A long-lasting anti-aging waterborne fluorocarbon waterproof coating and its preparation method
By introducing surface-modified double-shell microcapsules to encapsulate light stabilizers and antioxidants in waterborne fluorocarbon coatings, the problem of rapid aging and degradation of waterborne fluorocarbon coatings has been solved, achieving a long-lasting anti-aging effect.
Patent Information
- Application Number
- CN202611560857.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing waterborne fluorocarbon coatings age rapidly under long-term outdoor exposure, resulting in uneven protective effects. Traditional additives cannot adjust the protection according to the degree of aging, leading to a short effective period of protection.
The light stabilizer and antioxidant are encapsulated in surface-modified double-shell microcapsules, and the slow release is achieved through physical encapsulation. Combined with the design of the inner wall material and core material, the compatibility with the resin matrix is enhanced, and long-lasting anti-aging effect is achieved.
The prepared long-lasting anti-aging waterborne fluorocarbon waterproof coating showed no abnormalities such as loss of gloss, discoloration, or blistering after a 1000-hour aging test, maintained good adhesion, and significantly improved anti-aging ability.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention discloses a long-lasting anti-aging waterborne fluorocarbon waterproof coating and its preparation method, belonging to the field of waterproof coating technology. Background Technology
[0002] Waterborne fluorocarbon coatings are widely used for protection in long-term exposed environments such as building exteriors, metal roofs, and steel structures due to their excellent weather resistance, chemical resistance, and self-cleaning properties. However, under long-term outdoor exposure, aging and degradation of the coating are unavoidable, mainly manifested as decreased gloss, discoloration, chalking, and cracking, ultimately leading to the failure of waterproof and protective functions.
[0003] To address coating aging issues, existing technologies typically add various anti-aging additives to coatings, such as hindered amine light stabilizers, UV absorbers, and antioxidants. These additives can capture free radicals, absorb UV rays, and decompose hydrogen peroxide, thereby slowing down the coating aging process. However, small-molecule anti-aging additives have limited compatibility with the resin matrix and tend to migrate to the coating surface during long-term use, where they are washed away by rainwater or evaporated, leading to a rapid decline in protective effectiveness. Traditional additives are added directly to the coating and begin to be consumed upon exposure, making it impossible to adjust their effectiveness according to the degree of aging. This often results in excessive protection in the early stages and insufficient protection in the later stages, leading to a short period of effective protection.
[0004] Therefore, developing a long-lasting, anti-aging waterborne fluorocarbon waterproof coating has become a pressing technical problem to be solved in this field. Summary of the Invention
[0005] To address the aforementioned problems in the prior art, this invention provides a long-lasting anti-aging waterborne fluorocarbon waterproof coating and its preparation method. The waterborne fluorocarbon waterproof coating prepared by this invention achieves the objective of long-lasting anti-aging.
[0006] To achieve the above objectives, the following technical solution is adopted: A long-lasting, anti-aging water-based fluorocarbon waterproof coating, comprising the following raw materials by weight: 40-60 parts of waterborne fluorocarbon emulsion, 8-16 parts of surface-modified double-shell microcapsules, 10-14 parts of pigments and fillers, 15-20 parts of deionized water, 0.5-1.5 parts of dispersant, 0.8-1 part of defoamer, 1-3 parts of film-forming aid, and 0.5-1.2 parts of thickener.
[0007] The pigments and fillers are at least one of rutile titanium dioxide, sericite powder, and mica iron oxide.
[0008] The pigment and filler have a particle size of 5-20 μm.
[0009] The dispersant is at least one of hydrophobically modified polycarboxylate dispersant and sodium polyacrylate dispersant.
[0010] The hydrophobic modified polycarboxylate dispersant is SC-886 from Ausnutria Chemical (Beijing) Co., Ltd.
[0011] The sodium polyacrylate dispersant is RF-B5040 from Zhejiang Ruigao New Material Co., Ltd.
[0012] The defoamer is at least one of mineral oil defoamer and polyether-modified silicone defoamer.
[0013] The mineral oil defoamer is CK-6005 mineral oil defoamer from Tianjin Gaotian New Material Technology Co., Ltd.
[0014] The polyether-modified silicone defoamer mentioned above is THIX-299, a polyether-modified silicone defoamer from Yantai Hengxin Chemical Technology Co., Ltd.
[0015] The film-forming aid is 12-ol ester.
[0016] The thickener is at least one of nonionic polyurethane associative thickener and hydroxyethyl cellulose thickener.
[0017] The nonionic polyurethane associative thickener is Vesmody, a polyurethane associative thickener. ® U605.
[0018] The hydroxyethyl cellulose thickener is HECOCELL. ® HE400.
[0019] The aqueous fluorocarbon emulsion is a low surface energy hydroxyl fluorocarbon emulsion, with the grade HD-8666.
[0020] A long-lasting, anti-aging water-based fluorocarbon waterproof coating is prepared by the following steps: Step 1: Inner wall material cladding Polyvinyl alcohol was dissolved in deionized water by heating, and the core material was added dropwise. The mixture was then emulsified by high-speed shearing to obtain an emulsion. After pre-crosslinking of the emulsion, the reaction was maintained at this temperature for 2-3 hours to obtain an inner wall microcapsule emulsion.
[0021] The polyvinyl alcohol is PVA-1788.
[0022] The IPDI trimer has the following characteristics: the solvent is butyl acetate with a mass concentration of 70%, the NCO content is 12-15%, and the viscosity (23℃) is 600-1000 mPa·s.
[0023] The heating and dissolution process involves heating to 70-80℃ and stirring to dissolve the substances.
[0024] The shear emulsification process involves controlling the rotation speed at 2000-3000 r / min and the emulsification time at 15-30 min.
[0025] The core material is obtained by mixing dodecafluoroheptyl methacrylate, IPDI trimer, antioxidant 1010, and light stabilizer 944.
[0026] The pre-crosslinking process involves a crosslinking temperature of 40-50℃ and a crosslinking time of 0.5-1h.
[0027] The heat preservation reaction: the reaction temperature is 50-60℃.
[0028] In this step, the weight ratio of dodecyl fluoroheptyl methacrylate, antioxidant 1010, light stabilizer 944, polyvinyl alcohol, and IPDI trimer is as follows: dodecyl fluoroheptyl methacrylate 60-80 parts, antioxidant 1010 10-20 parts, light stabilizer 944 10-20 parts, polyvinyl alcohol 50-60 parts, and IPDI trimer 4-4.8 parts. The amount of deionized water used is 8-10 times the mass of polyvinyl alcohol.
[0029] Step 2: Modification of the outer wall material Urea and p-hydroxybenzaldehyde were added to water, and the pH of the system was adjusted to 7.5-8.0. This mixture was then added dropwise to the microcapsule emulsion on the inner wall, followed by the addition of formaldehyde solution. After adjusting the pH to acidity, the reaction was maintained at this temperature for 3-5 hours. The pH of the system was adjusted to neutral, and the solid was filtered and washed with ethanol to obtain the initial product of the double-shell microcapsules. The initial microcapsule product was dispersed in an ethanol-water solution, and perfluorobutylethyltrimethoxysilane was added under nitrogen protection. The pH was adjusted to 4.0-4.5 with acetic acid, and the reaction was maintained at this temperature for 3.5-5 hours. The solid was filtered and washed with ethanol and then vacuum dried to obtain surface-modified double-shell microcapsules.
[0030] The amount of water used is 4-6 times the amount of urine.
[0031] The formaldehyde solution has a mass concentration of 35-40%.
[0032] The pH adjustment involves using citric acid to adjust the system's pH to 3.5-4.5.
[0033] The heat preservation reaction: the reaction temperature is 55-65℃.
[0034] In this step, the weight ratio of urea, p-hydroxybenzaldehyde, and formaldehyde solution is: 55-65 parts urea, 2-3 parts p-hydroxybenzaldehyde, and 108-120 parts formaldehyde solution.
[0035] The volume fraction of the ethanol-water solution is 60-70%, and the amount used is 3.5-5 times the initial mass of the microcapsules.
[0036] The amount of perfluorobutyl ethyltrimethoxysilane used is 2-3% of the initial mass of the double-shell microcapsules.
[0037] The vacuum drying process involves controlling the temperature at 40-50℃, the vacuum level at <-0.06MPa, and the drying time at 12-15h.
[0038] Step 3, Compound Mixing A long-lasting anti-aging waterborne fluorocarbon waterproof coating is obtained by dispersing waterborne fluorocarbon emulsion, surface-modified double-shell microcapsules, deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener through high-speed stirring and filtration.
[0039] The high-speed stirring and dispersion is carried out at 1200-1800 r / min for 20-50 min.
[0040] In this step, the weight ratio of the aqueous fluorocarbon emulsion, surface-modified double-shell microcapsules, deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener is as follows: 40-60 parts aqueous fluorocarbon emulsion, 8-16 parts surface-modified double-shell microcapsules, 10-14 parts pigments and fillers, 15-20 parts deionized water, 0.5-1.5 parts dispersant, 0.8-1 part defoamer, 1-3 parts film-forming aid, and 0.5-1.2 parts thickener.
[0041] The beneficial effects of this invention are as follows: The long-lasting anti-aging waterborne fluorocarbon waterproof coating prepared by this invention has a long service life and strong anti-aging ability. After 1000 hours of damp heat resistance test, the damage level is level 1. In the water resistance test before and after aging treatment, there are no abnormal phenomena such as loss of gloss, discoloration, blistering, wrinkling, peeling, or corrosion. After 1000 hours of aging treatment, the coating adhesion level still remains at 0-1, which has good waterproof and anti-aging performance.
[0042] This invention introduces a surface-modified double-shell microcapsule adapted to waterborne fluorocarbon systems. Through the physical encapsulation of the double-shell microcapsule, light stabilizers and antioxidants are released in a sustained manner, achieving long-lasting anti-aging capabilities. The outer wall adopts a urea-formaldehyde-p-hydroxybenzaldehyde ternary system; the inner wall material is polyvinyl alcohol and IPDI trimer; the core material is dodecyl fluoroheptyl methacrylate, antioxidant 1010, and light stabilizer 944. Dodecyl fluoroheptyl methacrylate, as a repair monomer, has long fluorocarbon segments that are highly compatible with waterborne fluorocarbon resins. After release, it can quickly wet the microcracks on the coating surface, achieving surface repair. Detailed Implementation
[0043] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be described in further detail below. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.
[0044] Example 1: A long-lasting anti-aging waterborne fluorocarbon waterproof coating A long-lasting, anti-aging water-based fluorocarbon waterproof coating, the preparation method of which includes the following steps: Step 1: Inner wall material cladding The core material was prepared by mixing dodecafluoroheptyl methacrylate, IPDI trimer, antioxidant 1010, and light stabilizer 944. Polyvinyl alcohol was dissolved in deionized water at elevated temperature to obtain an aqueous phase. The core material was then added dropwise to the aqueous phase, and the mixture was emulsified at a high-speed shear rate of 3000 r / min for 15 min to obtain an emulsion. The emulsion was pre-crosslinked at 50℃ for 0.5 h, and then heated to 60℃ and held for 2 h to obtain an inner wall microcapsule emulsion.
[0045] In this step, the weight ratio of dodecyl fluoroheptyl methacrylate, antioxidant 1010, light stabilizer 944, polyvinyl alcohol, and IPDI trimer is as follows: 70 parts dodecyl fluoroheptyl methacrylate, 10 parts antioxidant 1010, 15 parts light stabilizer 944, 55 parts polyvinyl alcohol, and 4 parts IPDI trimer.
[0046] The amount of deionized water used is 10 times the mass of polyvinyl alcohol.
[0047] The heating and dissolution process involves heating to 80°C and stirring to dissolve the substances.
[0048] Step 2: Modification of the outer wall material Urea and p-hydroxybenzaldehyde were added to water, and the pH of the system was adjusted to 8.0 using triethanolamine to obtain a urea-p-hydroxybenzaldehyde mixture. This mixture was added dropwise to the inner wall microcapsule emulsion, stirred thoroughly, and then formaldehyde solution was added dropwise. The pH of the system was adjusted to 4.5 using citric acid, and the reaction was maintained at 55°C for 5 hours. After the reaction, the pH of the system was adjusted to neutral using triethanolamine, the mixture was filtered, and the solid was retained. The solid was washed with ethanol to obtain the initial product of the double-shell microcapsules.
[0049] The microcapsule sample was dispersed in a 60% (v / v) aqueous ethanol solution. Perfluorobutylethyltrimethoxysilane was added under nitrogen protection. The pH was adjusted to 4.0 with acetic acid, the temperature was raised to 50°C, and the reaction was maintained for 5 hours. The solid was filtered and washed with anhydrous ethanol and dried under vacuum to obtain surface-modified double-shell microcapsules.
[0050] In this step, the weight ratio of urea, p-hydroxybenzaldehyde, and formaldehyde solution is: 60 parts urea, 2 parts p-hydroxybenzaldehyde, and 110 parts formaldehyde solution.
[0051] The amount of water used is five times the amount of urine.
[0052] The amount of the ethanol-water solution used is 5 times the initial mass of the microcapsules.
[0053] The amount of perfluorobutyl ethyl trimethoxysilane used is 3% of the initial mass of the double-shell microcapsules.
[0054] The vacuum drying process involves controlling the temperature at 40°C, the vacuum level at <-0.06MPa, and the drying time at 15 hours.
[0055] Step 3, Compound Mixing Surface-modified double-shell microcapsules were added to an aqueous fluorocarbon emulsion and stirred to obtain a pre-dispersed masterbatch. Then, deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener were added in sequence. The mixture was stirred and dispersed at 1200 r / min for 50 min and filtered through a 300-mesh filter to obtain the finished product.
[0056] In this step, the weight ratio of the aqueous fluorocarbon emulsion, surface-modified double-shell microcapsules, deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener is as follows: 60 parts aqueous fluorocarbon emulsion, 15 parts surface-modified double-shell microcapsules, 20 parts deionized water, 14 parts pigments and fillers, 1 part dispersant, 1 part defoamer, 2 parts film-forming aid, and 0.5 parts thickener.
[0057] The dispersant is a hydrophobically modified polycarboxylate dispersant.
[0058] The defoamer is a polyether-modified silicone defoamer.
[0059] The film-forming aid is 12-ol ester.
[0060] The thickener is hydroxyethyl cellulose thickener.
[0061] The pigment and filler are sericite powder.
[0062] Example 2: A long-lasting anti-aging waterborne fluorocarbon waterproof coating A long-lasting, anti-aging water-based fluorocarbon waterproof coating, the preparation method of which includes the following steps: Step 1: Inner wall material cladding The core material was prepared by mixing dodecafluoroheptyl methacrylate, IPDI trimer, antioxidant 1010, and light stabilizer 944. Polyvinyl alcohol was dissolved in deionized water at elevated temperature to obtain an aqueous phase. The core material was then added dropwise to the aqueous phase, and the mixture was emulsified at a high-speed shear rate of 3000 r / min for 15 min to obtain an emulsion. The emulsion was pre-crosslinked at 50℃ for 0.5 h, and then heated to 60℃ and held for 3 h to obtain an inner wall microcapsule emulsion.
[0063] In this step, the weight ratio of dodecyl fluoroheptyl methacrylate, antioxidant 1010, light stabilizer 944, polyvinyl alcohol, and IPDI trimer is as follows: 80 parts dodecyl fluoroheptyl methacrylate, 20 parts antioxidant 1010, 10 parts light stabilizer 944, 60 parts polyvinyl alcohol, and 4.8 parts IPDI trimer.
[0064] The amount of deionized water used is 8 times the mass of polyvinyl alcohol.
[0065] The heating and dissolution process involves heating to 80°C and stirring to dissolve the substances.
[0066] Step 2: Modification of the outer wall material Urea and p-hydroxybenzaldehyde were added to water, and the pH of the system was adjusted to 8.0 using triethanolamine to obtain a urea-p-hydroxybenzaldehyde mixture. This mixture was added dropwise to the inner wall microcapsule emulsion, stirred thoroughly, and then formaldehyde solution was added dropwise. The pH of the system was adjusted to 4 using citric acid, and the reaction was maintained at 60°C for 5 hours. After the reaction, the pH of the system was adjusted to neutral using triethanolamine, the mixture was filtered, and the solid was retained. The solid was washed with ethanol to obtain the initial product of the double-shell microcapsules.
[0067] The microcapsule sample was dispersed in a 70% (v / v) aqueous ethanol solution. Perfluorobutylethyltrimethoxysilane was added under nitrogen protection. The pH was adjusted to 4.5 with acetic acid, the temperature was raised to 60°C, and the reaction was maintained for 3.5 h. The solid was filtered and washed with anhydrous ethanol and dried under vacuum to obtain surface-modified double-shell microcapsules.
[0068] In this step, the weight ratio of urea, p-hydroxybenzaldehyde, and formaldehyde solution is: 55 parts urea, 2 parts p-hydroxybenzaldehyde, and 108 parts formaldehyde solution.
[0069] The amount of water used is 6 times the amount of urine.
[0070] The amount of the ethanol-water solution used is 5 times the initial mass of the microcapsules.
[0071] The amount of perfluorobutyl ethyl trimethoxysilane used is 3% of the initial mass of the double-shell microcapsules.
[0072] The vacuum drying process involves controlling the temperature at 45℃, the vacuum level at <-0.06MPa, and the drying time at 12h.
[0073] Step 3, Compound Mixing Surface-modified double-shell microcapsules were added to an aqueous fluorocarbon emulsion and stirred to obtain a pre-dispersed masterbatch. Then, deionized water, pigments and fillers, dispersants, defoamers, film-forming aids, and thickeners were added in sequence. The mixture was stirred and dispersed at 1800 r / min for 20 min and filtered through a 300-mesh filter to obtain the finished product.
[0074] In this step, the weight ratio of the aqueous fluorocarbon emulsion, surface-modified double-shell microcapsules, deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener is as follows: 60 parts aqueous fluorocarbon emulsion, 16 parts surface-modified double-shell microcapsules, 20 parts deionized water, 10 parts pigments and fillers, 1.5 parts dispersant, 1 part defoamer, 3 parts film-forming aid, and 1.2 parts thickener.
[0075] The dispersant is sodium polyacrylate dispersant.
[0076] The defoamer is a mineral oil defoamer.
[0077] The film-forming aid is 12-ol ester.
[0078] The thickener is a nonionic polyurethane associative thickener.
[0079] The pigment and filler are rutile titanium dioxide.
[0080] Example 3: A long-lasting anti-aging waterborne fluorocarbon waterproof coating A long-lasting, anti-aging water-based fluorocarbon waterproof coating, the preparation method of which includes the following steps: Step 1: Inner wall material cladding The core material was prepared by mixing dodecafluoroheptyl methacrylate, IPDI trimer, antioxidant 1010, and light stabilizer 944. Polyvinyl alcohol was dissolved in deionized water at elevated temperature to obtain an aqueous phase. The core material was then added dropwise to the aqueous phase, and the mixture was emulsified at a high-speed shear rate of 2000 r / min for 30 min to obtain an emulsion. The emulsion was pre-crosslinked at 50℃ for 0.5 h, and then heated to 60℃ and held for 3 h to obtain an inner wall microcapsule emulsion.
[0081] In this step, the weight ratio of dodecyl fluoroheptyl methacrylate, antioxidant 1010, light stabilizer 944, polyvinyl alcohol, and IPDI trimer is as follows: 80 parts dodecyl fluoroheptyl methacrylate, 12 parts antioxidant 1010, 20 parts light stabilizer 944, 50 parts polyvinyl alcohol, and 4.5 parts IPDI trimer.
[0082] The amount of deionized water used is 10 times the mass of polyvinyl alcohol.
[0083] The heating and dissolution process involves heating to 70°C and stirring to dissolve the substances.
[0084] Step 2: Modification of the outer wall material Urea and p-hydroxybenzaldehyde were added to water, and the pH of the system was adjusted to 8.0 using triethanolamine to obtain a urea-p-hydroxybenzaldehyde mixture. This mixture was added dropwise to the inner wall microcapsule emulsion, stirred thoroughly, and then formaldehyde solution was added dropwise. The pH of the system was adjusted to 4.0 using citric acid, and the reaction was maintained at 60°C for 4 hours. After the reaction, the pH of the system was adjusted to neutral using triethanolamine, the mixture was filtered, and the solid was retained. The solid was washed with ethanol to obtain the initial product of the double-shell microcapsules.
[0085] The microcapsule sample was dispersed in a 60% (v / v) aqueous ethanol solution. Perfluorobutylethyltrimethoxysilane was added under nitrogen protection. The pH was adjusted to 4.0 with acetic acid, the temperature was raised to 60°C, and the reaction was maintained for 4 hours. The solid was filtered and washed with anhydrous ethanol and dried under vacuum to obtain surface-modified double-shell microcapsules.
[0086] In this step, the weight ratio of urea, p-hydroxybenzaldehyde, and formaldehyde solution is: 60 parts urea, 2 parts p-hydroxybenzaldehyde, and 120 parts formaldehyde solution.
[0087] The amount of water used is four times the amount of urine.
[0088] The vacuum drying process involves controlling the temperature at 50°C, the vacuum level at <-0.06MPa, and the drying time at 12 hours.
[0089] The amount of the ethanol-water solution used is 4 times the initial mass of the microcapsules.
[0090] The amount of perfluorobutyl ethyl trimethoxysilane used is 2% of the initial mass of the double-shell microcapsules.
[0091] Step 3, Compound Mixing Surface-modified double-shell microcapsules were added to an aqueous fluorocarbon emulsion and stirred to obtain a pre-dispersed masterbatch. Then, deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener were added in sequence. The mixture was stirred and dispersed at 1500 r / min for 30 min and filtered through a 300-mesh filter to obtain the finished product.
[0092] In this step, the weight ratio of the aqueous fluorocarbon emulsion, surface-modified double-shell microcapsules, deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener is as follows: 40 parts aqueous fluorocarbon emulsion, 8 parts surface-modified double-shell microcapsules, 15 parts deionized water, 10 parts pigments and fillers, 0.5 parts dispersant, 0.8 parts defoamer, 1 part film-forming aid, and 0.5 parts thickener.
[0093] The dispersant is a hydrophobically modified polycarboxylate dispersant.
[0094] The defoamer is a polyether-modified silicone defoamer.
[0095] The film-forming aid is 12-ol ester.
[0096] The thickener is a nonionic polyurethane associative thickener.
[0097] The pigment and filler are mica iron oxide.
[0098] Example 4: A long-lasting anti-aging waterborne fluorocarbon waterproof coating A long-lasting, anti-aging water-based fluorocarbon waterproof coating, the preparation method of which includes the following steps: Step 1: Inner wall material cladding The core material was prepared by mixing dodecafluoroheptyl methacrylate, IPDI trimer, antioxidant 1010, and light stabilizer 944. Polyvinyl alcohol was dissolved in deionized water at a heated temperature to obtain an aqueous phase. The core material was then added dropwise to the aqueous phase, and the mixture was emulsified at a high-speed shear rate of 2000 r / min for 30 min to obtain an emulsion. The emulsion was pre-crosslinked at 40℃ for 1 h, then heated to 50℃ and held for 3 h to obtain an inner wall microcapsule emulsion.
[0099] In this step, the weight ratio of dodecyl fluoroheptyl methacrylate, antioxidant 1010, light stabilizer 944, polyvinyl alcohol, and IPDI trimer is as follows: 60 parts dodecyl fluoroheptyl methacrylate, 10 parts antioxidant 1010, 13 parts light stabilizer 944, 50 parts polyvinyl alcohol, and 4 parts IPDI trimer.
[0100] The amount of deionized water used is 8 times the mass of polyvinyl alcohol.
[0101] The heating and dissolution process involves heating to 70°C and stirring to dissolve the substances.
[0102] Step 2: Modification of the outer wall material Urea and p-hydroxybenzaldehyde were added to water, and the pH of the system was adjusted to 7.5 using triethanolamine to obtain a urea-p-hydroxybenzaldehyde mixture. This mixture was added dropwise to the inner wall microcapsule emulsion, stirred thoroughly, and then formaldehyde solution was added dropwise. The pH of the system was adjusted to 3.5 using citric acid, and the reaction was maintained at 65°C for 3 hours. After the reaction, the pH of the system was adjusted to neutral using triethanolamine, the mixture was filtered, and the solid was retained. The solid was washed with ethanol to obtain the initial product of the double-shell microcapsules.
[0103] The microcapsule sample was dispersed in a 70% (v / v) aqueous ethanol solution. Perfluorobutylethyltrimethoxysilane was added under nitrogen protection. The pH was adjusted to 4.0 with acetic acid, the temperature was raised to 50°C, and the reaction was maintained for 5 hours. The solid was filtered and washed with anhydrous ethanol and dried under vacuum to obtain surface-modified double-shell microcapsules.
[0104] In this step, the weight ratio of urea, p-hydroxybenzaldehyde, and formaldehyde solution is: 65 parts urea, 3 parts p-hydroxybenzaldehyde, and 120 parts formaldehyde solution.
[0105] The amount of water used is 6 times the amount of urine.
[0106] The vacuum drying process involves controlling the temperature at 45℃, the vacuum level at <-0.06MPa, and the drying time at 12h.
[0107] The amount of the ethanol-water solution used is 3.5 times the initial mass of the microcapsules.
[0108] The amount of perfluorobutyl ethyl trimethoxysilane used is 2% of the initial mass of the double-shell microcapsules.
[0109] Step 3, Compound Mixing Surface-modified double-shell microcapsules were added to an aqueous fluorocarbon emulsion and stirred to obtain a pre-dispersed masterbatch. Then, deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener were added in sequence. The mixture was stirred and dispersed at 1500 r / min for 50 min and filtered through a 300-mesh filter to obtain the finished product.
[0110] In this step, the weight ratio of the aqueous fluorocarbon emulsion, surface-modified double-shell microcapsules, deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener is as follows: 50 parts aqueous fluorocarbon emulsion, 10 parts surface-modified double-shell microcapsules, 20 parts deionized water, 10 parts pigments and fillers, 0.5 parts dispersant, 1 part defoamer, 2 parts film-forming aid, and 0.5 parts thickener.
[0111] The dispersant is a hydrophobically modified polycarboxylate dispersant.
[0112] The defoamer is a polyether-modified silicone defoamer.
[0113] The film-forming aid is 12-ol ester.
[0114] The thickener is a nonionic polyurethane associative thickener.
[0115] The pigment and filler are sericite powder.
[0116] Comparative Example 1 Add dodecafluoroheptyl methacrylate, antioxidant 1010, and light stabilizer 944 to an aqueous fluorocarbon emulsion and stir to obtain a pre-dispersed masterbatch. Then, add deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener in sequence. Stir and disperse at 1500 r / min for 50 min and filter through a 300 mesh screen to obtain the finished product.
[0117] In this step, the weight ratio of each raw material component is as follows: 6 parts dodecafluoroheptyl methacrylate, 2 parts antioxidant 1010, 2 parts light stabilizer 944, 50 parts waterborne fluorocarbon emulsion, 20 parts deionized water, 10 parts pigments and fillers, 0.5 parts dispersant, 1 part defoamer, 2 parts film-forming aid, and 0.5 parts thickener.
[0118] The dispersant is a hydrophobically modified polycarboxylate dispersant.
[0119] The defoamer is a polyether-modified silicone defoamer.
[0120] The film-forming aid is 12-ol ester.
[0121] The thickener is a nonionic polyurethane associative thickener.
[0122] The pigment and filler are sericite powder.
[0123] Comparative Example 2 Step 1: Exterior wall material cladding The core material is obtained by mixing dodecafluoroheptyl methacrylate, antioxidant 1010, and light stabilizer 944.
[0124] Urea was dissolved in water, and the pH of the system was adjusted to 7.5 using triethanolamine to obtain a urea solution. The urea solution was mixed with the core material and emulsified at 3000 rpm for 30 min. After thorough stirring, formaldehyde solution was added dropwise, and the pH of the system was adjusted to 3.5 using citric acid. The reaction was maintained at 65°C for 3 h. After the reaction, the pH of the system was adjusted to neutral using triethanolamine. The mixture was filtered, and the solid was retained. The solid was washed with ethanol and vacuum dried to obtain single-walled microcapsules.
[0125] In this step, the weight ratio of dodecyl fluoroheptyl methacrylate, antioxidant 1010, light stabilizer 944, urea, and formaldehyde solution is as follows: 60 parts dodecyl fluoroheptyl methacrylate, 10 parts antioxidant 1010, 13 parts light stabilizer 944, 65 parts urea, and 120 parts formaldehyde solution.
[0126] The amount of water used is five times the amount of urine.
[0127] The vacuum drying process involves controlling the temperature at 50°C, the vacuum level at <-0.06MPa, and the drying time at 12 hours.
[0128] Step 2, Compound Mixing Single-walled microcapsules were added to an aqueous fluorocarbon emulsion and stirred to obtain a pre-dispersed masterbatch. Then, deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener were added in sequence. The mixture was stirred and dispersed at 1500 r / min for 50 min and filtered through a 300-mesh filter to obtain the finished product.
[0129] In this step, the weight ratio of aqueous fluorocarbon emulsion, single-walled microcapsules, deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener is as follows: 50 parts aqueous fluorocarbon emulsion, 10 parts single-walled microcapsules, 20 parts deionized water, 10 parts pigments and fillers, 0.5 parts dispersant, 1 part defoamer, 2 parts film-forming aid, and 0.5 parts thickener.
[0130] The dispersant is a hydrophobically modified polycarboxylate dispersant.
[0131] The defoamer is a polyether-modified silicone defoamer.
[0132] The film-forming aid is 12-ol ester.
[0133] The thickener is a nonionic polyurethane associative thickener.
[0134] The pigment and filler are sericite powder.
[0135] Performance testing 1. The performance tests of moisture and heat resistance, water resistance and coating adhesion of Examples 1-4 and Comparative Examples 1-2 were carried out. The test methods are as follows, and the test results are shown in Table 1.
[0136] Resistance to damp heat: Test panels were prepared according to the method provided in GB / T 1740-2007 "Test Method for Resistance to Damp Heat of Coatings", and the overall damage level was evaluated. The test conditions were: temperature 47±1℃, relative humidity 96±2%, and test time 1000h.
[0137] Water resistance: Test panels were prepared according to the method provided in GB / T 1733-1993 "Determination of Water Resistance of Paint Films" and tested using "9.1 Method A Immersion Test" for 28 days. The test panels were visually inspected and the presence of any loss of gloss, discoloration, blistering, wrinkling, peeling, or corrosion was recorded.
[0138] Aging treatment: The samples were aged for 1000 hours (irradiation intensity 1.0 W / m²) according to GB / T 1865-2009 "Artificial climate aging and artificial radiation exposure of paints and varnishes with filtered xenon arc radiation". 2 ).
[0139] Coating adhesion: Following the method provided in GB / T 9286-2021 "Cross-cut test for paint and varnish films", the coating adhesion was tested after aging treatment (irradiation intensity 1.0 W / m²). 2 The cross-cut test was performed on the sample (1000h).
[0140] Table 1. Performance test results of damp heat resistance, water resistance, and coating adhesion for the examples and comparative examples. 2. The retention rate of anti-aging additives in Examples 1-4 and Comparative Examples 1-2 under different aging times was tested. The test methods are as follows, and the test results are shown in Table 2.
[0141] Anti-aging additive retention rate: The coated test panels were subjected to 2000 hours of artificial accelerated aging with an irradiation intensity of 1.0 W / m². 2 Samples were taken at 0h, 500h, 1000h, and 2000h for testing. Tetrahydrofuran was refluxed in a Soxhlet extractor for 6h. The concentrations of antioxidant 1010 and light stabilizer 944 in the extract were determined by high performance liquid chromatography. The retention rate of the auxiliary agent was calculated as: concentration of the extraction auxiliary agent after aging / concentration of the original extraction auxiliary agent × 100%.
[0142] Table 2 Comparison of retention rates of anti-aging additives at different aging times Analysis of the data in Table 1 shows that the water-based fluorocarbon waterproof coating prepared by this invention exhibits a damage level of 1 after 1000 hours of damp heat resistance testing. No abnormal phenomena such as loss of gloss, discoloration, blistering, wrinkling, peeling, or corrosion were observed in the water resistance tests before and after aging treatment. After 1000 hours of aging treatment, the coating adhesion level remains at 0-1. Analysis of the data in Table 2 shows that after 2000 hours of artificial accelerated aging, the water-based fluorocarbon waterproof coating prepared by this invention retains 70.2-72.4% of antioxidant 1010 and 70.5-71.3% of light stabilizer 944. These data demonstrate that the water-based fluorocarbon waterproof coating prepared by this invention possesses good waterproof and anti-aging properties.
[0143] Obviously, there are many other specific implementation methods that can be varied under the concept of this invention. It should be stated here that any changes made under the inventive concept of this invention will fall within the protection scope of this invention.
Claims
1. A method for preparing a long-lasting anti-aging waterborne fluorocarbon waterproof coating, characterized in that, This includes the steps of inner wall material coating, outer wall material coating modification, and composite formulation. The inner wall material coating process involves dissolving polyvinyl alcohol in deionized water by heating, adding the core material dropwise, and emulsifying it under high-speed shear to obtain an emulsion. After pre-crosslinking the emulsion, the reaction is maintained at a high temperature for 2-3 hours to obtain an inner wall microcapsule emulsion. The outer wall material coating modification is as follows: Urea and p-hydroxybenzaldehyde are added to water, the pH of the system is adjusted to 7.5-8.0, and then added dropwise to the inner wall microcapsule emulsion. Formaldehyde solution is then added dropwise, the mixture is acidified, and the reaction is kept at a constant temperature for 3-5 hours. The pH of the system is adjusted to neutral, and the solid is filtered to obtain the initial product of the double-shell microcapsules. The initial product of the microcapsules is dispersed in an ethanol aqueous solution, and perfluorobutylethyltrimethoxysilane is added under nitrogen protection. The pH is adjusted to 4.0-4.5, the reaction is kept at a constant temperature for 3.5-5 hours, the solid is filtered to retain the solid, and the surface-modified double-shell microcapsules are obtained after washing with ethanol and vacuum drying. The compound formulation involves dispersing waterborne fluorocarbon emulsion, surface-modified double-shell microcapsules, deionized water, pigments and fillers, dispersants, defoamers, film-forming aids, and thickeners through high-speed stirring, followed by filtration to obtain a long-lasting anti-aging waterborne fluorocarbon waterproof coating.
2. The preparation method of a long-lasting anti-aging waterborne fluorocarbon waterproof coating according to claim 1, characterized in that, The heating and dissolution process in the inner wall material coating step involves heating to 70-80℃ and stirring to dissolve the material; the shear emulsification process involves controlling the rotation speed at 2000-3000 r / min and the emulsification time at 15-30 min; the amount of polyvinyl alcohol used is 50-60 parts; and the amount of deionized water used is 8-10 times the mass of polyvinyl alcohol.
3. The preparation method of a long-lasting anti-aging waterborne fluorocarbon waterproof coating according to claim 1, characterized in that, The core material described in the inner wall coating step has the following raw material weight ratio: 60-80 parts of dodecafluoroheptyl methacrylate, 10-20 parts of antioxidant 1010, 4-4.8 parts of IPDI trimer, and 10-20 parts of light stabilizer 944.
4. The preparation method of a long-lasting anti-aging waterborne fluorocarbon waterproof coating according to claim 3, characterized in that, The IPDI trimer has a mass concentration of 70%, uses butyl acetate as the solvent, has an NCO content of 12-15%, and a viscosity of 600-1000 mPa·s.
5. The preparation method of a long-lasting anti-aging waterborne fluorocarbon waterproof coating according to claim 1, characterized in that, The weight ratio of urea, p-hydroxybenzaldehyde, and formaldehyde solution in the outer wall material coating modification step is as follows: 55-65 parts urea, 2-3 parts p-hydroxybenzaldehyde, and 108-120 parts formaldehyde solution; the mass concentration of the formaldehyde solution is 35-40%.
6. The preparation method of a long-lasting anti-aging waterborne fluorocarbon waterproof coating according to claim 1, characterized in that, In the outer wall material coating modification step, the amount of water used is 4-6 times the amount of urea; the amount of perfluorobutyl ethyl trimethoxysilane used is 2-3% of the initial mass of the double-shell microcapsules; the volume fraction of the ethanol aqueous solution is 60-70%, and the amount used is 3.5-5 times the initial mass of the microcapsules.
7. The preparation method of a long-lasting anti-aging waterborne fluorocarbon waterproof coating according to claim 1, characterized in that, The heat preservation reaction in the outer wall material coating modification step is carried out at a temperature of 55-65℃; the vacuum drying step is carried out at a controlled temperature of 40-50℃, a vacuum degree of <-0.06MPa, and a drying time of 12-15h.
8. The preparation method of a long-lasting anti-aging waterborne fluorocarbon waterproof coating according to claim 1, characterized in that, The weight ratio of the aqueous fluorocarbon emulsion, surface-modified double-shell microcapsules, deionized water, pigments and fillers, dispersant, defoamer, film-forming aid, and thickener mentioned in the compounding step is as follows: 40-60 parts aqueous fluorocarbon emulsion, 8-16 parts surface-modified double-shell microcapsules, 10-14 parts pigments and fillers, 15-20 parts deionized water, 0.5-1.5 parts dispersant, 0.8-1 part defoamer, 1-3 parts film-forming aid, and 0.5-1.2 parts thickener.
9. The preparation method of a long-lasting anti-aging waterborne fluorocarbon waterproof coating according to claim 1, characterized in that, The pigments and fillers mentioned in the compounding step are at least one of rutile titanium dioxide, sericite powder, and mica iron oxide. The dispersant is at least one of hydrophobically modified polycarboxylate dispersant and sodium polyacrylate dispersant; The defoamer is at least one of mineral oil defoamer and polyether-modified silicone defoamer; The film-forming aid is alcohol ester dodecyl; The thickener is at least one of nonionic polyurethane associative thickener and hydroxyethyl cellulose thickener.
10. A long-lasting, anti-aging water-based fluorocarbon waterproof coating, characterized in that, The waterproof coating is prepared by the preparation method according to any one of claims 1 to 9.