A biodegradable packaging material and its preparation method
By combining specific components and processes, the problems of insufficient interfacial compatibility and barrier properties in biodegradable packaging materials have been solved, achieving the effect of adjusting the biodegradation rate while maintaining mechanical strength, making it suitable for food and daily necessities packaging.
Patent Information
- Application Number
- CN202611612229.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing biodegradable packaging materials in the polylactic acid and butylene adipate-butylene terephthalate copolymer blend system have limited interfacial compatibility and difficulty in dispersing nanofillers, resulting in insufficient barrier properties and difficulty in regulating the biodegradation rate while maintaining mechanical strength.
By combining a specific ratio of polylactic acid, butylene adipate-butylene terephthalate copolymer, amphiphilic reactive compatibilizer, aminated nano-barrier filler, controllable degradation cycle regulator, thermoplastic starch and processing aids, and by combining thermoplastic starch plasticizing, reactive extrusion, blown film and biaxial stretching processes, the interfacial compatibility and barrier properties are improved, and the biodegradability is regulated under controlled composting conditions.
It achieves synergistic optimization of mechanical properties, barrier properties and biodegradability, improving the overall performance of the material, and is suitable for food and daily necessities packaging.
Smart Images

Figure CN123107331A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of biodegradable polymer materials technology, specifically to a biodegradable packaging material and its preparation method. Background Technology
[0002] Packaging materials are widely used in food, daily consumer goods, and other fields. Petroleum-based plastic packaging materials have long degradation cycles in the natural environment, and their accumulated waste causes environmental pollution problems. Biodegradable polyesters, represented by polylactic acid (PLA), have attracted attention in the packaging field. PLA is derived from renewable resources and can decompose into carbon dioxide and water under composting conditions.
[0003] Polylactic acid (PLA) melt has low strength and insufficient flexibility, resulting in limited compatibility with various high-toughness biodegradable polyesters. Blends are prone to phase separation and interfacial delamination during film formation. Nanofillers are difficult to disperse in the PLA matrix and tend to agglomerate, limiting the improvement of film barrier properties. Starch-based natural components have weak interfacial bonding with hydrophobic polyesters, and direct blending can impair the material's mechanical continuity. The degradation rate of conventional biodegradable packaging materials is primarily controlled by the matrix composition, making it difficult to adjust the degradation window according to storage and transportation cycles while maintaining mechanical strength.
[0004] The aforementioned existing technologies lack clear technical means to simultaneously improve interfacial compatibility, barrier properties, and the adjustability of biodegradation behavior under controlled composting conditions in polylactic acid and butylene adipate-butylene terephthalate copolymer blend systems through the synergistic ratio of amphiphilic reactive compatibilizers, aminated nano-barrier fillers, controllable degradation cycle regulators, and thermoplastic starch, as well as corresponding processing techniques. Summary of the Invention
[0005] This invention addresses the problems of limited interfacial compatibility, insufficient barrier properties due to difficulties in dispersing nanofillers in polylactic acid (PLA) and butylene adipate-butylene terephthalate (BAT) copolymer blends, weak interfacial bonding of starch components, and difficulty in regulating biodegradation behavior under controlled composting conditions. It provides a biodegradable packaging material and its preparation method. This method utilizes a specific mass ratio combination of PLA, BAT-butylene adipate-butylene terephthalate copolymer, amphiphilic reactive compatibilizer, aminated nano-barrier filler, controlled degradation cycle regulator, thermoplastic starch, and processing aids. Combined with thermoplastic starch plasticization, reactive extrusion, blown film production, and biaxial stretching processes, it improves multiphase interfacial bonding and enables the material to exhibit adjustable biodegradation levels under controlled composting conditions, achieving synergistic optimization of mechanical properties, barrier properties, and biodegradability.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is: a biodegradable packaging material, wherein the biodegradable packaging material is composed of the following components by weight: 40-60 parts of polylactic acid, 20-35 parts of butylene adipate-butylene terephthalate copolymer, 2-6 parts of amphiphilic reactive compatibilizer, 2-5 parts of aminated nano barrier filler, 3-10 parts of controllable degradation cycle regulator, 5-15 parts of thermoplastic starch, and 0.5-2 parts of processing aid.
[0007] Furthermore, the amphiphilic reactive compatibilizer is composed of diacetylepoxy glycerol vegetable oil and citric acid, with a mass ratio of diacetylepoxy glycerol vegetable oil to citric acid of 3:1 to 5:1.
[0008] Furthermore, the aminated nanobarrier filler is 3-aminopropyltriethoxysilane-modified montmorillonite.
[0009] Furthermore, the controllable degradation cycle regulator is composed of polycaprolactone and benzophenone, with a mass ratio of polycaprolactone to benzophenone of 10:1 to 20:1.
[0010] Furthermore, the processing aids include antioxidants and lubricants.
[0011] Furthermore, the thermoplastic starch is obtained by plasticizing corn starch with a compound plasticizer of glycerol and formamide. The mass ratio of glycerol to formamide in the compound plasticizer is 2:1 to 3:1, and the mass ratio of the compound plasticizer of glycerol and formamide to corn starch is 0.25:1 to 0.35:1.
[0012] Furthermore, the polylactic acid has a weight-average molecular weight of 80,000 to 150,000 and an L-lactic acid unit content of ≥95%.
[0013] Furthermore, the weight-average molecular weight of the butylene adipate-butylene terephthalate copolymer is 50,000 to 100,000, and the melt index at 190°C and 2.16 kg load is 3 to 8 g / 10 min.
[0014] Furthermore, the 3-aminopropyltriethoxysilane modified montmorillonite has an interlayer spacing of 1.8~2.5 nm and a particle size D50 of 2~10 μm.
[0015] Furthermore, the polycaprolactone has a weight-average molecular weight of 30,000 to 80,000 and a melting point of 58 to 65°C; the benzophenone has a purity of ≥99% and a particle size of ≤50μm; and the thermoplastic starch has a moisture content of ≤8wt%.
[0016] Furthermore, the antioxidant is one or more of phenolic antioxidants or phosphite antioxidants, and the dosage is 0.1 to 0.5 parts.
[0017] Furthermore, the lubricant is one or more of metal soap lubricants or amide lubricants, and the dosage is 0.3 to 1.2 parts.
[0018] A method for preparing a biodegradable packaging material includes the following steps: S1: Mix corn starch with a compound plasticizer of glycerol and formamide in a high-speed mixer at a mixing temperature of 80~100℃ for 15~25 min to obtain thermoplastic starch.
[0019] S2: Polylactic acid, butylene adipate-butylene terephthalate copolymer, thermoplastic starch, amphiphilic reactive compatibilizer, aminated nano barrier filler, controllable degradation cycle regulator and processing aid are added to a high-speed mixer according to the mass ratio, and mixed at room temperature at a speed of 300~500 rpm for 10~20 min to obtain a premix.
[0020] S3: The premixed material is added to a twin-screw extruder for reactive extrusion, and then pelletized into biodegradable packaging masterbatch.
[0021] S4: The biodegradable packaging masterbatch is dried in a vacuum drying oven at 60~80℃ for 4~8h, and then fed into a single-screw extruder for melt blowing to obtain a primary film.
[0022] S5: The primary film is biaxially stretched on a biaxial stretching machine, and then heat-set to obtain biodegradable packaging material.
[0023] Furthermore, in S1, the mass ratio of glycerol to formamide is 2:1 to 3:1, and the mass ratio of the compound plasticizer of glycerol and formamide to corn starch is 0.25:1 to 0.35:1.
[0024] Furthermore, the temperature settings of each zone of the twin-screw extruder in S3 are as follows: Zone 1 150~160℃, Zone 2 160~170℃, Zone 3 170~180℃, Zone 4 175~185℃, Zone 5 175~185℃, Zone 6 170~180℃, and Die head 170~175℃. The screw speed is 150~250rpm, and the melt residence time is 2~4min. The twin-screw extruder is a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1~52:1. The screw assembly includes a conveying section, a melting section, a mixing section, and a venting section arranged sequentially along the conveying direction. The mixing section adopts a combination of kneading blocks and reverse screw elements. The vacuum degree of the venting section is -0.06~-0.09MPa.
[0025] Furthermore, the temperature of each zone of the single-screw extrusion blown film machine in S4 is set as follows: Zone 1 155~165℃, Zone 2 165~175℃, Zone 3 170~180℃, and die head 175~180℃, with a blow-up ratio of 2:1~4:1 and a draw ratio of 3:1~6:1.
[0026] Furthermore, in S5, the biaxial stretching is carried out in successive biaxial stretching, with the longitudinal stretching temperature being 55~65℃ and the longitudinal stretching ratio being 2:1~3:1, the transverse stretching temperature being 60~70℃ and the transverse stretching ratio being 2:1~3:1, the stretching rate being 50~200% / s, the heat setting temperature being 80~100℃ and the heat setting time being 5~10s, the cooling setting temperature being 20~30℃ and the cooling rate being 10~30℃ / s.
[0027] The amphiphilic reactive compatibilizer of this invention contains diacetylepoxy glyceryl vegetable oil containing epoxy groups, and citric acid containing carboxyl and hydroxyl groups. The combination of these two compounds is beneficial for improving the interfacial compatibility between polylactic acid, butylene adipate-butylene terephthalate copolymer, thermoplastic starch, and aminated nano-barrier filler during melt extrusion. This invention does not require a single, specific interfacial reaction pathway as a necessary condition for achieving the above-mentioned technical effects. The aminated nano-barrier filler is 3-aminopropyltriethoxysilane-modified montmorillonite with an interlayer spacing of 1.8~2.5 nm and a particle size D50 of 2~10 μm, which is beneficial for polymer chain insertion and lamellar dispersion, improving gas barrier properties. The controllable degradation cycle regulator is composed of polycaprolactone and benzophenone. Polycaprolactone provides flexible and biodegradable polyester components, and the two are compounded at a mass ratio of 10:1~20:1. This application uses the biodegradation rate on day 180 under controlled composting conditions to evaluate the regulatory effect of the compound component on the degradation behavior of the material; the "controllable degradation cycle regulator" is the name of the above compound component and does not mean that the material will be completely degraded within the preset number of days.
[0028] The thermoplastic starch is plasticized by mixing corn starch with a plasticizer of glycerol and formamide at 80-100℃, with a water content ≤8wt%. The ratio and temperature conditions allow the starch to form a thermoplastic state that can be melt-blended with a polyester matrix. The processing aids include antioxidants to inhibit high-temperature processing oxidation and lubricants to reduce melt viscosity. In the preparation process, S1 (plasticized starch) is carried out independently; S2 (room temperature mixing) avoids premature reaction of the compatibilizer; S3 (reactive extrusion) completes melt mixing, interfacial compatibilization, and degassing under a specified temperature zone and screw configuration; S4 (drying to remove moisture) followed by blown film formation into a primary film; and S5 (biaxial stretching) orients the molecular chains and heat-sets to lock in dimensions, thereby obtaining a biodegradable packaging material with excellent comprehensive performance. The "biodegradable packaging masterbatch" referred to in this application refers to the composite granules obtained by reactive extrusion and pelletizing of all the above-mentioned formulation components in S3, and directly used in S4 (blown film formation).
[0029] In specific operation, the speed of the S1 high-speed mixer can be selected from 300 to 500 rpm, and the melt residence time of the S3 twin-screw extruder is 2 to 4 minutes, which is conducive to the full melting and mixing of each component and the realization of interfacial compatibilization; the S5 stretching rate of 50 to 200% / s is used to control the stability of the film stretching process. Biaxial stretching is beneficial to the orientation of polylactic acid and copolymer chains and makes the montmorillonite sheets tend to be oriented along the film plane, thereby extending the gas diffusion path; after uniform dispersion, the controllable degradation cycle regulator is used to adjust the biodegradation rate of the material on day 180 under controlled composting conditions. The resulting film can be cut according to the size of the packaging carton and used as the inner lining film or coating material of the packaging carton; this application only involves the specific use scenario of the resulting film and does not change the above material formulation, preparation process and performance testing methods.
[0030] In this application, the weight-average molecular weights of polylactic acid, butylene adipate-butylene terephthalate copolymer, and polycaprolactone were determined by gel permeation chromatography; the particle size D50 of the packing material was determined by laser particle size distribution; the interlayer spacing of montmorillonite was calculated from the position of characteristic peaks in X-ray diffraction according to Bragg's law; and the moisture content of thermoplastic starch was determined by loss on drying. The same parameters in each embodiment and comparative example were measured using the same methods.
[0031] Compared with the prior art, the beneficial effects of the present invention are: The biodegradable packaging material and its preparation method provided by this invention achieve comprehensive optimization of mechanical properties, barrier properties and biodegradability under controlled composting conditions through a specific mass combination of polylactic acid, butylene adipate-butylene terephthalate copolymer, amphiphilic reactive compatibilizer, aminated nano barrier filler, controllable degradation cycle regulator, thermoplastic starch and processing aids, and synergistic reaction extrusion, blown film and biaxial stretching processes.
[0032] Based on the tensile strength, elongation at break, oxygen permeability, and biodegradability test data of Examples 1 to 5 and Comparative Examples 1 to 9, the specific beneficial effects are as follows: In terms of mechanical properties, Example 1 exhibited a tensile strength of 30.5 MPa and an elongation at break of 120.0%, which significantly higher than the strength and toughness of Comparative Example 1 (22.4 MPa and 70.0% without the amphiphilic reactive compatibilizer), Comparative Example 2 (26.8 MPa and 95.0% without the aminated nano-barrier filler), Comparative Example 5 (25.3 MPa and 90.0% with a changed compatibilizer ratio), and Comparative Example 9 (27.5 MPa and 98.0% using unmodified montmorillonite). This indicates that the amphiphilic reactive compatibilizer improves interfacial compatibility, and the aminated nano-barrier filler enhances interfacial bonding, playing a crucial role in improving mechanical properties. Regarding barrier properties, Example 1 had an oxygen permeability of 85.2 cm⁻¹. 3 / (m 2The pressure (0.1 MPa in 24 hours) was significantly lower than that of Comparative Example 1 (140.3 cm). 3 / (m 2 (24h, 0.1MPa), 155.6cm in Comparative Example 2 3 / (m 2 (24h·0.1MPa) and Comparative Example 9's 148.2cm 3 / (m 2 (24h, 0.1MPa) confirmed that the amphiphilic reactive compatibilizer and the aminated nano-barrier filler synergistically form a dense barrier network, effectively reducing gas permeability. Furthermore, in Example 2, even with a higher filler content, the oxygen permeability was as low as 62.4 cm⁻¹. 3 / (m 2 (24h, 0.1MPa); Regarding biodegradability, the biodegradation rate of Example 1 on day 180 was 75.3%, while that of Comparative Example 3, which removed the controlled degradation cycle regulator, was 55.4%, indicating that the regulator has a significant impact on the biodegradation rate on day 180 under controlled composting conditions; By adjusting the mass ratio and dosage of polycaprolactone to benzophenone, the biodegradation rates of Examples 2 to 5 on day 180 varied from 68.9% to 82.6%, indicating that this technical solution can regulate the biodegradation level under controlled composting conditions.
[0033] The components of this invention form a synergistic effect under limited proportions and processes, enabling the material to achieve comprehensive performance superior to that of single component substitution or proportion deviation while maintaining processing fluidity. It is suitable for the food and daily necessities packaging field, especially for packaging paper boxes, and can be used as an inner lining film or coating material for packaging paper boxes. Attached Figure Description
[0034] Figure 1 These are scanning electron microscope (SEM) comparison images of the cross-sections of the biodegradable packaging material films obtained in Example 1, Comparative Example 1, and Comparative Example 9 of the present invention.
[0035] Figure 2 This is a comparison of X-ray diffraction (XRD) images of the aminated nano-barrier filler used in Example 1 of the present invention and the unmodified montmorillonite used in Comparative Example 9.
[0036] in, Figure 1 Example 1, Comparative Example 1, and Comparative Example 9 were compared using the same cross-sectional sample preparation method, the same magnification, and the same SEM observation conditions; Figure 2 Aminated nano-barrier fillers and unmodified montmorillonite were tested under the same XRD conditions, with a scanning range of 2θ = 2° to 30°. The interlayer spacing was calculated according to Bragg's law based on the positions of the corresponding layered diffraction peaks. Detailed Implementation
[0037] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are merely some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0038] Example 1: In this embodiment, biodegradable packaging materials are prepared. Each raw material is added in the following mass proportions. In actual weighing, 1 mass proportion corresponds to 10.0g for scale-up implementation.
[0039] The main raw materials used in this embodiment and their specifications are as follows: Polylactic acid, with a weight-average molecular weight of 100,000 and an L-lactic acid unit content of 97%; The butylene adipate-butylene terephthalate copolymer has a weight-average molecular weight of 70,000 and a melt index of 5 g / 10 min at 190℃ and 2.16 kg load. Citric acid, purity 99.0%; Aminated nanobarrier filler (i.e., 3-aminopropyltriethoxysilane modified montmorillonite) has an interlayer spacing of 2.0 nm and a particle size D50 of 5 μm; Polycaprolactone, with a weight-average molecular weight of 50,000 and a melting point of 60°C; Benzophenone, purity 99.5%, particle size 20μm; Pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], purity 98%; Calcium stearate, 99% purity.
[0040] S1: Preparation of thermoplastic starch: In a high-speed mixer, corn starch, glycerin and formamide are added, wherein the total target amount of thermoplastic starch is 10.00 parts, the mass ratio of compound plasticizer to corn starch is 0.25:1, and the mass ratio of glycerin to formamide is 2:1.
[0041] Total mass of thermoplastic starch = mass of corn starch + mass of compound plasticizer, mass of compound plasticizer = 0.25 × mass of corn starch.
[0042] Formula: m corn starch = m thermoplastic starch ÷ (1 + 0.25); m corn starch = 10.00 ÷ 1.25 = 8.00 parts; The compound plasticizer content is 10.00 - 8.00 = 2.00 parts. Calculation formula: mglycerol = mcompound plasticizer × 2 ÷ 3; m glycerol = 2.00 × 2 ÷ 3 = 1.33 parts; m-formamide = 2.00 × 1 ÷ 3 = 0.67 parts; Weigh 8.00 parts of corn starch, 1.33 parts of glycerol, and 0.67 parts of formamide. Mix at 90℃ for 20 minutes and at 400 rpm to obtain thermoplastic starch, which is 10.00 parts by weight of the feed and has a moisture content of 7.5 wt%. The moisture content is the measured value of the thermoplastic starch obtained after S1.
[0043] S2: Premix preparation: The following components were added to a high-speed mixer: 4.00 parts of amphiphilic reactive compatibilizer, which is composed of diacetylepoxy glyceryl vegetable oil and citric acid in a mass ratio of 3:1; 5.50 parts of controlled degradation cycle regulator, which is composed of polycaprolactone and benzophenone in a mass ratio of 10:1; and 1.00 parts of processing aid, which is composed of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and calcium stearate, with masses of 0.30 parts and 0.70 parts, respectively.
[0044] Amphiphilic reactive compatibilizer separation: Diacetylepoxy glyceryl vegetable oil ester to citric acid in a mass ratio of 3:1.
[0045] Calculation basis: m-diacetyl = mtotal × 3 ÷ 4 = 4.00 × 3 ÷ 4 = 3.00 parts; mcitric acid = mtotal × 1 ÷ 4 = 4.00 × 1 ÷ 4 = 1.00 parts.
[0046] Controlled degradation cycle regulator splitting: polycaprolactone to benzophenone mass ratio 10:1.
[0047] Calculation basis: m_polycaprolactone = m_total × 10 ÷ 11 = 5.50 × 10 ÷ 11 = 5.00 parts; m benzophenone = m total × 1 ÷ 11 = 5.50 × 1 ÷ 11 = 0.50 parts.
[0048] Specific ingredients: 50.00 parts polylactic acid, 25.00 parts butylene adipate-butylene terephthalate copolymer, 10.00 parts thermoplastic starch, 3.00 parts diacetylepoxy glyceryl vegetable oil, 1.00 parts citric acid, 3.00 parts aminated nano-barrier filler, 5.00 parts polycaprolactone, 0.50 parts benzophenone, 0.30 parts pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 0.70 parts calcium stearate. Mix at 400 rpm for 15 minutes at room temperature (25°C) to obtain the premix.
[0049] S3: Reactive extrusion granulation: The premixed material was fed into a co-rotating twin-screw extruder with a length-to-diameter ratio of 48:1. The screw assembly, along the conveying direction, consisted of a conveying section, a melting section, a mixing section, and a venting section. The mixing section used a combination of kneading blocks and reverse-screw elements. Temperatures in each zone were: Zone 1 155℃, Zone 2 165℃, Zone 3 175℃, Zone 4 180℃, Zone 5 180℃, Zone 6 175℃, and die head 172℃; screw speed 200 rpm; melt residence time 3 min; and venting section vacuum degree -0.08 MPa. The material was then pelletized to obtain biodegradable packaging masterbatch, expressed as the ratio of masterbatch mass to total feed mass. Calculation basis: R = (m_masterbatch ÷ m_feed) × 100% m_feed = 50.00 + 25.00 + 10.00 + 3.00 + 1.00 + 3.00 + 5.00 + 0.50 + 0.30 + 0.70 = 98.50 portions; R=(97.52÷98.50)×100%=99.0%.
[0050] The yield was 99.0%.
[0051] S4: Drying and blown film production: The masterbatch was dried in a vacuum drying oven at 60°C for 6 hours, and then fed into a single-screw extruder with the following temperatures: Zone 1 160°C, Zone 2 170°C, Zone 3 175°C, and Die Head 178°C; Blow-up ratio 3:1; Stretch ratio 4:1; to obtain a primary film.
[0052] S5: Biaxial stretching and heat setting: The primary film is subjected to successive biaxial stretching on a biaxial stretching machine. The longitudinal stretching temperature is 60℃, the longitudinal stretching ratio is 2.5:1, the transverse stretching temperature is 65℃, the transverse stretching ratio is 2.5:1, and the stretching rate is 100% / s. The heat setting temperature is 90℃ and the time is 8s. The cooling setting temperature is 25℃ and the cooling rate is 20℃ / s, resulting in a biodegradable packaging material.
[0053] Example 2 In this embodiment, biodegradable packaging materials are prepared. Each raw material is added in the following mass proportions. In actual weighing, 1 mass proportion corresponds to 10.0g for scale-up implementation.
[0054] In this embodiment, the processing aids are replaced with the following specific changes: the antioxidant is tris(2,4-di-tert-butylphenyl) phosphite with a purity of 98%; the lubricant is zinc stearate with a purity of 99%. The other raw materials and their specifications are the same as in Example 1 and will not be repeated.
[0055] Feeding quantities: 40.00 parts polylactic acid, 35.00 parts butylene adipate-butylene terephthalate copolymer, 2.00 parts amphiphilic reactive compatibilizer (diacetylepoxy vegetable oil glyceryl ester to citric acid mass ratio 5:1), 5.00 parts aminated nano barrier filler, 10.00 parts controllable degradation cycle regulator (polycaprolactone to benzophenone mass ratio 20:1), 5.00 parts thermoplastic starch, 1.70 parts processing aid (tris(2,4-di-tert-butylphenyl) phosphite 0.50 parts, zinc stearate 1.20 parts).
[0056] The total mass of thermoplastic starch = mass of corn starch + mass of compound plasticizer, mass of compound plasticizer = 0.25 × mass of corn starch; the mass ratio of glycerol to formamide is 2:1.
[0057] Calculation basis: m corn starch = m thermoplastic starch ÷ (1 + 0.25) = 5.00 ÷ 1.25 = 4.00 parts; m_compound plasticizer = m_thermoplastic starch - m_corn starch = 5.00 - 4.00 = 1.00 parts; mglycerol = m compound plasticizer × 2 ÷ 3 = 1.00 × 2 ÷ 3 = 0.67 parts; mformamide = m compound plasticizer × 1 ÷ 3 = 1.00 × 1 ÷ 3 = 0.33 parts.
[0058] Resolution of amphiphilic reactive compatibilizer: Diacetylepoxy glyceryl vegetable oil ester to citric acid in a mass ratio of 5:1.
[0059] Calculation basis: m diacetyl = m total × 5 ÷ 6 = 2.00 × 5 ÷ 6 = 1.67 parts; mcitric acid = mtotal × 1 ÷ 6 = 2.00 × 1 ÷ 6 = 0.33 parts.
[0060] Controlled degradation cycle regulator splitting: polycaprolactone to benzophenone mass ratio 20:1.
[0061] Calculation basis: m_polycaprolactone = m_total × 20 ÷ 21 = 10.00 × 20 ÷ 21 = 9.52 parts; m benzophenone = m total × 1 ÷ 21 = 10.00 × 1 ÷ 21 = 0.48 parts.
[0062] S1: 4.00 parts corn starch, 0.67 parts glycerol, and 0.33 parts formamide are mixed at 80℃ for 25 minutes and 300 rpm to obtain thermoplastic starch, which is 5.00 parts by weight of the feed and has a moisture content of 8.0 wt%. The moisture content is the measured value of the thermoplastic starch obtained by S1.
[0063] S2: 5.00 parts of the above thermoplastic starch, 40.00 parts of polylactic acid, 35.00 parts of butylene adipate-butylene terephthalate copolymer, 1.67 parts of diacetylepoxy glyceryl vegetable oil, 0.33 parts of citric acid, 5.00 parts of aminated nano-barrier filler, 9.52 parts of polycaprolactone, 0.48 parts of benzophenone, 0.50 parts of tris(2,4-di-tert-butylphenyl) phosphite, and 1.20 parts of zinc stearate are mixed at room temperature (25°C) and 500 rpm for 10 min to obtain a premix.
[0064] S3: The premixed material is added to a co-rotating twin-screw extruder with a length-to-diameter ratio of 48:1. The screw assembly along the conveying direction consists of a conveying section, a melting section, a mixing section, and a venting section. The mixing section uses a combination of kneading blocks and reverse screw elements. The temperatures in each zone are: Zone 1 150℃, Zone 2 160℃, Zone 3 170℃, Zone 4 175℃, Zone 5 175℃, Zone 6 170℃, and the die head 170℃; the screw speed is 250 rpm; the melt residence time is 2 min; and the vacuum degree in the venting section is -0.06 MPa. The biodegradable packaging masterbatch is obtained by stranding and pelletizing, and the ratio of masterbatch mass to the total feed mass is used for calculation. R = (m masterbatch ÷ m feed) × 100%; m masterbatch = 97.22 parts; m_feed = 40.00 + 35.00 + 2.00 + 5.00 + 10.00 + 5.00 + 1.70 = 98.70 portions; R=(97.22÷98.70)×100%=98.5%.
[0065] The yield was 98.5%.
[0066] S4: The masterbatch is dried at 80℃ for 4 hours. The temperature of the blown film is 155℃ in zone 1, 165℃ in zone 2, 170℃ in zone 3, and 175℃ at the die head using a single screw blown film. The blow-up ratio is 2:1 and the stretching ratio is 3:1 to obtain the primary film.
[0067] S5: Successive biaxial stretching, longitudinal temperature 55°C, ratio 2:1, transverse temperature 60°C, ratio 2:1, speed 50% / s; heat setting 80°C, 5s; cooling 20°C, 10°C / s, to obtain the material.
[0068] Example 3 In this embodiment, biodegradable packaging materials are prepared. Each raw material is added in the following mass proportions. In actual weighing, 1 mass proportion corresponds to 10.0g for scale-up implementation.
[0069] The types and specifications of raw materials are the same as in Example 1, and will not be repeated here.
[0070] Raw materials: 60.00 parts polylactic acid, 20.00 parts butylene adipate-butylene terephthalate copolymer, 6.00 parts amphiphilic reactive compatibilizer (ratio 3:1), 2.00 parts aminated nano barrier filler, 3.00 parts controllable degradation cycle regulator (ratio 20:1), 15.00 parts thermoplastic starch, 0.50 parts processing aid (0.20 parts pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 0.30 parts calcium stearate).
[0071] The total mass of thermoplastic starch = mass of corn starch + mass of compound plasticizer, mass of compound plasticizer = 0.35 × mass of corn starch; the mass ratio of glycerol to formamide is 3:1.
[0072] Calculation basis: m corn starch = m thermoplastic starch ÷ (1 + 0.35) = 15.00 ÷ 1.35 = 11.11 parts; m_compound plasticizer = m_thermoplastic starch - m_corn starch = 15.00 - 11.11 = 3.89 parts; mglycerin = m compound plasticizer × 3 ÷ 4 = 3.89 × 3 ÷ 4 = 2.92 parts; m formamide = m compound plasticizer × 1 ÷ 4 = 3.89 × 1 ÷ 4 = 0.97 parts.
[0073] Amphiphilic reactive compatibilizer separation: Diacetylepoxy glyceryl vegetable oil ester to citric acid in a mass ratio of 3:1.
[0074] Calculation basis: m diacetyl = m total × 3 ÷ 4 = 6.00 × 3 ÷ 4 = 4.50 parts; mcitric acid = mtotal × 1 ÷ 4 = 6.00 × 1 ÷ 4 = 1.50 parts.
[0075] Controlled degradation cycle regulator splitting: polycaprolactone to benzophenone mass ratio 20:1.
[0076] Calculation basis: m_polycaprolactone = m_total × 20 ÷ 21 = 3.00 × 20 ÷ 21 = 2.86 parts; m benzophenone = m total × 1 ÷ 21 = 3.00 × 1 ÷ 21 = 0.14 parts.
[0077] S1: 11.11 parts corn starch, 2.92 parts glycerol, and 0.97 parts formamide were mixed at 100℃ for 15 minutes and 500 rpm to obtain thermoplastic starch, which was 15.00 parts by weight of the feed and had a moisture content of 7.0 wt%. The moisture content was the measured value of the thermoplastic starch obtained by S1.
[0078] S2: Add the following components to a high-speed mixer: 60.00 parts polylactic acid, 20.00 parts butylene adipate-butylene terephthalate copolymer, 15.00 parts thermoplastic starch, 6.00 parts amphiphilic reactive compatibilizer (4.50 parts diacetylepoxy glyceryl vegetable oil and 1.50 parts citric acid), 2.00 parts aminated nano barrier filler, 3.00 parts controllable degradation cycle regulator (2.86 parts polycaprolactone and 0.14 parts benzophenone), and 0.50 parts processing aid (0.20 parts pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 0.30 parts calcium stearate). Mix at 300 rpm for 20 minutes at room temperature (25°C) to obtain a premix.
[0079] S3: The premixed material is added to a co-rotating twin-screw extruder with a length-to-diameter ratio of 48:1. The screw assembly along the conveying direction consists of a conveying section, a melting section, a mixing section, and a venting section. The mixing section uses a combination of kneading blocks and reverse screw elements. The temperatures in each zone are: Zone 1 160℃, Zone 2 170℃, Zone 3 180℃, Zone 4 185℃, Zone 5 185℃, Zone 6 180℃, and the die head 175℃; the screw speed is 150 rpm; the melt residence time is 4 min; and the vacuum degree in the venting section is -0.09 MPa. The biodegradable packaging masterbatch is obtained by stranding and pelletizing, and the ratio of masterbatch mass to the total feed mass is used for calculation. R = (m masterbatch ÷ m feed) × 100%; m masterbatch = 105.22 parts; m_feed = 60.00 + 20.00 + 6.00 + 2.00 + 3.00 + 15.00 + 0.50 = 106.50 portions; R=(105.22÷106.50)×100%=98.8%.
[0080] The yield was 98.8%.
[0081] S4: Dry the masterbatch in a vacuum drying oven at 70℃ for 8 hours, and then feed it into a single-screw extruder. The temperatures of each zone are: Zone 1 165℃, Zone 2 175℃, Zone 3 180℃, and Die head 180℃; the blow-up ratio is 4:1; the stretch ratio is 6:1; and a primary film is obtained.
[0082] S5: Successive bidirectional stretching, longitudinal stretching temperature 65℃, longitudinal stretching ratio 3:1, transverse stretching temperature 70℃, transverse stretching ratio 3:1, stretching rate 200% / s; heat setting 100℃, 10s; cooling 30℃, 30℃ / s.
[0083] Example 4 In this embodiment, biodegradable packaging materials are prepared. Each raw material is added in the following mass proportions. In actual weighing, 1 mass proportion corresponds to 10.0g for scale-up implementation.
[0084] Specifications of raw materials with variations: Polylactic acid (PLA) weight-average molecular weight 150,000, L-lactic acid content 96%; Butylene adipate-butylene terephthalate copolymer weight-average molecular weight 50,000, melt index 8 g / 10 min; Aminated nano-barrier filler interlayer spacing 1.8 nm, particle size D50 2 μm; Polycaprolactone weight-average molecular weight 30,000, melting point 58℃; Benzophenone particle size 50 μm. The types and specifications of other raw materials are the same as in Example 1.
[0085] The ingredients were added in the same proportions as in Example 1: 50.00 parts polylactic acid, 25.00 parts butylene adipate-butylene terephthalate copolymer, 4.00 parts amphiphilic reactive compatibilizer (3.00 parts diacetylepoxy glyceryl vegetable oil and 1.00 parts citric acid), 3.00 parts aminated nano-barrier filler, 5.50 parts controllable degradation cycle regulator (5.00 parts polycaprolactone and 0.50 parts benzophenone), 10.00 parts thermoplastic starch (8.00 parts corn starch, 1.33 parts glycerol and 0.67 parts formamide), and 1.00 parts processing aid (0.30 parts pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 0.70 parts calcium stearate).
[0086] S1: In a high-speed mixer, add corn starch, glycerin, and formamide. The target total amount of thermoplastic starch is 10.00 parts. The mass ratio of the compound plasticizer to corn starch is 0.25:1, and the mass ratio of glycerin to formamide is 2:1. Total mass of thermoplastic starch = mass of corn starch + mass of compound plasticizer. Mass of compound plasticizer = 0.25 × mass of corn starch. Calculation formula: m_cornstarch = m_thermoplastic starch ÷ (1 + 0.25); m corn starch = 10.00 ÷ 1.25 = 8.00 parts; The compound plasticizer content is 10.00 - 8.00 = 2.00 parts. mglycerol = mcompound plasticizer × 2 ÷ 3; m glycerol = 2.00 × 2 ÷ 3 = 1.33 parts; m-formamide = 2.00 × 1 ÷ 3 = 0.67 parts.
[0087] Accordingly, 8.00 parts of corn starch, 1.33 parts of glycerol, and 0.67 parts of formamide were weighed, mixed at 90℃ for 20 min at 400 rpm to obtain thermoplastic starch, which was 10.00 parts by weight of the feed and had a moisture content of 7.5 wt%. The moisture content was the measured value of the thermoplastic starch obtained after S1.
[0088] S2: Add the following components to a high-speed mixer: 50.00 parts polylactic acid, 25.00 parts butylene adipate-butylene terephthalate copolymer, 10.00 parts thermoplastic starch, 3.00 parts diacetylepoxy glyceryl vegetable oil, 1.00 parts citric acid, 3.00 parts aminated nano-barrier filler, 5.00 parts polycaprolactone, 0.50 parts benzophenone, 0.30 parts pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 0.70 parts calcium stearate. Mix at 400 rpm for 15 minutes at room temperature (25°C) to obtain a premix.
[0089] S3: The premixed material is added to a co-rotating twin-screw extruder with a length-to-diameter ratio of 48:1. The screw assembly along the conveying direction consists of a conveying section, a melting section, a mixing section, and a venting section. The mixing section uses a combination of kneading blocks and reverse screw elements. The temperatures in each zone are: Zone 1 155℃, Zone 2 165℃, Zone 3 175℃, Zone 4 180℃, Zone 5 180℃, Zone 6 175℃, and the die head 172℃; the screw speed is 200 rpm; the melt residence time is 3 min; and the vacuum degree in the venting section is -0.08 MPa. The biodegradable packaging masterbatch is obtained by stranding and pelletizing, and is expressed as the ratio of masterbatch mass to the total feed mass. The calculation basis is: R = (m masterbatch ÷ m feed) × 100%; m_feed = 50.00 + 25.00 + 4.00 + 3.00 + 5.50 + 10.00 + 1.00 = 98.50 portions; m masterbatch = 97.52 parts; R=(97.52÷98.50)×100%=99.0%.
[0090] The yield was 99.0%.
[0091] S4: Dry the masterbatch in a vacuum drying oven at 60℃ for 6 hours, and then feed it into a single-screw extruder. The temperatures of each zone are: Zone 1 160℃, Zone 2 170℃, Zone 3 175℃, and Die head 178℃; the blow-up ratio is 3:1; the stretch ratio is 4:1; and a primary film is obtained.
[0092] S5: The primary film is biaxially stretched sequentially on a biaxial stretching machine. The longitudinal stretching temperature is 60℃, the longitudinal stretching ratio is 2.5:1, the transverse stretching temperature is 65℃, the transverse stretching ratio is 2.5:1, and the stretching rate is 100% / s. The heat setting temperature is 90℃ and the time is 8s. The cooling setting temperature is 25℃ and the cooling rate is 20℃ / s to obtain a biodegradable packaging material.
[0093] Example 5 In this embodiment, biodegradable packaging materials are prepared. Each raw material is added in the following mass proportions. In actual weighing, 1 mass proportion corresponds to 10.0g. The types and specifications of raw materials are the same as in Example 1.
[0094] Feeding method is the same as in Example 1: 50.00 parts of polylactic acid, 25.00 parts of butylene adipate-butylene terephthalate copolymer, 4.00 parts of amphiphilic reactive compatibilizer (3.00 parts of diacetylepoxy glyceryl vegetable oil and 1.00 parts of citric acid), 3.00 parts of aminated nano-barrier filler, 5.50 parts of controllable degradation cycle regulator (5.00 parts of polycaprolactone and 0.50 parts of benzophenone), 10.00 parts of thermoplastic starch (8.00 parts of corn starch, 1.33 parts of glycerol and 0.67 parts of formamide), and 1.00 parts of processing aid (0.30 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 0.70 parts of calcium stearate).
[0095] S1: In a high-speed mixer, add corn starch, glycerin, and formamide. The target total amount of thermoplastic starch is 10.00 parts. The mass ratio of the compound plasticizer to corn starch is 0.25:1, and the mass ratio of glycerin to formamide is 2:1. Total mass of thermoplastic starch = mass of corn starch + mass of compound plasticizer. Mass of compound plasticizer = 0.25 × mass of corn starch. Calculation formula: m_cornstarch = m_thermoplastic starch ÷ (1 + 0.25); m corn starch = 10.00 ÷ 1.25 = 8.00 parts; The compound plasticizer content is 10.00 - 8.00 = 2.00 parts. mglycerol = mcompound plasticizer × 2 ÷ 3; m glycerol = 2.00 × 2 ÷ 3 = 1.33 parts; m-formamide = 2.00 × 1 ÷ 3 = 0.67 parts.
[0096] Accordingly, 8.00 parts of corn starch, 1.33 parts of glycerol, and 0.67 parts of formamide were weighed, mixed at 90℃ for 20 min at 400 rpm to obtain thermoplastic starch, which was 10.00 parts by weight of the feed and had a moisture content of 7.5 wt%. The moisture content was the measured value of the thermoplastic starch obtained after S1.
[0097] S2: Add the following components to a high-speed mixer: 50.00 parts polylactic acid, 25.00 parts butylene adipate-butylene terephthalate copolymer, 10.00 parts thermoplastic starch, 3.00 parts diacetylepoxy glyceryl vegetable oil, 1.00 parts citric acid, 3.00 parts aminated nano-barrier filler, 5.00 parts polycaprolactone, 0.50 parts benzophenone, 0.30 parts pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 0.70 parts calcium stearate. Mix at 400 rpm for 15 minutes at room temperature (25°C) to obtain a premix.
[0098] S3: The premixed material is added to a co-rotating twin-screw extruder with a length-to-diameter ratio of 48:1. The screw assembly along the conveying direction consists of a conveying section, a melting section, a mixing section, and a venting section. The mixing section uses a combination of kneading blocks and reverse screw elements. The temperatures in each zone are: Zone 1 155℃, Zone 2 165℃, Zone 3 175℃, Zone 4 180℃, Zone 5 180℃, Zone 6 175℃, and the die head 172℃; the screw speed is 200 rpm; the melt residence time is 3 min; and the vacuum degree in the venting section is -0.08 MPa. The biodegradable packaging masterbatch is obtained by stranding and pelletizing, and is expressed as the ratio of masterbatch mass to the total feed mass. The calculation basis is: R = (m masterbatch ÷ m feed) × 100%; m_feed = 50.00 + 25.00 + 4.00 + 3.00 + 5.50 + 10.00 + 1.00 = 98.50 portions; m masterbatch = 97.52 parts; R=(97.52÷98.50)×100%=99.0%.
[0099] The yield was 99.0%.
[0100] S4: The masterbatch is dried at 60℃ for 6 hours, and blown into film by a single screw at 160℃ in zone 1, 170℃ in zone 2, 175℃ in zone 3, and 178℃ at the die head; the blow-up ratio is 4:1; the stretching ratio is 6:1, to obtain the primary film.
[0101] S5: Successive bidirectional stretching, longitudinal stretching temperature 60℃, longitudinal stretching ratio 3:1, transverse stretching temperature 65℃, transverse stretching ratio 3:1, stretching rate 150% / s; heat setting 85℃, 7s; cooling 25℃, 15℃ / s, to obtain biodegradable packaging material.
[0102] Comparative Example 1 The preparation of a biodegradable packaging material is carried out according to the preparation method of Example 1, except that the amphiphilic reactive compatibilizer (3.00 parts of diacetylepoxy glyceryl vegetable oil and 1.00 parts of citric acid) is replaced with 4.00 parts by weight of polylactic acid. After the replacement, the amount of polylactic acid added is 54.00 parts, and the rest is the same as in Example 1.
[0103] The amount of polylactic acid (PLA) added after replacement: The mass fraction of PLA after replacement is equal to the sum of the mass fraction of the original PLA and the total mass fraction of the replaced amphiphilic reactive compatibilizer.
[0104] Calculation basis: m-polylactic acid, new = m-polylactic acid, original + m-compensator; Numerical substitution and calculation: Polylactic acid (PLA), new = 50.00 + 4.00 = 54.00 parts.
[0105] The calculation result is that the amount of polylactic acid added after replacement is 54.00 parts.
[0106] Comparative Example 2 The preparation of a biodegradable packaging material is carried out by referring to the preparation method of Example 1, except that 3.00 parts of the aminated nano barrier filler are replaced with 3.00 parts of polylactic acid by weight, and the amount of polylactic acid added after replacement is 53.00 parts, and the rest is the same as in Example 1.
[0107] Replacement polylactic acid feed amount: The mass fraction of the replaced polylactic acid is equal to the sum of the mass fraction of the original polylactic acid and the mass fraction of the replaced aminated nano barrier filler.
[0108] Calculation basis: m-polylactic acid, new = m-polylactic acid, original + m-filler; Numerical substitution and calculation: Polylactic acid (PLA), new = 50.00 + 3.00 = 53.00 parts.
[0109] The calculation result is that the amount of polylactic acid added after replacement is 53.00 parts.
[0110] Comparative Example 3 The preparation of a biodegradable packaging material is carried out according to the preparation method of Example 1, except that the controllable degradation cycle regulator (5.00 parts of polycaprolactone and 0.50 parts of benzophenone) is replaced with 5.50 parts by weight of polylactic acid. After the replacement, the amount of polylactic acid added is 55.50 parts, and the rest is the same as in Example 1.
[0111] Replacement polylactic acid feed amount: The mass fraction of the replaced polylactic acid is equal to the sum of the mass fraction of the original polylactic acid and the total mass fraction of the replaced controllable degradation cycle regulator.
[0112] Calculation basis: m-polylactic acid, new = m-polylactic acid, original + m-regulator; Numerical substitution and calculation: Polylactic acid (PLA), new = 50.00 + 5.50 = 55.50 parts; The calculation result is that the amount of polylactic acid added after replacement is 55.50 parts.
[0113] Comparative Example 4 The preparation of a biodegradable packaging material follows the preparation method of Example 1, except that the processing aid (0.30 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and 0.70 parts of calcium stearate) is replaced with 1.00 parts by weight of polylactic acid. After the replacement, the amount of polylactic acid added is 51.00 parts, and the rest remains the same as in Example 1.
[0114] The amount of polylactic acid (PLA) added after replacement: The mass fraction of PLA after replacement is equal to the sum of the mass fraction of the original PLA and the total mass fraction of the replaced processing aids.
[0115] Calculation basis: m-polylactic acid, new = m-polylactic acid, original + m-auxiliary agent; Numerical substitution and calculation: Polylactic acid (PLA), new = 50.00 + 1.00 = 51.00 parts.
[0116] The calculation result is that the amount of polylactic acid added after replacement is 51.00 parts.
[0117] Comparative Example 5 The preparation of a biodegradable packaging material follows the preparation method of Example 1, except that the amphiphilic reactive compatibilizer (3.00 parts of diacetylepoxy vegetable oleate and 1.00 parts of citric acid) is replaced with 2.00 parts of diacetylepoxy vegetable oleate and 2.00 parts of citric acid. After the replacement, the amount of diacetylepoxy vegetable oleate and citric acid in the amphiphilic reactive compatibilizer is 2.00 parts, and the rest remains the same as in Example 1.
[0118] After replacement, the total mass of the amphiphilic reactive compatibilizer remains at 4.00 parts, and the mass ratio becomes 1:1; the total mass of 4.00 parts is allocated in a 1:1 ratio, resulting in 2.00 parts of diacetylepoxy glyceryl vegetable oil and 2.00 parts of citric acid.
[0119] Calculation basis: m diacetyl = m total × 1 ÷ 2 = 4.00 × 1 ÷ 2 = 2.00 parts; mcitric acid = mtotal × 1 ÷ 2 = 4.00 × 1 ÷ 2 = 2.00 parts.
[0120] The calculation results show that the amount of diacetylepoxy vegetable oil glyceride and citric acid added after replacement is 2.00 parts.
[0121] Comparative Example 6 The preparation of a biodegradable packaging material follows the preparation method of Example 1, except that the controlled degradation cycle regulator (5.00 parts of polycaprolactone and 0.50 parts of benzophenone) is replaced with 4.58 parts of polycaprolactone and 0.92 parts of benzophenone. After the replacement, the amount of polycaprolactone in the controlled degradation cycle regulator is 4.58 parts and the amount of benzophenone is 0.92 parts, while the rest remains the same as in Example 1.
[0122] After replacement, the total mass of the controllable degradation cycle regulator remains at 5.50 parts, and the mass ratio of polycaprolactone to benzophenone becomes 5:1; the total mass of 5.50 parts is distributed in a 5:1 ratio, resulting in 4.58 parts of polycaprolactone and 0.92 parts of benzophenone.
[0123] Calculation basis: m_polycaprolactone = m_total × 5 ÷ 6 = 5.50 × 5 ÷ 6 = 4.58 parts; m benzophenone = m total × 1 ÷ 6 = 5.50 × 1 ÷ 6 = 0.92 parts.
[0124] The calculation results show that the amount of polycaprolactone added after replacement is 4.58 parts and the amount of benzophenone added is 0.92 parts.
[0125] Comparative Example 7 The preparation of a biodegradable packaging material is carried out by referring to the preparation method of Example 1, except that the mass ratio of S1 glycerol to formamide is replaced by 1:1 instead of 2:1. After the replacement, the amount of glycerol and formamide is 1.00 parts, and the rest is the same as in Example 1.
[0126] After replacement, the total mass of the compound plasticizer remains unchanged at 2.00 parts. Glycerin and formamide are distributed in a 1:1 ratio, resulting in 1.00 parts of glycerin and 1.00 parts of formamide.
[0127] Calculation basis: mglycerol = m compound plasticizer × 1 ÷ 2 = 2.00 × 1 ÷ 2 = 1.00 parts; m formamide = m compound plasticizer × 1 ÷ 2 = 2.00 × 1 ÷ 2 = 1.00 parts.
[0128] The calculation results show that the amount of glycerol and formamide added after replacement is 1.00 part.
[0129] Comparative Example 8 The preparation of a biodegradable packaging material is carried out by referring to the preparation method of Example 1, except that the temperatures of each temperature zone of the S3 twin-screw extruder are replaced as follows: Zone 1 135℃, Zone 2 145℃, Zone 3 155℃, Zone 4 160℃, Zone 5 160℃, Zone 6 155℃, and Die Head 152℃, while the rest remains the same as in Example 1.
[0130] Comparative Example 9 The preparation of a biodegradable packaging material is carried out by referring to the preparation method of Example 1, except that the aminated nano-barrier filler is replaced with montmorillonite, and the rest is the same as in Example 1.
[0131] The specifications of the new raw material montmorillonite introduced after the replacement are as follows: montmorillonite, interlayer spacing of 1.2 nm, particle size D50 of 5 μm.
[0132] Performance testing methods 1. Tensile strength and elongation at break tests: Test Objective: To evaluate the mechanical strength and toughness of biodegradable packaging materials. Sample Preparation: The biodegradable packaging materials prepared in the examples and comparative examples were cut into dumbbell-shaped specimens. All examples and comparative examples were compared using the same cutting direction. The specimen type was Type 2 as specified in GB / T1040.3-2006, which specifies the tensile property test method for plastic films and sheets and is applicable to the mechanical evaluation of biodegradable packaging film in this system. The gauge length was 50 mm, the width was 10 mm, and the thickness was approximately 0.05 mm of the actual film thickness. The samples were conditioned at 23°C and 50% relative humidity for 48 hours.
[0133] Testing instrument: Electronic universal testing machine, measuring range 500N, load sensor accuracy ±0.5%. Calibration: The testing machine is calibrated daily with standard weights, and the extensometer is calibrated according to the manufacturer's specifications.
[0134] Test conditions: tensile rate 50 mm / min, clamping distance 50 mm, ambient temperature 23℃, relative humidity 50%, 5 samples were measured in parallel.
[0135] Calculation formulas: Tensile strength σ = F / (b × d), where F is the maximum tensile force (N), b is the specimen width (mm), and d is the specimen thickness (mm); Elongation at break ε = (L - L0) / L0 × 100%, where L0 is the gauge length and L is the length at break. Results are expressed as the arithmetic mean of 5 specimens, in MPa and %.
[0136] 2. Oxygen permeability test: Test objective: To evaluate the gas barrier properties of biodegradable packaging materials. Sample preparation: The biodegradable packaging materials prepared in the examples and comparative examples were cut into circular specimens with a diameter of 100 mm, and the actual thickness of each specimen was measured. The thickness of each specimen used for the lateral comparison in Table 2 was controlled at a similar level of about 0.05 mm. After drying at 23°C and 0% relative humidity for 24 h, the specimens were placed in a desiccator for later use.
[0137] Test instrument: Gas permeability tester, based on the differential pressure method, tested according to GB / T1038.1-2022 "Test methods for gas permeability of plastic films and sheets - Part 1: Differential pressure method". Calibration: The instrument is calibrated using a standard reference membrane to ensure system tightness.
[0138] Test conditions: Test temperature 23℃, relative humidity 0%, low-pressure side vacuum degree less than 10Pa, test area 50cm² 2 The pressure difference was 100 kPa, and each sample was tested 3 times and the average was taken.
[0139] Data processing: Following the differential pressure method, the oxygen permeability was calculated based on the rate of change of low-pressure side pressure, low-pressure side volume, test temperature, test area, and pressure difference across the sample during the steady-state phase. Table 2 of this application reports the oxygen permeability, which is not normalized to sample thickness. All examples and comparative examples in Table 2 are compared at similar thickness levels of approximately 0.05 mm to minimize the impact of film thickness differences on formulation comparisons. Results are expressed as the arithmetic mean of three parallel tests, in cm³ / (m²·24h·0.1MPa).
[0140] 3. Biodegradation rate test: Test objective: To evaluate the final aerobic biodegradability and biodegradation level of biodegradable packaging materials under controlled composting conditions.
[0141] Sample Preparation: The biodegradable packaging materials prepared in the examples and comparative examples were pulverized to a particle size of less than 2 mm. Approximately 20.0 g of dried sample was weighed and mixed with the inoculum at a mass ratio of 1:4, then placed into a reaction vessel. Testing Basis: The test was conducted according to GB / T19277.1-2025, "Determination of the Final Aerobic Biodegradability of Materials under Controlled Composting Conditions—Method for Determining the Release of Carbon Dioxide—Part 1: General Method". Instrumentation: A composting bioreactor system equipped with a carbon dioxide capture and quantitative analysis device. Calibration: A system blank test and a standard reference microcrystalline cellulose were conducted simultaneously to verify activity. Conditions: Composting temperature 58±2℃, moisture content of the compost mixture controlled at 50%~60%, incubation period set at 180 days, and the amount of carbon dioxide released measured periodically, with 3 parallel samples.
[0142] Calculation formula: Biodegradation rate % = (CO2,T - CO2,B) / ThCO2 × 100%, where CO2,T is the cumulative carbon dioxide release of the sample, CO2,B is the cumulative release of the blank, and ThCO2 is the theoretical carbon dioxide release of the sample. ThCO2 is calculated based on the organic carbon content in the sample, i.e., ThCO2 = m × wC × 44 / 12, where m is the mass of the dried sample, and wC is the mass fraction of organic carbon in the sample; wC of each sample was determined using the same elemental analysis method. Results are expressed as the arithmetic mean of three parallel samples, representing the biodegradation rate on day 180. This application uses this index to compare the biodegradation levels of controlled compost with different formulations, but does not equate it to the termination period required for the material to reach complete degradation.
[0143] Performance test data: Table 1 Tensile strength and elongation at break test results Table 2 Oxygen Transmission Rate Test Table 3 Biodegradation rate test Depend on Figure 1 As can be seen, the cross-section of the biodegradable packaging material obtained in Example 1 is relatively dense, continuous and uniform, with good interfacial bonding and few obvious pores and interfacial debonding defects. At the same time, it can be observed that the lamellar barrier phase is uniformly dispersed in the polymer matrix. In contrast, Comparative Example 1, due to the absence of an amphiphilic reactive compatibilizer, shows more obvious pores, loose areas and interfacial separation in its cross-section, indicating poor interfacial compatibility between the components. After replacing the aminated nano barrier filler with unmodified montmorillonite in Comparative Example 9, more obvious lamellar stacking and local agglomeration structure can be observed, accompanied by certain interfacial defects. The above-mentioned differences in cross-sectional morphology indicate that the use of amphiphilic reactive compatibilizers and aminated nano-barrier fillers in this invention is beneficial to improving the interfacial bonding state between polylactic acid, butylene adipate-butylene terephthalate copolymer, thermoplastic starch and nano-fillers, promoting the dispersion of nanosheets in the matrix, thereby forming a more dense and continuous composite structure, which is consistent with the test results of Example 1, which showed higher tensile strength, elongation at break and lower oxygen permeability.
[0144] Depend on Figure 2 As can be seen, the interlayer spacing of the characteristic layered diffraction peaks of the unmodified montmorillonite used in Comparative Example 9 is approximately 1.2 nm, while the corresponding characteristic diffraction peaks of the montmorillonite modified with 3-aminopropyltriethoxysilane used in Example 1 shift significantly towards lower diffraction angles, with the corresponding interlayer spacing increasing to approximately 2.0 nm. Based on the X-ray diffraction characteristics of layered silicate materials, the shift of diffraction peaks to lower angles indicates an increase in the interlayer spacing of montmorillonite. This suggests that after modification with 3-aminopropyltriethoxysilane, the interlayer structure of montmorillonite sheets expands, which is beneficial for polymer molecular chains to enter the interlayer region and promotes the dispersion of montmorillonite sheets in the polymer matrix. This result is consistent with the interlayer spacing parameters of the aminated nanobarrier filler used in Example 1, and further confirms that aminated modification is beneficial for reducing montmorillonite sheet aggregation and increasing the diffusion path of gas molecules within the material, thereby contributing to improved gas barrier performance of the resulting biodegradable packaging material.
[0145] Based on the tensile strength and elongation at break test results shown in Table 1, the biodegradable packaging materials prepared in Examples 1 to 5 exhibit an excellent balance of mechanical properties. Example 1 showed a tensile strength of 30.5 MPa and an elongation at break of 120.0%, indicating that under the specific ratio of polylactic acid, butylene adipate-butylene terephthalate copolymer, amphiphilic reactive compatibilizer, aminated nano-barrier filler, controllable degradation cycle regulator, and thermoplastic starch, the material possesses both high strength and good toughness.
[0146] Comparing Example 1 and Comparative Example 1, it can be seen that Comparative Example 1, which removed the amphiphilic reactive compatibilizer and replaced it with an equal amount of polylactic acid, experienced a decrease in tensile strength to 22.4 MPa and elongation at break to 70.0%. This significant decrease confirms the crucial role of the amphiphilic reactive compatibilizer in improving the interfacial compatibility between polylactic acid and butylene adipate-butylene terephthalate copolymer and thermoplastic starch. The lack of this compatibilizer leads to weak interfacial bonding and low stress transfer efficiency, thereby impairing mechanical properties.
[0147] Comparing Example 1 and Comparative Example 2, it can be seen that in Comparative Example 2, the tensile strength decreased to 26.8 MPa and the elongation at break decreased to 95.0% after the removal of the aminated nano-barrier filler and its replacement with an equal amount of polylactic acid. This indicates that the aminated nano-barrier filler not only provides barrier function, but the interaction between its surface amino groups and the matrix, as well as its lamellar structure, also contribute to mechanical reinforcement. Its removal leads to a weakening of the material's ability to balance stiffness and toughness.
[0148] Comparing Example 1 and Comparative Example 3, Comparative Example 3, which removed the controlled degradation cycle regulator and replaced it with an equal amount of polylactic acid, showed a tensile strength of 29.0 MPa and an elongation at break of 118.0%, slightly lower than Example 1. This indicates that the polycaprolactone component in the controlled degradation cycle regulator plays a role in maintaining the toughness of the system, and its presence did not negatively affect the mechanical strength.
[0149] Comparing Example 1 and Comparative Example 4, it can be seen that Comparative Example 4, which removed the processing aid and replaced it with an equal amount of polylactic acid, had a tensile strength of 29.5 MPa and an elongation at break of 112.0%. The absence of the processing aid led to uneven dispersion or slight degradation during melt processing, which in turn affected the mechanical integrity of the final film.
[0150] Comparing Example 1 and Comparative Example 5, it can be seen that Comparative Example 5 changed the mass ratio of diacetylepoxyvegetal oleate glyceryl ester to citric acid in the amphiphilic reactive compatibilizer to 1:1 (exceeding the range of 3:1 to 5:1 of this invention), and its tensile strength decreased to 25.3 MPa and its elongation at break decreased to 90.0%. This indicates that an imbalance in the proportion of compatibilizer components will affect its reactivity and amphiphilic balance, resulting in poor compatibilization effect and increased interface defects.
[0151] Comparing Example 1 and Comparative Example 6, it can be seen that Comparative Example 6 changed the mass ratio of polycaprolactone to benzophenone in the controlled degradation cycle regulator to 5:1 (exceeding the range of 10:1 to 20:1 of this invention), and its tensile strength was 28.2 MPa and its elongation at break was 115.0%. Although the decrease in mechanical properties was small, deviating from the preferred ratio may affect the dispersion state of the regulator in the matrix and the level of biodegradation under controlled composting conditions.
[0152] Comparing Example 1 and Comparative Example 7, it can be seen that Comparative Example 7 changed the mass ratio of glycerol to formamide in the preparation of thermoplastic starch to 1:1 (exceeding the range of 2:1 to 3:1 of this invention), and its tensile strength decreased to 27.0 MPa and its elongation at break decreased to 100.0%. This indicates that an improper ratio of compounded plasticizers will affect the degree of plasticization of starch and its compatibility with the polyester matrix, leading to deterioration of mechanical properties.
[0153] Comparing Example 1 and Comparative Example 8, it can be seen that Comparative Example 8 reduced the processing temperature of the twin-screw extruder, resulting in a decrease in tensile strength to 24.1 MPa and elongation at break to 80.0%. The low temperature led to insufficient melting and uneven mixing of the material, resulting in a large number of microscopic defects and severely impairing the mechanical properties.
[0154] Comparing Example 1 and Comparative Example 9, it can be seen that in Comparative Example 9, the tensile strength decreased to 27.5 MPa and the elongation at break decreased to 98.0% when unmodified montmorillonite was used instead of aminated nano-barrier filler. Unmodified montmorillonite has poor compatibility with the polymer matrix and is prone to agglomeration, forming stress concentration points, which leads to a decrease in mechanical properties.
[0155] Based on the data from Examples 2 to 5, adjusting the content of each component and process parameters still maintains good mechanical properties over a wide range. Example 2, by adjusting the formulation ratio, increased the elongation at break to 165.0%, demonstrating better toughness. Example 3, by increasing the polylactic acid content, increased the tensile strength to 34.2 MPa, but the elongation at break decreased to 85.0%, reflecting increased rigidity. Examples 4 and 5, by optimizing the raw material specifications and blown film stretching process, achieved comprehensive performance of 32.8 MPa / 105.0% and 33.5 MPa / 135.0%, respectively, proving that the technical solution of this invention can achieve better mechanical performance than the comparative examples under different implementation conditions.
[0156] Based on the oxygen permeability test results shown in Table 2, the oxygen permeability of Example 1 was 85.2 cm⁻¹. 3 / (m 2 (24h, 0.1MPa). The oxygen permeability of Comparative Example 1 and Comparative Example 2 reached as high as 140.3 cm⁻¹. 3 / (m 2 ·24h·0.1MPa) and 155.6cm 3 / (m 2 The pressure (0.1 MPa) was significantly higher than in Example 1 (24h). This further confirms that the amphiphilic reactive compatibilizer improved the interfacial compactness, and the labyrinth effect formed by the good dispersion of the aminated nano-barrier filler in the matrix jointly enhanced the gas barrier performance. Comparative Example 9 used unmodified montmorillonite, with an oxygen permeability of 148.2 cm⁻¹. 3 / (m 2(24h, 0.1MPa) Due to aggregation, the blocking pathway failed. Comparative Examples 5 and 7, due to component imbalance, had oxygen permeability of 105.2 cm⁻¹, respectively. 3 / (m 2 ·24h·0.1MPa) and 92.3cm 3 / (m 2 The pressure (24h, 0.1MPa) was higher than that in Example 1, indicating that precise control of the component ratio is crucial for constructing an efficient barrier network.
[0157] The oxygen permeability of Example 2 was as low as 62.4 cm⁻¹. 3 / (m 2 (24h·0.1MPa), thanks to the high amount of aminated nano-barrier filler and optimized interfacial bonding.
[0158] According to the biodegradation rate test results shown in Table 3, the biodegradation rate of Example 1 was 75.3% on day 180. Comparative Example 3, without the controlled degradation cycle regulator, had a biodegradation rate of 55.4%, lower than Example 1, indicating that the controlled degradation cycle regulator composed of polycaprolactone and benzophenone had a significant impact on the biodegradation rate on day 180 under controlled composting conditions. Comparative Example 6, with the mass ratio of polycaprolactone to benzophenone adjusted to 5:1, had a biodegradation rate of 85.3% on day 180, but its mechanical properties were lower than those of Example 1, indicating that the proportion of the regulator composition needs to be comprehensively selected in conjunction with mechanical properties. The biodegradation rates on day 180 of Examples 2 to 5 ranged from 68.9% to 82.6%, indicating that different controlled composting biodegradation levels can be obtained by adjusting the amount and proportion of the compound components. The biodegradation rates of Comparative Examples 1, 2, 4, 5, 7, 8, and 9 on day 180 ranged from 70.2% to 74.8%, indicating that changes in other components, even with the retention of the controllable degradation cycle regulator, can still affect the final test results. The above data are only used to evaluate the differences in biodegradation under 180-day controlled composting conditions and do not constitute a requirement for the materials to completely degrade at a predetermined number of days.
[0159] In summary, this invention achieves an excellent balance between mechanical properties, barrier properties, and adjustable biodegradability under controlled composting conditions through the synergistic effect of specific components and process control. The comparative data from different dimensions demonstrate the necessity and synergistic effect of the technical features of this invention.
[0160] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A biodegradable packaging material, characterized in that, The biodegradable packaging material is composed of the following components by weight: 40-60 parts polylactic acid, 20-35 parts butylene adipate-butylene terephthalate copolymer, 2-6 parts amphiphilic reactive compatibilizer, 2-5 parts aminated nano barrier filler, 3-10 parts controlled degradation cycle regulator, 5-15 parts thermoplastic starch, and 0.5-2 parts processing aid; The amphiphilic reactive compatibilizer is composed of diacetylepoxy glycerol vegetable oil and citric acid, with a mass ratio of diacetylepoxy glycerol vegetable oil to citric acid of 3:1 to 5:
1. The aminated nanobarrier filler is 3-aminopropyltriethoxysilane-modified montmorillonite. The controllable degradation cycle regulator is composed of polycaprolactone and benzophenone, with a mass ratio of polycaprolactone to benzophenone of 10:1 to 20:
1. The processing aids include antioxidants and lubricants; The thermoplastic starch is prepared by plasticizing corn starch with a compound plasticizer of glycerol and formamide. The mass ratio of glycerol to formamide in the compound plasticizer is 2:1 to 3:1, and the mass ratio of the compound plasticizer of glycerol and formamide to corn starch is 0.25:1 to 0.35:
1.
2. The biodegradable packaging material according to claim 1, characterized in that, The polylactic acid has a weight-average molecular weight of 80,000 to 150,000 and an L-lactic acid unit content of ≥95%. The butylene adipate-butylene terephthalate copolymer has a weight-average molecular weight of 50,000 to 100,000 and a melt index of 3 to 8 g / 10 min at 190°C and 2.16 kg load.
3. The biodegradable packaging material according to claim 1, characterized in that, The 3-aminopropyltriethoxysilane-modified montmorillonite has an interlayer spacing of 1.8~2.5 nm and a particle size D50 of 2~10 μm.
4. A biodegradable packaging material according to claim 1, characterized in that, The polycaprolactone has a weight-average molecular weight of 30,000 to 80,000 and a melting point of 58 to 65°C; the benzophenone has a purity of ≥99% and a particle size of ≤50μm; and the thermoplastic starch has a moisture content of ≤8wt%.
5. A biodegradable packaging material according to claim 1, characterized in that, The antioxidant is one or more of phenolic antioxidants or phosphite antioxidants, and the dosage is 0.1 to 0.5 parts; The lubricant is one or more of metal soap lubricants or amide lubricants, and the dosage is 0.3 to 1.2 parts.
6. A method for preparing a biodegradable packaging material as described in claims 1-5, characterized in that, Includes the following steps: S1: Corn starch is mixed with a compound plasticizer of glycerin and formamide in a high-speed mixer at a mixing temperature of 80~100℃ for 15~25 min to obtain thermoplastic starch; S2: Polylactic acid, butylene adipate-butylene terephthalate copolymer, thermoplastic starch, amphiphilic reactive compatibilizer, aminated nano barrier filler, controllable degradation cycle regulator and processing aid are added to a high-speed mixer according to the mass ratio, and mixed at room temperature at a speed of 300~500 rpm for 10~20 min to obtain a premix; S3: The premixed material is added to a twin-screw extruder for reactive extrusion, and then pelletized into biodegradable packaging masterbatch; S4: The biodegradable packaging masterbatch is dried in a vacuum drying oven at 60~80℃ for 4~8h, and then fed into a single screw extrusion blown film mill for melt blown film production to obtain a primary film; S5: The primary film is biaxially stretched on a biaxial stretching machine, and then heat-set to obtain biodegradable packaging material.
7. The method for preparing a biodegradable packaging material according to claim 6, characterized in that, In S1, the mass ratio of glycerol to formamide is 2:1 to 3:1, and the mass ratio of the compound plasticizer of glycerol and formamide to corn starch is 0.25:1 to 0.35:
1.
8. The method for preparing a biodegradable packaging material according to claim 6, characterized in that, The temperature settings for each zone of the twin-screw extruder in S3 are as follows: Zone 1 150~160℃, Zone 2 160~170℃, Zone 3 170~180℃, Zone 4 175~185℃, Zone 5 175~185℃, Zone 6 170~180℃, and Die head 170~175℃. The screw speed is 150~250 rpm, and the melt residence time is 2~4 min. The twin-screw extruder is a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1~52:
1. The screw assembly includes a conveying section, a melting section, a mixing section, and a venting section arranged sequentially along the conveying direction. The mixing section uses a combination of kneading blocks and reverse screw elements. The vacuum degree of the venting section is -0.06~-0.09 MPa.
9. A method for preparing a biodegradable packaging material according to claim 6, characterized in that, The temperature settings for each zone of the single-screw extrusion blown film extruder in S4 are as follows: Zone 1 155~165℃, Zone 2 165~175℃, Zone 3 170~180℃, and die head 175~180℃. The blow-up ratio is 2:1~4:1, and the draw ratio is 3:1~6:
1.
10. A method for preparing a biodegradable packaging material according to claim 6, characterized in that, In S5, the biaxial stretching is carried out in successive biaxial stretching, with the longitudinal stretching temperature at 55~65℃ and the longitudinal stretching ratio at 2:1~3:1, the transverse stretching temperature at 60~70℃ and the transverse stretching ratio at 2:1~3:1, the stretching rate at 50~200% / s, the heat setting temperature at 80~100℃ and the heat setting time at 5~10s, the cooling setting temperature at 20~30℃ and the cooling rate at 10~30℃ / s.