A multi-level gas-storing superhydrophobic structure on a metal surface and its preparation method

By constructing a partitioned gas storage layer, a confined gas replenishment layer, and a low surface energy gas-locking layer on the metal surface, the problem of easy failure of the gas film in the existing superhydrophobic structure under complex environments is solved, and the gas film retention and anti-corrosion and anti-fouling performance are improved under conditions such as mechanical disturbance, interface peeling, and fluid scouring.

CN123107434APending Publication Date: 2026-11-17HAINAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611424246.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing superhydrophobic structures are prone to overall wetting failure due to local air film rupture in complex service environments, making it difficult to maintain a continuous or locally continuous air layer under conditions such as mechanical disturbance, interface peeling, fluid scouring, pressure, temperature change and chemical corrosion.

Method used

A multi-level gas storage superhydrophobic structure is constructed on a metal surface, including a partitioned gas storage layer, a confined gas replenishment layer, and a low surface energy gas-locking layer. Independent or semi-independent gas storage units are formed by isolation boundaries and buffer trenches. Combined with nanoscale residual gas storage space and low surface energy modification, the lateral expansion of liquid is blocked and the intrusion tendency is reduced.

Benefits of technology

It effectively inhibits the lateral spread of liquid, maintains the local gas film layer, improves anti-corrosion and anti-fouling performance, enhances the gas film retention ability of metal surfaces in complex environments, and prevents overall wetting failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107434A_ABST
    Figure CN123107434A_ABST
Patent Text Reader

Abstract

This application relates to a multi-level gas-storage superhydrophobic structure on a metal surface and its preparation method, belonging to the field of metal material surface modification technology. The multi-level gas-storage superhydrophobic structure on a metal surface of this application includes a partitioned gas storage layer, a confined gas replenishment layer, and a low surface energy gas-locking layer. The partitioned gas storage layer includes multiple microscale gas storage units, and adjacent microscale gas storage units are separated by isolation boundaries, buffer trenches, or liquid lateral expansion blocking structures. The confined gas replenishment layer is disposed on the top, sidewall, edge, or inner wall of the microscale gas storage units, or in the trench area between adjacent microscale gas storage units, to form a nanoscale residual gas storage space. The low surface energy gas-locking layer covers the surfaces of the partitioned gas storage layer and the confined gas replenishment layer, to reduce the tendency of liquid to intrude into the microscale gas storage units and the nanoscale residual gas storage space. The multi-level gas-storage superhydrophobic structure on a metal surface provided by this application has the ability to isolate local wetting failure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of surface modification technology for metallic materials, and in particular to a multi-level gas-storing superhydrophobic structure for a metallic surface and its preparation method. Background Technology

[0002] Superhydrophobic surfaces typically achieve the Cassie-Baxter wetting state through a combination of micro / nano rough structures and low surface energy chemical modifications. In this state, an air layer exists between the liquid and the solid surface, and the liquid primarily contacts the solid protrusions at the air-solid composite interface. Therefore, the surface can exhibit a high water contact angle and a low roll-off angle.

[0003] However, in actual service environments, superhydrophobic surfaces not only need to have a high initial contact angle, but also need to maintain an air film layer for a long time under external disturbances. For marine engineering equipment, ship structures, port facilities, bridge components and outdoor metal facilities, the surface is often subjected to multiple factors such as mechanical wear, tape peeling, fluid erosion, hydrostatic pressure, temperature changes, acid and alkali corrosion and salt spray corrosion.

[0004] When external disturbances cause the gas film layer to rupture or the gas storage structure to fail, the liquid will gradually penetrate into the interior of the micro / nano structure, causing the surface to change from a Cassie-Baxter wetted state to a Wenzel wetted state. This change will significantly increase the actual contact area between the liquid and the metal substrate, causing a rapid decline in superhydrophobicity, self-cleaning properties, antifouling properties, and corrosion resistance.

[0005] Existing technologies have disclosed methods for suppressing the transition from the Cassie state to the Wenzel state by covering the surface of micro / nano structures with two-dimensional materials, as well as methods for constructing biomimetic non-smooth structures on metal surfaces using laser processing. However, existing technologies mainly focus on delaying liquid intrusion through two-dimensional material covering, micro / nano rough structures, and low surface energy modification, and still primarily belong to the overall gas film maintenance approach. Once liquid intrusion occurs in a local area of ​​this type of structure, it is easy to induce continuous wetting and expansion in adjacent areas, leading to the overall failure of the gas film layer.

[0006] Therefore, how to construct a multi-level air-storage superhydrophobic structure on a metal surface that can maintain a continuous or partially continuous air layer under mechanical disturbance, interface peeling, fluid scouring, pressure, temperature change and chemical corrosion, and can inhibit the continuous lateral intrusion of liquid, is a key technical problem that urgently needs to be solved in the field of metal corrosion and antifouling. Summary of the Invention

[0007] In view of this, this application provides a multi-level gas-storage superhydrophobic structure on a metal surface and its preparation method. The multi-level gas-storage superhydrophobic structure on a metal surface has the ability to isolate local wetting failure, which can effectively overcome the defect of existing superhydrophobic structures that are prone to overall wetting failure due to local gas film rupture in complex service environments.

[0008] This application provides a multi-level gas storage superhydrophobic structure on a metal surface, comprising a partitioned gas storage layer, a confined gas replenishment layer, and a low surface energy gas-locking layer; the partitioned gas storage layer comprises multiple independent microscale gas storage units spaced apart from each other, and adjacent microscale gas storage units are provided with isolation boundaries, buffer trenches, or liquid lateral expansion blocking structures; the confined gas replenishment layer is disposed on the top, sidewall, edge, or inner wall of the microscale gas storage unit or in the trench area between adjacent microscale gas storage units, for forming a nanoscale residual gas storage space; the low surface energy gas-locking layer covers the surfaces of the partitioned gas storage layer and the confined gas replenishment layer, for reducing the tendency of liquid to intrude into the microscale gas storage unit and the nanoscale residual gas storage space.

[0009] Preferably, the microscale gas storage unit is selected from at least one of the following: biomimetic scale-like unit, hexagonal unit, arc-shaped groove unit, closed pit unit, semi-closed pit unit, and grid unit.

[0010] Preferably, the microscale gas storage unit is a periodically arranged array of regular hexagonal protrusions. The equivalent circumcircle diameter of each hexagonal protrusion is 50-250 μm, the spacing between adjacent hexagonal protrusions is 10-80 μm, and the height of each hexagonal protrusion is 10-100 μm. Isolation trenches, semi-continuous trenches, or buffer trenches are formed between adjacent hexagonal protrusions. The width of each isolation trench, semi-continuous trench, or buffer trench is 5-60 μm, and the depth is 10-100 μm. Preferably, the equivalent circumcircle diameter of each hexagonal protrusion is 80-180 μm, the spacing between adjacent hexagonal protrusions is 20-50 μm, the height of each hexagonal protrusion is 20-60 μm, and the trench width is 10-40 μm.

[0011] Specifically, the microscale gas storage units are not continuous, open, monolithic recessed structures, but rather form locally independent or semi-independent gas storage regions through isolation boundaries, semi-closed boundaries, or buffer trenches. Each hexagonal protrusion is surrounded by trenches, which are distributed around the edge of the hexagonal protrusion. This ensures that each hexagonal protrusion is relatively independent, resulting in optimal isolation between gas storage regions. A liquid lateral propagation blocking structure is used to prevent liquid from continuously spreading along the surface and trench areas between adjacent microscale gas storage units to adjacent microscale gas storage units after local liquid intrusion.

[0012] A second aspect of this application also provides a method for preparing the above-mentioned multi-level gas-storing superhydrophobic structure on a metal surface, comprising the following steps:

[0013] S1. Construct a partitioned gas storage layer on the surface of a metal substrate;

[0014] S2. Confinement gas replenishment layer is constructed in the trench area at the top, sidewall, edge or inner wall of the partitioned gas storage layer or between adjacent microscale gas storage units.

[0015] S3. Construct a low surface energy gas-locking layer on the surface of the partitioned gas storage layer and the confined gas replenishment layer, and form a multi-level gas storage type superhydrophobic structure on the metal surface after curing, drying or heat treatment.

[0016] Preferably, the specific process of step S1 is as follows: grinding, cleaning and drying the metal substrate to remove oxide layer, oil and loose particles; then using laser processing, plasma etching, mechanical imprinting, chemical etching, micro milling, sandblasting, template replication or a combination thereof to construct microscale gas storage units on the surface of the metal substrate.

[0017] Preferably, the specific process of step S2 is as follows: a dispersion containing hydrophobic nanoparticles and / or two-dimensional sheet materials is loaded onto the top, sidewall, edge or inner wall of a microscale gas storage unit or the trench area between adjacent microscale gas storage units by spraying, dipping, dripping, spin coating, scraping, electrophoretic deposition, in-situ growth or a combination thereof, to form a confined gas replenishment layer.

[0018] The confined gas replenishment layer does not continuously cover the entire surface of the partitioned gas storage layer. Instead, it is distributed in a bridging, overlapping, embedding, semi-suspended, or partially covering manner on the top, sidewalls, edges, or inner walls of the microscale gas storage units, or in the grooved areas between adjacent microscale gas storage units. Even after local damage or wetting of the microscale gas storage unit, the nanoscale residual gas storage space can still retain an air layer, thus maintaining a locally superhydrophobic state. The nanoscale residual gas storage space can retain an air layer because its pore size is small, its surface is modified with a low surface energy gas-locking layer, and liquid entry requires overcoming a high capillary ingress pressure. Simultaneously, the semi-enclosed, tortuous confined space formed by nanoparticles and two-dimensional sheets can impede liquid infiltration and slow down air escape. Therefore, even if the microscale gas storage unit is locally wetted, residual air can still be retained in the nanoscale space, maintaining a locally located residual air layer between the liquid and solid surfaces.

[0019] The multi-level gas-storage superhydrophobic structure on the metal surface of this application has a multi-level failure-resistant structure, including a microscale partitioned gas storage structure, a nanoscale residual gas storage structure, and a low surface energy anti-liquid intrusion structure. The microscale partitioned gas storage structure and the nanoscale residual gas storage structure can retain air in the microscale gas storage unit and the nanoscale residual gas storage space, so that the retained air is located between the corrosive medium and the solid surface and forms an interfacial gas film layer, thereby reducing the actual contact area between the corrosive medium and the metal substrate; at the same time, the two-dimensional sheet structure can extend the diffusion path of the corrosive medium to the metal substrate, thereby improving the corrosion resistance of the metal substrate. The partitioned gas storage layer, the confined gas replenishment layer, and the low surface energy gas-locking layer together constitute an anti-disturbance gas film retention structure. The anti-disturbance gas film retention structure is used to retain a continuous or locally continuous interfacial gas film layer in the microscale gas storage unit and / or the nanoscale residual gas storage space after mechanical wear, tape peeling, water erosion, hydrostatic pressure, acid and alkali media, salt environment, or temperature change.

[0020] Preferably, the hydrophobic nanoparticles are selected from at least one of silicon dioxide, aluminum oxide, titanium oxide, zinc oxide, silicon nitride, silicon carbide, calcium carbonate, or their hydrophobic modifiers; the two-dimensional sheet material is selected from at least one of graphene, graphene oxide, reduced graphene oxide, boron nitride, MXene, molybdenum disulfide, or their modifiers.

[0021] Preferably, the specific process of step S3 is as follows: the surface of the partitioned gas storage layer and the confined gas replenishment layer is modified by using a low surface energy material through silanization reaction, thermosetting, ultraviolet curing, room temperature curing, adsorption assembly or a combination thereof to form a low surface energy gas-locking layer, which is then cured, dried or heat-treated to form a multi-level gas storage type superhydrophobic structure on the metal surface.

[0022] Preferably, the low surface energy material is selected from at least one of fluorosilanes, long-chain alkylsilanes, fluoropolymers, siloxane resins, polydimethylsiloxanes, and stearic acid.

[0023] Preferably, the specific conditions for the heat treatment are: the heat treatment temperature is 40~120℃, and the treatment time is 0.5~4 h. Curing, drying, or heat treatment is used to enhance the bonding stability between the confined gas replenishment layer and the low surface energy gas-locking layer and the partitioned gas storage layer.

[0024] This application does not merely delay liquid wetting by covering the surface of micro / nano structures with two-dimensional materials, nor does it aim solely to increase the initial water contact angle. Instead, it focuses on "preventing wetting spread even after local gas film damage." By constructing a partitioned gas storage layer, a confined gas replenishment layer, and a low surface energy gas-locking layer, the multi-level gas storage superhydrophobic structure on the metal surface can maintain a continuous or locally continuous gas film layer even after being subjected to mechanical disturbances, interface peeling, fluid scouring, pressure, temperature changes, and acid / alkali environments. The mechanism of this application lies in constructing an anti-disturbance gas film retention structure through partitioned gas storage layers, confined gas replenishment layers, and low surface energy gas-locking layers. The partitioned gas storage layer divides the gas film into multiple independent or semi-independent gas storage units. The isolation boundaries or longitudinal trenches can prevent the lateral expansion of liquid. The confined gas replenishment layer forms nanoscale residual gas storage spaces on the top of the protrusion, sidewalls and trench edges, which can maintain the local gas film even after local damage. The low surface energy gas-locking layer reduces the tendency of liquid to wet and enter the gas cavity. The three work together to enable the multi-level gas storage superhydrophobic structure on the metal surface to achieve failure isolation after local wetting occurs, avoiding overall wetting failure, thereby improving the resistance to erosion, hydrostatic pressure, wear, acid and alkali and corrosion resistance.

[0025] The partitioned gas storage layer is the main bottom gas storage structure, composed of periodically arranged microscale gas storage units. In one specific embodiment, the microscale gas storage units are a regular hexagonal array of protrusions, appearing trapezoidal or stepped when viewed in cross-section. Isolation boundaries or trench structures are set between adjacent microscale gas storage units, allowing each microscale gas storage unit to form a relatively independent gas storage region. When one microscale gas storage unit experiences localized wetting, the isolation boundaries or trench structures can inhibit the lateral spread of liquid to adjacent microscale gas storage units, thereby reducing the possibility of further localized wetting. A confined gas replenishment layer is disposed at least at one location on the top, sidewall, edge, or inner wall of the microscale gas storage unit, and in the trench region between adjacent microscale gas storage units, and is composed of nanoparticles, two-dimensional sheet materials, or their composite structures. The confined gas replenishment layer is distributed in a bridging, overlapping, embedded, semi-suspended, or partially covering manner, forming nanoscale residual gas storage spaces at the edges of the microscale gas storage units and in the trench regions between adjacent microscale gas storage units. When the interfacial gas film layer within a microscale gas storage unit is locally damaged by abrasion, erosion, or pressure, the nanoscale residual gas storage space can still retain some air and delay further liquid intrusion. A low surface energy gas-locking layer covers the surfaces of the partitioned gas storage layer and the confined gas replenishment layer to reduce the tendency of liquid to spread and wet on the surface and increase the capillary ingress pressure that liquid needs to overcome to enter the microscale gas storage unit and the nanoscale residual gas storage space. The partitioned gas storage layer, the confined gas replenishment layer, and the low surface energy gas-locking layer work together to enable the formation of an interfacial gas film layer within the microscale gas storage unit and / or the nanoscale residual gas storage space, and maintain a continuous or partially continuous state after external disturbances.

[0026] A confined gas replenishment layer is set on the top, sidewall, edge, or inner wall of a microscale gas storage unit, or in the trench area between adjacent microscale gas storage units, forming a nanoscale residual gas storage space. A low surface energy gas-locking layer covers the surfaces of the partitioned gas storage layer and the confined gas replenishment layer to reduce the tendency of liquid to enter the microscale gas storage unit and the nanoscale residual gas storage space. The low surface energy gas-locking layer is made of hydrophobic materials such as fluorinated silanes, long-chain alkyl silanes, PDMS, and siloxane resins, and covers the surfaces of the partitioned gas storage layer and the confined gas replenishment layer to reduce the tendency of liquid to spread and adhere on the surfaces of the partitioned gas storage layer and the confined gas replenishment layer after being modified by the low surface energy gas-locking layer, and to increase the capillary entry pressure that liquid needs to overcome to enter the microscale gas storage unit and the nanoscale residual gas storage space, thereby improving the stability of the interfacial gas film layer within the microscale gas storage unit and / or the nanoscale residual gas storage space. Because the low surface energy gas-locking layer makes the outer surface of the multi-level gas-storage superhydrophobic structure on the metal surface hydrophobic or superhydrophobic, liquids need to overcome high capillary ingress pressures when entering the trenches, pores, or gas-storage cavities. Therefore, it can effectively inhibit the intrusion of liquids into the gas-storage space and maintain the air layer at the solid-liquid interface. The partitioned gas-storage layer, the confined gas-replenishing layer, and the low surface energy gas-locking layer together form an anti-disturbance gas film retention structure, enabling the multi-level gas-storage superhydrophobic structure on the metal surface to maintain a continuous or locally continuous gas film layer even after mechanical disturbances, interface peeling, fluid erosion, pressure, temperature changes, or acid-base environments, and to inhibit the spread of local wetting to adjacent areas.

[0027] Compared with the prior art, this application has the following advantages:

[0028] (1) This application shifts from “constructing a surface with a high contact angle” to “constructing a disturbance-resistant gas film retention structure”, which solves the problem that the existing superhydrophobic structure is prone to overall instability of the gas film layer in complex environments.

[0029] (2) This application achieves the partitioned maintenance of the gas film and the isolation of local failures through the partitioned gas storage layer, which can avoid the continuous wetting and expansion of adjacent areas after local liquid intrusion.

[0030] (3) This application constructs a nanoscale confined gas storage space through a confined gas replenishment layer, so that the air layer can still be maintained in the nanoscale region after the local gas film is disturbed, thereby improving the gas film's ability to resist disturbance failure.

[0031] (4) This application reduces the tendency of liquid to invade microscale gas storage units and nanoscale confined gas storage space by using a low surface energy gas-locking layer, thereby improving the gas film retention ability of multi-level gas storage superhydrophobic structures on metal surfaces after mechanical wear, tape peeling, water flow scouring, hydrostatic pressure, high temperature, low temperature and acid and alkali environment.

[0032] (5) The multi-level gas-storage superhydrophobic structure on the metal surface of this application, through the synergistic effect of microscale gas film partitioning, nanoscale residual gas storage, and isolation from local wetting failure, enables the multi-level gas-storage superhydrophobic structure on the metal surface to maintain a continuous or locally continuous gas film layer after mechanical disturbance, interface peeling, fluid scouring, pressure, temperature change, and acid and alkali environment, thus avoiding the overall wetting failure induced by local liquid intrusion. This multi-level gas-storage superhydrophobic structure on the metal surface can be used for corrosion protection, antifouling, and self-cleaning protection of marine engineering equipment, ship structures, port facilities, bridge components, and other metal structural parts. Attached Figure Description

[0033] To more clearly illustrate the technical solutions in this application or the prior art, the drawings used in the description of this application or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0034] Figure 1 This is a schematic diagram of the structure and gas film retention state of the multi-level gas storage superhydrophobic structure on the metal surface of this application, wherein (a) is a schematic diagram of the normal gas film retention state, (b) is a schematic diagram of the liquid local intrusion state, and (c) is a schematic diagram of the isolation state after the local gas storage area has experienced wetting failure.

[0035] Figure 2 This is a flowchart illustrating the fabrication process of the multi-level gas storage superhydrophobic structure on the metal surface described in this application.

[0036] Figure 3 This is a SEM image of the multi-level gas storage superhydrophobic structure on the metal surface of this application;

[0037] Figure 4 The following are the superhydrophobic test results of the multi-level gas storage superhydrophobic structure on the metal surface of this application: (a) is the superhydrophobic test result of the sample in hydrochloric acid solution with pH=1, (b) is the superhydrophobic test result of the sample in deionized water, (c) is the superhydrophobic test result of the sample in sodium hydroxide solution with pH=14, and (d) is the superhydrophobic test result of the sample in muddy water.

[0038] Figure 5 The following are self-cleaning test diagrams of the multi-level gas storage type superhydrophobic structure on the metal surface of this application: (a) is a self-cleaning test diagram of sodium chloride contaminants on the surface of the superhydrophobic sample; (b) is a self-cleaning test diagram of sand contaminants on the surface of the superhydrophobic sample; (c) is a control test diagram of sodium chloride contaminants on the surface of untreated Q235 steel; and (d) is a control test diagram of sand contaminants on the surface of untreated Q235 steel.

[0039] Figure 6This is a weather resistance test diagram of the multi-level gas storage superhydrophobic structure on the metal surface of this application;

[0040] Figure 7 The following are stability tests of the multi-level gas storage superhydrophobic structure on the metal surface of this application: wide pH range, tape adhesion performance, abrasion resistance, water flow erosion resistance and high and low temperature performance graphs; (a) is the wide pH range stability graph, (b) is the tape adhesion stability graph, (c) is the abrasion resistance stability graph, (d) is the water flow erosion resistance stability graph, and (e) is the high and low temperature stability graph.

[0041] Figure 8 This is a water pressure test diagram of the multi-level gas storage type superhydrophobic structure on the metal surface of this application;

[0042] Figure 9 Electrochemical impedance spectroscopy of Q235 steel samples with different surface treatments, where (a) is the Bode impedance modulus diagram and (b) is the Nyquist impedance spectrum.

[0043] Explanation of reference numerals in the attached figures:

[0044] 1. Zoned gas storage layer; 11. Zoned gas storage unit; 12. Isolation boundary; 2. Confined gas replenishment layer; 3. Low surface energy gas-locking layer; 4. Metal substrate; 5. Gas film; 6. Water body; 7. Local failure zone. Detailed Implementation

[0045] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0046] Unless otherwise specified, the experimental methods used in the embodiments of this application are all conventional methods.

[0047] Example

[0048] like Figure 1 As shown in the embodiment of this application, the multi-level gas storage type superhydrophobic structure on the metal surface specifically includes:

[0049] First, a partitioned gas storage layer 1 is constructed on the surface of a metal substrate. The partitioned gas storage layer 1 comprises multiple microscale gas storage units 11, and these units 11 can be biomimetic scale-like, hexagonal, arc-shaped groove-like, closed pit-like, semi-closed pit-like, grid-like, or combinations thereof. Isolation boundaries 12 are set between adjacent partitioned gas storage units 11 to form locally independent or semi-independent partitioned gas storage spaces.

[0050] In this embodiment, the partitioned gas storage layer 1 differs from ordinary rough structures. The partitioned gas storage layer 1 is not merely used to improve surface roughness, but rather to achieve partitioned air retention during liquid contact, scouring, pressurization, or mechanical disturbance. When the gas film in a single area is damaged or liquid intrudes, adjacent microscale gas storage units can still maintain the gas film layer, thereby reducing the risk of overall gas film failure.

[0051] Secondly, a confined gas replenishment layer 2 is constructed in the top, sidewalls, edges, inner walls, and isolation boundary 12 regions of the partitioned gas storage unit 11 of the partitioned gas storage layer 1. The confined gas replenishment layer 2 is composed of nano-rough structures and two-dimensional sheet structures. The nano-rough structures form nanopores and nano-protrusions, while the two-dimensional sheet structures are distributed between the nano-rough structures or between adjacent microscale gas storage units in a covering, bridging, overlapping, embedding, or semi-overhanging manner, thereby forming a nanoscale confined gas storage space.

[0052] The confined gas replenishment layer 2 can form an auxiliary gas storage space on the surface of a microscale gas storage unit or between adjacent microscale gas storage units. When external disturbances cause damage to the local gas film 5, the nanoscale confined gas storage space can delay the continued infiltration of liquid and maintain the local air layer, thereby improving the gas film layer's resistance to disturbance failure.

[0053] Next, a low surface energy gas-locking layer 3 is constructed on the surfaces of the partitioned gas storage layer 1 and the confined gas replenishment layer 2. The low surface energy gas-locking layer 3 serves to reduce the spread of liquid on the multi-level gas storage superhydrophobic structure on the metal surface and to reduce the possibility of liquid entering the microscale gas storage unit and the nanoscale confined gas storage space. The low surface energy gas-locking layer 3 can be formed from fluorinated silanes, long-chain alkyl silanes, fluoropolymers, siloxane resins, polydimethylsiloxane, stearic acid, or combinations thereof.

[0054] like Figure 1 As shown, through the synergistic effect of the partitioned gas storage layer 1, the confined gas replenishment layer 2, and the low surface energy gas-locking layer 3, this application forms an anti-disturbance gas film retention structure. The partitioned gas storage layer 1 includes multiple partitioned gas storage units 11, with isolation boundaries 12 set between adjacent partitioned gas storage units 11. Under normal wetting conditions, air can be retained within the partitioned gas storage unit 11, forming a gas film 5 between the metal substrate 4 and the water body 6. When subjected to mechanical disturbance, fluid scouring, hydrostatic pressure, or other external forces, the gas film 5 within some partitioned gas storage units 11 may be damaged, and the water body 6 may further enter the partitioned gas storage unit 11, forming a locally wetting area. The area where local wetting occurs is defined as the local failure zone 7. The local failure zone 7 is the state area formed after the local gas film of the partitioned gas storage unit 11 fails, and is not an independently set structure.

[0055] Once the local failure zone 7 is formed, the isolation boundary 12 restricts the continuous lateral expansion of liquid from this region to adjacent partitioned gas storage units 11, allowing the adjacent partitioned gas storage units 11 to still maintain a portion of the gas film 5. The confined gas replenishment layer 2 forms a nanoscale auxiliary gas storage space in the partitioned gas storage units 11 and the isolation boundary 12 region, and also hinders further liquid infiltration; the low surface energy gas-locking layer 3 is used to reduce the tendency of water 6 to spread and wet on the structural surface. Thus, the partitioned gas storage layer 1 provides microscale air retention space and local failure isolation, the confined gas replenishment layer 2 provides nanoscale air retention space and liquid infiltration resistance, and the low surface energy gas-locking layer 3 reduces the tendency of liquid to wet the structural surface. Together, these three elements improve the retention capacity of the gas film 5 on the surface of the metal substrate 4 under external disturbance conditions and reduce the risk of local wetting further expanding into overall wetting failure. The multi-level gas-storage superhydrophobic structure on the metal surface prepared in this application has excellent interfacial gas film retention capability, and also possesses self-cleaning, antifouling, anti-corrosion, and environmental aging resistance properties. It is suitable for surface protection of marine engineering equipment, ship structures, bridge components, port facilities, and other metal structural parts. Its structural schematic diagram is shown below. Figure 1 As shown.

[0056] like Figure 2 As shown in the figure, this application provides a method for preparing a multi-level gas-storing superhydrophobic structure on a metal surface, including the following steps:

[0057] 1. In this embodiment, a metal sheet is selected as the metal substrate, preferably a Q235 carbon steel sheet. Before the test, the surface of the metal sheet is polished with sandpaper to remove the surface oxide layer, rust layer and processing contaminants; then it is cleaned with acetone, anhydrous ethanol and deionized water respectively, and then kept dry for later use.

[0058] 2. Subsequently, a periodic array of regular hexagonal protrusions is constructed on the surface of the metal substrate 4 using a laser processing method to form a partitioned gas storage layer 1. Each regular hexagonal protrusion constitutes a partitioned gas storage unit 11, and grooves are formed between adjacent partitioned gas storage units 11, which constitute an isolation boundary 12. The top, sidewalls, and isolation boundary 12 of the partitioned gas storage unit 11 together form a microscale gas storage space for retaining air. The isolation boundary 12 is used to inhibit the continuous lateral spread of liquid from the partially wetted partitioned gas storage unit 11 to adjacent partitioned gas storage units 11.

[0059] 3. After forming the partitioned gas storage layer 1, hydrophobic nano-silica and graphene-like two-dimensional sheet materials are dispersed in ethanol or other organic solvents and ultrasonically treated to form a uniform dispersion. Then, the dispersion is loaded onto the surface of the partitioned gas storage layer 1 by spraying, dipping, dripping, or scraping, so that the nanoparticles and two-dimensional sheet materials are distributed on the top, sidewalls, and isolation boundary 12 areas of the partitioned gas storage unit 11, thereby forming a confined gas replenishment layer 2.

[0060] 4. Finally, the above structure is modified with low surface energy materials such as fluorinated silane, long-chain alkyl silane, PDMS, siloxane resin or stearic acid to form a low surface energy gas-locking layer 3. The modified sample is cured and dried or heat-treated at 40~120℃ for 0.5~4 h to obtain a multi-level gas-storage superhydrophobic structure on the metal surface with a partitioned gas storage layer 1, a confined gas replenishment layer 2 and a low surface energy gas-locking layer 3.

[0061] In this application, a periodic array of regular hexagonal protrusions is constructed on the surface of a metal substrate using laser processing to form a partitioned gas storage layer 1. The periodic array of regular hexagonal protrusions constitutes the partitioned gas storage layer 1, wherein each regular hexagonal protrusion constitutes a partitioned gas storage unit 11, and the grooves between adjacent partitioned gas storage units 11 constitute an isolation boundary 12. Isolation grooves are formed between adjacent microscale gas storage units. These isolation grooves are used to prevent liquid from spreading laterally from a microscale gas storage unit that has experienced localized wetting to adjacent microscale gas storage units through the groove area between adjacent microscale gas storage units, thereby inhibiting the expansion of localized wetting into overall wetting failure. The size of the regular hexagonal protrusions and the size of the grooves have a significant impact on the gas film retention capability. When the size of the regular hexagonal protrusions is too small or the grooves are too shallow, the gas storage space is insufficient, making it difficult to maintain a stable air layer in a liquid environment; when the size of the regular hexagonal protrusions is too large or the grooves are too wide, liquid can easily enter the interior of the grooves under water pressure or scouring, leading to gas film instability. Therefore, this application adopts a parameter range of 50-250 μm for the equivalent circumcircle diameter of the regular hexagonal protrusions, 10-80 μm for the spacing between adjacent protrusions, 10-100 μm for the protrusion height, and 5-60 μm for the groove width, in order to balance gas storage capacity, structural stability, and resistance to liquid intrusion. Preferably, the equivalent circumcircle diameter of the regular hexagonal protrusions is 80-180 μm, the spacing between adjacent protrusions is 20-50 μm, the protrusion height is 20-60 μm, and the groove width is 10-40 μm; this size range can balance gas storage space, structural stability, and resistance to liquid intrusion.

[0062] The construction of the confined gas replenishment layer 2 is a key step in improving the gas film retention capacity after local damage. Nanoparticles form a nano-rough structure, and two-dimensional sheet materials form bridging, covering, or overlapping structures. Together, they form nanoscale residual gas storage spaces on the top of the protrusion, sidewalls, and groove edges. Even if the microscale gas storage unit is locally wetted, the nanoscale residual gas storage space can still retain some air, thereby maintaining a local superhydrophobic state.

[0063] The construction of the low surface energy gas-locking layer 3 is a key step in improving anti-wetting ability. The low surface energy gas-locking layer 3 reduces the tendency of liquids to spread and adhere to the surfaces of the partitioned gas storage layer 1 and the confined gas replenishment layer 2 after modification with the low surface energy gas-locking layer 3, and increases the capillary ingress pressure that liquids need to overcome to enter the microscale gas storage unit and the nanoscale residual gas storage space, thereby reducing the degree of air displacement within the microscale gas storage unit and the nanoscale residual gas storage space by water or corrosive media. The curing or heat treatment step can improve the bonding stability between the confined gas replenishment layer 2 and the low surface energy gas-locking layer 3 and the partitioned gas storage layer 1, thereby reducing the risk of the confined gas replenishment layer 2 and the low surface energy gas-locking layer 3 detaching or failing under the influence of water erosion, mechanical wear, tape peeling, and acid / alkali environments.

[0064] Test case

[0065] Performance test results show that the multi-level gas storage superhydrophobic structure on the metal surface prepared in this application exhibits obvious non-wetting characteristics in various liquid environments.

[0066] Depend on Figure 3 As can be seen, the multi-level gas storage superhydrophobic structure on the metal surface prepared in this application exhibits a distinct multi-scale surface morphology. At lower magnification, periodically arranged near-hexagonal partitioned gas storage units 11 can be observed, with obvious isolation boundaries 12 formed between adjacent partitioned gas storage units 11. Upon further magnification, it can be observed that the surface of the partitioned gas storage units 11 is covered with a large number of nanoscale particles and fine protrusions, forming the secondary nano-rough structure required for the confined gas replenishment layer 2.

[0067] Depend on Figure 4 It can be seen that after the sample was immersed in aqueous solutions of different colors, the surface still maintained a clear air film, and no obvious liquid adhesion appeared on the surface after it was taken out. This indicates that the multi-level gas storage superhydrophobic structure of the metal surface can effectively capture and maintain an air layer in the liquid environment.

[0068] Depend on Figure 5 (a) and Figure 5(b) As can be seen, after placing powdered contaminants on the multi-level gas-storage superhydrophobic structure on the metal surface prepared in this application, the water droplets can maintain a relatively complete droplet shape and move along the surface. During the movement, the contaminants are carried away from the sample surface, and no obvious contaminant residue is observed in the area after the water droplets pass through. Figure 5 (c) and Figure 5 (d) As can be seen, the liquid on the control sample exhibits more obvious adhesion and spreading phenomena, accompanied by contaminant residue. The above comparison shows that the multi-level gas-storing superhydrophobic structure on the metal surface prepared in this application has low liquid adhesion characteristics and can remove surface contaminants by means of rolling or sliding droplets, thus having good self-cleaning performance.

[0069] Depend on Figure 6 It can be seen that after the sample was placed in water and air environments for a certain period of time, the contact angle remained at a high level and the sliding angle changed little, indicating that the multi-level gas storage superhydrophobic structure on the metal surface has good long-term wetting stability and gas film retention ability.

[0070] Depend on Figure 7 It is evident that the sample maintained a high contact angle and a low sliding angle even after undergoing different pH environments, tape peeling, mechanical wear, salt resistance treatment, and different temperature treatments. This indicates that the multi-level gas-storage superhydrophobic structure on the metal surface has excellent resistance to acids and alkalis, adhesion and peeling, wear, salt, and temperature changes.

[0071] Depend on Figure 8 It is evident that at a water depth of 0.2 m, the gas film retention time on the sample surface is approximately 7 hours; when the water depth increases to 0.5 m, the gas film retention time is approximately 3.4 hours. With increasing water depth, the hydrostatic pressure on the sample increases, and the gas film retention time shortens somewhat, but it can still maintain a gas film state for several hours at a water depth of 0.5 m. These results demonstrate that the multi-level gas-storage superhydrophobic structure on the metal surface prepared in this application exhibits good gas film retention capability under certain hydrostatic pressure conditions.

[0072] To compare the effects of different surface components on the corrosion resistance of metal substrates, five groups of samples were subjected to electrochemical tests. Q represents a Q235 steel substrate without surface functionalization; QF represents a sample obtained by spraying only a low surface energy FAS material onto the Q235 steel surface; QFG represents a sample obtained by spraying a mixture of FAS and graphene onto the Q235 steel surface; QFS represents a sample obtained by spraying a mixture of FAS and SiO2 onto the Q235 steel surface; and QFGS represents a sample obtained by spraying a mixture of FAS, graphene, and SiO2 onto the Q235 steel surface. QFGS corresponds to the multi-level gas-storing superhydrophobic structure on the metal surface constructed in this application. Preferably, all samples used Q235 steel substrates of the same specifications and were prepared and tested under the same substrate pretreatment and testing conditions to evaluate the effects of different functional components on corrosion resistance. Figure 9 (a) It can be seen that the QFGS sample has the highest impedance modulus in the low-frequency region, significantly higher than that of the Q, QF, QFG, and QFS samples; Figure 9 (b) As can be seen, the QFGS sample has the largest impedance arc, followed by the QFS sample, while the Q, QF, and QFG samples have relatively low impedance responses. These results indicate that the multi-level gas-storage superhydrophobic structure on the metal surface constructed using FAS, graphene, and SiO2 in this application can effectively improve the electrochemical impedance of the Q235 steel surface, reduce the contact between the corrosive medium and the metal substrate, and decrease the degree of transport of the corrosive medium into the substrate, thereby improving the corrosion resistance of the metal substrate.

[0073] The partitioned gas storage-limited gas replenishment-low surface energy gas-locking composite structure constructed in this application can maintain good gas film stability and superhydrophobic properties under conditions such as liquid immersion, mechanical wear, tape peeling, water pressure, acid and alkali, salt environment and temperature change, and further improve the corrosion protection capability of metal surface.

[0074] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.

Claims

1. A multi-level gas-storage superhydrophobic structure on a metal surface, characterized in that, It includes a partitioned gas storage layer, a confined gas replenishment layer, and a low surface energy gas-locking layer. The partitioned gas storage layer comprises multiple independent microscale gas storage units spaced apart from each other, and adjacent microscale gas storage units are provided with isolation boundaries, buffer trenches, or liquid lateral expansion blocking structures. The confined gas replenishment layer is disposed on the top, sidewall, edge, or inner wall of the microscale gas storage unit or in the trench area between adjacent microscale gas storage units to form a nanoscale residual gas storage space. The low surface energy gas-locking layer covers the surfaces of the partitioned gas storage layer and the confined gas replenishment layer to reduce the tendency of liquid to invade the microscale gas storage unit and the nanoscale residual gas storage space.

2. The multi-level gas storage type superhydrophobic structure on a metal surface according to claim 1, characterized in that, The microscale gas storage unit is selected from at least one of the following: biomimetic scale-like unit, hexagonal unit, arc-shaped groove unit, closed pit unit, semi-closed pit unit, and grid unit.

3. The multi-level gas storage type superhydrophobic structure on a metal surface according to claim 2, characterized in that, The microscale gas storage unit is a periodically arranged array of regular hexagonal protrusions. The equivalent circumcircle diameter of the regular hexagonal protrusion is 50~250μm, the spacing between adjacent regular hexagonal protrusions is 10~80μm, and the height of the regular hexagonal protrusion is 10~100μm. An isolation trench, a semi-continuous trench, or a buffer trench is formed between adjacent regular hexagonal protrusions; the width of the isolation trench, semi-continuous trench, or buffer trench is 5~60 μm and the depth is 10~100 μm.

4. A method for preparing a multi-level gas-storing superhydrophobic structure on a metal surface according to any one of claims 1 to 3, characterized in that, Includes the following steps: S1. Construct a partitioned gas storage layer on the surface of a metal substrate; S2. Confinement gas replenishment layer is constructed in the trench area at the top, sidewall, edge or inner wall of the partitioned gas storage layer or between adjacent microscale gas storage units. S3. Construct a low surface energy gas-locking layer on the surface of the partitioned gas storage layer and the confined gas replenishment layer, and form a multi-level gas storage type superhydrophobic structure on the metal surface after curing, drying or heat treatment.

5. The method for preparing a multi-level gas-storage superhydrophobic structure on a metal surface according to claim 4, characterized in that, The specific process of step S1 is as follows: grinding, cleaning and drying the metal substrate to remove oxide layer, oil and loose particles; then using laser processing, plasma etching, mechanical imprinting, chemical etching, micro milling, sandblasting, template replication or a combination thereof to construct microscale gas storage units on the surface of the metal substrate.

6. The method for preparing a multi-level gas-storage superhydrophobic structure on a metal surface according to claim 5, characterized in that, The specific process of step S2 is as follows: a dispersion containing hydrophobic nanoparticles and / or two-dimensional sheet materials is loaded onto the top, sidewall, edge or inner wall of a microscale gas storage unit or the trench area between adjacent microscale gas storage units by spraying, dip coating, drop coating, spin coating, scraping coating, electrophoretic deposition, in-situ growth or a combination thereof, to form a confined gas replenishment layer.

7. The method for preparing a multi-level gas-storage superhydrophobic structure on a metal surface according to claim 6, characterized in that, The hydrophobic nanoparticles are selected from at least one of silicon dioxide, aluminum oxide, titanium oxide, zinc oxide, silicon nitride, silicon carbide, calcium carbonate, or their hydrophobic modifiers; the two-dimensional sheet material is selected from at least one of graphene, graphene oxide, reduced graphene oxide, boron nitride, MXene, molybdenum disulfide, or their modifiers.

8. The method for preparing a multi-level gas-storage superhydrophobic structure on a metal surface according to claim 4, characterized in that, The specific process of step S3 is as follows: the surface of the partitioned gas storage layer and the confined gas replenishment layer is modified by using a low surface energy material through silanization reaction, thermosetting, ultraviolet curing, room temperature curing, adsorption assembly or a combination thereof to form a low surface energy gas-locking layer. After curing, drying or heat treatment, a multi-level gas storage type superhydrophobic structure on the metal surface is formed.

9. The method for preparing a multi-level gas-storing superhydrophobic structure on a metal surface according to claim 8, characterized in that, The low surface energy material is selected from at least one of fluorosilanes, long-chain alkylsilanes, fluoropolymers, siloxane resins, polydimethylsiloxanes, and stearic acid.

10. The method for preparing a multi-level gas-storing superhydrophobic structure on a metal surface according to claim 4, characterized in that, The specific conditions for the heat treatment are as follows: the heat treatment temperature is 40~120℃, and the treatment time is 0.5~4 h.