A modified bamboo powder / PLA / PBAT composite film with borate ester epoxy chain extender and its preparation method
By combining borate ester epoxy chain extender with tannic acid-modified bamboo powder in the PLA/PBAT blend system, the problem of insufficient interfacial bonding was solved, the mechanical properties and processing stability of the composite film were improved, and the interfacial interaction between bamboo powder and polyester matrix was enhanced.
Patent Information
- Application Number
- CN202611479768.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
PLA/PBAT blend films suffer from insufficient interfacial bonding during melt processing, which affects their mechanical properties and processing stability. Furthermore, the interfacial compatibility between unmodified bamboo powder and the polyester matrix is poor, making them prone to agglomeration and stress concentration.
A borate ester epoxy chain extender (TDBE) is combined with tannic acid deposition to modify bamboo powder. Through the reaction of the epoxy groups in TDBE with the chain ends of PLA/PBAT, the cyclic borate ester structure interacts with the ortho- and tho-diol or polyhydroxy sites on the surface of bamboo powder, thereby enhancing the interfacial bonding.
It improves the mechanical properties and melt processing stability of the composite film, enhances the dispersion and interfacial adhesion of bamboo powder in the polyester matrix, strengthens the connection between polyester segments and bamboo powder, and improves tensile strength, elongation at break and melt viscosity.
Smart Images

Figure CN123107329A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of biodegradable polymer composite material processing technology, specifically relating to a modified bamboo powder / PLA / PBAT composite film containing borate ester epoxy chain extender and its preparation method. Background Technology
[0002] Traditional petroleum-based plastic films are difficult to degrade naturally after disposal, easily causing cumulative environmental pollution. PLA / PBAT blend films have biodegradable properties and can be used to replace some traditional plastic films. PLA has high rigidity and good strength, but limited toughness and melt strength; PBAT has good flexibility and film-forming properties, but relatively insufficient strength. Blending the two can achieve complementary properties, but due to differences in molecular structure and phase characteristics, insufficient interfacial bonding is prone to occur during melt processing, which in turn affects the mechanical properties and processing stability of the composite film.
[0003] Existing improvement schemes still have certain shortcomings: single epoxy chain extenders mainly improve the molecular weight and interfacial bonding of the PLA / PBAT matrix through the reaction of epoxy groups with polyester end groups, but have limited effect on improving the interface between natural plant fillers and the polyester matrix; unmodified bamboo powder contains a large number of hydrophilic hydroxyl groups on its surface, resulting in insufficient interfacial compatibility with the PLA / PBAT polyester matrix, easily leading to agglomeration and stress concentration; ordinary alkali treatment is mainly used to remove impurities on the bamboo powder surface and expose hydroxyl groups, resulting in a relatively simple interfacial interaction mechanism. Bamboo powder is widely available and renewable, and its cellulose and lignin structures contain abundant hydroxyl groups; tannic acid surface deposition can further introduce polyphenols and polyhydroxyl sites into the bamboo powder surface, providing binding sites for the interaction between the borate ester structure and the bamboo powder interface. Therefore, it is necessary to develop a modification system that combines polyester chain extension and bamboo powder interface regulation functions. Summary of the Invention
[0004] This invention aims to improve the interfacial bonding and melt processing properties of PLA / PBAT blends, and to improve the dispersion and interfacial adhesion of bamboo powder filler in a polyester matrix. The epoxy groups in TDBE can participate in the chain-end reactions of PLA / PBAT, and the cyclic borate ester structure interacts with the ortho- and polyhydroxy sites on the surface of tannic acid-modified bamboo powder, thereby improving the mechanical properties and processing stability of the composite film.
[0005] To achieve the above objectives, the present invention provides a modified bamboo powder / PLA / PBAT composite film containing a borate ester epoxy chain extender, comprising PLA, PBAT, tannic acid deposition-modified bamboo powder, TDBE, antioxidant, and lubricant; wherein the TDBE is a reaction product obtained by forming a bicyclic borate ester intermediate from 3,5-dihydroxyphenylboronic acid and α,α′-diglycerol, and then subjecting the intermediate to glycidyl etherification with epichlorohydrin in the presence of an alkali and a phase transfer catalyst, wherein the TDBE contains a cyclic borate ester structure and a glycidyl ether type epoxy group.
[0006] Further, using 100 parts by weight of PLA and PBAT as the matrix, wherein PLA comprises 50-70 parts and PBAT comprises 30-50 parts; relative to 100 parts by weight of the matrix, there are 5-20 parts of tannic acid deposition-modified bamboo powder, 0.5-3 parts of TDBE, 0.1-0.8 parts of antioxidant, and 0.1-0.8 parts of lubricant. The surface of the tannic acid deposition-modified bamboo powder is deposited with a tannic acid layer containing ortho- and polyhydroxy structures.
[0007] Furthermore, the antioxidant is preferably a compound of antioxidant 1010 and antioxidant 168, and the lubricant is preferably calcium stearate.
[0008] Furthermore, the TDBE contains a cyclic borate ester structure and a glycidyl ether type epoxy group; according to the target reaction structure, cyclic borate esters are formed at both ends of its α,α′-diglycerol skeleton, and the phenolic hydroxyl groups on the two aromatic rings are etherified with glycidyl ether to form epoxy functional groups.
[0009] Furthermore, the modified bamboo powder has a particle size of 200-500 mesh and a moisture content of no more than 1.0% after vacuum drying. Its preparation employs a single route: first, it is treated with a 2-5 wt% NaOH solution at 60-80℃ for 1-3 hours and washed with water until neutral; then, it is treated with a 0.5-2.0 wt% tannic acid aqueous solution at a solid-liquid ratio of 1g bamboo powder to 10-30mL solution at 20-40℃ for 2-8 hours; after filtration, washing with water, and vacuum drying, a tannic acid layer containing ortho-diol and polyhydroxyl structures is deposited on the surface of the bamboo powder.
[0010] Furthermore, the antioxidant is selected from antioxidant 1010, antioxidant 168, or a combination of the two; the lubricant is selected from one or more of stearate, erucamide, and polyethylene wax.
[0011] The present invention also provides a method for preparing the composite film, comprising the following steps: S1, raw material pre-drying: PLA and PBAT are vacuum dried at 60-90℃ for 6-10h, and modified bamboo powder is vacuum dried at 50-70℃ for 8-12h; S2, mixing: the dried PLA, PBAT, modified bamboo powder, TDBE, antioxidant and lubricant are uniformly mixed; S3, melt blending, extrusion and granulation: the mixed material is fed into a twin-screw extruder, melt blended at 150-185℃ and screw speed of 100-350rpm, extruded, cooled and granulated to obtain composite masterbatch; S4, blow molding film formation: the composite masterbatch is blow molded into a film to obtain the composite film.
[0012] Furthermore, the processing temperature of the twin-screw extruder is 160–180°C, and the blow molding film temperature is 160–180°C.
[0013] Further, the synthesis of TDBE comprises two steps. M1: 3,5-Dihydroxyphenylboronic acid and α,α′-diglycerol are reacted in a molar ratio of 2:1 in toluene under nitrogen protection at 110°C for 6 hours to remove water, yielding a bicyclic borate intermediate. M2: The intermediate is reacted with epichlorohydrin, wherein the molar ratio of epichlorohydrin to the intermediate is not less than 8:1, at 55–65°C for 6 hours in the presence of NaOH and a phase transfer catalyst, causing the phenolic hydroxyl group to undergo etherification and ring closure to form a glycidyl ether group; unreacted epichlorohydrin is removed under reduced pressure, the mixture is washed with water until neutral, and dried under vacuum to obtain the TDBE reaction product.
[0014] In this invention, the glycidyl ether-type epoxy groups in TDBE can undergo ring-opening reactions with the terminal hydroxyl or carboxyl groups of PLA / PBAT; the cyclic borate ester structure in TDBE interacts with the ortho- and polyhydroxy sites on the surface of bamboo powder modified by tannic acid deposition. These effects enhance the connection between the polyester segments and the bamboo powder interface.
[0015] In this invention, the composite film can be used as packaging film, agricultural mulch film and other biodegradable film products.
[0016] The composite membrane of the present invention participates in the PLA / PBAT chain-end reaction through the glycidyl ether type epoxy group in TDBE, and utilizes the interfacial interaction generated by the cyclic borate ester structure and the ortho-diol or polyhydroxy sites on the surface of bamboo powder modified by tannic acid deposition, which is beneficial to improving the interfacial bonding between the polyester matrix and the bamboo powder filler.
[0017] The present invention has the following beneficial effects:
[0018] The glycidyl ether-type epoxy group of TDBE in this invention can undergo a ring-opening reaction with the active groups at the chain ends of PLA / PBAT, which is beneficial for improving melt viscosity and processing stability. The cyclic borate ester structure of TDBE interacts with the ortho- and choline sites on the surface of tannic acid-modified bamboo powder, enhancing the interfacial interaction between the bamboo powder and the polyester matrix. Under the formulation and test conditions listed in this invention, the composite film containing TDBE and tannic acid-modified bamboo powder exhibits higher tensile strength, elongation at break, and low-frequency storage modulus, indicating that this specific formulation is beneficial for improving the mechanical properties and melt processing performance of the composite film.
[0019] This invention uses bamboo powder as a renewable filler; residual epichlorohydrin after TDBE synthesis is removed by vacuum desorption and water washing. The degradation performance, residues, and safety of the resulting material should be evaluated according to the appropriate testing methods for the target application. The composite material of this invention can be used in packaging films, agricultural mulch films, and other biodegradable film products, depending on the film-forming process. Attached Figure Description
[0020] Figure 1 This is a schematic diagram of the target structure of TDBE and the functional group connection relationship of the present invention.
[0021] Figure 2 This diagram illustrates the ring-opening reaction between the glycidyl ether-type epoxy group in the TDBE of this invention and the terminal hydroxyl or carboxyl group of PLA / PBAT, as well as the interfacial interaction between the cyclic borate ester structure and the ortho-diol or polyhydroxy sites on the surface of bamboo powder modified by tannic acid deposition.
[0022] Figure 3 This is a schematic diagram illustrating the preparation of modified bamboo powder using a single route of alkali treatment and tannic acid deposition according to the present invention.
[0023] Figure 4 This is a schematic diagram of the two-step reaction route for the preparation of TDBE using 3,5-dihydroxyphenylboronic acid, α,α′-diglycerol and epichlorohydrin according to the present invention. Detailed Implementation
[0024] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] Reference Figures 1-4This invention provides a modified bamboo powder / PLA / PBAT composite film containing a borate ester epoxy chain extender. PLA and PBAT form a polyester matrix; the TDBE molecular backbone is used for polyester chain-end reactions and bamboo powder interface regulation; antioxidants and lubricants are used to improve processing stability and flowability, respectively.
[0026] The matrix consists of 100 parts by weight of PLA and PBAT, with PLA comprising 50-70 parts and PBAT comprising 30-50 parts. Relative to the 100 parts by weight matrix, the matrix contains 5-20 parts modified bamboo powder, 0.5-3 parts TDBE, 0.1-0.8 parts antioxidant, and 0.1-0.8 parts lubricant. PLA and PBAT form a polyester matrix; tannic acid deposition-modified bamboo powder serves as a renewable filler and provides multi-hydroxyl interface sites; TDBE is used for polyester chain-end reactions and bamboo powder interface regulation; antioxidants and lubricants are used to improve processing stability and flowability, respectively.
[0027] Reference Figure 1 TDBE is a reaction product obtained by forming a bicyclic borate intermediate from 3,5-dihydroxyphenylboronic acid and α,α′-diglycerol, followed by epichlorohydrin glycidyl etherification. According to the target reaction structure, cyclic borate esters are formed at both ends of α,α′-diglycerol, and the phenolic hydroxyl groups on the two aromatic rings further form glycidyl ether-type epoxy groups. Figure 1 Used to represent target connectivity and functional group type.
[0028] In a preferred embodiment of the present invention, the modified bamboo powder is tannic acid deposition-modified bamboo powder. The embodiments of this application employ a modification route involving NaOH treatment followed by tannic acid surface deposition; the embodiments and corresponding test data all correspond to the described modification route.
[0029] The glycidyl ether type epoxy group in TDBE can undergo ring-opening reaction with the terminal hydroxyl or terminal carboxyl group of PLA / PBAT, which is beneficial to improve the degree of connection between polyester segments.
[0030] Reference Figure 2 The glycidyl ether-type epoxy groups in TDBE can undergo ring-opening reactions with the terminal hydroxyl or carboxyl groups of PLA / PBAT; the cyclic borate ester structure in TDBE interacts with the ortho- and polyhydroxy sites on the surface of bamboo powder modified by tannic acid deposition. Both of these interactions contribute to improving the interfacial bonding between the polyester matrix and the bamboo powder filler.
[0031] Reference Figure 3 Bamboo powder was first treated with NaOH solution and washed with water until neutral, then surface deposition was performed using a tannic acid aqueous solution. (Refer to...) Figure 4 TDBE is first formed by dehydration of 3,5-dihydroxyphenylboronic acid and α,α′-diglycerol to form a ring, and then the phenolic hydroxyl group of the intermediate is glycidyl etherified by epichlorohydrin.
[0032] Furthermore, a matrix of 100 parts is used, consisting of 60 parts PLA and 40 parts PBAT. Relative to the 100 parts matrix, there are 10 parts modified bamboo powder, 1.2 parts TDBE, 0.3 parts antioxidant, and 0.3 parts lubricant. This formulation balances the mechanical and processing properties of the composite film.
[0033] TDBE is prepared according to the method described in this invention and is a reaction product containing a cyclic borate ester structure and a glycidyl ether type epoxy group.
[0034] In a preferred embodiment of the present invention, the modified bamboo powder has a particle size of 200-500 mesh and a moisture content of ≤1.0% after vacuum drying. Using finer-particle-size bamboo powder is beneficial for improving its dispersion in the film and reducing surface defects caused by large particles; controlling the moisture content is beneficial for reducing the risk of polyester hydrolysis during melt processing.
[0035] The preparation of modified bamboo powder includes an alkali treatment step: bamboo powder is treated with a 2-5 wt% NaOH solution at 60-80℃ for 1-3 hours. This treatment helps remove the wax and some soluble impurities from the surface of the bamboo powder and exposes the hydroxyl groups. After washing with water until neutral, it is used for subsequent tannic acid deposition.
[0036] The alkali-treated bamboo powder was then subjected to tannic acid deposition: 1 g of bamboo powder was dispersed in 10–30 mL of an aqueous tannic acid solution with a concentration of 0.5–2.0 wt%, stirred at 20–40 °C for 2–8 h, filtered, washed with deionized water, and then vacuum dried. This route is used to introduce ortho- and hydroxyl sites onto the surface of bamboo powder. The data in the examples correspond only to the tannic acid deposition products described.
[0037] Antioxidants such as antioxidant 1010, antioxidant 168, or a combination of both can be used to reduce the risk of thermo-oxidative degradation of PLA / PBAT during extrusion and blown film processes.
[0038] The lubricant can be one or more of stearates, erucamides, and polyethylene waxes, used to improve the melt processing fluidity and discharge stability of the mixture.
[0039] The preparation of the composite film includes the following steps: S1, PLA and PBAT are vacuum dried at 60-90℃ for 6-10h, and modified bamboo powder is vacuum dried at 50-70℃ for 8-12h; S2, the dried PLA, PBAT, modified bamboo powder, TDBE, antioxidant and lubricant are uniformly mixed; S3, the mixture is fed into a twin-screw extruder, melt-blended at 150-185℃ and 100-350rpm, extruded, cooled and pelletized to obtain composite masterbatch; S4, the composite masterbatch is blow-molded into a film to obtain the composite film.
[0040] In a preferred embodiment of the present invention, S2 involves uniformly mixing the dried PLA, PBAT, modified bamboo powder, TDBE, antioxidant, and lubricant to improve the dispersion uniformity of each component during subsequent melt processing.
[0041] In a preferred embodiment of the present invention, in step S3, the mixture is fed into a twin-screw extruder and melt-blended at 150–185°C and a screw speed of 100–350 rpm. The resulting material is then extruded, cooled, and pelletized to obtain composite masterbatch. The aforementioned temperature and speed range are designed to balance the melt processing of PLA / PBAT with the chain-end reactions and interfacial interactions of TDBE.
[0042] S4. The composite masterbatch is blown into a film to obtain a composite film.
[0043] In a preferred embodiment of the present invention, the processing temperature range of the twin-screw extruder is 160–180°C, and the blow molding film forming processing temperature is 160–180°C. This temperature range is beneficial for balancing melt processing stability and composite film formation.
[0044] The M1 step of TDBE is as follows: 3,5-dihydroxyphenylboronic acid and α,α′-diglycerol are added to a reactor equipped with a water separator in a molar ratio of 2:1. Using toluene as solvent, the mixture is refluxed at 110°C for 6 hours under nitrogen protection to remove water, yielding a bicyclic borate intermediate retaining the phenolic hydroxyl groups. The target dehydration rate for this step is 4 mol of water per mole of the intermediate.
[0045] The M2 step of TDBE is as follows: the bicyclic borate intermediate is mixed with epichlorohydrin, wherein the molar ratio of epichlorohydrin to the intermediate is not less than 8:1. NaOH and a phase transfer catalyst are added, and the mixture is reacted at 55–65 °C for 6 h, causing the phenolic hydroxyl groups to undergo etherification and ring closure to form glycidyl ether groups. The chlorine leaving during the reaction enters the inorganic salt phase in the form of chloride and is removed during subsequent water washing. After the reaction, unreacted epichlorohydrin is removed under reduced pressure, and the mixture is washed with water until neutral and then dried under vacuum to obtain TDBE.
[0046] Composite films can be used in packaging films, agricultural mulch films, and other biodegradable film products; their specific application performance and safety should be evaluated according to the test methods corresponding to their intended use.
[0047] In this embodiment of the invention, PLA can be selected from polylactic acid resin suitable for film processing, and PBAT can be selected from polybutylene adipate / terephthalate resin suitable for blown film processing. Antioxidants can be antioxidant 1010, antioxidant 168, or a combination thereof, and lubricants can be stearate, erucamide, polyethylene wax, or a combination thereof.
[0048] TDBE is a product obtained by a two-step reaction of α,α′-diglycerol, 3,5-dihydroxyphenylboronic acid, and epichlorohydrin. According to the target reaction structure, cyclic borate esters are formed at both ends of α,α′-diglycerol, and the phenolic hydroxyl groups on the aromatic ring are etherified with glycidyl to form epoxy functional groups.
[0049] According to the target reaction design, the TDBE reaction product contains a cyclic borate ester structure and a glycidyl ether type epoxy group.
[0050] The two-step synthesis process of TDBE is as follows: M1: 3,5-Dihydroxyphenylboronic acid and α,α′-diglycerol are refluxed in toluene at a molar ratio of 2:1 to remove water, causing the 1,2-diols at both ends of the diglycerol to form rings with one molecule of borate group, forming a bicyclic borate ester intermediate. M2: In the presence of NaOH and a phase transfer catalyst, the phenolic hydroxyl groups in the intermediate are etherified with glycidyl ether using epichlorohydrin in an amount not less than 8 molar amounts of the intermediate; the epichlorohydrin is removed under reduced pressure, and the intermediate is washed with water and dried under vacuum to obtain TDBE.
[0051] TDBE has two main functions: the glycidyl ether type epoxy group can undergo ring-opening reaction with the terminal hydroxyl or carboxyl groups of PLA / PBAT; the cyclic borate ester structure can generate interfacial interactions with the ortho- and polyhydroxy sites on the surface of bamboo powder modified by tannic acid deposition. These functions are beneficial to improving the connectivity of polyester segments and enhancing the interfacial bonding between bamboo powder and the polyester matrix.
[0052] The preparation of modified bamboo powder includes: crushing bamboo raw materials and sieving them to 200-500 mesh to reduce film surface defects caused by large particles;
[0053] Alkali treatment: Treat with 2-5 wt% NaOH solution at 60-80℃ for 1-3 hours to remove surface wax and some soluble impurities and expose hydroxyl groups; then filter and wash with water until neutral.
[0054] Tannic acid deposition: Alkaline-treated bamboo powder, washed to neutral pH, was dispersed in a 1.0 wt% tannic acid aqueous solution at a solid-liquid ratio of 1 g bamboo powder to 20 mL solution. The solution was stirred at 25 °C for 4 h; filtered, and washed with deionized water until the washing solution was colorless, followed by vacuum drying at 60 °C. This treatment is used to deposit a tannic acid layer containing ortho- and polyhydroxy structures on the surface of bamboo powder.
[0055] Vacuum drying: Dry at 50-70℃ for 8-12 hours to reduce the moisture content to no more than 1.0% to reduce the risk of PLA hydrolysis caused by moisture.
[0056] The epoxy groups in TDBE can react with the active groups at the ends of PLA / PBAT chains; the cyclic borate ester structure interacts with the ortho- and hydroxyl sites on the surface of tannic acid-modified bamboo powder. These interactions facilitate the formation of interfacial bonds between the polyester segments and the modified bamboo powder.
[0057] Covalent epoxy effect: The epoxy groups of TDBE participate in the chain-end reaction of PLA / PBAT, which is beneficial to improving the melt strength and processing stability of the polyester matrix.
[0058] Borate ester interfacial interaction: The cyclic borate ester structure in TDBE interacts with the ortho-diol or polyhydroxy sites on the surface of bamboo powder modified by tannic acid deposition, which is beneficial to improving the interfacial interaction between the filler and the matrix.
[0059] Target linkage structure: α,α′-diglycerol backbone connects two cyclic borate ester units, and glycidyl ether-type epoxy groups on the aromatic ring provide reaction sites at the polyester chain ends.
[0060] Under the given formulation and testing conditions of this application, the tensile strength, elongation at break, tensile impact strength, low-frequency storage modulus, complex viscosity, and antibacterial rate of Example 3 are all higher than those of the comparative examples; at the same time, its MFR is lower than that of the comparative examples, indicating that the combined use of TDBE and tannic acid deposition-modified bamboo powder is beneficial to improve the degree of polyester chain segment connection, improve the interfacial effect of bamboo powder, and enhance the melt processing stability.
[0061] Example 1: Preparation of TDBE. 0.20 mol of 3,5-dihydroxyphenylboronic acid and 0.10 mol of α,α′-diglycerol were added to a reactor equipped with a water separator. Using toluene as solvent, the mixture was heated to 110°C under nitrogen protection and refluxed for 6 hours to separate the water, yielding a bicyclic borate intermediate. After cooling, 0.80 mol of epichlorohydrin and a catalytic amount of the phase transfer catalyst tetrabutylammonium bromide were added. NaOH was added in batches under stirring at 55–65°C, ensuring a molar ratio of NaOH to the total molar amount of phenolic hydroxyl groups in the intermediate of 1.1:1, and the reaction continued for 6 hours. In this step, the chlorine on the epichlorohydrin acts as a leaving group and enters the inorganic salt phase. After the reaction, unreacted epichlorohydrin was removed under reduced pressure, and the mixture was washed with deionized water until neutral and then vacuum dried to obtain the TDBE reaction product, which was used for subsequent composite membrane preparation.
[0062] Example 2: Preparation of tannic acid deposition-modified bamboo powder. Bamboo was pulverized and sieved to 300 mesh. It was then placed in a 3wt% NaOH solution at a solid-liquid ratio of 1g bamboo powder to 20mL solution and treated at 70℃ for 2h. The mixture was washed with deionized water until neutral and filtered. The alkali-treated bamboo powder was dispersed in a 1.0wt% tannic acid aqueous solution at a solid-liquid ratio of 1g bamboo powder to 20mL solution and stirred at 25℃ for 4h. The mixture was filtered, washed with deionized water, and vacuum dried at 60℃ to obtain tannic acid deposition-modified bamboo powder.
[0063] Example 3: Preparation of composite film. 60 parts by weight of PLA, 40 parts by weight of PBAT, 10 parts by weight of modified bamboo powder obtained in Example 2, 1.2 parts by weight of TDBE obtained in Example 1, 0.3 parts by weight of antioxidant 1010 / 168 compound, and 0.3 parts by weight of calcium stearate were weighed. PLA and PBAT were vacuum dried at 80℃ for 8 hours, and modified bamboo powder was vacuum dried at 60℃ for 10 hours. After the components were mixed evenly, they were fed into a twin-screw extruder and melt-extruded at 160–180℃ and 200 rpm, cooled, and pelletized. The resulting masterbatch was blow-molded into a film at 165–175℃.
[0064] Except for the differences in components listed in Table 1, the drying, mixing, extrusion, and film-forming conditions of Comparative Examples 1-4 were the same as those of Example 3. Comparative Example 1 was a PLA / PBAT blank; Comparative Example 2 had 10 parts of unmodified bamboo powder added; Comparative Example 3 had 1.2 parts of common epoxy chain extender Joncryl ADR4468 (manufactured by BASF) added; Comparative Example 4 had 1.2 parts of TDBE added but no bamboo powder added.
[0065] The drying, mixing, extrusion, and film-forming conditions for Comparative Examples 5–7 were the same as those for Example 3. Comparative Example 5 included 10 parts of tannic acid-modified bamboo powder without a chain extender; Comparative Example 6 included 10 parts of tannic acid-modified bamboo powder and 1.2 parts of the common epoxy chain extender Joncryl ADR4468; Comparative Example 7 included 10 parts of tannic acid-modified bamboo powder and 1.2 parts of the bicyclic borate ester intermediate obtained in step M1 of Example 1, without M2 glycidyl etherification.
[0066] Comparative Example 5 was used to evaluate the effect of tannic acid deposition on bamboo powder itself; Comparative Example 6 was used to compare the differences between ordinary epoxy chain extenders and TDBE in the modified bamboo powder system; Comparative Example 7 was used to evaluate the effect of glycidyl ether type epoxy groups. All comparative examples and Example 3 used the same drying, mixing, extrusion, and film-forming conditions to ensure comparability of performance results.
[0067] Table 1. Formulations of Examples and Comparative Examples (parts by weight)
[0068] sample PLA PBAT Modified bamboo powder Unmodified bamboo powder TDBE Common epoxy chain extender illustrate Example 3 60 40 10 — 1.2 — Tannic acid deposition modified bamboo powder + TDBE Comparative Example 1 60 40 — — — — PLA / PBAT blank Comparative Example 2 60 40 — 10 — — Unmodified bamboo powder Comparative Example 3 60 40 — — — 1.2 Common epoxy chain extender Comparative Example 4 60 40 — — 1.2 — TDBE only Comparative Example 5 60 40 10 — — — Modified bamboo powder, without chain extenders Comparative Example 6 60 40 10 — — 1.2 Modified bamboo powder + ordinary epoxy chain extender Comparative Example 7 60 40 10 — — — Modified bamboo powder + 1.2 parts of bicyclic borate ester intermediate (without glycidyl ether type epoxy group)
[0069] Table 2 lists the mechanical properties, melt flow rate, and antibacterial properties of each composite membrane sample, used to compare the differences in the effects of modified bamboo powder, ordinary epoxy chain extender, bicyclic borate intermediate, and TDBE.
[0070] Note: The types and amounts of antioxidants and lubricants are the same in each group, and are omitted from the table.
[0071] Performance tests were conducted on the composite films of the examples and comparative examples. Tensile properties were determined using a CMT6104 electronic universal testing machine. After conditioning the samples at 23±2℃ and 50±5% relative humidity for 24 hours, tests were performed according to GB / T1040.3-2006. The film thickness was 50±5μm, and samples were taken longitudinally along the blown film. The sample width was 15mm, the effective gauge length was 50mm, and the test speed was 50mm / min. Tensile impact strength was measured using an XJU-5.5 tensile impact testing machine. After conditioning the samples under the same conditions, tests were performed according to GB / T13525-1992. The sample size was 80mm×10mm, the pendulum energy was 2J, and the results are expressed as kJ·m⁻². Melt flow rate was measured using an XNR-400A melt flow rate meter at 190℃ and 2.16kg. Dynamic rheological properties were measured using a parallel plate mode on an MCR302 rotational rheometer at a test temperature of 180℃. The parallel plate diameter was 25mm and the gap was 1.0mm. A 3% strain was applied in the linear viscoelastic region, and frequency scanning was performed from 0.1 to 100 rad / s. The low-frequency storage modulus G′ and complex viscosity η* in Table 3 were taken as values when ω=1 rad / s. The equilibrium torque was measured using an RM-200C torque rheometer at a mixing temperature of 180℃, a rotation speed of 60 rpm, and a charge of 60g. The average torque during the 8–10 min stable mixing period was taken as the equilibrium torque. Antibacterial rate was determined according to GB / T31402-2023 using the plate count method with *Escherichia coli* ATCC25922 and *Staphylococcus aureus* ATCC6538. The bacterial concentration was 1.0 × 10⁻⁶. 6 The concentration of CFU / mL was measured, with a contact time of 24 h. The samples were incubated at 37℃ for 24 h before counting. For the soil condition mass loss test, a constant temperature and humidity incubator was used. The soil was a 1:1 mixture of sieved garden soil and humus, with a moisture content of 30±5%. The incubation temperature was 28±2℃, and the sample burial depth was 5 cm. After sampling, the surface soil was gently washed with deionized water to remove the soil, and the samples were vacuum dried at 60℃ to constant weight before calculating the mass loss rate. The test results are shown in Tables 2-4. Tensile strength, elongation at break, and tensile impact strength were measured using five parallel samples for each sample; melt flow rate, rheological properties, antibacterial rate, and soil condition mass loss were measured using three independent parallel samples for each sample. The data listed in Tables 2-4 are all arithmetic means. The data in Tables 2-4 are used to evaluate the performance differences of each sample under the same test conditions.
[0072] Table 2 Mechanical, flow and antibacterial properties of the composite membrane
[0073] sample Tensile strength / MPa Elongation at break / % Tensile impact strength / (kJ·m⁻²) MFR / (g / 10min) E. coli antibacterial rate / % Staphylococcus aureus antibacterial rate / % Comparative Example 1 (PLA / PBAT) 28.4 118 7.6 8.9 18.3 21.5 Comparative Example 2 (PLA / PBAT + Unmodified Bamboo Powder) 25.8 82 6.8 9.4 28.6 31.4 Comparative Example 3 (PLA / PBAT + ordinary epoxy chain extender) 34.7 205 10.8 5.1 24.5 28.1 Comparative Example 4 (PLA / PBAT + TDBE) 36.5 246 12.1 4.4 31.6 35.2 Comparative Example 5 (Modified bamboo powder, without chain extender) 29.7 106 8.3 8.1 62.4 66.8 Comparative Example 6 (Modified bamboo powder + ordinary epoxy chain extender) 37.8 220 13.5 4.6 65.7 70.2 Comparative Example 7 (Modified bamboo powder + bicyclic borate ester intermediate (without glycidyl ether type epoxy group)) 33.2 154 10.9 6.8 70.9 75.3 Example 3 (Modified bamboo powder + TDBE) 41.6 265 15.8 3.3 78.4 82.1
[0074] Table 2 shows that the combined use of TDBE and tannic acid-modified bamboo powder can improve the antibacterial properties of the composite membrane. Due to the functional group structure of TDBE, the cyclic borate ester structure interacts with the ortho- and polyhydroxy sites on the surface of the modified bamboo powder, which helps reduce the migration or loss of the active tannic acid components, allowing more phenolic hydroxyl sites to be retained and exert their antibacterial effect.
[0075] Table 3 Rheological properties of the composite membrane
[0076] sample Low-frequency energy storage modulus G′ / Pa Complex viscosity η* / (Pa·s) Balance torque / (N·m) illustrate Comparative Example 1 (PLA / PBAT) 2.8×10² 620 18.2 The interfacial bonding is weak, and the melt strength is low. Comparative Example 2 (Unmodified bamboo powder) 3.2×10² 710 20.5 Bamboo powder has poor dispersibility, and melt fluctuations are slightly increased. Comparative Example 3 (Common Epoxy Chain Extender) 6.2×10² 1180 24.6 Forming a certain extended chain structure Comparative Example 4 (TDBE) 8.1×10² 1460 27.3 Multifunctional chain extension improves melt strength Comparative Example 5 (Modified bamboo powder, without chain extender) 4.6×10² 820 21.6 Modified bamboo powder improves dispersion, but its chain extension effect is limited. Comparative Example 6 (Modified bamboo powder + ordinary epoxy chain extender) 9.4×10² 1680 29.1 Chain extension increases melt strength, but interfacial anchoring is insufficient. Comparative Example 7 (Modified bamboo powder + bicyclic borate ester intermediate (without glycidyl ether type epoxy group)) 7.2×10² 1250 25.4 It has some interfacial function, but lacks epoxy chain extender. Example 3 (Modified bamboo powder + TDBE) 1.35×10³ 2260 33.9 Enhanced interfacial interaction and improved melt elasticity
[0077] Table 4. Mass loss of composite membrane under soil conditions
[0078] sample 30d mass loss / % 60d mass loss / % 90d mass loss / % 180d mass loss / % Comparative Example 1 (PLA / PBAT) 8.5 22.7 41.3 79.6 Comparative Example 2 (Unmodified bamboo powder) 9.8 25.6 44.8 81.6 Comparative Example 3 (Common Epoxy Chain Extender) 7.2 19.6 36.9 72.8 Comparative Example 4 (TDBE) 7.9 21.4 39.0 76.8 Comparative Example 5 (Modified bamboo powder, without chain extender) 10.6 27.1 47.2 83.0 Comparative Example 6 (Modified bamboo powder + ordinary epoxy chain extender) 8.8 23.4 42.1 78.8 Comparative Example 7 (Modified bamboo powder + bicyclic borate ester intermediate (without glycidyl ether type epoxy group)) 10.1 26.3 45.8 82.4 Example 3 (Modified bamboo powder + TDBE) 10.2 28.7 49.5 84.3
[0079] As shown in Tables 2-4, under the formulations and test conditions listed in this application, Example 3 exhibits higher tensile strength, elongation at break, tensile impact strength, low-frequency storage modulus, complex viscosity, and equilibrium torque than the comparative examples, while its melt flow rate is lower. This indicates that the combined use of TDBE and tannic acid-modified bamboo powder is beneficial for improving the mechanical properties and melt processing performance of the composite film. The addition of bamboo powder generally increased the mass loss rate of each group. Specifically, the 180-day mass loss rates of Comparative Examples 5, 6, and 7 were 83.0%, 78.8%, and 82.4%, respectively, while Example 3 reached 84.3%. This demonstrates that under the formulations and test conditions listed in this application, the material maintains a high level of mass loss under soil conditions even after the combined use of tannic acid-modified bamboo powder and TDBE. The antibacterial rate of Example 3 is also higher than that of the comparative examples. The above data only correspond to the specific formulations and test conditions listed in this application and are not extrapolated to other formulations and test conditions.
[0080] In this embodiment of the invention, PLA can be selected from polylactic acid resin suitable for film processing, and PBAT can be selected from polybutylene adipate / terephthalate resin suitable for blown film processing. Antioxidants can be antioxidant 1010, antioxidant 168, or a combination thereof, and lubricants can be stearate, erucamide, polyethylene wax, or a combination thereof.
[0081] TDBE is a product obtained through a two-step reaction of α,α′-diglycerol, 3,5-dihydroxyphenylboronic acid, and epichlorohydrin. According to the target reaction structure, cyclic borate esters are formed at both ends of the α,α′-diglycerol, and the phenolic hydroxyl groups on the aromatic ring are etherified with glycidyl ether to form epoxy functional groups. The TDBE reaction product contains cyclic borate ester structures and glycidyl ether-type epoxy groups.
[0082] TDBE has two main functions: the glycidyl ether type epoxy group can undergo ring-opening reaction with the terminal hydroxyl or carboxyl groups of PLA / PBAT; the cyclic borate ester structure can generate interfacial interactions with the ortho- and polyhydroxy sites on the surface of bamboo powder modified by tannic acid deposition. These functions are beneficial to improving the connectivity of polyester segments and enhancing the interfacial bonding between bamboo powder and the polyester matrix.
[0083] In summary, this invention utilizes the ring-opening reaction between the glycidyl ether-type epoxy groups in TDBE and the terminal hydroxyl or carboxyl groups of PLA / PBAT to enhance the connectivity between polyester segments, thereby improving melt viscosity and processing stability. The interfacial interaction between the cyclic borate ester structure in TDBE and the ortho-diol or polyhydroxy sites on the surface of tannic acid-modified bamboo powder enhances the interfacial bonding between bamboo powder and the polyester matrix, improving the dispersion of bamboo powder filler in the matrix. Integrating the epoxy chain-extending function and the borate ester interfacial regulation function into the same molecule (TDBE) and using it in conjunction with tannic acid-modified bamboo powder creates a dual interfacial connection between the polyester matrix and the bamboo powder filler. Under the formulation and testing conditions listed in this application, the composite film (Example 3) with TDBE and tannic acid-modified bamboo powder exhibited a tensile strength of 41.6 MPa, an elongation at break of 265%, a tensile impact strength of 15.8 kJ / m², a melt flow rate of 3.3 g / 10 min, a low-frequency storage modulus of 1.35 × 10³ Pa, a complex viscosity of 2260 Pa·s, and a balance torque of 33.9 N·m. Compared with the PLA / PBAT blank sample (Comparative Example 1), the tensile strength increased from 28.4 MPa to 41.6 MPa, the elongation at break increased from 118% to 265%, and the low-frequency storage modulus increased from 2.8 × 10² Pa to 1.35 × 10³ Pa. The above data are based on the formulation (60 parts PLA, 40 parts PBAT, 10 parts modified bamboo powder, and 1.2 parts TDBE) and corresponding testing conditions listed in Example 3, and are not extrapolated to other formulations and testing conditions. Using tannic acid-modified bamboo powder as a renewable filler, under the formulation and testing conditions listed in this application, the composite membrane of Example 3 achieved an antibacterial rate of 78.4% against Escherichia coli and an antibacterial rate of 82.1% against Staphylococcus aureus; the mass loss under soil conditions was 84.3% after 180 days. The above data are based on the formulation and corresponding testing conditions listed in Example 3 and are not extrapolated to other formulations and testing conditions.
[0084] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A modified bamboo powder / PLA / PBAT composite film containing a borate ester epoxy chain extender, characterized in that, The product includes PLA, PBAT, tannic acid-modified bamboo powder, TDBE, antioxidants, and lubricants. The TDBE is a reaction product obtained by forming a bicyclic borate intermediate from 3,5-dihydroxyphenylboronic acid and α,α′-diglycerol, and then subjecting the intermediate to glycidyl etherification with epichlorohydrin in the presence of an alkaline environment and a phase transfer catalyst. The TDBE contains a cyclic borate structure and a glycidyl ether type epoxy group.
2. The composite membrane according to claim 1, characterized in that, The matrix consists of 100 parts by weight of PLA and PBAT, of which PLA is 50-70 parts and PBAT is 30-50 parts. Relative to the 100 parts by weight of the matrix, there are 5-20 parts of tannic acid deposition-modified bamboo powder, 0.5-3 parts of TDBE, 0.1-0.8 parts of antioxidant, and 0.1-0.8 parts of lubricant. The surface of the tannic acid deposition-modified bamboo powder is deposited with a tannic acid layer containing ortho-diphenol and polyhydroxyl structures.
3. The composite membrane according to claim 2, characterized in that, The PLA is 60 parts, PBAT is 40 parts, the tannic acid deposition modified bamboo powder is 10 parts, TDBE is 1.2 parts, antioxidant is 0.3 parts, and lubricant is 0.3 parts; the antioxidant is a compound of antioxidant 1010 and antioxidant 168, and the lubricant is calcium stearate.
4. The composite membrane according to claim 1, characterized in that, The TDBE is a reaction product prepared by the following method: 3,5-dihydroxyphenylboronic acid and α,α′-diglycerol are subjected to a reflux dehydration reaction at a molar ratio of 2:1 to obtain a bicyclic borate intermediate; the intermediate is then reacted with epichlorohydrin in the presence of NaOH and a phase transfer catalyst to cause the phenolic hydroxyl groups of the intermediate to undergo glycidyl etherification, thereby obtaining TDBE; the resulting TDBE reaction product contains a cyclic borate structure and a glycidyl ether type epoxy group.
5. The composite membrane according to claim 1, characterized in that, The tannic acid-modified bamboo powder has a particle size of 200-500 mesh and a moisture content of no more than 1.0%. The preparation of the tannic acid-modified bamboo powder includes: treating bamboo powder with 2-5 wt% NaOH solution at 60-80℃ for 1-3 hours, washing with water until neutral; then placing the alkali-treated bamboo powder in 0.5-2.0 wt% tannic acid aqueous solution, treating it at 20-40℃ for 2-8 hours at a solid-liquid ratio of 1g bamboo powder to 10-30mL tannic acid aqueous solution, filtering, washing with water, and vacuum drying.
6. The composite membrane according to claim 1, characterized in that, The antioxidant is antioxidant 1010, antioxidant 168, or a combination of both; the lubricant is one or more of stearate, erucamide, and polyethylene wax.
7. A method for preparing the composite membrane according to any one of claims 1 to 6, characterized in that, Includes the following steps: S1: Dry PLA and PBAT under vacuum at 60-90℃ for 6-10 hours, and dry tannic acid-modified bamboo powder under vacuum at 50-70℃ for 8-12 hours. S2: Mix the dried PLA, PBAT, tannic acid deposited modified bamboo powder, TDBE, antioxidant and lubricant evenly; S3: The mixture is fed into a twin-screw extruder and melt-blended at 150–185°C and 100–350 rpm. The mixture is then extruded, cooled, and pelletized to obtain composite masterbatch. S4: The composite masterbatch is blow-molded into a film to obtain the composite film.
8. The preparation method according to claim 7, characterized in that, The processing temperature of the twin-screw extruder is 160–180℃, and the blow molding film temperature is 160–180℃.
9. The preparation method according to claim 7, characterized in that, The preparation of TDBE includes: M1, adding 3,5-dihydroxyphenylboronic acid and α,α′-diglycerol in a molar ratio of 2:1 to a reactor equipped with a water separator, using toluene as solvent, and reacting under nitrogen protection at 110°C under reflux to separate water, to obtain a bicyclic borate intermediate; M2, reacting the bicyclic borate intermediate with epichlorohydrin, wherein the molar ratio of epichlorohydrin to the bicyclic borate intermediate is not less than 8:1, reacting at 55-65°C in the presence of NaOH and a phase transfer catalyst, causing the phenolic hydroxyl groups of the intermediate to undergo etherification and ring closure to form glycidyl ether groups; subsequently removing unreacted epichlorohydrin under reduced pressure, washing with water until neutral, and vacuum drying to obtain TDBE.