A polyacrylic acid cement waterproof coating and its preparation method
By using a specific ratio and mixing process of modified polyacrylate emulsion and composite functional additives, the problems of easy cracking and weak weather resistance in low-temperature construction of polyacrylic acid cement waterproof coatings have been solved. Stable film formation and high weather resistance over a wide temperature range have been achieved, making it suitable for building waterproofing projects.
Patent Information
- Application Number
- CN202611204542.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polyacrylic acid cement waterproof coatings suffer from poor low-temperature application, easy cracking, weak weather resistance, and insufficient mass production stability.
The liquid components, consisting of modified polyacrylate emulsion, composite functional additives, defoamers, preservatives, and deionized water, and the powder components, consisting of silicate cement, quartz sand, and heavy calcium carbonate powder, are mixed and stirred in a specific ratio to form a coating that is filled with nanoparticles, reinforced with flexible micro powder and coupling agent, achieving stable film formation from -20℃ to 60℃.
It achieves continuous film formation within a temperature range of -20℃ to 60℃, without powdering, film breakage, or cracking. It exhibits no cracking after 50 dry and wet cycles, significantly improving its weather resistance and lifespan. The batch index deviation is ≤1.5%, making it suitable for building waterproofing scenarios across the country.
Smart Images

Figure CN123107470A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the technical field of building waterproofing materials, specifically relating to a polyacrylic acid cement waterproof coating and its preparation method. Background Technology
[0002] Polyacrylic acid cement waterproof coatings combine the flexibility and adhesion of organic emulsions with the high strength, aging resistance, and environmentally friendly flame retardancy of inorganic cement, making them the most widely used and mature general-purpose waterproof material in China. Existing publicly available technologies almost entirely focus on macroscopic formulation modifications such as emulsion type replacement, filler ratio adjustment, and simple addition of conventional additives. Reports on solutions to the problems of poor low-temperature application, easy cracking, weak weather resistance, and insufficient mass production stability of existing polyacrylic acid cement waterproof coatings are relatively few. Summary of the Invention
[0003] This application provides a polyacrylic acid cement waterproof coating and its preparation method, aiming to solve the problems of poor low-temperature construction, easy cracking, weak weather resistance, and insufficient mass production stability of existing polyacrylic acid cement waterproof coatings.
[0004] The first aspect of this application provides a polyacrylic acid cement waterproof coating, comprising a liquid component and a powder component; The liquid component comprises the following raw materials in parts by weight: 45-55 parts modified polyacrylate emulsion, 3-6 parts composite functional additives, 0.2-0.5 parts defoamer, 0.1-0.3 parts preservative, and 20-25 parts deionized water. The composite functional additive comprises the following raw materials in parts by weight: 55-65 parts of modified dodecyl alcohol ester film-forming aid, 15-20 parts of hydrophilic modified nano-silica dispersion powder, 10-15 parts of ultrafine acrylic flexible crack-resistant micro powder, and silane coupling agent KH. 570 3-10 copies; The powder composition includes the following raw materials in parts by weight: 35-45 parts silicate cement, 25-30 parts quartz sand, and 10-15 parts heavy calcium carbonate powder.
[0005] According to some embodiments of the polyacrylic acid cement waterproof coating described in this application, the liquid component includes the following raw materials in parts by weight: 50 parts modified polyacrylate emulsion, 4 parts composite functional additives, 0.3 parts defoamer, 0.2 parts preservative, and 22 parts deionized water. The composite functional additive comprises the following raw materials in parts by weight: 60 parts of modified dodecyl alcohol ester film-forming aid, 18 parts of hydrophilic modified nano silica dispersion powder, 12 parts of ultrafine acrylic flexible crack-resistant micro powder, and silane coupling agent KH. 570 10 copies; The powder composition includes the following raw materials in parts by weight: 40 parts silicate cement, 28 parts quartz sand, and 12 parts heavy calcium carbonate powder.
[0006] According to some embodiments of the polyacrylic acid cement waterproof coating described in this application, the mass ratio of the liquid component to the powder component is 1:(1-1.5).
[0007] According to some embodiments of the polyacrylic acid cement waterproof coating described in this application, the defoamer includes polydimethylsiloxane and / or glyceryl stearate.
[0008] According to some embodiments of the polyacrylic acid cement waterproof coating described in this application, the preservative includes methylisothiazolinone and / or thiazolinone.
[0009] The second aspect of this application provides a method for preparing the polyacrylic acid cement waterproof coating described in the first aspect of this application, comprising the following steps: (1) Mix the composite functional additive with deionized water to obtain a pre-dispersion of the composite functional additive; (2) The pre-dispersed liquid of the composite functional additive is added dropwise to the modified polyacrylate emulsion. After the addition is complete, the defoamer and preservative are added in sequence and mixed to obtain the liquid component. (3) The silicate cement, quartz sand and heavy calcium carbonate powder are mixed to obtain the powder composition.
[0010] According to some embodiments of the preparation method of polyacrylic acid cement waterproof coating described in this application, in step (2), the dripping time of the pre-dispersed liquid of the composite functional additive is controlled at 10-15 min.
[0011] According to some embodiments of the preparation method of polyacrylic acid cement waterproof coating described in this application, in step (2), the mixing temperature is 25-30℃ and the time is 30-50min.
[0012] The third aspect of this application provides the application of the polyacrylic acid cement waterproof coating described in the first aspect of this application or the polyacrylic acid cement waterproof coating prepared by the method described in the second aspect of this application in low-temperature waterproofing projects for building roofs, basements, tunnels or outdoor floors.
[0013] According to some embodiments of the application described in this application, the application temperature of the polyacrylic acid cement waterproof coating is -20°C to 60°C.
[0014] The beneficial effects of this application include: the nanoparticles contained in the polyacrylic cement waterproof coating fill the micropores, the flexible micro powder can offset the shrinkage of cement hydration, and the coupling agent contained enhances the organic-inorganic interface bonding, enabling the cement waterproof coating to achieve stable and continuous film formation from -20℃ to 60℃, without powdering, film breakage, or cracking, greatly expanding the construction window in northern regions and winter; and without cracking or peeling after 50 dry-wet cycles, significantly improving its weather resistance life.
[0015] The polyacrylic acid cement waterproof coating preparation process described in this application is simple and fully compatible with existing raw materials and equipment. The method ensures that the batch index deviation of the product is ≤1.5%, which is far superior to the industry standard. Detailed Implementation
[0016] The embodiments of the present invention are described in detail below. These embodiments are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0017] In this invention, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0018] This application provides a polyacrylic acid cement waterproof coating, comprising a liquid component and a powder component; The liquid component comprises the following raw materials in parts by weight: 45-55 parts modified polyacrylate emulsion, 3-6 parts composite functional additives, 0.2-0.5 parts defoamer, 0.1-0.3 parts preservative, and 20-25 parts deionized water. The composite functional additive comprises the following raw materials in parts by weight: 55-65 parts of modified dodecyl alcohol ester film-forming aid, 15-20 parts of hydrophilic modified nano-silica dispersion powder, 10-15 parts of ultrafine acrylic flexible crack-resistant micro powder, and silane coupling agent KH. 570 3-10 copies; The powder composition includes the following raw materials in parts by weight: 35-45 parts silicate cement, 25-30 parts quartz sand, and 10-15 parts heavy calcium carbonate powder.
[0019] The polyacrylic acid cement waterproof coating described in this application contains nanoparticles that fill micropores, and flexible micro powders that can counteract cement hydration shrinkage. The coupling agent it contains enhances the organic-inorganic interface bonding, enabling the cement waterproof coating to achieve stable and continuous film formation from -5℃ to 5℃, without powdering, film breakage, or cracking, greatly expanding the construction window in northern regions and winter; and it does not crack or peel after 50 dry-wet cycles, significantly improving its weather resistance life.
[0020] The modified dodecyl alcohol ester contained in the waterproof coating described in this application can continuously reduce the minimum film-forming temperature of the emulsion. The hydrophilic modified nano-silica fills the micro-pores of the coating film to improve its density. The ultrafine acrylic flexible crack-resistant micro powder offsets the stress caused by cement hydration and low-temperature thermal shrinkage. The silane coupling agent KH-570 strengthens the interfacial bonding between the organic emulsion and the inorganic cement filler. It can form a stable and continuous film at temperatures below -20°C, completely breaking through the traditional JS coating's 5°C construction limit and expanding the construction window in northern winters and cold regions.
[0021] The nano-silica and silane cross-linked network contained in the waterproof coating described in this application enhances the heat resistance, UV resistance, and freeze-thaw resistance of the coating film. The cured waterproof coating film can withstand long-term low-temperature freeze-thaw cycles of -20℃ and high-temperature exposure of 60℃. It can withstand 50 dry and wet cycles without cracking or peeling, making it suitable for various building waterproofing scenarios across the country, from the cold Northeast to the high-temperature South China.
[0022] In some embodiments of this application, the liquid component includes the following raw materials in parts by weight: 50 parts modified polyacrylate emulsion, 4 parts composite functional additives, 0.3 parts defoamer, 0.2 parts preservative, and 22 parts deionized water. The composite functional additive comprises the following raw materials in parts by weight: 60 parts of modified dodecyl alcohol ester film-forming aid, 18 parts of hydrophilic modified nano silica dispersion powder, 12 parts of ultrafine acrylic flexible crack-resistant micro powder, and silane coupling agent KH. 570 10 copies; The powder composition includes the following raw materials in parts by weight: 40 parts silicate cement, 28 parts quartz sand, and 12 parts heavy calcium carbonate powder.
[0023] In some embodiments of this application, the mass ratio of the liquid component to the powder component is 1:(1-1.5); for example, 1:1, 1:1.2, 1:1.3, 1:1.5, etc.
[0024] In some embodiments of this application, the defoamer includes polydimethylsiloxane and / or glyceryl stearate.
[0025] In some embodiments of this application, the preservatives include methylisothiazolinone and / or thiazolinone.
[0026] This application also provides a method for preparing the polyacrylic acid cement waterproof coating described in the first aspect of this application, comprising the following steps: (1) Mix the composite functional additive with deionized water to obtain a pre-dispersion of the composite functional additive; (2) The pre-dispersed liquid of the composite functional additive is added dropwise to the modified polyacrylate emulsion. After the addition is complete, the defoamer and preservative are added in sequence and mixed to obtain the liquid component. (3) The silicate cement, quartz sand and heavy calcium carbonate powder are mixed to obtain the powder composition.
[0027] The polyacrylic acid cement waterproof coating preparation process described in this application is simple and fully compatible with existing raw materials and equipment. The method ensures that the batch index deviation of the product is ≤1.5%, which is far superior to the industry standard.
[0028] In some embodiments of this application, in step (2), the dripping time of the pre-dispersion liquid of the composite functional additive is controlled at 10-15 min; for example, 10 min, 11 min, 12 min, 15 min, etc.
[0029] In some embodiments of this application, in step (2), the mixing temperature is 25-30°C, such as 25°C, 28°C, 30°C, etc., and the time is 30-50 min; such as 30 min, 33 min, 35 min, 43 min, 50 min, etc.
[0030] This application also provides an application of the polyacrylic acid cement waterproof coating described in the first aspect of this application or the polyacrylic acid cement waterproof coating prepared by the method described in the second aspect of this application in low-temperature waterproofing projects for building roofs, basements, tunnels, or outdoor floors. The polyacrylic acid cement waterproof coating described in this application, through additive pre-dispersion, gradient dripping, and segmented variable-speed stirring, completely solves the problems of powder agglomeration, system inhomogeneity, and batch fluctuations, making the polyacrylic acid cement waterproof coating more stable and possessing higher weather resistance.
[0031] In some embodiments of this application, the application temperature of the polyacrylic acid cement waterproof coating is -20℃ to 60℃. When applied in a low-temperature environment of -20℃ to -10℃, simple insulation treatment of the substrate can achieve continuous, crack-free film formation without powdering or film breakage defects. The waterproof coating described in this application, after 50 dry-wet cycles under conditions of -20℃ freeze-thaw cycles and 60℃ high-temperature exposure, showed no cracking, peeling, or flaking.
[0032] The technical solution of this application will be further described below with reference to specific embodiments.
[0033] Example 1 A method for preparing a polyacrylic acid cement waterproof coating includes the following steps: (1) 60g of modified dodecyl alcohol ester film-forming aid, 18g of hydrophilic modified nano silica dispersion powder, 12g of ultrafine acrylic flexible crack-resistant micro powder, and 10g of silane coupling agent KH 570 g of deionized water and 22 g of deionized water were mixed and stirred at 25 °C and 300 r / min for 20 min to obtain a pre-dispersion of the composite functional additive. (2) Add 50g of modified polyacrylate emulsion to the reactor and stir for 10min at 25℃ and 250r / min. Then add 7.6g of pre-dispersed composite functional additive to the modified polyacrylate emulsion and control the dripping time to 15min. After the dripping is completed, mix and stir for 30min at 400r / min. Then add 0.3g of defoamer polydimethylsiloxane and 0.2g of preservative methylisothiazolinone in sequence. Stir for 15min at 25℃ and 300r / min. Filter to obtain liquid components. (3) Mix 35g silicate cement, 25g quartz sand and 10g heavy calcium carbonate powder in a closed mixer for 25min to obtain powder components.
[0034] Example 2 The only difference between the preparation method of the polyacrylic acid cement waterproof coating in Example 2 and that in Example 1 is that the amount of composite functional additives added during the preparation of the polyacrylic acid cement waterproof coating in Example 2 is different from that in Example 1.
[0035] The specific operating steps include: (2) Add 50g of modified polyacrylate emulsion to the reactor and stir for 10min at 25℃ and 250r / min. Then add 3.6g of pre-dispersed composite functional additive liquid dropwise into the modified polyacrylate emulsion and control the dropwise addition time to 15min. After the dropwise addition is completed, mix and stir at 400r / min for 30min. Then add 0.3g of defoamer polydimethylsiloxane and 0.2g of preservative methylisothiazolinone in sequence. Stir for 15min at 25℃ and 300r / min. Filter to obtain the liquid component. The remaining operation steps are the same as in Example 1.
[0036] Example 3 The only difference between the preparation method of the polyacrylic acid cement waterproof coating in Example 3 and that in Example 1 is that the amount of composite functional additives added during the preparation of the polyacrylic acid cement waterproof coating in Example 3 is different from that in Example 1.
[0037] The specific operating steps include: (2) Add 50g of modified polyacrylate emulsion to the reactor and stir for 10min at 25℃ and 250r / min. Then add 2.5g of pre-dispersed composite functional additive to the modified polyacrylate emulsion and control the dripping time to 15min. After the dripping is completed, mix and stir for 30min at 400r / min. Then add 0.3g of defoamer polydimethylsiloxane and 0.2g of preservative methylisothiazolinone in sequence. Stir for 15min at 25℃ and 300r / min. Filter to obtain the liquid component. The remaining operation steps are the same as in Example 1.
[0038] Example 4 The only difference between the preparation method of the polyacrylic acid cement waterproof coating in Example 4 and that in Example 1 is that the amount of composite functional additives added during the preparation process of the polyacrylic acid cement waterproof coating in Example 4 is different from that in Example 1.
[0039] The specific operating steps include: (2) Add 50g of modified polyacrylate emulsion to the reactor and stir for 10min at 25℃ and 250r / min. Then add 9.6g of pre-dispersed composite functional additive liquid dropwise into the modified polyacrylate emulsion and control the dropwise addition time to 15min. After the dropwise addition is completed, mix and stir at 400r / min for 30min. Then add 0.3g of defoamer polydimethylsiloxane and 0.2g of preservative methylisothiazolinone in sequence. Stir for 15min at 25℃ and 300r / min. Filter to obtain the liquid component. The remaining operation steps are the same as in Example 1.
[0040] Comparative Example 1 The only difference between the preparation method of the polyacrylic acid cement waterproof coating in Comparative Example 1 and Example 1 is that no raw material composite functional additives were added during the preparation process of the polyacrylic acid cement waterproof coating in Comparative Example 1.
[0041] Performance Study of Polyacrylic Cement Waterproof Coatings as Described in Examples 1-4 and Comparative Example 1 of this Application The tensile strength and elongation at break of the low-temperature resistant polymer cement waterproof coatings described in Examples 1-4 and Comparative Example 1 of this application were tested at -5℃ in accordance with GB / T 23445-2009 Polymer Cement Waterproof Coatings. The results are shown in Table 1.
[0042] The film-forming temperature of the polyacrylic acid cement waterproof coatings described in Examples 1-4 and Comparative Example 1 of this application was tested according to GB / T 9267, and the results are shown in Table 1.
[0043] Table 1
[0044] Although the above embodiments have been shown and described, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Any changes, modifications, substitutions and variations made to the above embodiments by those skilled in the art are within the protection scope of the present invention.
Claims
1. A polyacrylic acid cement waterproof coating, characterized in that, Includes liquid components and powder components; The liquid component comprises the following raw materials in parts by weight: 45-55 parts modified polyacrylate emulsion, 3-6 parts composite functional additives, 0.2-0.5 parts defoamer, 0.1-0.3 parts preservative, and 20-25 parts deionized water. The composite functional additive comprises the following raw materials in parts by weight: 55-65 parts of modified dodecyl alcohol ester film-forming aid, 15-20 parts of hydrophilic modified nano-silica dispersion powder, 10-15 parts of ultrafine acrylic flexible crack-resistant micro powder, and silane coupling agent KH. 5703-10 copies; The powder composition includes the following raw materials in parts by weight: 35-45 parts silicate cement, 25-30 parts quartz sand, and 10-15 parts heavy calcium carbonate powder.
2. The polyacrylic acid cement waterproof coating according to claim 1, characterized in that, The liquid component comprises the following raw materials in parts by weight: 50 parts modified polyacrylate emulsion, 4 parts composite functional additives, 0.3 parts defoamer, 0.2 parts preservative, and 22 parts deionized water. The composite functional additive comprises the following raw materials in parts by weight: 60 parts of modified dodecyl alcohol ester film-forming aid, 18 parts of hydrophilic modified nano silica dispersion powder, 12 parts of ultrafine acrylic flexible crack-resistant micro powder, and silane coupling agent KH. 570 10 copies; The powder composition includes the following raw materials in parts by weight: 40 parts silicate cement, 28 parts quartz sand, and 12 parts heavy calcium carbonate powder.
3. The polyacrylic acid cement waterproof coating according to claim 1, characterized in that, The mass ratio of the liquid component to the powder component is 1:(1-1.5).
4. The polyacrylic acid cement waterproof coating according to claim 1, characterized in that, The defoamer includes polydimethylsiloxane and / or glyceryl stearate; And / or, the preservative includes methylisothiazolinone and / or thiazolinone.
5. The method for preparing the polyacrylic acid cement waterproof coating according to any one of claims 1-4, characterized in that, Includes the following steps: (1) Mix the composite functional additive with deionized water to obtain a pre-dispersion of the composite functional additive; (2) The pre-dispersed liquid of the composite functional additive is added dropwise to the modified polyacrylate emulsion. After the addition is complete, the defoamer and preservative are added in sequence and mixed to obtain the liquid component. (3) The silicate cement, quartz sand and heavy calcium carbonate powder are mixed to obtain the powder composition.
6. The method for preparing the polyacrylic acid cement waterproof coating according to claim 5, characterized in that, In step (2), the dripping time of the pre-dispersion liquid of the composite functional additive is controlled at 10-15 min.
7. The method for preparing the polyacrylic acid cement waterproof coating according to claim 5, characterized in that, In step (2), the mixing temperature is 25-30℃ and the time is 30-50min.
8. The application of the polyacrylic acid cement waterproof coating according to any one of claims 1-4 or the polyacrylic acid cement waterproof coating obtained by the preparation method according to any one of claims 5-7 in low-temperature waterproofing projects for building roofs, basements, tunnels or outdoor floors.
9. The application according to claim 8, characterized in that, The application temperature of the polyacrylic acid cement waterproof coating is -20℃ to 60℃.