Thermochromic coatings, energy storage devices and energy storage systems
By applying a coating containing silicone organic resin and thermochromic pigments to the surface of the energy storage device, the problem of the energy storage device being unable to be monitored due to temperature rise is solved, realizing intuitive warning of temperature changes and corrosion resistance and durability, thus improving the safety of the device.
Patent Information
- Application Number
- CN202510633693.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-16
- Publication Date
- 2026-11-17
AI Technical Summary
During use, energy storage devices may overheat due to factors such as heat generated during operation or high ambient temperature. This overheating cannot be effectively monitored or visually alerted, which may cause damage. Furthermore, existing temperature detectors have limited detection range.
A thermochromic coating is applied to the surface of the main components of the energy storage device. The coating consists of an adhesive matrix and a thermochromic pigment. The adhesive matrix uses a silicone-containing organic resin, combined with polyester compounds and a capsule-structured thermochromic pigment, to achieve temperature change monitoring and intuitive warning.
While meeting the requirements for corrosion resistance and durability, it enables real-time monitoring and intuitive warning of temperature changes in energy storage devices, thereby improving the safety and reliability of the devices.
Smart Images

Figure CN123107436A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of energy storage device technology, and in particular to a thermosensitive color-changing coating, an energy storage device, and an energy storage system. Background Technology
[0002] During operation, energy storage devices may experience temperature rise or even overheating in some components due to factors such as heat generation or high ambient temperatures. If not addressed promptly, this could damage the energy storage device. However, due to space or technological limitations, it is impossible to install temperature detectors within energy storage devices to monitor the temperature of all components. Furthermore, temperature detectors have limited detection ranges and lack intuitiveness, failing to meet the requirements for direct warning. Summary of the Invention
[0003] This application provides a thermochromic coating with good corrosion resistance and durability, and can provide a visual warning of temperature changes. Furthermore, it provides an energy storage device and energy storage system treated with this thermochromic coating.
[0004] A first aspect of this application provides an energy storage device, including a body component and a thermochromic coating disposed on the outer surface of the body component; the thermochromic coating includes an adhesive matrix and a thermochromic pigment; the resin of the adhesive matrix includes a silicone-containing organic resin.
[0005] The aforementioned energy storage device, by applying a thermochromic coating comprising an adhesive matrix and a thermochromic pigment to the surface of its main components, and by using a silicone-containing organic resin as the adhesive matrix resin, can impart thermochromic properties to the energy storage device while meeting the requirements for corrosion resistance and durability, thereby enabling the monitoring and intuitive warning of its temperature changes.
[0006] In some embodiments, the silicone-containing organic resin includes at least one of a hydroxyl-containing silicone-containing organic resin and a silicone-modified epoxy resin; optionally, the hydroxyl-containing silicone-containing organic resin includes a silicone-modified hydroxyl-type acrylic resin.
[0007] Hydroxyl-containing silicone organic resins contain hydroxyl groups, and silicone-modified epoxy resins are rich in hydroxyl groups after curing, which is beneficial for adhesion to substrates. Furthermore, silicone-modified hydroxyl-type acrylic resins and silicone-modified epoxy resins combine the excellent film-forming properties and adhesion of acrylic or epoxy resins with the high and low temperature resistance, water repellency, aging resistance, and corrosion resistance of silicone, enabling good adhesion and film formation on energy storage device components, giving them better insulation, corrosion resistance, and durability.
[0008] In some embodiments, the silicone-containing organic resin is an aqueous silicone-containing organic resin; optionally, the aqueous silicone-containing organic resin includes at least one of silicone-modified aqueous hydroxyl-type acrylic resin and silicone-modified aqueous epoxy resin.
[0009] Waterborne silicone-containing organic resins are solvent-free, safe, and environmentally friendly, avoiding the adverse effects of residual solvents on energy storage devices. Furthermore, silicone-modified waterborne hydroxyl-type acrylic resins and silicone-modified waterborne epoxy resins are rich in hydroxyl groups, exhibiting excellent adhesion to various substrates and good film-forming properties, which helps improve the overall performance of the coating.
[0010] In some embodiments, the adhesive matrix comprises a polyester compound.
[0011] Polyester compounds can promote film formation and reduce film formation temperature. They have good compatibility with silicone-containing organic resins. When used in combination with silicone-containing organic resins, they can promote film formation and adhesion to the substrate, and improve the insulation and corrosion resistance of thermochromic coatings.
[0012] In some embodiments, the polyester compound includes C10-C20 polyester compounds, and optionally, the polyester compound includes at least one of alcohol ester twelve, alcohol ester fourteen, and alcohol ester sixteen.
[0013] C10-C20 polyester compounds have long chains, which is beneficial for improving toughness; alcohol esters twelve, fourteen, and sixteen have moderately long chains and can lower the film-forming temperature, which is beneficial for promoting film formation and improving the insulation and corrosion resistance of thermochromic coatings.
[0014] In some embodiments, the thermochromic pigment has a capsule structure.
[0015] Microencapsulated thermochromic pigments exhibit good stability, strong reversibility of color change, and are easy to disperse, thus meeting the application requirements for real-time color-changing warnings in response to temperature changes.
[0016] In some embodiments, the outer shell of the capsule structure is made of at least one of silicone hybrid polyurethane and silicone hybrid epoxy resin.
[0017] Organosilicon hybrid polyurethane and organosilicon hybrid epoxy resin have good transparency, weather resistance, chemical resistance and mechanical properties. Thermosensitive color-changing pigments with capsule structures prepared using them as shells can maintain stable working performance in a variety of complex environments.
[0018] In some embodiments, the color-changing substance in the capsule structure comprises an electron-transfer organic compound.
[0019] Electron-transfer type organic compounds are a class of organic chromogenic systems with special chemical structures. The electron transitions that occur at different temperatures are different, resulting in different electron densities and thus different colors. This can meet the application requirements of real-time color-coding warnings based on temperature changes.
[0020] In some embodiments, the electron-transfer organic compound includes at least one of phenylenediamine compounds, triarylmethanephthalides, indolinephthalides, fluorane compounds, triphenylmethane compounds, spiropyran compounds, spirocyclic compounds, dianthrone compounds, and α-naphthoquinone derivatives; optionally, at least one of spiropyran compounds and phenylenediamine compounds.
[0021] The aforementioned electron transfer organic compounds exhibit good stability, are not easily oxidized or decomposed, and show significant color changes with temperature, which is beneficial for stable color-based warning.
[0022] In some embodiments, the spiropyran compound includes organosilicon-modified spiropyran compound, optionally spiro[1,3,3-trimethylindole-(8-methoxysilanebenzodihydropyran)]; the phenylenediamine compound includes N,N'-bis(3-hydroxysalicylyl)-1,2-phenylenediamine.
[0023] Spiropyran compounds and phenylenediamine compounds have good resistance to oxidation and aging, and are not easily discolored by environmental factors such as oxidation or high temperature, which is conducive to stable color-based warning.
[0024] In some embodiments, the adhesive matrix further includes additives; the additives include at least one of wetting agents, dispersants, fillers, leveling agents, defoamers, pH adjusters, and thickeners;
[0025] Optionally, the wetting agent includes at least one of acetylenic diol wetting agents, hydrophobically modified acrylate wetting agents, and polyether modified polysiloxane wetting agents;
[0026] Optionally, the dispersant includes at least one of polyphosphate, sodium polyacrylate, and ammonium polyacrylate;
[0027] Optionally, the filler includes at least one of mica powder, calcium carbonate, and kaolin.
[0028] Optionally, the leveling agent includes at least one of polyether-modified silicone leveling agents, acrylate leveling agents, and fluorocarbon-modified acrylate leveling agents;
[0029] Optionally, the defoamer includes at least one of mineral oil-based defoamers and silicone-based defoamers;
[0030] Optionally, the pH adjuster includes at least one of 2-amino-2-methyl-1-propanol and ammonia water;
[0031] Optionally, the thickener includes at least one of associative polyacrylate, non-associative polyacrylate, and hydrophobically modified associative polyurethane.
[0032] Choosing the above-mentioned additives is beneficial for adjusting the application performance of thermochromic coatings.
[0033] A second aspect of this application provides a method for preparing an energy storage device, the method comprising the following steps:
[0034] The energy storage device is prepared by curing the thermo-color-sensitive coating onto the surface of the main component of the energy storage device to form a thermo-color-sensitive coating.
[0035] The thermochromic coating comprises a binder matrix and a thermochromic pigment; the resin of the binder matrix comprises a silicone-containing organic resin.
[0036] By curing a thermosensitive color-changing coating on the surface of the main components of an energy storage device, a thermosensitive color-changing coating is formed, and an energy storage device is prepared. The resin of the bonding matrix includes a silicone-containing organic resin. On the basis of meeting the requirements of corrosion resistance and durability, the energy storage device can be endowed with thermosensitive color-changing characteristics, so as to realize the monitoring and intuitive warning of its temperature changes.
[0037] In some embodiments, the thermochromic coating includes single-component coatings and / or two-component coatings.
[0038] Single-component coatings can be used directly without mixing, making them suitable for rapid application and easy to use; two-component coatings allow for adjustable curing time and offer good adhesion, bond strength, and durability, allowing you to choose the appropriate option based on your specific needs.
[0039] In some embodiments, the thermochromic coating is a two-component coating, wherein component A includes resin, thermochromic pigment and film-forming aid; and component B includes curing agent.
[0040] The two-component coating has component A consisting of resin, thermochromic pigment, and film-forming aid, and component B consisting of curing agent. This allows for adjustment of curing time and ensures the storage durability of the adhesive, thereby improving its adhesion, bond strength, and durability.
[0041] In some embodiments, the curing agent includes isocyanate-based curing agents; optionally, it includes hexamethylene diisocyanate-based polyisocyanates.
[0042] The isocyanate groups in isocyanate curing agents exhibit high reactivity with hydroxyl-containing silicone organic resins, which is beneficial for improving curing efficiency. Furthermore, hexamethylene diisocyanate-based polyisocyanates, belonging to aliphatic isocyanate curing agents, possess a stable six-membered ring structure and excellent heat and chemical resistance, which is beneficial for improving the flexibility, adhesion strength, and durability of the coating.
[0043] In some embodiments, the molar ratio of the hydroxyl groups of the matrix resin in component A to the isocyanate groups of the curing agent in component B is 1:1.3-1:1.5.
[0044] Controlling the molar ratio of hydroxyl groups in the matrix resin in component A to isocyanate groups in the curing agent in component B to 1:1.3-1:1.5 is beneficial to improve the degree of curing and enhance the adhesion strength and durability of the coating.
[0045] In some embodiments, component A comprises, by weight, 50-70 parts resin, 10-20 parts thermochromic pigment, and 2.5-3.5 parts film-forming aid.
[0046] Controlling the dosage of component A in the above-mentioned ratio is beneficial to improving the dispersion uniformity and film formation uniformity of the coating, as well as improving the insulation, corrosion resistance and durability of the coating.
[0047] A third aspect of this application provides an energy storage system including the energy storage device described in the first aspect.
[0048] The energy storage devices in the above-mentioned energy storage system can change color to indicate temperature changes, which facilitates temperature monitoring.
[0049] A fourth aspect of this application provides a thermochromic coating comprising an adhesive matrix and a thermochromic pigment; wherein the resin of the adhesive matrix comprises a silicone-containing organic resin.
[0050] The aforementioned thermochromic coating, comprising a resin including a silicone-containing organic resin binder and thermochromic pigments, can impart thermochromic properties to the coating while meeting corrosion resistance and durability requirements. When applied to energy storage devices, it enables the monitoring and visual warning of temperature changes. Attached Figure Description
[0051] To better describe and illustrate the embodiments or examples provided in this application, reference may be made to one or more accompanying drawings. Additional details or examples used to describe the drawings should not be considered as limiting the scope of any of the disclosed applications, the currently described embodiments or examples, or the best mode of conduct of these applications as currently understood. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:
[0052] Figure 1 This is a schematic diagram illustrating the color development mechanism of electron-transfer type organic compounds in some embodiments of this application;
[0053] Figure 2 This application provides schematic diagrams of the structure of an energy storage system according to some embodiments.
[0054] Figure 3 This is a color change diagram of Embodiment 1 of this application;
[0055] Explanation of reference numerals in the attached drawings: 100, energy storage system; 200, energy storage device; 300, power conversion equipment; 400, power generation equipment. Detailed Implementation
[0056] Hereinafter, some embodiments of the thermochromic coating, energy storage device, and energy storage system of this application are described in detail with appropriate reference to the accompanying drawings. However, some unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of actually identical structures may be omitted. This is to avoid making the following description unnecessarily lengthy and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0057] The "range" disclosed in this application can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints; any endpoint can be independently included or excluded, and they can be combined arbitrarily, meaning any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values 1 and 2 are listed, and maximum range values 3, 4, and 5 are also listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0" and "5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when describing a parameter as an integer ≥ 2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12 for that parameter. For instance, when describing a parameter as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.
[0058] In this application, the terms "multiple" or "various" are used unless otherwise specified, referring to a quantity greater than or equal to 2. For example, "one or more" means one or more types.
[0059] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0060] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. The term "implementation" as used herein has a similar understanding.
[0061] Those skilled in the art will understand that the order in which the steps are written in the methods of various embodiments or examples does not imply a strict execution order and does not constitute any limitation on the implementation process. The detailed execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps of this application may be performed sequentially or randomly, preferably sequentially. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, if the method may also include step (c), it means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0062] In this application, open-ended technical features or solutions described using terms such as "containing," "including," or "comprising" do not exclude additional members beyond those listed unless otherwise specified. They can be considered as providing both closed-ended features or solutions comprised of the listed members and open-ended features or solutions that include additional members beyond the listed members. For example, if A includes a1, a2, and a3, it may also include other members or exclude additional members unless otherwise specified. This can be considered as providing both the feature or solution that "A consists of a1, a2, and a3" and the feature or solution that "A includes not only a1, a2, and a3, but also other members." In this application, unless otherwise specified, A (e.g., B) indicates that B is a non-limiting example of A, and it can be understood that A is not limited to B.
[0063] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "optional" entry shall be independent.
[0064] In this application, the room temperature refers to -30℃ to 40℃, optionally 10℃ to 35℃, and further optionally 20℃ to 30℃.
[0065] In this application, "polyester compounds" refers to products obtained by esterification of polyacids and polyols, which may contain one or more ester groups. Polyester compounds can effectively reduce the minimum film-forming temperature (MFFT) of coatings, enabling coatings to form continuous films at lower temperatures, improving coating performance, and also have a certain plasticizing effect.
[0066] During operation, energy storage devices may experience temperature rise or even overheating in some components due to heat generation or high ambient temperatures. Failure to address this promptly can damage the device. However, space and technology limitations often prevent the installation of temperature detectors to monitor all components within the device. Furthermore, temperature detectors have limited detection ranges and lack intuitiveness, failing to meet the requirement for direct temperature warnings. While coating the surface of the energy storage device with a thermochromic coating can provide a direct warning of temperature changes, the surface requires excellent corrosion resistance and durability (e.g., resistance to aging, heat, and chemicals). General thermochromic coatings cannot simultaneously meet both these requirements.
[0067] Based on this, this application provides a thermochromic coating with good corrosion resistance and durability, and can provide a direct warning of temperature changes, and further provides an energy storage device and energy storage system treated with the thermochromic coating.
[0068] In a first aspect, some embodiments of this application provide an energy storage device, including a body component and a thermochromic coating disposed on the outer surface of the body component; the thermochromic coating includes an adhesive matrix and a thermochromic pigment; the resin of the adhesive matrix includes a silicone-containing organic resin.
[0069] The aforementioned energy storage device, by applying a thermochromic coating comprising an adhesive matrix and a thermochromic pigment to the surface of its main components, and by using a silicone-containing organic resin as the adhesive matrix resin, can impart thermochromic properties to the energy storage device while meeting the requirements for corrosion resistance and durability, thereby enabling the monitoring and intuitive warning of its temperature changes.
[0070] In some embodiments, the silicone-containing organic resin includes at least one of a hydroxyl-containing silicone-containing organic resin and a silicone-modified epoxy resin; optionally, the hydroxyl-containing silicone-containing organic resin includes a silicone-modified hydroxyl-type acrylic resin.
[0071] Hydroxyl-containing silicone organic resins contain hydroxyl groups, and silicone-modified epoxy resins are rich in hydroxyl groups after curing, which is beneficial for adhesion to substrates. Furthermore, silicone-modified hydroxyl-type acrylic resins and silicone-modified epoxy resins combine the excellent film-forming properties and adhesion of acrylic or epoxy resins with the high and low temperature resistance, water repellency, aging resistance, and corrosion resistance of silicone, enabling good adhesion and film formation on energy storage device components, giving them better insulation, corrosion resistance, and durability.
[0072] In some embodiments, the silicone-containing organic resin is an aqueous silicone-containing organic resin; optionally, the aqueous silicone-containing organic resin includes at least one of silicone-modified aqueous hydroxyl-type acrylic resin and silicone-modified aqueous epoxy resin.
[0073] Waterborne silicone-containing organic resins are solvent-free, safe, and environmentally friendly, avoiding the adverse effects of residual solvents on energy storage devices. Furthermore, silicone-modified waterborne hydroxyl-type acrylic resins and silicone-modified waterborne epoxy resins are rich in hydroxyl groups, exhibiting excellent adhesion to various substrates and good film-forming properties, which helps improve the overall performance of the coating.
[0074] In some embodiments, the adhesive matrix comprises a polyester compound.
[0075] Polyester compounds can promote film formation and reduce film formation temperature. They have good compatibility with silicone-containing organic resins. When used in combination with silicone-containing organic resins, they can promote film formation and adhesion to the substrate, and improve the insulation and corrosion resistance of thermochromic coatings.
[0076] In one specific example, the polyester compounds include C10-C20 polyester compounds.
[0077] C10-C20 polyester compounds have long chains, which helps improve toughness.
[0078] In a specific example, C10-C20 polyester compounds can be C10, C11, C12, C13, C14, C15, C16, C17, C18, C19, or C20 polyester compounds.
[0079] In some embodiments, the polyester compound includes at least one of alcohol ester twelve, alcohol ester fourteen, and alcohol ester sixteen.
[0080] Alcohol esters twelve, fourteen, and sixteen have moderately long chains and can lower the film-forming temperature, which is beneficial for promoting film formation and improving the insulation and corrosion resistance of thermochromic coatings.
[0081] In some embodiments, the thermochromic pigment has a capsule structure.
[0082] Microencapsulated thermochromic pigments exhibit good stability, strong reversibility of color change, and are easy to disperse, thus meeting the application requirements for real-time color-changing warnings in response to temperature changes.
[0083] In some embodiments, the outer shell of the capsule structure is made of at least one of silicone hybrid polyurethane and silicone hybrid epoxy resin.
[0084] Organosilicon hybrid polyurethane and organosilicon hybrid epoxy resin have good transparency, weather resistance, chemical resistance and mechanical properties. Thermosensitive color-changing pigments with capsule structures prepared using them as shells can maintain stable working performance in a variety of complex environments.
[0085] In some embodiments, the color-changing substance in the capsule structure comprises an electron-transfer organic compound.
[0086] Electron-transfer type organic compounds are a class of organic chromogenic systems with special chemical structures. Different electron transitions occur at different temperatures, resulting in varying electron densities and thus different colors. This allows them to meet the application requirements of real-time color-changing warnings based on temperature changes. Their color-changing mechanism is as follows: Figure 1 As shown.
[0087] In some embodiments, the electron-transfer organic compound includes at least one of phenylenediamine compounds, triarylmethanephthalides, indolinephthalides, fluorane compounds, triphenylmethane compounds, spiropyran compounds, spirocyclic compounds, dianthrone compounds, and α-naphthoquinone derivatives; optionally, at least one of spiropyran compounds and phenylenediamine compounds.
[0088] The aforementioned electron transfer organic compounds exhibit good stability, are not easily oxidized or decomposed, and show significant color changes with temperature, which is beneficial for stable color-based warning.
[0089] In some embodiments, the spiropyran compound includes organosilicon-modified spiropyran compound, optionally spiro[1,3,3-trimethylindole-(8-methoxysilanebenzodihydropyran)]; the phenylenediamine compound includes N,N'-bis(3-hydroxysalicylyl)-1,2-phenylenediamine.
[0090] Spiropyran compounds and phenylenediamine compounds have good resistance to oxidation and aging, and are not easily discolored by environmental factors such as oxidation or high temperature, which is conducive to stable color-based warning.
[0091] In some embodiments, the adhesive matrix further includes additives; the additives include at least one of wetting agents, dispersants, fillers, leveling agents, defoamers, pH adjusters, and thickeners;
[0092] Optionally, the wetting agent includes at least one of acetylenic diol wetting agents, hydrophobically modified acrylate wetting agents, and polyether modified polysiloxane wetting agents;
[0093] Optionally, the dispersant includes at least one of polyphosphate, sodium polyacrylate, and ammonium polyacrylate;
[0094] Optionally, the filler includes at least one of mica powder, calcium carbonate, and kaolin.
[0095] Optionally, the leveling agent includes at least one of polyether-modified silicone leveling agents, acrylate leveling agents, and fluorocarbon-modified acrylate leveling agents;
[0096] Optionally, the defoamer includes at least one of mineral oil-based defoamers and silicone-based defoamers;
[0097] Optionally, the pH adjuster includes at least one of 2-amino-2-methyl-1-propanol and ammonia water;
[0098] Optionally, the thickener includes at least one of associative polyacrylate, non-associative polyacrylate, and hydrophobically modified associative polyurethane.
[0099] Choosing the above-mentioned additives is beneficial for adjusting the application performance of thermochromic coatings.
[0100] In some embodiments, the thickness of the thermochromic coating is 100μm-400μm, optionally 150μm-350μm, such as 100μm, 150μm, 200μm, 250μm, 300μm, 350μm, 400μm, etc.
[0101] Secondly, some embodiments of this application provide a method for preparing an energy storage device, the method comprising the following steps:
[0102] The energy storage device is prepared by curing the thermo-color-sensitive coating onto the surface of the main component of the energy storage device to form a thermo-color-sensitive coating.
[0103] The thermochromic coating comprises a binder matrix and a thermochromic pigment; the resin of the binder matrix comprises a silicone-containing organic resin.
[0104] Understandably, the surface of the body component refers to the outer surface of the body component.
[0105] In some embodiments, the curing conditions for the thermochromic coating are 1-7 days at room temperature, such as 1 day, 2 days, 3 days, 4 days, 5 days, 6 days, 7 days, etc. The curing time is adjusted according to the temperature.
[0106] By curing a thermosensitive color-changing coating on the surface of the main components of an energy storage device, a thermosensitive color-changing coating is formed, and an energy storage device is prepared. The resin of the bonding matrix includes a silicone-containing organic resin. On the basis of meeting the requirements of corrosion resistance and durability, the energy storage device can be endowed with thermosensitive color-changing characteristics, so as to realize the monitoring and intuitive warning of its temperature changes.
[0107] In some embodiments, the thermochromic coating includes single-component coatings and / or two-component coatings.
[0108] Single-component coatings can be used directly without mixing, making them suitable for rapid application and easy to use; two-component coatings allow for adjustable curing time and offer good adhesion, bond strength, and durability, allowing you to choose the appropriate option based on your specific needs.
[0109] In some embodiments, the thermochromic coating is a two-component coating, wherein component A includes resin, thermochromic pigment and film-forming aid; and component B includes curing agent.
[0110] The two-component coating has component A consisting of resin, thermochromic pigment, and film-forming aid, and component B consisting of curing agent. This allows for adjustment of curing time and ensures the storage durability of the adhesive, thereby improving its adhesion, bond strength, and durability.
[0111] In some embodiments, the curing agent includes isocyanate-based curing agents; optionally, it includes hexamethylene diisocyanate-based polyisocyanates.
[0112] The isocyanate groups in isocyanate curing agents exhibit high reactivity with hydroxyl-containing silicone organic resins, which is beneficial for improving curing efficiency. Furthermore, hexamethylene diisocyanate-based polyisocyanates, belonging to aliphatic isocyanate curing agents, possess a stable six-membered ring structure and excellent heat and chemical resistance, which is beneficial for improving the flexibility, adhesion strength, and durability of the coating.
[0113] In some embodiments, the molar ratio of the hydroxyl groups of the matrix resin in component A to the isocyanate groups of the curing agent in component B is 1:1.3-1:1.5, for example, 1:1.3, 1:1.35, 1:1.4, 1:1.45, 1:1.5, etc.
[0114] Controlling the molar ratio of hydroxyl groups in the matrix resin in component A to isocyanate groups in the curing agent in component B to 1:1.3-1:1.5 is beneficial to improve the degree of curing and enhance the adhesion strength and durability of the coating.
[0115] In some embodiments, component A comprises, by weight, 50-70 parts resin, 10-20 parts thermochromic pigment, and 2.5-3.5 parts film-forming aid.
[0116] Controlling the dosage of component A in the above-mentioned ratio is beneficial to improving the dispersion uniformity and film formation uniformity of the coating, as well as improving the insulation, corrosion resistance and durability of the coating.
[0117] In some specific examples, the amount of resin used can be 50 parts, 52 parts, 54 parts, 55 parts, 60 parts, 65 parts, 66 parts, 68 parts, 70 parts, etc.; 55-65 parts can be selected.
[0118] In some specific examples, the amount of thermochromic pigment used can be 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, etc.; 12 to 18 parts can be selected.
[0119] In some specific examples, the amount of film-forming aid can be 2.5 parts, 2.6 parts, 2.7 parts, 2.8 parts, 2.9 parts, 3.0 parts, 3.1 parts, 3.2 parts, 3.3 parts, 3.4 parts, 3.5 parts, etc.; 2.7 parts to 3.3 parts are optional.
[0120] Thirdly, some embodiments of this application provide an energy storage system including the energy storage device described in the first aspect.
[0121] The energy storage devices in the above-mentioned energy storage system can change color to indicate temperature changes, which facilitates temperature monitoring.
[0122] Fourthly, some embodiments of this application provide a thermochromic coating, including an adhesive matrix and a thermochromic pigment; the resin of the adhesive matrix includes a silicone-containing organic resin.
[0123] The aforementioned thermochromic coating, comprising a resin including a silicone-containing organic resin binder and thermochromic pigments, can impart thermochromic properties to the coating while meeting corrosion resistance and durability requirements. When applied to energy storage devices, it enables the monitoring and visual warning of temperature changes.
[0124] The energy storage device of this application will be described below with appropriate reference to the accompanying drawings.
[0125] Please refer to Figure 2 , Figure 2 The diagram shows the structure of an energy storage system provided in some embodiments of this application.
[0126] In some embodiments, the energy storage system 100 may include one or more energy storage devices 200 and a power converter system (PCS), wherein the power converter system 300 is connected between the power generation device 400 and the energy storage device 200. The power generation device 400 generates electrical energy, which can be stored in the energy storage device 200 through the power converter system 300, and the electrical energy stored in the energy storage device 200 can be released back to the power generation device 400 through the power converter system 300. As an example, the power generation device 400 may specifically be a power grid, a solar panel, a hydroelectric power generation device 400, a thermal power generation device 400, a wind power generation device 400, etc. The specific type of the power generation device 400 is not limited in this application.
[0127] This application provides an energy storage device 200, including one or more battery clusters to increase the voltage and capacity of the energy storage device 200. The battery cluster may include multiple battery devices, which are connected in series via a busbar to increase the voltage of the energy storage device 200. When the energy storage device 200 includes multiple battery clusters, the multiple battery clusters are connected in parallel to increase the capacity of the energy storage device 200. The energy storage device 200 can be used in energy storage power stations, wind power generation systems, solar power generation systems, mobile power systems, or temporary power supply systems, etc. The energy storage device 200 can store electrical energy as needed and output electrical energy when appropriate. For example, the energy storage device 200 can store electrical energy during off-peak hours and provide power to relevant users or electrical equipment during peak hours. The energy storage system provided in this application can be any power system that requires the energy storage device 200.
[0128] In some embodiments, the energy storage device 200 is an energy storage container or an energy storage cabinet.
[0129] In some embodiments, the energy storage device 200 may include a cabinet and one or more battery clusters housed in the cabinet.
[0130] In some embodiments, the energy storage device 200 may include modules such as a thermal management module, a main control module, a central control module, a power distribution module, and a fire protection module.
[0131] As an example, the thermal management module may include a liquid cooling unit that supplies coolant to each battery device via piping to regulate the temperature of the individual battery cells.
[0132] As an example, the main control module can serve as the battery management unit for the battery cluster, used to monitor and manage the battery cluster. The main control module can monitor information such as the current, voltage, power, or temperature of the battery cluster. For instance, it can control the charging and discharging current and voltage of the battery cluster. The main control module includes modules such as an auxiliary battery management unit (SBMU) and a fusion switch.
[0133] As an example, the central control module can serve as the battery management unit of the energy storage device 200, used to monitor and manage the energy storage device 200. The central control module can monitor information such as the current, voltage, power, state of charge, or temperature of the energy storage device 200. For example, it can control the charging and discharging current and voltage of the energy storage device 200. As an example, the central control module includes modules such as an insulation monitoring module (IMM), a master battery management unit (MBMU), an Ethernet (ETH) module, and a fiber optic conversion module.
[0134] As an example, a fire protection system includes control panels, detectors, alarm devices, etc., used to detect, alarm, or extinguish fires in energy storage systems.
[0135] As an example, the power distribution unit can be used to distribute power to the power modules of the energy storage device 200.
[0136] In some embodiments, the main body component includes at least one of the following: main control box of electrical cabinet, sheet metal of electrical control box, sheet metal of radiator exterior, internal metal wiring, high-voltage transmission line and compressor.
[0137] Example
[0138] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where the technology or conditions are not specified in the embodiments, they are performed according to the technology or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0139] The following are exemplary descriptions of some of the raw materials used in the embodiments and comparative examples:
[0140] Organosilicon-modified waterborne hydroxyl-type acrylic dispersion: solid content 50-55%, number average molecular weight 50,000-100,000, hydroxyl content (as a percentage of resin content) 3%-5%, silicon content (as a percentage of resin content) 0.2%-0.4%, denoted as resin 1;
[0141] Organosilicon-modified waterborne epoxy resin dispersion: solid content 55%-60%, number average molecular weight 60,000-110,000, silicon mass content (as a percentage of resin content) 0.3%-0.5%, epoxy resin type is bisphenol A, epoxy value 0.2-0.4 mol / 100g, denoted as resin 2;
[0142] Aqueous hydroxyl-type acrylic dispersion: solid content 50%-60%, number average molecular weight 50,000-100,000, hydroxyl mass content (as a percentage of resin content) 2.5%-3.5%, denoted as resin 1-1;
[0143] Thermosensitive color-changing pigments: Thermosensitive color-changing capsule 1: The color-changing substance is spiro[1,3,3-trimethylindole-(8-methoxysilanebenzodihydropyran)], and the outer shell is an organosilicon hybrid polyurethane (number average molecular weight 200,000-300,000, silicon mass content 0.25%-0.45%); Thermosensitive color-changing capsule 2: The color-changing substance is spiro[1,3,3-trimethylindole-(8-methoxysilanebenzodihydropyran)], and the outer shell is an organosilicon hybrid epoxy resin (number average molecular weight 180,000-250,000, epoxy resin type is bisphenol A, silicon mass content 0.1%-0.3%); Thermosensitive color-changing capsule 3: The color-changing substance is N,N'-bis(3-hydroxysalicylyl)-1,2-phenylenediamine, and the outer shell is an organosilicon hybrid polyurethane (number average molecular weight 200,000-300,000, silicon mass content 0.15%-0.35%).
[0144] Dispersant: Ammonium polyacrylate, solid content 30%-40%, number average molecular weight 3000-6000;
[0145] Wetting agent: Polyether-modified polydimethylsiloxane, molecular weight 30,000-50,000, solid content 99.5%;
[0146] Fillers: mica powder, 1500-2000 mesh; calcium carbonate, 2000-2500 mesh; kaolin, 1500-2000 mesh;
[0147] Leveling agent: Polyether-modified polysiloxane, number average molecular weight 10,000-30,000, solid content 99.5%;
[0148] Defoamer: Polyether-modified polydimethylsiloxane, molecular weight 10,000-30,000, solid content 99.5%;
[0149] Thickener: Associative alkali-swellable polyacrylate, molecular weight 50,000-100,000, solid content 25%-35%;
[0150] Film-forming agents: Dodecyl alcohol ester, 99.5% solid content; hexadecyl alcohol ester, 99.5% solid content, commercially available; tetradecyl alcohol ester, 99.5% solid content, purchased from Eastman.
[0151] pH adjuster: 2-amino-2-methyl-1-propanol, AMP-95, solid content 95%;
[0152] Curing agent: Hexamethylene diisocyanate-based polyisocyanate (i.e., HDI trimer), solid content 99.5%;
[0153] Diluent: Propylene glycol methyl ether acetate, solid content 99.5%.
[0154] Example of preparation of energy storage cabinet with thermochromic coating
[0155] 1) Preparation of thermochromic coatings:
[0156] The formulations of the thermochromic coatings used in the examples and comparative examples are shown in Tables 1-2, and the preparation methods are as follows:
[0157] Component A: Pour water into a disperser, and add wetting agent, dispersant, and half of the defoamer in sequence while stirring at low speed (350 rpm) for 2 minutes; then add thermosensitive color-changing pigment and filler in sequence at 1200 rpm and stir for 15 minutes; after that, add film-forming aid, pH adjuster, leveling agent, thickener, resin dispersion, and the remaining half of the defoamer at 650 rpm and stir for 15 minutes to obtain Component A;
[0158] Component B: Pour the curing agent into a disperser, add the diluent while stirring at low speed (350 r / min), and stop stirring after 4 minutes to obtain component B.
[0159] 2) Spray coating
[0160] The molar ratio of hydroxyl groups in the matrix resin in component A to isocyanate groups in the curing agent in component B is 1:1.4. Components A and B of the thermochromic coatings of each example and comparative example are mixed and stirred evenly at a speed of 350 r / min. The mixture is then sprayed onto the energy storage cabinet and cured and dried at room temperature (25°C) for 2 days to obtain a sample with a thermochromic coating (200 μm) on the surface.
[0161] The color development of the sample in Example 1 as a function of temperature is shown in the figure. Figure 3 As can be seen, the color of the coating changed significantly from 25℃ to 75℃, gradually changing from dark red to light pink.
[0162] Comparative Example 1
[0163] Except for replacing the silicone-modified waterborne hydroxyl acrylic dispersion (resin 1) with waterborne hydroxyl acrylic dispersion (resin 1), the rest is the same as in Example 11.
[0164] Comparative Example 2
[0165] Except for replacing the silicone-modified waterborne hydroxyl acrylic dispersion (resin 1) with waterborne hydroxyl acrylic dispersion (resin 1), the rest is the same as in Example 1.
[0166] The testing procedures for the relevant parameters of the coatings in the examples and comparative examples are as follows:
[0167] 1. Paint film color
[0168] Visual inspection and comparison with the standard color chart are shown in the figure. The color development results of Example 1 at different temperatures are as follows. Figure 2 .
[0169] 2. Adhesion test
[0170] The test was conducted according to GB / T 9286-1998, "Cross-cut Test for Paint and Varnish Films," with results graded from 0 to 5. Grade 0 indicates a completely smooth cut edge with no peeling. Grade 1 indicates minor coating peeling at the cut intersections, but the affected cross-cut area cannot be significantly greater than 5%. Grade 2 indicates coating peeling at the cut intersections and / or along the cut edges, with the affected cross-cut area significantly greater than 5%, but not significantly greater than 15%. Grade 3 indicates partial or complete coating peeling along the cut edge in large fragments, and / or partial or complete peeling at different locations on the grid, with the affected cross-cut area significantly greater than 15%, but not significantly greater than 35%. Grade 4 indicates large fragment peeling along the cut edge, and / or partial or complete peeling of some squares, with the affected cross-cut area significantly greater than 35%, but not significantly greater than 65%. Grade 5 indicates peeling exceeding Grade 4. Higher grades indicate weaker adhesion.
[0171] 3. Flexibility test
[0172] Referring to GB / T6742-2007 Paint and Varnish Bending Test (Cylindrical Shaft), a Φ2mm cylindrical shaft was used for the test. The screw handle was lifted at a constant speed within 1-2 seconds to rotate it 180°.
[0173] 4. Insulation resistance and withstand voltage test
[0174] Test conditions: Hold DC 5000V for 60 seconds, repeat 25 times, to test insulation resistance and contact leakage current.
[0175] 5. Volume resistivity and dielectric strength testing
[0176] The test was conducted in accordance with GB / T 1410-2006 Test Methods for Volume Resistivity and Surface Resistivity of Materials.
[0177] Volume resistivity: The sample is a sheet with a size of 2cm×2cm×1mm. It is placed on the testing equipment with a voltage of 1000V. The corresponding value is measured according to the corresponding volume resistivity calculation formula and then calculated.
[0178] Dielectric strength: The sample is a sheet with dimensions of 2cm×2cm×1mm. After connecting the positive and negative electrodes, the voltage rises at a rate of 10V / min until the sample is broken down and the equipment stops running. The dielectric strength is the ratio of the corresponding voltage value to the thickness.
[0179] 6. Salt spray resistance test:
[0180] The test was conducted in accordance with GB / T 1771-2007 Determination of resistance to neutral salt spray in paints and varnishes, with a test duration of 720 hours.
[0181] The sodium chloride concentration was (50±5) g / L, and the pH value was 6.5-7.2;
[0182] 7. Artificial accelerated aging test:
[0183] The test was conducted according to GB / T 1865-2009 Artificial Climate Aging and Artificial Radiation Exposure to Filtered Xenon Arc Radiation for Paints and Varnishes, with a test duration of 800 hours. The wavelength was 320-360 nm, and the irradiance was 60 W / m². 2 .
[0184] The test results of the examples and comparative examples are shown in Tables 1-2.
[0185] Table 1 Formulations for Examples 1-10
[0186]
[0187] Table 2 Formulation of the Example (Total amount of component A is 100 parts)
[0188]
[0189] As can be seen from Table 1-2, Examples 1-11 have good comprehensive performance, which can meet the requirements of corrosion prevention and durability, and have temperature-sensitive color-changing characteristics, which facilitates the monitoring and intuitive warning of temperature changes. In particular, Examples 1-9 use a combination of silicone organic resin and polyester compounds, which simultaneously achieves excellent insulation, corrosion prevention and durability.
[0190] Comparing Example 10 and Comparative Example 1, it can be seen that the use of silicone-containing organic resin (organosilicon-modified waterborne hydroxy acrylic resin) has significantly improved insulation, corrosion resistance and durability compared to silicone-free organic resin (waterborne hydroxy acrylic resin).
[0191] Comparing Example 1 and Examples 10-11, it can be seen that using polyester compounds as film-forming aids has significantly improved insulation and corrosion resistance compared to using non-polyester compounds as film-forming agents.
[0192] Comparing Examples 1, 10, and 1-2, it can be seen that the combined use of silicone-containing organic resins and polyester compounds can achieve synergistic effects and simultaneously obtain excellent insulation, corrosion resistance, and durability.
[0193] The description of the various embodiments above tends to emphasize the differences between the various embodiments. The similarities or similarities between them can be referred to, and for the sake of brevity, they will not be repeated here.
[0194] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. An energy storage device, characterized in that, It includes a body component and a thermochromic coating disposed on the outer surface of the body component; the thermochromic coating includes an adhesive matrix and a thermochromic pigment; the adhesive matrix includes a silicone-containing organic resin.
2. The energy storage device as described in claim 1, characterized in that, The silicon-containing organic resin includes at least one of hydroxyl-containing silicon-containing organic resin and silicone-modified epoxy resin; optionally, the hydroxyl-containing silicon-containing organic resin includes silicone-modified hydroxyl-type acrylic resin.
3. The energy storage device as described in claim 1, characterized in that, The silicon-containing organic resin is a water-based silicon-containing organic resin; optionally, the water-based silicon-containing organic resin includes at least one of silicone-modified water-based hydroxyl-type acrylic resin and silicone-modified water-based epoxy resin.
4. The energy storage device according to any one of claims 1-3, characterized in that, The adhesive matrix comprises polyester compounds.
5. The energy storage device as described in claim 4, characterized in that, The polyester compounds include C10-C20 polyester compounds, and optionally, the polyester compounds include at least one of alcohol ester twelve, alcohol ester fourteen, and alcohol ester sixteen.
6. The energy storage device according to any one of claims 1-5, characterized in that, The thermosensitive color-changing pigment has a capsule structure.
7. The energy storage device as described in claim 6, characterized in that, The outer shell of the capsule structure is made of at least one of silicone hybrid polyurethane and silicone hybrid epoxy resin.
8. The energy storage device as described in claim 6 or 7, characterized in that, The color-changing substances in the capsule structure include electron-transfer type organic compounds.
9. The energy storage device as described in claim 8, characterized in that, The electron-transfer type organic compound includes at least one of phenylenediamine compounds, triarylmethane phthalides, indoline phthalides, fluorane compounds, triphenylmethane compounds, spiropyran compounds, spirocyclic compounds, dianthrone compounds, and α-naphthoquinone derivatives; optionally, at least one of spiropyran compounds and phenylenediamine compounds.
10. The energy storage device as described in claim 9, characterized in that, The spiropyran compounds include organosilicon-modified spiropyran compounds, optionally spiro[1,3,3-trimethylindole-(8-methoxysilanebenzodihydropyran)]; the phenylenediamine compounds include N,N'-bis(3-hydroxysalicylyl)-1,2-phenylenediamine.
11. The energy storage device according to any one of claims 1-10, characterized in that, The adhesive matrix further includes additives; the additives include at least one of wetting agents, dispersants, fillers, leveling agents, defoamers, pH adjusters, and thickeners; Optionally, the wetting agent includes at least one of acetylenic diol wetting agents, hydrophobically modified acrylate wetting agents, and polyether modified polysiloxane wetting agents; Optionally, the dispersant includes at least one of polyphosphate, sodium polyacrylate, and ammonium polyacrylate; Optionally, the filler includes at least one of mica powder, calcium carbonate, and kaolin. Optionally, the leveling agent includes at least one of polyether-modified silicone leveling agents, acrylate leveling agents, and fluorocarbon-modified acrylate leveling agents; Optionally, the defoamer includes at least one of mineral oil-based defoamers and silicone-based defoamers; Optionally, the pH adjuster includes at least one of 2-amino-2-methyl-1-propanol and ammonia water; Optionally, the thickener includes at least one of associative polyacrylate, non-associative polyacrylate, and hydrophobically modified associative polyurethane.
12. A method for preparing an energy storage device, characterized in that, The preparation method includes the following steps: The energy storage device is prepared by curing the thermo-color-sensitive coating onto the surface of the main component of the energy storage device to form a thermo-color-sensitive coating. The thermochromic coating comprises a binder matrix and a thermochromic pigment; the resin of the binder matrix comprises a silicone-containing organic resin.
13. The preparation method according to claim 12, characterized in that, The thermosensitive color-changing coating includes single-component coatings and / or two-component coatings.
14. The energy storage device as described in claim 11 or 12, characterized in that, The thermochromic coating is a two-component coating, wherein component A includes resin, thermochromic pigment and film-forming aid; and component B includes curing agent.
15. The energy storage device as described in claim 14, characterized in that, The curing agent includes isocyanate-based curing agents; optionally, it includes hexamethylene diisocyanate-based polyisocyanate.
16. The energy storage device as described in claim 14 or 15, characterized in that, The molar ratio of the hydroxyl groups of the matrix resin in component A to the isocyanate groups of the curing agent in component B is 1:1.3-1:1.
5.
17. The energy storage device according to any one of claims 14-16, characterized in that, Component A comprises, by weight, 50-70 parts of resin, 10-20 parts of thermosensitive color-changing pigment, and 2.5-3.5 parts of film-forming aid.
18. An energy storage system, characterized in that, Includes the energy storage device and other devices as described in any one of claims 1-16.
19. A thermosensitive color-changing coating, characterized in that, It includes a binder matrix and a thermosensitive color-changing pigment; the resin of the binder matrix includes a silicone-containing organic resin.