A method for preparing a composite microcapsule smart protective coating with self-healing, self-early warning and wave absorption functions.

By constructing a multi-layered composite microcapsule structure, the problem of damage identification and repair of existing microwave absorbing protective coatings in service environments has been solved. This enables visualized early warning and autonomous repair of damage locations, improving electromagnetic protection and corrosion resistance. It is suitable for metal structure protection in aerospace, shipbuilding, and electronic equipment.

CN123107437APending Publication Date: 2026-11-17SOUTHWEST JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611448563.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing electromagnetic wave absorbing protective coatings cannot achieve visual early warning of damage location and autonomous repair after being damaged in complex service environments, and it is difficult to simultaneously meet the multi-functional protection requirements of electromagnetic wave absorption, corrosion resistance and damage self-sensing.

Method used

A multi-layered composite microcapsule structure is adopted, in which the repair agent isophorone diisocyanate (IPDI) and the early warning agent crystal violet lactone (CVL) are encapsulated in a polyurethane (PU) shell. The stability is enhanced by a polydopamine (PDA) interface layer, and a conductive functional layer of polyaniline (PANI) is constructed on the outer layer to achieve damage recognition and repair.

Benefits of technology

It enables rapid identification and autonomous repair of damaged locations, enhances electromagnetic protection and corrosion resistance, and possesses multi-functional synergistic effects, making it suitable for metal structure protection in aerospace, shipbuilding, and electronic equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107437A_ABST
    Figure CN123107437A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of intelligent protective coating technology and discloses a method for preparing a composite microcapsule intelligent protective coating with self-healing, self-early warning, and wave absorption functions. Addressing the technical problems of existing wave-absorbing protective coatings failing to achieve visual early warning and autonomous repair of damage locations in complex service environments, and struggling to simultaneously meet the multi-functional protection requirements of electromagnetic wave absorption, corrosion resistance, and damage self-sensing, this invention adopts the following technical solution: First, a repair agent and an early warning agent are emulsified at high speed and then reacted with isocyanate monomers and chain extenders to prepare polyurethane shell microcapsules; subsequently, a polydopamine interface layer is coated onto the surface of the microcapsules through dopamine self-polymerization; then, a polyaniline functional layer is formed through in-situ oxidative polymerization of aniline monomers to obtain composite microcapsules; finally, the obtained composite microcapsules are dispersed and mixed uniformly with a coating matrix resin and a curing agent, then coated onto the substrate surface and cured to form a protective coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of microwave absorbing coatings and provides a method for preparing a composite microcapsule intelligent protective coating with self-healing, self-early warning and microwave absorbing functions. Background Technology

[0002] With the development of aerospace, naval equipment, and electronic devices, electromagnetic interference and metal structure corrosion problems in complex service environments are becoming increasingly prominent. Electromagnetic absorbing coatings, due to their ability to attenuate electromagnetic waves and protect the substrate, have significant application value in the field of equipment protection.

[0003] However, existing electromagnetic shielding coatings are susceptible to damage from mechanical shocks and environmental corrosion during long-term service, resulting in localized damage such as cracks and scratches. On the one hand, the damaged areas disrupt the continuous electromagnetic loss structure within the coating, leading to a decrease in electromagnetic protection performance; on the other hand, corrosive media can penetrate the substrate through the defective areas, causing further corrosion failure.

[0004] In recent years, microcapsule self-healing technology has provided a new solution for active protection after coating damage. It repairs damaged areas by encapsulating repair agents and utilizing a crack-triggered release mechanism. However, existing microcapsule repair systems typically only focus on crack filling and structural restoration, making it difficult to quickly identify the damage location. Furthermore, directly introducing microwave-absorbing functional layers into self-healing microcapsule systems can easily lead to problems such as insufficient interfacial bonding between the functional layer and the flexible encapsulation structure, and decreased stability.

[0005] Therefore, there is an urgent need to develop a novel intelligent protective coating structure that can achieve synergistic effects of packaging stability, electromagnetic absorption, damage identification, and active repair. Summary of the Invention

[0006] The purpose of this invention is to solve the technical problems that existing electromagnetic absorbing protective coatings cannot achieve visual early warning and autonomous repair of damage location after being damaged in complex service environments, and it is difficult to simultaneously meet the multi-functional protection requirements such as electromagnetic wave absorption, corrosion resistance and damage self-sensing.

[0007] To achieve the above objectives, the present invention employs the following technical means:

[0008] This invention provides a method for preparing a composite microcapsule intelligent protective coating with self-healing, self-early warning, and wave-absorbing functions, comprising the following steps:

[0009] Step (1) Preparation of polyurethane shell microcapsules: Dissolve emulsifier in water to form an aqueous phase; mix repair agent, early warning agent and organic solvent to form an oil phase; add the oil phase to the aqueous phase for high-speed emulsification to form an oil-in-water emulsion; add isocyanate monomer and chain extender to the oil-in-water emulsion, stir and react at 300-800 rpm at 60-80℃ for 2-5 hours, centrifuge and wash to obtain polyurethane shell microcapsules;

[0010] Step (2) Polydopamine interface layer coating: Disperse the polyurethane shell microcapsules obtained in step (1) in water, adjust the pH of the system to 8-10, add dopamine hydrochloride, and react at 20-35℃ for 8-16 h to allow dopamine to self-polymerize on the surface of the microcapsules. After centrifugation and washing, polydopamine-coated microcapsules are obtained.

[0011] Step (3) Polyaniline functional layer coating: The polydopamine-coated microcapsules obtained in step (2) are dispersed in a doped acid aqueous solution, aniline monomer is added, and the mixture is stirred and protonated at 0~5℃ for 1~4 h; then an oxidant of the same molar amount as the aniline monomer is added, and the mixture is reacted at 0~5℃ for 12~20 h. After centrifugation and washing, polyaniline / polydopamine / polyurethane composite microcapsules are obtained.

[0012] Step (4) Coating preparation: The composite microcapsules obtained in step (3) are dispersed in a solvent, mixed with the coating matrix resin and curing agent, degassed and coated on the surface of the substrate, and cured at 20~30℃ for 5~10 days to obtain the composite microcapsule protective coating.

[0013] In the above scheme, in step (1), the repair agent is isophorone diisocyanate, the warning agent is crystal violet lactone, and the organic solvent is phenyl acetate; the mass ratio of the repair agent to the organic solvent is 3:7; and the mass ratio of the repair agent to the warning agent is 3:1.

[0014] In the above scheme, in step (1), the emulsifier is gum arabic, and the mass ratio of the emulsifier to water is 1:10; the high-speed emulsification speed is 5000~8000 rpm, and the emulsification time is 5~15 min; the chain extender is 1,4-butanediol.

[0015] In the above scheme, in step (2), the mass ratio of the dopamine hydrochloride to the polyurethane shell microcapsules obtained in step (1) is 1:(10~30); the pH is adjusted by ammonia water; the temperature of the self-polymerization reaction is 22~28℃, and the reaction time is 10~14h.

[0016] In the above scheme, in step (3), the doping acid is camphor sulfonic acid, and the concentration of the aqueous solution of the doping acid is 0.05~0.2 mol / L;

[0017] The oxidant is ammonium persulfate;

[0018] The aniline monomer is protonated by stirring at 0-2°C for 2-4 h before being added to the oxidant;

[0019] The reaction temperature is 0~2℃, and the reaction time is 14~18 h.

[0020] In the above scheme, in step (4), the mass ratio of the coating matrix resin to the curing agent is 8:1 to 12:1;

[0021] The composite microcapsules are added to the coating matrix resin at an amount of 25-40 wt%.

[0022] In the above scheme, the isocyanate monomer in step (1) is diphenylmethane diisocyanate or toluene diisocyanate; the particle size of the polyurethane shell microcapsules in step (1) is 4~5μm.

[0023] The present invention also provides a composite microcapsule, which is prepared by steps (1) to (3) of the preparation method. The composite microcapsule comprises, from the inside to the outside, a functional core material containing a repair agent and a warning agent, a polyurethane shell, a polydopamine interface layer and a polyaniline functional layer.

[0024] The present invention also provides a composite microcapsule protective coating, which is prepared by the aforementioned preparation method, wherein the coating contains composite microcapsules uniformly dispersed in a resin matrix.

[0025] The above-mentioned solution describes the application of the composite microcapsule protective coating in electromagnetic and corrosion protection of metal structures in aerospace equipment, ship equipment, or electronic equipment.

[0026] Because the present invention employs the above-mentioned technical means, it has the following beneficial effects:

[0027] 1. Multifunctional composite structure design:

[0028] This invention achieves the integration of multiple functions, including wave absorption, corrosion protection, self-warning, and self-repair, by constructing a multi-layered composite microcapsule structure consisting of an IPDI / CVL functional core material, a polyurethane (PU) shell, a polydopamine (PDA) interface layer, and a polyaniline (PANI) functional layer, from the inside out. This structure avoids the problems of poor interfacial bonding and insufficient functional synergy caused by the simple stacking of different functional materials in traditional multifunctional coatings.

[0029] 2. Synergistic effect of damage warning and self-repair function:

[0030] This invention encapsulates isophorone diisocyanate (IPDI) repair agent and crystal violet lactone (CVL) early warning agent within a microcapsule. When the coating is subjected to mechanical damage and cracks are generated, the microcapsule can rupture due to crack propagation, releasing IPDI and causing a polymerization reaction to achieve autonomous repair of the cracked area. At the same time, the release of CVL generates a visual response, enabling rapid identification of early damage locations and improving the active protection capability of the coating during service.

[0031] 3. Improved stability of microcapsule structure:

[0032] This invention utilizes polydopamine (PDA) as an interface control layer between the PU shell and the PANI functional layer. Its excellent adhesion properties enhance the bonding stability between different layers, while improving the surface functionalization capability of microcapsules. This provides a stable carrier for subsequent in-situ polymerization of polyaniline, thereby improving the structural integrity and environmental stability of the composite microcapsules.

[0033] 4. Enhanced electromagnetic wave absorption performance:

[0034] This invention enables the composite microcapsules to absorb electromagnetic waves by constructing a polyaniline (PANI) conductive functional layer on the outer layer of the microcapsules. The PANI conductive network can attenuate electromagnetic wave energy through mechanisms such as dielectric loss and interfacial polarization loss, thereby improving the electromagnetic protection performance of the coating.

[0035] 5. Improved performance of intelligent protective coating applications:

[0036] The preparation method of this invention is simple and the process conditions are mild. The resulting composite microcapsules can be uniformly dispersed in a resin matrix to form an intelligent protective coating. When damaged, this coating can achieve damage recognition, active repair, and continuous electromagnetic protection. It can be applied to corrosion protection and electromagnetic protection of metal structures in aerospace, naval equipment, electronic equipment, and other complex service environments. Attached Figure Description

[0037] Figure 1 SEM image of the microcapsules;

[0038] Figure 2 RL diagram of microcapsules;

[0039] Figure 3 SEM images of the coating before and after damage;

[0040] Figure 4 LSCM image after coating damage. Detailed Implementation

[0041] The embodiments of the present invention will be described in detail below. Although the present invention will be described and illustrated in conjunction with some specific embodiments, it should be noted that the present invention is not limited to these embodiments. On the contrary, any modifications or equivalent substitutions made to the present invention should be covered within the scope of the claims of the present invention.

[0042] Furthermore, to better illustrate the present invention, numerous specific details are set forth in the following detailed embodiments. Those skilled in the art will understand that the present invention can be practiced without these specific details.

[0043] This invention belongs to the field of intelligent protective coating technology, and discloses a self-healing, self-early warning and wave-absorbing composite microcapsule intelligent protective coating based on gradient interface regulation and its preparation method.

[0044] To address the problems of existing microwave absorbing protective coatings, such as difficulty in detecting damage, inability to self-repair, and difficulty in synergizing multiple functions, this invention constructs a composite microcapsule with a gradient structure of "flexible encapsulation layer—interface regulation layer—electromagnetic loss layer". First, isophorone diisocyanate (IPDI) and crystal violet lactone (CVL) are co-encapsulated in a polyurethane (PU) shell. Then, an interface regulation layer is constructed using polydopamine (PDA), and polyaniline (PANI) is induced to grow in situ to form a conductive functional layer.

[0045] This gradient structure achieves a synergistic effect of stable storage of functional core materials, enhanced interfacial bonding, and electromagnetic loss regulation. When the coating is damaged, the microcapsules rupture to release IPDI and CVL, respectively enabling crack repair and visual early warning of damage. The intelligent protective coating prepared by this invention has the functions of wave absorption, corrosion prevention, self-early warning, and self-repair, and can be applied to the protection of metal structures in complex environments such as aerospace, ships, and electronic equipment.

[0046] I. Overall Structure of Composite Microcapsule Intelligent Protective Coating

[0047] This embodiment provides a composite microcapsule intelligent protective coating with self-healing, self-warning, and wave-absorbing functions. The composite microcapsule, from the inside out, comprises a repair / warning functional core material, a polyurethane (PU) shell, a polydopamine (PDA) interface layer, and a polyaniline (PANi) functional layer. The repair / warning functional core material contains the repair agent isophorone diisocyanate (IPDI) and the warning agent crystal violet lactone (CVL). The polyurethane shell encapsulates the functional core material and ruptures to release it when the coating is damaged. The PDA interface layer enhances the interfacial bonding stability between the polyurethane shell and the polyaniline functional layer and provides a stable carrier for the in-situ polymerization of polyaniline. The polyaniline functional layer endows the composite microcapsule with electromagnetic wave absorption capabilities.

[0048] II. Preparation of Composite Microcapsules and Protective Coatings

[0049] Step 1: Preparation of PU@IPDI / CVL microcapsules

[0050] Add 5 g of gum arabic (GA) to 50 mL of deionized water and stir at 600 rpm / min until the solution is clear, forming an aqueous phase.

[0051] 1 g of crystal violet lactone (CVL) was added to 7 g of phenyl acetate (PA) and sonicated for 10 min to dissolve it completely. Then, 5 g of isocyanate monomer and 3 g of repair agent isophorone diisocyanate (IPDI) were added and mixed evenly to form an oily solution, which was used as the oil phase.

[0052] The oil phase was slowly added dropwise to the aqueous solution, and emulsified at a high speed of 6000 rpm / min for 8 min to form a stable oil-in-water (O / W) emulsion.

[0053] Subsequently, a chain extender solution of 1,4-butanediol (BDO) was slowly added dropwise to the oil-in-water emulsion, and the temperature was raised to 70°C. The mixture was stirred at 500 rpm / min for 3.5 h to allow the isocyanate monomer and the chain extender to undergo interfacial polymerization at the oil droplet interface, forming a polyurethane shell.

[0054] After the reaction was completed, the microcapsule product was recovered from the suspension by centrifugation. The obtained product was washed three times with deionized water by centrifugation to remove residual emulsifier and unreacted monomers, thus obtaining PU@IPDI / CVL microcapsules.

[0055] Step 2: Preparation of PDA / PU@IPDI / CVL microcapsules

[0056] Disperse the PU@IPDI / CVL microcapsules obtained in step 1 into 100 mL of deionized water, and slowly add ammonia to adjust the pH of the system to 8-9.

[0057] Add 0.5 g of dopamine hydrochloride to 20 mL of deionized water and stir until completely dissolved.

[0058] The dopamine hydrochloride solution was slowly added to the microcapsule dispersion and reacted continuously at 25°C for 12 hours, so that dopamine under alkaline conditions underwent oxidative self-polymerization on the surface of the microcapsules to form a polydopamine (PDA) interface layer.

[0059] After the reaction was completed, the microcapsule product was recovered from the suspension by centrifugation. The obtained product was washed three times with deionized water by centrifugation to obtain PDA / PU@IPDI / CVL microcapsules.

[0060] Step 3: Preparation of PANi / PDA / PU@IPDI / CVL microcapsules

[0061] To prepare an aqueous solution of camphor sulfonic acid (CSA) doped with camphor sulfonic acid: Take 360 ​​mL of deionized water, add camphor sulfonic acid to make the concentration reach 0.1 mol / L, and the total system volume is 400 mL. Stir until completely dissolved.

[0062] The PDA / PU@IPDI / CVL microcapsules obtained in step 2 were added to the camphor sulfonic acid solution and stirred for 1 h to allow the microcapsules to be fully dispersed and adsorb the doped acid.

[0063] Add 5 mL of aniline (ANi) monomer to the above system and stir continuously for 3 h at a low temperature of 0~2℃ to allow the aniline monomer to be fully protonated in an acidic environment.

[0064] Take another 40 mL of deionized water, add ammonium persulfate (APS) powder in an equimolar ratio with aniline, stir at low temperature and pre-cool for 30 min to obtain an oxidant solution.

[0065] Under low temperature conditions of 0~2℃, the ammonium persulfate solution is added dropwise to the aniline protonation solution to initiate the in-situ oxidative polymerization reaction of aniline. The reaction is carried out at low temperature for 16 h, so that polyaniline is deposited and grown on the surface of microcapsules to form a PANi functional layer.

[0066] After the reaction was completed, the microcapsule product was recovered from the suspension by centrifugation. The obtained product was washed three times with deionized water by centrifugation to remove residual oxidant and unreacted monomers, thus obtaining PANi / PDA / PU@IPDI / CVL composite microcapsules.

[0067] Step 4: Preparation of composite microcapsule intelligent protective coating

[0068] The PANi / PDA / PU@IPDI / CVL composite microcapsules obtained in step 3 were dispersed in an appropriate amount of solvent, thoroughly mixed with the coating matrix resin, and then a curing agent was added. The mass ratio of the resin to the curing agent was 10:1. The mixture was then degassed to remove air bubbles.

[0069] The degassed coating is uniformly applied to the surface of the substrate and cured at room temperature for 7 days to obtain the composite microcapsule intelligent protective coating.

[0070] III. Performance Characterization of Composite Microcapsules and Coatings

[0071] (I) Morphological characterization of composite microcapsules

[0072] like Figure 1The image shows a scanning electron microscope (SEM) image of the prepared composite microcapsules. As can be seen from the figure, the composite microcapsules exhibit a regular spherical structure with a particle size of approximately 4–5 μm, indicating that the emulsification polymerization process in this embodiment can form a stable microcapsule structure. Furthermore, the microcapsule surface exhibits a distinctly rough morphology, accompanied by granular protrusions. This is mainly attributed to the formation of the PDA interface layer and the deposition of conductive polymers on the microcapsule surface during the in-situ polymerization of PANi. This rough surface structure not only demonstrates the successful construction of each functional layer but also enhances the interfacial bonding between the microcapsules and the resin matrix, improving the overall stability of the coating.

[0073] (II) Coating Absorption Performance Test

[0074] like Figure 2 The results show the microwave absorption performance of the coatings with different amounts of composite microcapsules, characterized by reflection loss (RL) values. Under the same coating thickness (3.3 mm), the reflection loss gradually decreased as the amount of composite microcapsules increased from 25 wt% to 40 wt%, indicating that the introduction of composite microcapsules effectively enhances the coating's attenuation capability for electromagnetic waves. When the amount of composite microcapsules was 40 wt%, the coating achieved the lowest reflection loss value of −51 dB at 10.2 GHz, demonstrating excellent electromagnetic wave absorption performance.

[0075] The main reason for the enhanced microwave absorption performance mentioned above is that as the microcapsule content increases, the content of the polyaniline functional layer in the coating also increases accordingly. This enhances the conductive loss and interfacial polarization effect, allowing more incident electromagnetic wave energy to be converted into heat energy for dissipation, thereby improving the microwave absorption performance of the coating. Simultaneously, the multi-layered shell structure (PU / PDA / PANi) of the composite microcapsules provides abundant heterogeneous interfaces, enhancing interfacial polarization loss and further promoting the attenuation of electromagnetic wave energy.

[0076] (III) Verification of Coating Self-Healing Performance

[0077] like Figure 3 As shown, this is a comparison of the surface morphology of the composite microcapsule coating before and after damage. Figure 3 (a) is a SEM image of the coating after mechanical scratching, showing obvious cracks on the coating surface, which have destroyed the continuous protective structure of the coating. After a certain period of self-healing, as... Figure 3 As shown in (b), the original crack area is significantly reduced, the crack width is significantly reduced, and the crack interior shows signs of filling.

[0078] The above results indicate that mechanical damage causes the microcapsules in the cracked area to rupture, releasing the internally encapsulated IPDI repair agent into the cracked area. The IPDI reacts with moisture in the environment and polymerizes, forming a new polymer network that effectively fills the damaged area, achieving self-repair of the coating cracks. These results demonstrate that the prepared composite microcapsule coating exhibits excellent damage response and self-healing capabilities.

[0079] (iv) Verification of self-early warning performance of coating damage

[0080] To verify the damage warning performance of the composite microcapsule coating, the coating was observed under ultraviolet light excitation after mechanical damage. Figure 4 As shown, under ultraviolet light irradiation (laser scanning confocal microscope, LSCM observation), the cracked area showed obvious blue fluorescence signal, while no obvious fluorescence response was observed in the undamaged area.

[0081] The above results indicate that during mechanical damage, crack propagation leads to microcapsule rupture, releasing the encapsulated CVL warning component along with the repair agent into the damaged area. This component generates a fluorescence response under ultraviolet light excitation, enabling rapid and visual identification of the coating damage location. These results demonstrate that the prepared composite microcapsule coating possesses excellent damage response and self-warning capabilities, providing intuitive visual signals for timely maintenance and proactive protection of the coating.

Claims

1. A method for preparing a composite microcapsule intelligent protective coating with self-healing, self-early warning, and wave-absorbing functions, characterized in that, Includes the following steps: Step (1) Preparation of polyurethane shell microcapsules: Emulsifier gum arabic is dissolved in water to form an aqueous phase; repair agent, early warning agent and organic solvent are mixed to form an oil phase; the oil phase is added to the aqueous phase for high-speed emulsification to form an oil-in-water emulsion; isocyanate monomer and chain extender are added to the oil-in-water emulsion, and the mixture is stirred at 300-800 rpm at 60-80℃ for 2-5 h. After centrifugation and washing, polyurethane shell microcapsules are obtained. Step (2) Polydopamine interface layer coating: Disperse the polyurethane shell microcapsules obtained in step (1) in water, adjust the pH of the system to 8-10, add dopamine hydrochloride, and react at 20-35℃ for 8-16 h to allow dopamine to self-polymerize on the surface of the microcapsules. After centrifugation and washing, polydopamine-coated microcapsules are obtained. Step (3) Polyaniline functional layer coating: The polydopamine-coated microcapsules obtained in step (2) are dispersed in a doped acid aqueous solution, aniline monomer is added, and the mixture is stirred and protonated at 0~5℃ for 1~4 h; then an oxidant of the same molar amount as the aniline monomer is added, and the mixture is reacted at 0~5℃ for 12~20 h. After centrifugation and washing, polyaniline / polydopamine / polyurethane composite microcapsules are obtained. Step (4) Coating preparation: The composite microcapsules obtained in step (3) are dispersed in a solvent, mixed with the coating matrix resin and curing agent, degassed and coated on the surface of the substrate, and cured at 20~30℃ for 5~10 days to obtain the composite microcapsule protective coating.

2. The preparation method according to claim 1, characterized in that, In step (1), the repair agent is isophorone diisocyanate, the warning agent is crystal violet lactone, and the organic solvent is phenyl acetate; the mass ratio of the repair agent to the organic solvent is 3:7; and the mass ratio of the repair agent to the warning agent is 3:

1.

3. The preparation method according to claim 1, characterized in that, In step (1), the emulsifier is gum arabic, and the mass ratio of the emulsifier to water is 1:10; the high-speed emulsification speed is 5000~8000 rpm, and the emulsification time is 5~10 min; the chain extender is 1,4-butanediol.

4. The preparation method according to claim 1, characterized in that, In step (2), the mass ratio of the dopamine hydrochloride to the polyurethane shell microcapsules obtained in step (1) is 1:(10~30); the pH is adjusted using ammonia water; the temperature of the self-polymerization reaction is 22~28℃, and the reaction time is 10~12 h.

5. The preparation method according to claim 1, characterized in that, In step (3), the doping acid is camphor sulfonic acid, and the concentration of the aqueous solution of the doping acid is 0.05~0.2 mol / L; The oxidant is ammonium persulfate; The aniline monomer is protonated by stirring at 0-2°C for 2-4 h before being added to the oxidant; The reaction temperature is 0~2℃, and the reaction time is 14~18 h.

6. The preparation method according to claim 1, characterized in that, In step (4), the mass ratio of the coating matrix resin to the curing agent is 8:1 to 12:1; The composite microcapsules are added to the coating matrix resin at an amount of 25-40 wt%.

7. The preparation method according to any one of claims 1-6, characterized in that, The isocyanate monomer in step (1) is diphenylmethane diisocyanate or toluene diisocyanate; the particle size of the polyurethane shell microcapsules in step (1) is 4~5μm.

8. A composite microcapsule, characterized in that, The composite microcapsule is prepared by steps (1) to (3) of the preparation method according to any one of claims 1 to 7, and comprises, from the inside out: a functional core material containing a repair agent and an early warning agent, a polyurethane shell, a polydopamine interface layer, and a polyaniline functional layer.

9. A composite microcapsule protective coating, characterized in that, The coating is prepared by any one of claims 1 to 7, wherein the composite microcapsules of claim 8 are uniformly dispersed in the resin matrix.

10. The application of the composite microcapsule protective coating of claim 9 in electromagnetic and corrosion protection of metal structures of aerospace equipment, ship equipment, or electronic equipment.