester polyols. Chinese patent application CN102970964A, published on March 13, 2013, discloses the monoesterification reaction of polyols with C6-C21 monocarboxylic acids for the preparation of polyglycerol low-polyesters, but does not address the issues of hydrolysis resistance and low-temperature resistance of polyester polyols.

[0005] Furthermore, Chinese patent application CN121592243A, published on March 3, 2026, discloses a biodegradable bio-based polyurethane wood protective coating, which mentions a synergistic approach of capturing long-chain alkyl hydrophobic groups and carbodiimide carboxyl groups, but its hydrophobic chain source and system differ from this solution. Chinese patent application CN1189179A, published on July 29, 1998, discloses a general concept of partially esterifying polyols with monocarboxylic acids, but does not specifically address the monoesterification of trifunctional alcohols with C8-C18 monocarboxylic acids for hydrolysis / low-temperature resistance modification of polyester polyols.

[0006] In summary, while existing technologies disclose methods for improving hydrolysis resistance with carbodiimide and improving low-temperature or hydrophobic properties with long-chain side chains, a scheme that simultaneously achieves synergistic improvement in low-temperature resistance and hydrolysis resistance by pre-esterifying C8-C18 long-chain monocarboxylic acids with trifunctional alcohols to form long-chain hydrophobic side-chain intermediates, then stepwise polycondensing them with branched diols and aliphatic diacids, and finally adding polymerizable polycarbodiimide at 130-150℃ after polycondensation, has not yet been clearly disclosed. Furthermore, direct polycondensation of trifunctional alcohols can easily lead to gelation, and improper selection of the subsequent addition temperature can result in uneven dispersion or excessively rapid reactions, problems that remain to be solved. Summary of the Invention

[0007] In view of the shortcomings of the prior art, the purpose of this invention is to provide a method for preparing a hydrolysis-resistant and low-temperature-resistant polyester polyol. By using a stepwise esterification process, long carbon chain hydrophobic side chains are orderly introduced into the polyester main chain, and combined with medium- and low-temperature end-group passivation technology, the overall performance of the polyester polyol is improved.

[0008] This invention is achieved using the following technical solution: The method for preparing the hydrolysis-resistant and low-temperature-resistant polyester polyol includes the following steps: (1) An aliphatic trifunctional polyol is subjected to an esterification and dehydration reaction with a C8-C18 aliphatic monoacid until the acid value of the system is ≤5 mgKOH / g, thereby obtaining a long-chain hydrophobic side-chain modified alcohol intermediate; wherein, the molar ratio of the aliphatic trifunctional polyol to the C8-C18 aliphatic monoacid is 1:(0.8-1.2), preferably 1:(0.9-1.1); (2) Add branched diol and aliphatic diacid to the intermediate obtained in step (1) and perform atmospheric pressure esterification. After the water output is stable, perform negative compression polymerization and polycondensation until the acid value of the system is ≤1.0 mgKOH / g. (3) After the polycondensation reaction is completed, the system is cooled to 130-150 °C, and polymeric polycarbodiimide is added. The mixture is kept warm and stirred to obtain the hydrolysis-resistant and low-temperature-resistant polyester polyol.

[0009] Preferably, the aliphatic trifunctional polyol in step (1) is glycerol or trimethylolpropane; the C8-C18 aliphatic monocarboxylic acid is a saturated aliphatic monocarboxylic acid selected from one or more of octanoic acid, lauric acid, myristic acid, and stearic acid.

[0010] Aliphatic monoacids with C8 or higher are chosen because short carbon chains (such as C6 and below) lack sufficient steric hindrance and hydrophobic effects, making it difficult to provide adequate physical shielding. Conversely, carbon chains longer than C18 are solid at room temperature and have low reactivity, hindering the smooth progress of esterification. Controlling the molar ratio of trifunctional polyol to monoacid at 1:(0.9-1.1) aims to selectively consume one hydroxyl group in the trifunctional polyol, reducing its overall average functionality to approximately 2.0. This effectively avoids the risk of gelation caused by trifunctional monomers in subsequent polycondensation steps. Requiring the acid value to be ≤5 mgKOH / g in this step ensures the monoacid reacts completely, preventing competitive disordered reactions when adding the dicarboxylic acid in the second step and maintaining the relative regularity of the side chain distribution.

[0011] Preferably, the branched diol in step (2) is selected from at least one of neopentyl glycol, 2-methyl-1,3-propanediol, 3-methyl-1,5-pentanediol, and 2-butyl-2-ethyl-1,3-propanediol; and the aliphatic dicarboxylic acid is selected from one or more of succinic acid, octanoic acid, azelaic acid, and sebacic acid.

[0012] The introduction of branched diol side groups can have a synergistic effect with the long carbon chain hydrophobic side chains formed in step (1), further disrupting the regular stacking of the polyester main chain, reducing the tendency to crystallize, and giving the material better low-temperature flexibility.

[0013] Preferably, the esterification dehydration reaction in step (1) is carried out at a temperature of 180-200 °C and under the protection of an organotitanium catalyst and an inert gas. The organotitanium catalyst is selected from one or more of tetrabutyl titanate, tetraethyl titanate, and tetraisopropyl titanate, and its addition amount is 10-200 ppm of the total monomer mass.

[0014] Organotitanium catalysts have high catalytic efficiency. The temperature range of 180-200 ℃ can ensure the efficient esterification and dehydration while avoiding side reactions such as etherification caused by excessive high temperature. The inert gas protection helps to prevent the material from oxidizing and turning yellow at high temperature.

[0015] Preferably, the heating temperature for atmospheric pressure esterification in step (2) is 210-230 °C; the hydroxyl value of the system obtained by negative compression polycondensation is 50-150 mgKOH / g.

[0016] The above-mentioned hydroxyl value range corresponds to a specific polyester molecular weight, which can meet the conventional processing requirements for it as a polyurethane prepolymer or elastomer soft segment, balancing the mechanical strength and processing viscosity of polyurethane products.

[0017] Preferably, the negative compression polymerization in step (2) adopts a two-stage gradient vacuum polymerization: the first stage has a vacuum degree of -0.03 to -0.05 MPa and a reaction time of 1 to 2 h; the second stage has a vacuum degree of -0.07 to -0.09 MPa and a reaction time of 2 to 4 h.

[0018] The use of gradient negative pressure instead of direct high vacuum is to smoothly extract a large amount of generated water in the first stage, preventing low-boiling-point monomers (such as diols) from being removed in large quantities with water vapor, which would lead to an imbalance in the ratio. The use of high vacuum in the second stage aims to break the chemical equilibrium, promote the condensation reaction towards higher molecular weight, and ensure that the final acid value meets the standard.

[0019] Preferably, in step (2), when feeding materials, the ratio of the total hydroxyl equivalent of the long-chain hydrophobic side-chain modified alcohol intermediate and the branched diol to the carboxyl equivalent of the aliphatic dicarboxylic acid is (1.1-1.8):1; the molar ratio of the long-chain hydrophobic side-chain modified alcohol intermediate obtained in step (1) to the branched diol in step (2) is 1:(3-10).

[0020] The above-mentioned ratio limits ensure that the polyester polyol is capped with hydroxyl groups; at the same time, the specific molar ratio of intermediate to branched diol is intended to balance the relationship between the hydrophobic modification effect brought by the long carbon chain side chain and the mechanical properties of the main chain. If the proportion of intermediate is too high, it may lead to a decrease in the mechanical strength of the polyester; if it is too low, it will be difficult to achieve the expected hydrolysis resistance and low temperature resistance.

[0021] Preferably, the amount of polymeric polycarbodiimide added in step (3) is 0.5%-2.0% of the mass of the polyester polyol, and the time for heat preservation and stirring is 30-60 min.

[0022] In step (3), after the polycondensation reaches the target, the temperature is lowered to 130-150℃ before adding the polymeric polycarbodiimide. The selection of this temperature window is based on the following considerations: when the temperature is below 130℃, the viscosity of the specific polyester polyol (containing long-chain hydrophobic side chains and branched diol structures) in this scheme is too high, making it difficult to achieve uniform dispersion of the polycarbodiimide; when the temperature is above 150℃, the reaction rate between the carbodiimide and the terminal carboxyl groups is too fast, which may lead to local reactions before uniform dispersion, resulting in uneven crosslinking or gelation. This temperature window is a suitable range for achieving uniform dispersion and controllable reaction, rather than being limited by the thermal decomposition temperature of the carbodiimide (the 5% thermogravimetric temperature of polymeric carbodiimide is usually above 330℃).

[0023] This invention combines physical structure design with chemical end-group passivation to achieve synergistic mechanism: (1) Physical regulation of aggregated structure: This invention uses a pre-esterification process to graft long-chain alkyl groups of C8-C18 into polyester molecules to form pendant side chains. At the macroscopic mechanical level, these flexible long side chains act like internal plasticizers, increasing the free volume between molecular chains and inhibiting the crystallization behavior of polyester at low temperatures, thereby maintaining the low-temperature resilience and flexibility of the material. At the hydrolysis resistance level, due to their strong hydrophobicity, the long alkyl side chains form a local hydrophobic microenvironment (hydrophobic shielding layer) inside the polyester matrix, which can effectively block the penetration and diffusion of external water molecules into the polar ester bond region, reducing the probability of contact between water molecules and ester bonds.

[0024] (2) Construction of a chemical defense: The hydrolysis of polyester is usually an autocatalytic process (the carboxyl groups generated by the hydrolysis of ester bonds accelerate further hydrolysis). This invention introduces polymeric polycarbodiimide into a specific cooling window as a "proton scavenger" to precisely capture the residual terminal carboxyl groups in the system. This effectively cuts off the autocatalytic cycle of the hydrolysis reaction at the chemical level. Physical shielding prevents water molecules from entering, and chemical passivation eliminates catalytic factors. The combination of these two measures improves the intrinsic resistance of the material to wet hot water hydrolysis.

[0025] (3) Stepwise controllable synthesis process: Traditional single-step methods are prone to triggering gel crosslinking points if trifunctional monomers are used directly. The stepwise synthesis method of this invention first consumes one site of the trifunctional alcohol and converts it into a near-bifunctional monomer with a longer side chain, which effectively avoids the risk of crosslinking in the later stage of polycondensation and ensures the relative regularity of the polyester main chain structure and the stability of batch production.

[0026] Compared with the prior art, the beneficial effects of the present invention are: (1) This invention utilizes the hydrophobic side chains of long alkyl groups with C8 or higher and the branched diols to synergistically disrupt the regularity of the main chain and inhibit low-temperature crystallization behavior. The elastomer prepared from this polyester polyol exhibits little change in hardness under low-temperature environments such as -20 ℃, and has good low-temperature compression set performance, which can meet the application requirements of frozen packaging, extremely cold working conditions and other applications.

[0027] (2) This invention reduces the risk of ester bond breakage through the synergistic effect of "long carbon chain hydrophobic physical shielding" and "carbodiimide terminal carboxyl group chemical removal". Under damp heat aging (e.g., 85 ℃, 85% RH) treatment, the materials prepared using the polyester of this invention can maintain a high tensile strength retention rate and elongation at break retention rate, and the mechanical properties have a low degree of degradation.

[0028] (3) The stepwise pre-esterification process used in this invention has a wide operating window, effectively avoiding the risk of gelation caused by crosslinking. The synthesized polyester molecules have regular structures and stable batch quality. At the same time, the raw materials used are all bulk industrial products, and the synthesis route is compatible with existing polyester production equipment. No complicated equipment modifications are required, and it has excellent prospects for large-scale production. Detailed Implementation

[0029] To make the objectives and technical solutions of this invention clearer, the invention will be further described in detail below.

[0030] All raw materials used in the embodiments of this invention are commercially available industrial-grade products. Among them: polycarbodiimide: HyMax ® 2010H, HyMax ® 213, industrial grade, Shanghai Langyi; the remaining small molecule diols, diacids and organotitanium catalysts are all commercially available analytical grade or industrial grade reagents, and their specific specifications will not be repeated.

[0031] Example 1 This embodiment provides a method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyols, including the following steps: (1) Take 134.2g (1.0mol) of trimethylolpropane and 200.3g (1.0mol) of lauric acid, add tetrabutyl titanate (80ppm of the total monomer mass), stir and heat to 190℃ for esterification and dehydration, and react until the acid value of the system is 4.3mgKOH / g to obtain a long carbon chain hydrophobic side chain modified alcohol intermediate.

[0032] (2) Add 792.0 g (7.61 mol) of neopentyl glycol and 966.0 g (6.61 mol) of adipic acid to the above intermediate, heat to 220 °C, and esterify under normal pressure to remove water. After the water removal is stable, start gradient negative compression polymerization: the first stage vacuum degree is -0.04 MPa and the reaction is 1.5 h; the second stage vacuum degree is -0.08 MPa and the reaction is 3 h, and the polycondensation is carried out until the acid value of the system is 0.48 mg KOH / g and the hydroxyl value is 110.7 mg KOH / g.

[0033] (3) After the polycondensation reaches the standard, the vacuum is broken, the temperature is lowered to 140℃, and 1.0% (by weight) of polycarbodiimide (HyMax) is added to the polyester polyol. ® 2010H), keep warm and stir for 45 minutes; continue to cool and discharge to obtain hydrolysis-resistant and low-temperature resistant polyester polyol A1.

[0034] Example 2 This embodiment provides a method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyols, including the following steps: (1) Take 92.1g (1.0mol) of glycerol and 256.4g (0.9mol) of stearic acid, add tetraisopropyl titanate (10ppm of the total monomer mass), under nitrogen protection, heat to 200℃ and keep warm for esterification and dehydration, and react until the acid value of the system is 4.1mgKOH / g to obtain a long carbon chain hydrophobic side chain modified alcohol intermediate.

[0035] (2) Add 901.2 g (10.0 mol) of 2-methyl-1,3-propanediol and 1957 g (9.67 mol) of sebacic acid to the above intermediate, heat to 230 °C, and esterify under normal pressure to remove water. After the water removal is stable, start gradient negative compression polymerization: the first stage vacuum degree is -0.03 MPa, and the reaction is carried out for 2 h; the second stage vacuum degree is -0.09 MPa, and the reaction is carried out for 2 h, and polycondensation is carried out until the acid value of the system is 0.8 mg KOH / g and the hydroxyl value is 53.1 mg KOH / g.

[0036] (3) After the polycondensation reaches the standard, the vacuum is broken, the temperature is lowered to 130℃, and 0.5% of polycarbodiimide (HyMax) by mass of polyester polyol is added. ® 2010H), keep warm and stir for 30 minutes; continue to cool and discharge to obtain hydrolysis-resistant and low-temperature resistant polyester polyol A2.

[0037] Example 3 This embodiment provides a method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyols, including the following steps: (1) Take 134.2 g (1.0 mol) of trimethylolpropane and 129.8 g (0.9 mol) of octanoic acid, add tetraethyl titanate (60 ppm of total monomer mass), under nitrogen protection, heat to 190 °C and keep warm for esterification and dehydration, and react until the acid value of the system is 3.9 mg KOH / g to obtain a long carbon chain hydrophobic side chain modified alcohol intermediate.

[0038] (2) Add 312.2g (3.0mol) of neopentyl glycol and 451.3g (3.09mol) of adipic acid to the above intermediate, heat to 220℃, esterify under normal pressure to remove water, and after the water removal is stable, start gradient negative compression polymerization: the first stage vacuum degree is -0.03MPa, and the reaction is carried out for 1h; the second stage vacuum degree is -0.07MPa, and the reaction is carried out for 4h, and the polycondensation is carried out until the acid value of the system is 0.76mgKOH / g and the hydroxyl value is 97.6mgKOH / g.

[0039] (3) After the polycondensation reaches the standard, the vacuum is broken, the temperature is lowered to 150℃, and 2.0% (by weight) of polycarbodiimide (HyMax) is added to the polyester polyol. ® 2010H), keep warm and stir for 60 minutes; continue to cool and discharge to obtain hydrolysis-resistant and low-temperature resistant polyester polyol A3.

[0040] Example 4 This embodiment provides a method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyols, including the following steps: (1) Take 92.1g (1.0mol) of glycerol and 251.4g (1.1mol) of myristic acid, add tetrabutyl titanate (180ppm of total monomer mass), under nitrogen protection, heat to 195℃ and keep warm for esterification and dehydration, and react until the acid value of the system is 4.5mgKOH / g to obtain a long carbon chain hydrophobic side chain modified alcohol intermediate.

[0041] (2) Add 1602.5g (10.0mol) of 2-butyl-2-ethyl-1,3-propanediol and 1258.3g (6.22mol) of sebacic acid to the above intermediate, heat to 225℃, esterify under normal pressure to remove water, and after the water removal is stable, start gradient negative compression polymerization: the first stage vacuum degree is -0.05MPa, and the reaction is carried out for 2h; the second stage vacuum degree is -0.09MPa, and the reaction is carried out for 2h, and polycondensation is carried out until the acid value of the system is 0.48mgKOH / g and the hydroxyl value is 148.7mgKOH / g.

[0042] (3) After the polycondensation reaches the standard, the vacuum is broken, the temperature is lowered to 150°C, and 1.0% (by weight) of polycarbodiimide (HyMax) is added to the polyester polyol. ® 213), keep warm and stir for 60 minutes; continue to cool down and discharge the material to obtain hydrolysis-resistant and low-temperature resistant polyester polyol A4.

[0043] Comparative Example 1 A method for preparing polyester polyols includes the following steps: Polyester polyols were synthesized using the traditional one-pot method without preparing long-chain hydrophobic side-chain modified alcohol intermediates. 134.2 g (1.0 mol) of trimethylolpropane, 200.3 g (1.0 mol) of lauric acid, 792.0 g (7.61 mol) of neopentyl glycol, and 966.0 g (6.61 mol) of adipic acid were added to the reactor in one batch, along with tetrabutyl titanate (80 ppm of the total monomer mass). Under nitrogen protection, the mixture was heated to 220 °C and subjected to atmospheric pressure for esterification to produce water. After the water output stabilized, gradient negative compression polymerization was initiated: the first stage was carried out under a vacuum of -0.04 MPa for 1.5 h; the second stage was carried out under a vacuum of -0.08 MPa for 3 h. During the polymerization process, the system gelled to obtain liquid polyester polyol D1.

[0044] Comparative Example 2 A method for preparing polyester polyols includes the following steps: The long-chain hydrophobic side-chain modified alcohol intermediate in step (1) is replaced with a hydroxyl equivalent of a common diol; (1) Take 90.1g (1mol) of 1,4-butanediol, 792.0g (7.61mol) of neopentyl glycol and 966.0g (6.61mol) of adipic acid, heat to 220℃, esterify under normal pressure to remove water, and after the water removal is stable, start gradient negative compression polymerization: the first stage vacuum degree is -0.04MPa, and the reaction is 1.5h; the second stage vacuum degree is -0.08MPa, and the reaction is 3h, and the polycondensation is carried out until the acid value of the system is 0.42mgKOH / g and the hydroxyl value is 110.9mgKOH / g.

[0045] (2) After the polycondensation reaches the standard, the vacuum is broken, the temperature is lowered to 140℃, and 1.0% (by weight) of polycarbodiimide (HyMax) is added to the polyester polyol. ® 2010H), keep warm and stir for 45 minutes; continue to cool and discharge to obtain hydrolysis-resistant and low-temperature resistant polyester polyol D2.

[0046] Comparative Example 3 A method for preparing polyester polyols includes the following steps: No polycarbodiimide added; (1) Take 134.2g (1.0mol) of trimethylolpropane and 200.3g (1.0mol) of lauric acid, add tetrabutyl titanate (80ppm of the total monomer mass), stir and heat to 190℃ for esterification and dehydration, and react until the acid value of the system is 4.3mgKOH / g to obtain a long carbon chain hydrophobic side chain modified alcohol intermediate.

[0047] (2) Add 792.0 g (7.61 mol) of neopentyl glycol and 966.0 g (6.61 mol) of adipic acid to the above intermediate, heat to 220 °C, and esterify under normal pressure to remove water. After the water removal is stable, start gradient negative compression polymerization: the first stage vacuum degree is -0.04 MPa and the reaction is 1.5 h; the second stage vacuum degree is -0.08 MPa and the reaction is 3 h, and the polycondensation is carried out until the acid value of the system is 0.48 mg KOH / g and the hydroxyl value is 110.5 mg KOH / g.

[0048] (3) After the polycondensation reaches the standard, the vacuum is broken, the material is cooled and discharged to obtain hydrolysis-resistant and low-temperature resistant polyester polyol D3.

[0049] Comparative Example 4 A method for preparing polyester polyols includes the following steps: C6 short-chain monocarboxylic acid, hexanoic acid replaces lauric acid; (1) Take 134.2g (1.0mol) of trimethylolpropane and 116.2g (1.0mol) of hexanoic acid, add tetrabutyl titanate (80ppm of the total monomer mass), stir and heat to 190℃ for esterification and dehydration, and react until the acid value of the system is 4.2mgKOH / g to obtain the modified alcohol intermediate.

[0050] (2) Add 792.0 g (7.61 mol) of neopentyl glycol and 966.0 g (6.61 mol) of adipic acid to the above intermediate, heat to 220 °C, and esterify under normal pressure to remove water; after the water removal is stable, start gradient negative compression polymerization: the first stage vacuum degree is -0.04 MPa, and the reaction is 1.5 h; the second stage vacuum degree is -0.08 MPa, and the reaction is 3 h, and the polycondensation is carried out until the acid value of the system is 0.78 mg KOH / g and the hydroxyl value is 110.4 mg KOH / g.

[0051] (3) After the polycondensation reaches the standard, the vacuum is broken and the temperature is lowered to 140°C. 1.0% of the mass of polycarbodiimide (HyMax®2010H) of polyester polyol is added and stirred for 45 minutes. The temperature is then lowered and the material is discharged to obtain polyester polyol D4.

[0052] Comparative Example 5 A method for preparing polyester polyols includes the following steps: (1) Take 134.2g (1.0mol) of trimethylolpropane and 312.5g (1.0mol) of icosanoic acid, add tetrabutyl titanate (80ppm of the total monomer mass), stir and heat to 190℃ for esterification and dehydration, and react until the acid value of the system is 4.6mgKOH / g to obtain the modified alcohol intermediate.

[0053] (2) Add 792.0 g (7.61 mol) of neopentyl glycol and 966.0 g (6.61 mol) of adipic acid to the above intermediate, heat to 220 °C, and esterify under normal pressure to remove water; after the water removal is stable, start gradient negative compression polymerization: the first stage vacuum degree is -0.04 MPa, and the reaction is 1.5 h; the second stage vacuum degree is -0.08 MPa, and the reaction is 3 h, and the polycondensation is carried out until the acid value of the system is 0.75 mg KOH / g and the hydroxyl value is 111.0 mg KOH / g.

[0054] (3) After the polycondensation reaches the standard, the vacuum is broken and the temperature is lowered to 140°C. 1.0% of the mass of polycarbodiimide (HyMax®2010H) of polyester polyol is added and the mixture is kept warm and stirred for 45 minutes. The material is discharged after cooling to obtain polyester polyol D5.

[0055] Comparative Example 6 A method for preparing polyester polyols includes the following steps: (1) Take 134.2g (1.0mol) of trimethylolpropane and 200.3g (1.0mol) of lauric acid, add tetrabutyl titanate (80ppm of the total monomer mass), stir and heat to 190℃ for esterification and dehydration, and react until the acid value of the system is 4.3mgKOH / g to obtain a long carbon chain hydrophobic side chain modified alcohol intermediate.

[0056] (2) Add 792.0 g (7.61 mol) of neopentyl glycol and 966.0 g (6.61 mol) of adipic acid to the above intermediate, heat to 220 °C, and esterify under normal pressure to remove water; after the water removal is stable, start gradient negative compression polymerization: the first stage vacuum degree is -0.04 MPa, and the reaction is 1.5 h; the second stage vacuum degree is -0.08 MPa, and the reaction is 3 h, and the polycondensation is carried out until the acid value of the system is 0.48 mg KOH / g and the hydroxyl value is 110.7 mg KOH / g.

[0057] (3) After the polycondensation reaches the standard, the vacuum is broken and the temperature is lowered to 110°C. 1.0% of the mass of polycarbodiimide (HyMax®2010H) of polyester polyol is added and stirred for 45 minutes. The temperature is then lowered and the material is discharged to obtain polyester polyol D6.

[0058] Comparative Example 7 A method for preparing polyester polyols includes the following steps: (1) Take 134.2g (1.0mol) of trimethylolpropane and 200.3g (1.0mol) of lauric acid, add tetrabutyl titanate (80ppm of the total monomer mass), stir and heat to 190℃ for esterification and dehydration, and react until the acid value of the system is 4.3mgKOH / g to obtain a long carbon chain hydrophobic side chain modified alcohol intermediate.

[0059] (2) Add 792.0 g (7.61 mol) of neopentyl glycol and 966.0 g (6.61 mol) of adipic acid to the above intermediate, heat to 220 °C, and esterify under normal pressure to remove water; after the water removal is stable, start gradient negative compression polymerization: the first stage vacuum degree is -0.04 MPa, and the reaction is 1.5 h; the second stage vacuum degree is -0.08 MPa, and the reaction is 3 h, and the polycondensation is carried out until the acid value of the system is 0.48 mg KOH / g and the hydroxyl value is 110.7 mg KOH / g.

[0060] (3) After the polycondensation reaches the standard, the vacuum is broken and the temperature is lowered to 170°C. 1.0% of the mass of polycarbodiimide (HyMax®2010H) of polyester polyol is added and stirred for 45 minutes. The temperature is then lowered and the material is discharged to obtain polyester polyol D7.

[0061] Comparative Example 8 A method for preparing polyester polyols includes the following steps: (1) Take 134.2g (1.0mol) of trimethylolpropane and 100.15g (0.5mol) of lauric acid, add tetrabutyl titanate (80ppm of the total monomer mass), under nitrogen protection, stir and heat to 190℃ for esterification and dehydration, and react until the acid value of the system is 4.1mgKOH / g to obtain the modified alcohol intermediate.

[0062] (2) Add 792.0 g (7.61 mol) of neopentyl glycol and 966.0 g (6.61 mol) of adipic acid to the above intermediate, heat to 220°C, and esterify under normal pressure to remove water; after the water removal is stable, start gradient negative compression polymerization and perform the same gradient vacuum process polycondensation as in Example 1 to produce gel, and obtain polyester polyol D8.

[0063] Comparative Example 9 A method for preparing polyester polyols includes the following steps: (1) Take 134.2g (1.0mol) of trimethylolpropane and 300.45g (1.5mol) of lauric acid, add tetrabutyl titanate (80ppm of the total monomer mass), stir and heat to 190℃ for esterification and dehydration, and react until the acid value of the system is 4.9mgKOH / g to obtain the modified alcohol intermediate.

[0064] (2) Add 792.0 g (7.61 mol) of neopentyl glycol and 966.0 g (6.61 mol) of adipic acid to the above intermediate, heat to 220 °C, and esterify under normal pressure to remove water; after the water removal is stable, start gradient negative compression polymerization: the first stage vacuum degree is -0.04 MPa, and the reaction is 1.5 h; the second stage vacuum degree is -0.08 MPa, and the reaction is 3 h, and the polycondensation is carried out until the acid value of the system is 0.71 mg KOH / g and the hydroxyl value is 101.3 mg KOH / g.

[0065] (3) After the polycondensation reaches the standard, the vacuum is broken and the temperature is lowered to 140°C. 1.0% of the mass of polycarbodiimide (HyMax®2010H) of polyester polyol is added and stirred for 45 minutes. The temperature is then lowered and the material is discharged to obtain polyester polyol D9.

[0066] The polyester polyols obtained in the examples and comparative examples were prepolymerized with diphenylmethane diisocyanate (MDI) at an isocyanate index (NCO / OH molar ratio) of 1.05:1. 1,4-Butanediol was used as the chain extender, and the molar ratio of prepolymer to chain extender was 1:2. The prepolymer was cast using the prepolymer method. The vulcanization conditions were 110 ℃ × 2 h, followed by curing at room temperature (23 ℃) for 7 days before performance testing.

[0067] The testing methods for each indicator of this invention are as follows: The hydroxyl value was determined using the acetylation method, referring to HG / T 2709-2022 (Determination of hydroxyl value of polyester polyols used in the production of polyurethane in plastics).

[0068] The acid value was determined according to HG / T 2708-1995 (Determination of Acid Value in Polyester Polyols). The sample was dissolved in ethanol and titrated with potassium hydroxide ethanol solution to the phenolphthalein endpoint.

[0069] Evaluation of hydrolysis resistance (characterized by retention rate of mechanical properties after damp heat aging): (1) Moist heat aging treatment In accordance with ISO 4611 standard, the elastomer samples were placed in a constant temperature and humidity chamber at 85 ℃ and 85% RH for 28 days of aging treatment. After removal, the samples were conditioned at 23 ℃ and 50% RH for 24 hours before mechanical property testing.

[0070] (2) Determination of tensile property retention rate Referring to GB / T 528 "Determination of Tensile Stress-Strain Properties of Vulcanized Rubber or Thermoplastic Rubber", dumbbell-shaped specimens were used, and the tensile speed was 500 mm / min. The tensile strength and elongation at break before and after aging were determined, and the retention rate was calculated using the following formula: Tensile strength retention rate (%) = (Tensile strength after aging / Tensile strength before aging) × 100% Elongation at break retention rate (%) = (Elongation at break after aging / Elongation at break before aging) × 100% Low-temperature performance evaluation: Low-temperature hardness change determination, referring to GB / T 2411 and ASTM D2240 standards, involves placing the sample in a -20℃ low-temperature chamber for 2 hours and measuring the Shore A hardness at -20℃ in situ within the chamber; simultaneously, the Shore A hardness at 23℃ room temperature is also measured. A smaller change in low-temperature hardness indicates a smaller increase in rigidity at low temperatures and better low-temperature flexibility.

[0071] Compression set test: The compression set rate of the elastomer was tested at 23 ℃ or low temperature (-20 ℃) ​​according to GB / T 7759.1 and ISO 815-2 standards. The cylindrical specimen was compressed to 75% of its original height, held for 24 h, unloaded, and allowed to recover at 23 ℃ for 30 min. The residual deformation was then measured.

[0072] Test data for the examples and comparative examples are shown in Table 1.

[0073] Table 1: Test data for examples and comparative examples

[0074] Note: Comparative Examples 1 and 8 gels, no data available.

[0075] As shown in Table 1, after 28 days of wet heat aging, the elastomers in Examples 1-4 exhibited tensile strength retention of ≥87% and elongation at break retention of ≥82%; the difference in Shore A hardness between room temperature and -20℃ was ≤5, indicating low low-temperature compression set and excellent hydrolysis resistance and low-temperature flexibility. Comparative Example 2, lacking long carbon chain hydrophobic side chains, showed decreased hydrolysis resistance and low-temperature performance, confirming that long carbon chain side chains can simultaneously provide hydrophobic shielding and disrupt molecular chain crystallization. Comparative Example 3, without the addition of polycarbodiimide, lacked end-carboxyl passivation, resulting in significant hydrolysis autocatalysis and a marked decrease in mechanical retention rate after wet heat aging, demonstrating that carbodiimide chemical end-group passivation is a necessary condition for improving hydrolysis resistance. Example D4 used a C6 short-chain unit acid with insufficient alkyl carbon chains, resulting in limited hydrophobicity and anti-crystallization effects; its hydrolysis resistance and low-temperature performance were inferior to the examples, verifying that the number of carbon atoms in the unit acid should not be lower than C8. D5 uses a C20 monoacid. The excessively long carbon chain easily leads to self-aggregation and crystallization, resulting in decreased elongation and low-temperature toughness of the elastomer, indicating that the carbon number of the monoacid should not exceed C18. D6, carbodiimide, was added at 110℃. The excessively high melt viscosity led to uneven dispersion, poor carboxyl group capture, and decreased hydrolysis resistance. D7 was added at 170℃. The excessively fast reaction rate caused localized micro-crosslinking, impairing elongation, proving that 130-150℃ is a suitable temperature window balancing dispersion and controllable reaction. Comparative Example 8 (D8) had a trifunctional alcohol to monoacid molar ratio of 1:0.5. Insufficient monoacid caused direct gelation during polycondensation, failing to obtain liquid polyester polyol. D9 had a molar ratio of 1:1.5, with excessive monoacid, resulting in reduced grafting efficiency and significantly weakened modification effect. This indicates that the molar ratio of trifunctional polyol to monoacid needs to be controlled within 1:(0.8-1.2). A ratio that is too low easily leads to gelation, while a ratio that is too high impairs performance.

[0076] In summary, only when the following conditions are met simultaneously: ① the molar ratio of trifunctional polyol to C8-C18 monoacid in the pre-esterification stage is 1:(0.8-1.2) to prepare an intermediate with approximately bifunctional hydrophobic side chains; ② the addition of polymeric polycarbodiimide at 130-150℃ after polycondensation, can high hydrolysis resistance and excellent low-temperature flexibility be synergistically achieved; deviation from any of these conditions will result in synthesis failure or significant deterioration of material properties.

Claims

1. A method for preparing a hydrolysis-resistant and low-temperature-resistant polyester polyol, characterized in that, Includes the following steps: (1) An aliphatic trifunctional polyol is subjected to an esterification and dehydration reaction with a C8-C18 aliphatic monoacid until the acid value of the system is ≤5 mgKOH / g, thereby obtaining a long-chain hydrophobic side-chain modified alcohol intermediate; wherein the molar ratio of the aliphatic trifunctional polyol to the C8-C18 aliphatic monoacid is 1:(0.8-1.2). (2) Add branched diol and aliphatic diacid to the intermediate obtained in step (1) and perform atmospheric pressure esterification. After the water output is stable, perform negative compression polymerization and polycondensation until the acid value of the system is ≤1.0 mgKOH / g. (3) After the polycondensation reaction is completed, the system is cooled to 130-150 °C, and polymeric polycarbodiimide is added. The mixture is kept warm and stirred to obtain the hydrolysis-resistant and low-temperature-resistant polyester polyol.

2. The method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyol according to claim 1, characterized in that, The aliphatic trifunctional polyol mentioned in step (1) is glycerol or trimethylolpropane; The C8-C18 aliphatic monocarboxylic acid is a saturated aliphatic monocarboxylic acid selected from one or more of octanoic acid, lauric acid, myristic acid, and stearic acid.

3. The method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyol according to claim 1, characterized in that, The branched diol mentioned in step (2) is selected from at least one of neopentyl glycol, 2-methyl-1,3-propanediol, 3-methyl-1,5-pentanediol, and 2-butyl-2-ethyl-1,3-propanediol; The aliphatic dicarboxylic acid is selected from one or more of the following: succinic acid, octanoic acid, azelaic acid, and sebacic acid.

4. The method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyol according to claim 1, characterized in that, The esterification dehydration reaction described in step (1) is carried out at a temperature of 180-200 °C, and the reaction is carried out under the protection of an organotitanium catalyst and an inert gas.

5. The method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyol according to claim 4, characterized in that, The organotitanium catalyst is selected from one or more of tetrabutyl titanate, tetraethyl titanate, and tetraisopropyl titanate, and its addition amount is 10-200 ppm of the total monomer mass.

6. The method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyol according to claim 1, characterized in that, The heating temperature for atmospheric pressure esterification in step (2) is 210-230 °C; the hydroxyl value of the negative compression polymerization system is 50-150 mgKOH / g.

7. The method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyols according to claim 1 or 6, characterized in that, The negative compression polycondensation described in step (2) employs a two-stage gradient vacuum polycondensation: The first stage has a vacuum of -0.03 to -0.05 MPa and a reaction time of 1 to 2 hours. The second stage has a vacuum level of -0.07 to -0.09 MPa and a reaction time of 2 to 4 hours.

8. The method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyol according to claim 1, characterized in that, When feeding materials in step (2), the ratio of the total hydroxyl equivalent of the long-chain hydrophobic side-chain modified alcohol intermediate and the branched diol to the carboxyl equivalent of the aliphatic dicarboxylic acid is (1.1-1.8):

1.

9. The method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyol according to claim 1, characterized in that, The molar ratio of the long-chain hydrophobic side-chain modified alcohol intermediate obtained in step (1) to the branched diol in step (2) is 1:(3-10).

10. The method for preparing hydrolysis-resistant and low-temperature-resistant polyester polyol according to claim 1, characterized in that, The amount of polymeric polycarbodiimide added in step (3) is 0.5%-2.0% of the mass of the polyester polyol, and the time for heat preservation and stirring is 30-60 min.

Citation Information

Patent Citations

  • Novel oligoester

    CN102970964A

  • Bi-component composite adhesive for solar power back panel, and preparation method thereof

    CN104804698A

  • Polyester resin composition and molded article using said polyester resin composition

    CN105940053A

  • Modified polyester polyol, preparation method thereof and hydrolysis-resistant polyester type TPU prepared from modified polyester polyol

    CN114634616A

  • Coating composition comprising polyacetoacetate, crosslinker and organosilane

    CN1189179A