Composite flame retardants and their preparation methods, polyolefin composite materials

By using a composite flame retardant containing components such as piperazine pyrophosphate, the problem of dripping in traditional halogen-free flame retardant materials has been solved, achieving fluorine-free anti-dripping and high-efficiency flame retardancy, thus improving the stability and environmental performance of polyolefin composite materials.

CN123107366APending Publication Date: 2026-11-17DONGGUAN HONGTAIJI FLAME RETARDANT MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611524583.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional halogen-free flame-retardant polymer materials are prone to dripping during combustion, making it difficult to meet flame-retardant rating requirements, and the use of fluorinated additives does not comply with environmental access standards.

Method used

Piperazine pyrophosphate was used as the main flame retardant, combined with specific types of charring agents and anti-dripping agents to form a synergistic anti-dripping system of inorganic framework and organosilicon continuous phase. Antioxidants and coupling agents were added to prepare a composite flame retardant without the use of halogenated harmful substances such as chlorine and bromine and fluorinated anti-dripping components such as polytetrafluoroethylene.

Benefits of technology

It achieves fluorine-free anti-dripping flame retardant effect, improves the hydrolysis and damp heat resistance of composite flame retardants, inhibits the migration and precipitation of flame retardant components, and improves the long-term use stability and mechanical properties of polyolefin composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application relates to a composite flame retardant and its preparation method, as well as a polyolefin composite material. By weight, the composite flame retardant comprises the following components: 18-28 parts flame retardant, 4-10 parts charring agent, 1-5 parts anti-dripping agent, 0.1-1 parts antioxidant, and 0.1-1 parts coupling agent. The flame retardant includes a first flame retardant, which includes piperazine pyrophosphate; the charring agent includes a first charring agent and a second charring agent, the first charring agent including melamine cyanurate, and the second charring agent including at least one of calcium borate and barium metaborate; the anti-dripping agent includes a first anti-dripping agent and a second anti-dripping agent, the first anti-dripping agent including silicate, and the second anti-dripping agent including polysiloxane. Using piperazine pyrophosphate as the main flame retardant, combined with specific types of first and second charring agents, first and second anti-dripping agents, and supplemented with antioxidants and coupling agents, the anti-dripping performance can be effectively improved, giving the composite flame retardant a better flame retardant effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of flame retardant materials technology, and in particular to composite flame retardants and their preparation methods, and polyolefin composite materials. Background Technology

[0002] Polymer flame retardant formulations using phosphorus-nitrogen or intumescent halogen-free flame retardants as the main flame retardant avoid harmful halogenated substances such as chlorine and bromine, representing the mainstream direction of halogen-free polymer modification. However, to overcome combustion dripping defects and meet flame retardant rating requirements, it is still commonly necessary to compound fluorinated anti-dripping agents such as polytetrafluoroethylene (PTFE). If these fluorinated anti-dripping additives are removed, traditional halogen-free flame-retardant polymer materials are prone to melt flow and continuous high-temperature dripping during combustion, making it difficult to meet flame retardant rating requirements. Furthermore, with the continuous upgrading of environmental and safety requirements for polymer materials in fields such as home appliances, new energy components, cables, and automotive parts, the use of fluorinated additives and fluorinated flame-retardant materials is gradually becoming more restrictive. This traditional halogen-free flame-retardant modification scheme, which relies on fluorinated additives to achieve anti-dripping performance, is no longer suitable for environmental access and usage standards.

[0003] Therefore, it is necessary to improve traditional technologies. Summary of the Invention

[0004] Based on this, this application provides a fluorine-free composite flame retardant with good flame retardant properties, its preparation method, and a polyolefin composite material.

[0005] The technical solution to the above-mentioned technical problems in this application is as follows.

[0006] The first aspect of this application provides a composite flame retardant, comprising the following components by mass parts:

[0007] Flame retardant 18-28 parts, charring agent 4-10 parts, anti-dripping agent 1-5 parts, antioxidant 0.1-1 parts, and coupling agent 0.1-1 parts;

[0008] The flame retardant includes a first flame retardant, which includes piperazine pyrophosphate;

[0009] The char-forming agent includes a first char-forming agent and a second char-forming agent, wherein the first char-forming agent includes melamine cyanurate and the second char-forming agent includes at least one of calcium borate and barium metaborate.

[0010] The anti-dripping agent includes a first anti-dripping agent and a second anti-dripping agent, wherein the first anti-dripping agent includes a silicate and the second anti-dripping agent includes a polysiloxane.

[0011] In some embodiments, the composite flame retardant comprises, by mass parts, the following components:

[0012] Flame retardant 18-22 parts, charring agent 6-10 parts, anti-dripping agent 1.5-4 parts, antioxidant 0.3-0.5 parts and coupling agent 0.3-1 parts.

[0013] In some embodiments, the composite flame retardant satisfies at least one of the following conditions:

[0014] (1) The mass ratio of the char-forming agent to the flame retardant is 1:1.8~3.5;

[0015] (2) The mass ratio of the anti-dripping agent to the flame retardant is 1:4.5~14.

[0016] In some embodiments, the composite flame retardant further includes a second flame retardant, which includes at least one of cage-like phosphate ester and aluminum hypophosphite.

[0017] In some embodiments, the composite flame retardant satisfies at least one of the following conditions:

[0018] (1) The mass ratio of the first flame retardant to the second flame retardant is 1:0.15~0.35;

[0019] (2) The mass ratio of the first charring agent to the second charring agent is 1:0.1~0.3;

[0020] (3) The mass ratio of the first anti-dripping agent to the second anti-dripping agent is 1:0.5~2.

[0021] In some embodiments, the second anti-dripping agent in the composite flame retardant further includes at least one of zinc oxide and lanthanum oxide.

[0022] In some embodiments, the silicate in the composite flame retardant satisfies at least one of the following conditions:

[0023] (1) The silicate is a sheet silicate;

[0024] (2) The silicate includes at least one of montmorillonite, talc, kaolin, mica and attapulgite.

[0025] In some embodiments, the composite flame retardant satisfies at least one of the following conditions:

[0026] (1) The antioxidants include at least one of hindered phenolic antioxidants, phosphite antioxidants and thioether antioxidants;

[0027] (2) The coupling agent includes at least one of silane coupling agent, titanate coupling agent and aluminate coupling agent.

[0028] The second aspect of this application provides a method for preparing a composite flame retardant, comprising the following steps;

[0029] A composite flame retardant is prepared by mixing 18-28 parts of flame retardant, 4-10 parts of charring agent, 1-5 parts of anti-dripping agent, 0.1-1 parts of antioxidant and 0.1-1 parts of coupling agent by weight.

[0030] The flame retardant includes a first flame retardant, which includes piperazine pyrophosphate;

[0031] The char-forming agent includes a first char-forming agent and a second char-forming agent, wherein the first char-forming agent includes melamine cyanurate and the second char-forming agent includes at least one of calcium borate and barium metaborate.

[0032] The anti-dripping agent includes a first anti-dripping agent and a second anti-dripping agent, wherein the first anti-dripping agent includes a silicate and the second anti-dripping agent includes a polysiloxane.

[0033] A third aspect of this application provides a polyolefin composite material, comprising polyolefin, and further comprising the aforementioned composite flame retardant or a composite flame retardant prepared by the aforementioned method of preparing the composite flame retardant.

[0034] The composite flame retardant of this application uses piperazine pyrophosphate as the main flame retardant, combined with specific types of first charring agent, second charring agent, first anti-dripping agent, and second anti-dripping agent, and supplemented with antioxidant and coupling agent. The components are compatible and synergistic with each other, which can effectively improve the combustion state, enhance anti-dripping performance, inhibit melt flow, and give the composite flame retardant a better flame retardant effect.

[0035] The aforementioned specific compound system achieves anti-dripping flame retardancy without using halogenated harmful substances such as chlorine and bromine, and without the need for adding fluorinated anti-dripping components such as polytetrafluoroethylene. Simultaneously, it effectively improves the hydrolysis resistance and damp heat resistance of the composite flame retardant. Applying this composite flame retardant to polyolefin composites inhibits the migration and precipitation of flame retardant components, reduces blooming on the composite surface, and significantly improves the long-term stability of polyolefin composites. Detailed Implementation

[0036] The present application will be further described in detail below with reference to the embodiments and examples. It should be understood that these embodiments and examples are only used to illustrate the present application and are not intended to limit the scope of the present application. The purpose of providing these embodiments and examples is to make the disclosure of the present application more thorough and comprehensive.

[0037] It should also be understood that this application can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various alterations or modifications without departing from the spirit of this application, and the resulting equivalent forms also fall within the protection scope of this application. For example, features described or illustrated as part of one embodiment can be combined in a suitable manner in another embodiment to produce new embodiments. Furthermore, numerous specific details are set forth in the following description to provide a fuller understanding of this application; it should be understood that this application can be implemented without one or more of these details.

[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein in the specification of this application is for descriptive purposes only and is not intended to be limiting of the application.

[0039] Unless otherwise stated or in case of contradiction, the terms or phrases used herein shall have the following meanings:

[0040] In this application, the terms "multiple", "various", "multiple times", etc., unless otherwise specified, refer to a quantity greater than or equal to 2. For example, "one or more" means one or more than or equal to two.

[0041] The terms “combinations of,” “any combination of,” and “any combination of” used in this article include all suitable combinations of any two or more of the listed items.

[0042] In this document, the term "suitable" as used in "suitable combination", "suitable method", "any suitable method", etc., refers to the ability to implement the technical solution of this application, solve the technical problem of this application, and achieve the expected technical effect of this application.

[0043] In this document, terms such as "preferred," "better," "more suitable," and "ideal" are merely descriptions of more effective implementation methods or embodiments, and should be understood not to limit the scope of protection of this application. If multiple "preferred" terms appear in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "preferred" term shall be independent.

[0044] In this application, terms such as "further," "even further," and "particularly" are used to describe purposes and indicate differences in content, but should not be construed as limiting the scope of protection of this application.

[0045] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified, and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0046] In this application, the terms "first aspect," "second aspect," "third aspect," "fourth aspect," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," "third," "fourth," etc., serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on quantity.

[0047] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0048] In this application, when numerical intervals (i.e., numerical ranges) are mentioned, unless otherwise specified, the distribution of selectable numerical values ​​within the numerical interval is considered continuous, and includes the two endpoints of the numerical interval (i.e., the minimum and maximum values), as well as every numerical value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that numerical interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints, which is equivalent to directly listing every integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be merged. In other words, unless otherwise specified, the numerical ranges disclosed herein should be understood to include any and all subranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, percentage, ratio, etc. The term "numerical interval" can be broadly included to include numerical interval types such as percentage intervals, ratio intervals, and proportion intervals.

[0049] Unless otherwise specified, the temperature parameters in this application are permitted to be either constant-temperature treatment or variations within a certain temperature range. It should be understood that the constant-temperature treatment allows temperature fluctuations within the precision range of the instrument control, such as ±5℃, ±4℃, ±3℃, ±2℃, or ±1℃.

[0050] In this application, the terms "room temperature" or "normal temperature" generally refer to 4℃ to 35℃, for example, 20℃ ± 5℃. In some embodiments of this application, "room temperature" or "normal temperature" refers to 10℃ to 30℃. In some embodiments of this application, "room temperature" or "normal temperature" refers to 20℃ to 30℃.

[0051] In this application, if the unit of a data range is only followed by the right endpoint, it indicates that the units of the left and right endpoints are the same. For example, 3~5 h means that the units of the left endpoint "3" and the right endpoint "5" are both h (hours).

[0052] The mass or weight of the relevant components mentioned in the embodiments of this application can refer not only to the specific content of each component, but also to the proportional relationship of mass or weight between the components. Therefore, any scaling up or down of the content of the relevant components according to the embodiments of this application is within the scope disclosed in the embodiments of this application. Specifically, the mass or weight mentioned in the embodiments of this application can be units known in the chemical industry, such as μg, mg, g, and kg.

[0053] Traditional halogen-free flame retardants suitable for polymers, such as the "ammonium polyphosphate-pentaerythritol-melamine" phosphorus-nitrogen-based intumescent halogen-free flame retardant system, have drawbacks such as the need to compound with fluorinated anti-dripping agents such as polytetrafluoroethylene, making it difficult to meet environmental access and usage standards. In addition, they have drawbacks such as large addition amounts, poor water resistance, easy precipitation and frosting, flame retardant failure after damp heat aging, and significant mechanical damage.

[0054] One embodiment of this application provides a composite flame retardant, comprising the following components by mass parts:

[0055] Flame retardant 18-28 parts, charring agent 4-10 parts, anti-dripping agent 1-5 parts, antioxidant 0.1-1 parts, and coupling agent 0.1-1 parts;

[0056] Flame retardants include a first flame retardant, which includes piperazine pyrophosphate;

[0057] The char-forming agent includes a first char-forming agent and a second char-forming agent. The first char-forming agent includes melamine cyanurate (MCA), and the second char-forming agent includes at least one of calcium borate and barium metaborate.

[0058] The anti-dripping agent includes a first anti-dripping agent and a second anti-dripping agent, wherein the first anti-dripping agent includes a silicate and the second anti-dripping agent includes a polysiloxane.

[0059] Piperazine pyrophosphate is used as the main flame retardant, serving as both a gas source and an acid source in the composite flame retardant, and the main body expands into char. It is combined with specific types of first and second charring agents. The first charring agent undergoes endothermic decomposition, releasing nitrogen-containing gas and expanding and foaming, while the second charring agent forms a glassy / semi-glassy protective layer at high temperatures, promoting the formation of a continuous and dense char layer. It is also combined with specific types of first and second anti-dripping agents. The first anti-dripping agent is responsible for the inorganic framework and improves the stability of the melt / carbon layer structure. The second anti-dripping agent is responsible for interface, rheological regulation, and the Si-O ceramic barrier after combustion. The combination of the first and second anti-dripping agents can form a synergistic anti-dripping system of "inorganic skeleton + organosilicon continuous phase", which can resist melt flow and inhibit dripping. In addition, antioxidants and coupling agents are added to improve the resistance to yellowing, degradation and thermal stability, and improve the compatibility with the matrix. The components are compatible and synergistic with each other, which can effectively improve the combustion state, enhance the anti-dripping performance, inhibit melt flow, and give the composite flame retardant a good flame retardant effect.

[0060] This specific compound system achieves anti-dripping flame retardancy without using harmful halogenated substances such as chlorine and bromine, and without the need for fluorinated anti-dripping components such as polytetrafluoroethylene. It also effectively improves the hydrolysis and damp heat resistance of the composite flame retardant. Applying this composite flame retardant to polyolefin composites can inhibit the migration and precipitation of flame retardant components while reducing the amount of flame retardant added, thus reducing blooming on the composite surface and significantly improving the long-term stability of the polyolefin composite. Furthermore, it exhibits good compatibility with the polyolefin matrix, improving mechanical retention.

[0061] In some of these examples, the coupling agent is coated on the surface of the flame retardant in the flame retardant main agent.

[0062] It is understood that, in some of these examples, the raw materials for the composite flame retardant, by weight, include the following components:

[0063] Flame retardant 18-28 parts, charring agent 4-10 parts, anti-dripping agent 1-5 parts, antioxidant 0.1-1 parts and coupling agent 0.1-1 parts.

[0064] It is understood that, by mass percentage, the flame retardant includes, but is not limited to, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, and 28 parts; the charring agent includes, but is not limited to, 4, 5, 6, 7, 8, 9, and 10 parts; the anti-dripping agent includes, but is not limited to, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, and 5 parts; the antioxidant includes, but is not limited to, 0.1 to 1 part; and the coupling agent includes, but is not limited to, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1 part. In some examples, any two of these point values ​​can be used as endpoints within a range.

[0065] In some of these examples, the composite flame retardant comprises, by mass parts, the following components:

[0066] Flame retardant 18-22 parts, charring agent 6-10 parts, anti-dripping agent 1.5-4 parts, antioxidant 0.3-0.5 parts and coupling agent 0.3-1 parts.

[0067] In some examples, the mass ratio of charring agent to flame retardant in the composite flame retardant is 1:1.8 to 3.5. It is understood that the mass ratio of charring agent to flame retardant includes, but is not limited to, 1:1.8, 1:1.9, 1:2.0, 1:2.1, 1:2.2, 1:2.3, 1:2.4, 1:2.5, 1:2.6, 1:2.7, 1:2.8, 1:2.9, 1:3.0, 1:3.1, 1:3.2, 1:3.3, 1:3.4, and 1:3.5; in some examples, it can be any two of these point values ​​forming a range. Optionally, the mass ratio of charring agent to flame retardant is 1:2 to 3.5. Further, the mass ratio of charring agent to flame retardant is 1:2 to 3. By controlling the mass ratio of char-forming agent to flame retardant, the density and continuity of the char layer during combustion can be effectively improved, promoting the formation of a more stable and denser expanded char layer. This more effectively isolates heat and oxygen, inhibits molten dripping, and further enhances the anti-dripping performance and flame retardant effect of the composite flame retardant.

[0068] In some examples, the mass ratio of anti-dripping agent to flame retardant in the composite flame retardant is 1:4.5 to 14. It is understood that the mass ratio of charring agent to flame retardant includes, but is not limited to, 1:4.5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5, 1:10, 1:10.5, 1:11, 1:11.5, 1:12, 1:12.5, 1:13, 1:13.5, and 1:14; in some examples, it can be any two of these values ​​forming a range. By controlling the mass ratio of anti-dripping agent to flame retardant, the flow and dripping of the polymer melt can be effectively suppressed, while simultaneously enhancing the heat and oxygen barrier effect of the char layer, thereby further improving the anti-dripping performance and flame retardant effect of the composite flame retardant.

[0069] In some of these examples, the composite flame retardant further includes a second flame retardant, which includes at least one of cage-like phosphate ester and aluminum hypophosphite.

[0070] By synergizing a specific type of second flame retardant with a first flame retardant, and combining it with specific types of first charring agent, second charring agent, first anti-dripping agent, and second anti-dripping agent, the second flame retardant and the first flame retardant work together to be responsible for phosphorus-based flame retardancy and charring. The first charring agent and the second charring agent are responsible for nitrogen supply and foaming expansion. The second charring agent focuses on changing the physical state of the char layer. The first anti-dripping agent and the second anti-dripping agent solidify the char and strengthen the skeleton. Finally, a thick, fine-pore, dense, high-strength, crack-resistant, and non-detachable PNB-Si-Al-C composite expanded char layer is formed, which also suppresses flames in the gas phase.

[0071] In some examples, the mass ratio of the first flame retardant to the second flame retardant in the composite flame retardant is 1:0.15 to 0.35. It can be understood that the mass ratio of the first flame retardant to the second flame retardant includes, but is not limited to, 1:0.15, 1:0.16, 1:0.17, 1:0.18, 1:0.19, 1:0.20, 1:0.21, 1:0.22, 1:0.23, 1:0.24, 1:0.25, 1:0.26, 1:0.27, 1:0.28, 1:0.29, 1:0.30, 1:0.31, 1:0.32, 1:0.33, 1:0.34, and 1:0.35; in some examples, it can be any two of these point values ​​within a range defined by the endpoints. By controlling the mass ratio of the first flame retardant to the second flame retardant, the PNC-rich barrier carbon layer becomes more continuous and dense, while further flame retardant treatment of the material is achieved in the gas phase.

[0072] In some examples, the mass ratio of the first charring agent to the second charring agent in the composite flame retardant is 1:0.1 to 0.3. It can be understood that the mass ratio of the first charring agent to the second charring agent includes, but is not limited to, 1:0.1, 1:0.11, 1:0.12, 1:0.13, 1:0.14, 1:0.15, 1:0.16, 1:0.17, 1:0.18, 1:0.19, 1:0.20, 1:0.21, 1:0.22, 1:0.23, 1:0.24, 1:0.25, 1:0.26, 1:0.27, 1:0.28, 1:0.29, and 1:0.3; in some examples, it can be any two of these point values ​​within a range defined by the endpoints. By controlling the mass ratio of the first charring agent to the second charring agent, a low amount of the second charring agent can stabilize the carbon layer formed by the thermal decomposition and expansion of the first charring agent, cyanuric acid melamine, forming an inorganic phase of BO-Ca / BO-Ba, thus improving the high-temperature integrity of the carbon layer.

[0073] In some examples, the mass ratio of the first anti-dripping agent to the second anti-dripping agent in the composite flame retardant is 1:0.5 to 2. It is understood that the mass ratio of the first charring agent to the second charring agent includes, but is not limited to, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, and 1:2; in some examples, it can be any two of these values ​​forming a range. Optionally, the mass ratio of the first anti-dripping agent to the second anti-dripping agent is 1:0.8 to 1.2. By controlling the mass ratio of the first anti-dripping agent to the second anti-dripping agent, the synergistic effect of the two anti-dripping agents can be brought into play, forming a more uniform and denser network-like char layer structure during combustion. This effectively inhibits the fluidity of the polymer melt, reduces melt dripping, and enhances the thermal stability and insulation properties of the char layer, thereby significantly improving the anti-dripping performance and flame retardant effect of the composite flame retardant.

[0074] In some of these examples, the second anti-dripping agent in the composite flame retardant also includes at least one of zinc oxide and lanthanum oxide.

[0075] In some of these examples, the anti-dripping agent in the composite flame retardant is composed of a first anti-dripping agent and a second anti-dripping agent, wherein the first anti-dripping agent is a silicate and the second anti-dripping agent is a polysiloxane, or the second anti-dripping agent is selected from at least one of zinc oxide and lanthanum oxide and a mixture of polysiloxanes.

[0076] Understandably, in some of these examples, the composite flame retardant does not contain fluorinated substances such as polytetrafluoroethylene.

[0077] In some of these examples, the silicate in the composite flame retardant is a flake silicate.

[0078] In some of these examples, the silicate in the composite flame retardant includes at least one of montmorillonite, talc, kaolin, mica, and attapulgite.

[0079] In some of these examples, the antioxidant in the composite flame retardant includes at least one of hindered phenolic antioxidants, phosphite antioxidants, and thioether antioxidants.

[0080] Optionally, the hindered phenolic antioxidants include at least one of antioxidant 1010, antioxidant 1076, antioxidant 1098 and antioxidant 3114;

[0081] Optionally, the phosphite antioxidants include at least one of antioxidant 168 and antioxidant 626;

[0082] Optionally, thioether antioxidants include at least one of dioctadecyl thiodipropionate and didodecyl thiodipropionate.

[0083] In some of these examples, the coupling agent in the composite flame retardant includes at least one of a silane coupling agent, a titanate coupling agent, and an aluminate coupling agent.

[0084] Optionally, the silane coupling agent includes at least one of KH-550, KH-560 and KH-570;

[0085] Optionally, the titanate coupling agent includes at least one of NDZ-201, NDZ-101 and NDZ-311;

[0086] Optionally, the aluminate coupling agent includes at least one of DL-411 and DL-411AF.

[0087] In some of these examples, the composite flame retardant, by weight, consists of the following components:

[0088] Flame retardant 18-28 parts, charring agent 4-10 parts, anti-dripping agent 1-5 parts, antioxidant 0.1-1 parts, and coupling agent 0.1-1 parts;

[0089] The flame retardant is composed of a first flame retardant and a second flame retardant. The first flame retardant is piperazine pyrophosphate, and the second flame retardant is selected from at least one of cage-like phosphate ester and aluminum hypophosphite.

[0090] The charring agent consists of a first charring agent and a second charring agent. The first charring agent is melamine cyanurate (MCA); the second charring agent is selected from at least one of calcium borate and barium metaborate.

[0091] The anti-dripping agent is composed of a first anti-dripping agent and a second anti-dripping agent, wherein the first anti-dripping agent is a silicate and the second anti-dripping agent is a polysiloxane, or the second anti-dripping agent is selected from at least one of zinc oxide and lanthanum oxide and a mixture of polysiloxane.

[0092] One embodiment of this application provides a method for preparing a composite flame retardant, comprising the following steps;

[0093] A composite flame retardant is prepared by mixing 18-28 parts of flame retardant, 4-10 parts of charring agent, 1-5 parts of anti-dripping agent, 0.1-1 parts of antioxidant and 0.1-1 parts of coupling agent by weight.

[0094] Flame retardants include a first flame retardant, which includes piperazine pyrophosphate;

[0095] The char-forming agent includes a first char-forming agent and a second char-forming agent. The first char-forming agent includes melamine cyanurate, and the second char-forming agent includes at least one of calcium borate and barium metaborate.

[0096] The anti-dripping agent includes a first anti-dripping agent and a second anti-dripping agent, wherein the first anti-dripping agent includes a silicate and the second anti-dripping agent includes a polysiloxane.

[0097] It is understood that the preparation method of the composite flame retardant provided in this application can produce the above-mentioned composite flame retardant, and the specific adaptability of the above-mentioned composite flame retardant is used in the preparation method of the composite flame retardant.

[0098] In some of these examples, the mixing step in the preparation method of the composite flame retardant includes:

[0099] The flame retardant and char-forming agent are mixed, and an alcohol solution of the coupling agent is added. The mixture is stirred at 60℃~80℃ to obtain the flame retardant main agent.

[0100] A composite flame retardant is prepared by mixing flame retardant, anti-dripping agent, antioxidant and coupling agent.

[0101] It is understood that the stirring temperature includes, but is not limited to, 60℃, 61℃, 62℃, 63℃, 64℃, 65℃, 66℃, 67℃, 68℃, 69℃, 70℃, 71℃, 72℃, 73℃, 74℃, 75℃, 76℃, 77℃, 78℃, 79℃, and 80℃; in some examples, it can be a range formed by any two of these point values ​​as endpoints. Further, the stirring time is 10 min to 20 min. It is understood that the stirring time includes, but is not limited to, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, and 20 min. In some examples, it can be a range formed by any two of these point values ​​as endpoints. Optionally, the stirring time is 15 min to 20 min.

[0102] In some examples, in the preparation method of the composite flame retardant, the concentration of the coupling agent in the alcohol solution is 5 wt% to 20 wt%. It is understood that the concentration of the coupling agent in the alcohol solution includes, but is not limited to, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, and 20 wt%; in some examples, it can be within a range formed by any two of these values ​​as endpoints. Optionally, the concentration of the coupling agent in the alcohol solution is 10 wt% to 15 wt%.

[0103] In some of these examples, the alcohol in the alcohol solution of the coupling agent in the preparation method of the composite flame retardant includes ethanol.

[0104] In some of these examples, the preparation method of the composite flame retardant involves mixing the flame retardant and the charring agent in a high-speed mixer.

[0105] In some of these examples, the preparation method of the composite flame retardant involves mixing a first anti-dripping agent and a second anti-dripping agent to obtain the anti-dripping agent.

[0106] One embodiment of this application provides the application of the above-described composite flame retardant or the composite flame retardant prepared by the above-described composite flame retardant preparation method in the preparation of polyolefin composite materials.

[0107] One embodiment of this application provides a polyolefin composite material, including polyolefin, and also including the above-described composite flame retardant or a composite flame retardant prepared by the above-described composite flame retardant preparation method.

[0108] The polyolefin composite material provided in this application includes the above-mentioned composite flame retardant or the composite flame retardant prepared by the above-mentioned composite flame retardant preparation method. It can achieve anti-dripping and inhibit melt flow without adding traditional fluorine-based anti-dripping components, thereby achieving anti-flame retardant effect. It can significantly reduce the amount of flame retardant added, retain the mechanical properties of polyolefin composite material such as impact strength, and improve the long-term stability of polyolefin composite material in terms of hydrolysis resistance, damp heat resistance, migration resistance, and non-frosting.

[0109] It is understandable that the composite flame retardant is distributed in the polyolefin.

[0110] In some of these examples, the olefin composite material contains polyolefins including, but not limited to, at least one of polyethylene (PE), polypropylene (PP), and polyolefin elastomer (POE).

[0111] In some examples, the mass ratio of the composite flame retardant to the polyolefin in the olefin composite is 0.2 to 0.4:1. It is understood that the mass ratio of the composite flame retardant to the polyolefin includes, but is not limited to, 0.2:1, 0.21:1, 0.22:1, 0.23:1, 0.24:1, 0.25:1, 0.26:1, 0.27:1, 0.28:1, 0.29:1, 0.3:1, 0.31:1, 0.32:1, 0.33:1, 0.34:1, 0.35:1, 0.36:1, 0.37:1, 0.38:1, 0.39:1, and 0.4:1. Optionally, the mass ratio of the composite flame retardant to the polyolefin is 0.29 to 0.36:1.

[0112] One embodiment of this application provides a method for preparing a polyolefin composite material, comprising the following steps:

[0113] A polyolefin composite material is prepared by mixing a composite flame retardant with a polyolefin.

[0114] The present application will be described in further detail below with reference to specific embodiments, but the embodiments of the present application are not limited thereto.

[0115] Unless otherwise specified, all raw materials used in the following examples and comparative examples are commercially available.

[0116] Example 1

[0117] (1) Inorganic nanopowder raw materials: by mass parts, flame retardant 18 parts, charring agent 8 parts, anti-dripping agent 3 parts, antioxidant 0.4 parts and coupling agent 0.6 parts; the mass ratio of charring agent to flame retardant is about 1:2.25, and the mass ratio of anti-dripping agent to flame retardant is 1:6;

[0118] The flame retardant includes piperazine pyrophosphate and cage-like phosphate ester, with a mass ratio of piperazine pyrophosphate to cage-like phosphate ester of 1:0.25.

[0119] The charring agent includes melamine cyanurate and calcium borate, with a mass ratio of melamine cyanurate to calcium borate of 1:0.2;

[0120] The anti-dripping agent includes a composite material of montmorillonite and polysiloxane. The polysiloxane composite material is composed of polysiloxane and lanthanum oxide in a mass ratio of 1:0.5, and the mass ratio of montmorillonite to polysiloxane composite material is 1:1.

[0121] Antioxidants include hindered phenols and phosphites, with a mass ratio of hindered phenols to phosphites of 1:1;

[0122] The coupling agent is silane coupling agent KH-550;

[0123] The inorganic nanopowder raw material was dried in a 100℃ oven for 3 hours to remove surface adsorbed moisture and was ready for use.

[0124] (2) Piperazine pyrophosphate, cage-like phosphate, calcium borate and melamine cyanurate were put into a high-speed mixer and premixed at room temperature for 5 min. 0.6 parts of coupling agent were diluted with anhydrous ethanol to a concentration of 10 wt%, and slowly sprayed into the mixed powder with an atomizing nozzle. The temperature was raised to 70℃ and stirred at 1000 r / min for 20 min to make the coupling agent uniformly coat the surface of the flame retardant. The heating was stopped, and stirring was continued and cooled to room temperature to obtain the activated flame retardant main agent.

[0125] (3) Add 1.5 parts of montmorillonite and 1.5 parts of polysiloxane micro powder to a high-speed mixer and premix at room temperature for 10 minutes to obtain a premixed anti-dripping agent;

[0126] (4) Add the activated flame retardant, premixed anti-dripping agent, hindered phenol antioxidant, and phosphite antioxidant to the mixer and mix at 400 r / min for 10 min until uniform to obtain polyolefin composite flame retardant.

[0127] Example 2

[0128] The method is basically the same as in Example 1, except that 20 parts of flame retardant and 6 parts of charring agent are used. The mass ratio of charring agent to flame retardant is approximately 1:3.3.

[0129] Example 3

[0130] The method is basically the same as in Example 1, except that there are 22 parts of flame retardant and 10 parts of charring agent. The mass ratio of charring agent to flame retardant is approximately 1:2.2.

[0131] Example 4

[0132] The method is basically the same as in Example 1, except that there are 2 parts of anti-dripping agent. The mass ratio of anti-dripping agent to flame retardant is 1:9.

[0133] Example 5

[0134] The process is basically the same as in Example 1, except that the anti-dripping agent includes montmorillonite and polysiloxane, with a mass ratio of 1:1 between montmorillonite and polysiloxane.

[0135] Example 6

[0136] It is basically the same as Example 1, except that the flame retardant is piperazine pyrophosphate in all cases.

[0137] Example 7

[0138] It is basically the same as Example 1, except that the mass ratio of montmorillonite and polysiloxane composite material is 1:0.5.

[0139] Example 8

[0140] It is basically the same as Example 1, except that the flame retardant includes piperazine pyrophosphate and aluminum hypophosphite, and the mass ratio of piperazine pyrophosphate to aluminum hypophosphite is 1:0.25.

[0141] The charring agent includes melamine cyanurate and barium metaborate, with a mass ratio of melamine cyanurate to barium metaborate of 1:0.2;

[0142] The anti-dripping agent includes a talc and polysiloxane composite material. The polysiloxane composite material is composed of a mixture of polysiloxane and lanthanum oxide in a mass ratio of 1:0.5, and the mass ratio of talc to the polysiloxane composite material is 1:1.

[0143] Comparative Example 1

[0144] By weight, 15 parts ammonium polyphosphate, 5 parts pentaerythritol, 5 parts melamine, 0.5 parts anti-dripping agent (polytetrafluoroethylene), and 1 part antioxidant (hindered phenol and phosphite in a 1:1 mass ratio); place in an oven at 100℃ and dry for 3 hours to remove surface adsorbed moisture.

[0145] Ammonium polyphosphate, pentaerythritol, and melamine were added to a high-speed mixer and mechanically stirred for 10 minutes at room temperature. Then, polytetrafluoroethylene and antioxidants were added and stirred for another 5 minutes. The mixture was then passed through a 300-mesh sieve and vacuum-packed to obtain a traditional halogen-free intumescent polyolefin composite flame retardant.

[0146] Comparative Example 2

[0147] The process is basically the same as in Example 1, except that the inorganic nanopowder raw materials are: by mass parts, 16 parts flame retardant, 10 parts charring agent, 3 parts anti-dripping agent, 0.4 parts antioxidant and 0.6 parts coupling agent.

[0148] Comparative Example 3

[0149] It is basically the same as Example 1, except that the charring agent is melamine phosphate.

[0150] Comparative Example 4

[0151] It is basically the same as Example 1, except that the charring agent includes melamine cyanurate and zinc borate in a mass ratio of 1:0.2.

[0152] Comparative Example 5

[0153] It is basically the same as Example 1, except that the anti-dripping agent is montmorillonite in all cases.

[0154] Each of the embodiments or comparative examples of the composite flame retardant was blended with 100 parts of polyolefin resin, 4 parts of maleic anhydride-grafted polypropylene compatibilizer, and 0.2 parts of ethylene bis-stearamide lubricant. The mixture was melt-extruded using a twin-screw extruder, water-cooled into strips, and pelletized to obtain a polyolefin composite material. The sample was then injection-molded / extruded for performance testing.

[0155] UL94 Vertical Burning (1.6mm): GB / T 2408-2021. Observe whether dripping occurs during the burning process and judge based on the self-extinguishing time and dripping situation.

[0156] Notched impact strength of simply supported beams: GB / T 1043.1-2008;

[0157] Limiting oxygen index: GB / T 2406.2-2009; a higher value indicates better flame retardancy of the material.

[0158] Flame retardant stability in boiling water: The test material was immersed in deionized water, heated to 82°C in a water bath, and kept stable. The water was changed every 24 hours. After 168 hours, the material was removed from the water bath and dried in an oven at 82°C to constant weight. After cooling to room temperature and standing for 24 hours, the surface of the sample was observed for white exudates and frost. The UL94 vertical burning performance and notched impact strength of a simply supported beam were tested. The impact strength retention rate was the ratio of the impact strength after boiling water aging to the original impact strength.

[0159] The results are shown in Table 1.

[0160] Table 1

[0161]

[0162] As shown in Table 1, compared to Comparative Example 1, which uses a traditional phosphorus-nitrogen-based intumescent flame retardant system of ammonium polyphosphate-pentaerythritol-melamine-polytetrafluoroethylene, the composite flame retardants provided in each example do not require the addition of fluorine-containing substances such as polytetrafluoroethylene to achieve anti-dripping flame retardant effects. Furthermore, they exhibit good flame retardant stability after 168 hours of boiling in water, with no precipitation or frosting. Comparative Example 1 showed slight frosting after 7 days, indicating the migration and precipitation of small molecules in the flame retardant, leading to surface whitening, decreased insulation, and long-term flame retardant attenuation. Comparative Example 2 had an inappropriate ratio of flame retardant to charring agent, resulting in poor initial combustion performance and flame retardant stability after 500 hours of boiling in water. Comparative Examples 3 and 4 did not use specific charring agents, and Comparative Example 5 did not use specific anti-dripping agents, resulting in varying degrees of deterioration in flame retardant performance and / or flame retardant stability.

[0163] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0164] The embodiments described above are merely illustrative of several implementation methods of this application, intended to facilitate a detailed understanding of the technical solutions of this application, but should not be construed as limiting the scope of protection of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the scope of protection of this application. It should be understood that technical solutions obtained by those skilled in the art based on the technical solutions provided in this application through logical analysis, reasoning, or limited experimentation are all within the scope of protection of the appended claims. Therefore, the scope of protection of this patent application should be determined by the content of the appended claims, and the specification can be used to interpret the content of the claims.

Claims

1. A composite flame retardant, characterized in that, By mass parts, it includes the following components: Flame retardant 18-28 parts, charring agent 4-10 parts, anti-dripping agent 1-5 parts, antioxidant 0.1-1 parts, and coupling agent 0.1-1 parts; The flame retardant includes a first flame retardant, which includes piperazine pyrophosphate; The char-forming agent includes a first char-forming agent and a second char-forming agent, wherein the first char-forming agent includes melamine cyanurate and the second char-forming agent includes at least one of calcium borate and barium metaborate. The anti-dripping agent includes a first anti-dripping agent and a second anti-dripping agent, wherein the first anti-dripping agent includes a silicate and the second anti-dripping agent includes a polysiloxane.

2. The composite flame retardant as described in claim 1, characterized in that, By mass parts, it includes the following components: Flame retardant 18-22 parts, charring agent 6-10 parts, anti-dripping agent 1.5-4 parts, antioxidant 0.3-0.5 parts and coupling agent 0.3-1 parts.

3. The composite flame retardant as described in claim 2, characterized in that, The composite flame retardant satisfies at least one of the following conditions: (1) The mass ratio of the char-forming agent to the flame retardant is 1:1.8~3.5; (2) The mass ratio of the anti-dripping agent to the flame retardant is 1:4.5~14.

4. The composite flame retardant as described in claim 1, characterized in that, The flame retardant also includes a second flame retardant, which includes at least one of cage-like phosphate ester and aluminum hypophosphite.

5. The composite flame retardant as described in claim 4, characterized in that, The composite flame retardant satisfies at least one of the following conditions: (1) The mass ratio of the first flame retardant to the second flame retardant is 1:0.15~0.35; (2) The mass ratio of the first charring agent to the second charring agent is 1:0.1~0.3; (3) The mass ratio of the first anti-dripping agent to the second anti-dripping agent is 1:0.5~2.

6. The composite flame retardant as described in claim 1, characterized in that, The second anti-dripping agent also includes at least one of zinc oxide and lanthanum oxide.

7. The composite flame retardant according to any one of claims 1 to 6, characterized in that, The silicate satisfies at least one of the following conditions: (1) The silicate is a sheet silicate; (2) The silicate includes at least one of montmorillonite, talc, kaolin, mica and attapulgite.

8. The composite flame retardant according to any one of claims 1 to 6, characterized in that, The composite flame retardant satisfies at least one of the following conditions: (1) The antioxidants include at least one of hindered phenolic antioxidants, phosphite antioxidants and thioether antioxidants; (2) The coupling agent includes at least one of silane coupling agent, titanate coupling agent and aluminate coupling agent.

9. A method for preparing a composite flame retardant, characterized in that, Includes the following steps; A composite flame retardant is prepared by mixing 18-28 parts of flame retardant, 4-10 parts of charring agent, 1-5 parts of anti-dripping agent, 0.1-1 parts of antioxidant and 0.1-1 parts of coupling agent by weight. The flame retardant includes a first flame retardant, which includes piperazine pyrophosphate; The char-forming agent includes a first char-forming agent and a second char-forming agent, wherein the first char-forming agent includes melamine cyanurate and the second char-forming agent includes at least one of calcium borate and barium metaborate. The anti-dripping agent includes a first anti-dripping agent and a second anti-dripping agent, wherein the first anti-dripping agent includes a silicate and the second anti-dripping agent includes a polysiloxane.

10. A polyolefin composite material, characterized in that, It includes polyolefins, and also includes composite flame retardants prepared by the method of preparing composite flame retardants as described in any one of claims 1 to 8 or as described in claim 9.