A double-layer epoxy fire-retardant coating, coating material and its preparation method
By designing a double-layer epoxy fire-retardant coating, the bottom layer improves the bonding performance with the steel substrate, while the top layer forms a high-expansion char layer. This solves the problem of cracking and peeling of existing epoxy intumescent fire-retardant coatings at high temperatures, achieving better heat insulation and stability of the expanded char layer, and improving the fire resistance of the steel structure.
Patent Information
- Application Number
- CN202611584116.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing epoxy-based intumescent fire retardant coatings are prone to cracking and peeling at high temperatures, making it difficult to balance heat insulation performance and the stability of the intumescent char layer.
The coating employs a double-layer epoxy fire-retardant structure. The bottom layer contains polyboron siloxane-modified epoxy resin, hexagonal boron nitride, and nano-silica, while the top layer contains epoxy resin, ammonium polyphosphate, dipentaerythritol, melamine, expandable graphite, and low-melting-point glass powder. Through functional layering design, the bottom layer improves the bonding performance with the steel substrate, while the top layer forms a high-expansion carbon layer for heat insulation.
It effectively inhibits heat transfer to the steel substrate, improves the structural integrity and airflow erosion resistance of the expanded carbon layer, delays the temperature rise of the steel substrate, and enhances the overall fire resistance.
Smart Images

Figure CN123107499A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of fire-retardant coating technology, specifically relating to a double-layer epoxy fire-retardant coating, the coating itself, and its preparation method. Background Technology
[0002] Steel structures are widely used in modern construction and industrial fields due to their high strength and excellent workability. However, the yield strength of steel rapidly decreases under high temperatures (typically exceeding 500°C) during a fire, leading to structural failure. Intumescent fire-retardant coatings, when heated, can generate a porous carbon layer dozens of times thicker than the original layer, making them a primary means of protecting steel structures.
[0003] When heated, epoxy-based intumescent fire-retardant coatings form an expanded char layer, which slows down the temperature rise of the steel substrate by increasing heat transfer resistance. Its protective effect depends not only on the thickness of the char layer but also on factors such as the integrity of the char layer, the bonding state between the coating and the steel substrate, and the heating conditions.
[0004] Existing epoxy-based intumescent fire-retardant coatings are prone to cracking, peeling, or damage from airflow when heated, which can affect their continuous heat insulation performance.
[0005] Therefore, there is a need to provide an improved technical solution that addresses the shortcomings of the existing technology. Summary of the Invention
[0006] The purpose of this invention is to provide a double-layer epoxy fire-retardant coating, coating material and preparation method thereof, so as to solve the problem that existing epoxy intumescent fire-retardant coatings cannot simultaneously achieve thermal insulation performance and stability of the intumescent char layer.
[0007] To achieve the above objectives, the present invention provides the following technical solution: a double-layer epoxy fire-retardant coating, wherein the double-layer epoxy fire-retardant coating comprises a separately stored base coating and a top coating; by weight parts, the base coating comprises: 40-50 parts of polyboron siloxane modified epoxy resin, 15-25 parts of hexagonal boron nitride, 1-3 parts of nano-silica, 1-2 parts of epoxy silane coupling agent, 5-10 parts of diluent, and 10-15 parts of first curing agent; by weight parts, the top coating comprises: 30-40 parts of epoxy resin, 18-24 parts of ammonium polyphosphate, 8-12 parts of dipentaerythritol, 6-10 parts of melamine, 10-15 parts of expandable graphite, 5-10 parts of low-melting-point glass powder, 1-3 parts of boric acid, 5-10 parts of diluent, and 10-15 parts of second curing agent.
[0008] Preferably, the polyborosiloxane-modified epoxy resin is prepared by compounding and modifying bisphenol A type epoxy resin with a polyborosiloxane modifier; the mass of the polyborosiloxane modifier is 5%-15% of the mass of the bisphenol A type epoxy resin.
[0009] Preferably, the softening point temperature of the low-melting-point glass powder is 400℃-600℃, and the median particle size is 5-15μm; the particle size of the hexagonal boron nitride is 1-10μm, and the nano-silica is fumed silica with an average particle size of 10-30nm; the initial expansion temperature of the expandable graphite is 180℃-220℃, and the expansion ratio is 200-400 times.
[0010] The present invention also provides a double-layer epoxy fire-retardant coating, which adopts the following technical solution: a double-layer epoxy fire-retardant coating, wherein the double-layer epoxy fire-retardant coating is prepared by the double-layer epoxy fire-retardant coating described above; the double-layer epoxy fire-retardant coating includes a base layer coating formed by curing the base layer coating and a surface layer coating formed by curing the surface layer coating; the base layer coating is in contact with the surface of the steel substrate, and the surface layer coating is located on the side of the base layer coating away from the steel substrate.
[0011] The present invention also provides a method for preparing a double-layer epoxy fire-retardant coating, which adopts the following technical solution: The method for preparing a double-layer epoxy fire-retardant coating as described above includes the following steps: S1, applying the bottom coating to the surface of a steel substrate to obtain a bottom coating; S2, after the bottom coating is surface dry to the point where it is not sticky to the touch, applying the top coating to the surface of the bottom coating; S3, curing at room temperature to obtain the double-layer epoxy fire-retardant coating.
[0012] Preferably, the undercoat is prepared by a method comprising the following steps: mixing polyborosiloxane modified epoxy resin, epoxy silane coupling agent and diluent evenly, adding hexagonal boron nitride and nano silica for shear dispersion, and then adding the first curing agent and mixing evenly to obtain the undercoat.
[0013] Preferably, the dry film thickness of the bottom coating formed after the bottom coating has been fully cured is 0.5~1.0 mm; and the dry film thickness of the surface coating formed after the surface coating has been fully cured is 1.5~2.5 mm.
[0014] Preferably, the surface coating is prepared by a method comprising the following steps: mixing epoxy resin and diluent uniformly, sequentially adding ammonium polyphosphate, dipentaerythritol, melamine, low melting point glass powder and boric acid for shear dispersion, then reducing the shear speed and adding expandable graphite for uniform dispersion, and finally adding the second curing agent and mixing uniformly to obtain the surface coating.
[0015] Preferably, the expandable graphite is added after the shearing speed is reduced to 500-800 r / min.
[0016] Beneficial effects: (1) To address the problem of localized heat accumulation and easy detachment of the expanded char layer that may occur in traditional single-layer epoxy fireproof coatings under high temperatures, the double-layer epoxy fireproof coating of this invention forms a high-ratio expanded char layer on the surface layer after heating, which can effectively inhibit the transfer of heat to the steel substrate along the coating thickness direction; the bottom layer has a high thermal conductivity, which is conducive to the diffusion of localized heat transferred to the bottom layer along the surface of the substrate, thereby reducing localized heat concentration and improving the stability of the expanded char layer. The double-layer epoxy fireproof coating of this invention, through the longitudinal heat insulation effect of the surface layer (reducing the conduction of heat to the steel substrate) and the heat diffusion effect of the bottom layer, helps to delay the temperature rise of the unexposed surface of the steel substrate and improve the overall fire resistance of the double-layer epoxy fireproof coating.
[0017] (2) To address the problems of loose structure and easy cracking and peeling after heating in traditional expanded carbon layers, this invention introduces low-melting-point glass powder and boric acid into the surface coating. During heating, the low-melting-point glass powder softens to form a high-viscosity inorganic liquid phase, which wets and connects the carbon skeleton and phosphate high-temperature residues in the surface expanded carbon layer formed by the thermal reaction of ammonium polyphosphate, dipentaerythritol, melamine, and expandable graphite. Under continuous high temperature, a continuous glassy / ceramic-like inorganic protective phase is further formed inside and on the surface of the surface expanded carbon layer, thereby helping to improve the structural integrity and airflow erosion resistance of the surface expanded carbon layer. The formed glassy / ceramic-like inorganic protective phase can connect, coat, and strengthen the structure of the surface expanded carbon layer, thereby reducing the risk of cracking, local peeling, and structural damage of the surface expanded carbon layer under the action of high-temperature airflow, which is beneficial to maintaining the continuity and heat insulation protection of the surface expanded carbon layer.
[0018] (3) This invention achieves a layered configuration with different functions through a double-layer structure: the bottom coating does not primarily function as a high-expansion layer; the bottom coating uses polyborosiloxane-modified epoxy resin as the resin matrix, which is beneficial for improving the interfacial bonding performance between the bottom coating and the steel substrate and enhancing the structural stability of the bottom coating during heating; the top coating mainly forms an expanded char layer through the expansion flame-retardant system to provide thermal insulation and protection. Through the above functional layered design, it helps to reduce the adverse effects of the surface coating on the bottom coating and its interface with the steel substrate during the thermal expansion process, thereby helping to maintain the overall integrity of the double-layer epoxy fireproof coating during the fire process.
[0019] The double-layer epoxy fireproof coating of the present invention can be applied to petrochemical equipment, offshore platforms, high-rise steel structures, and other steel structure substrates that have both fire protection and thermal management requirements. Attached Figure Description
[0020] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. Wherein: Figure 1 These are comparative images of the cross-sectional morphology and expansion height of the expanded carbon layer formed after high-temperature burning of the double-layer epoxy fireproof coatings of Examples 1-5 of the present invention. Detailed Implementation
[0021] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention are within the scope of protection of the present invention.
[0022] The present invention will now be described in detail with reference to embodiments. It should be noted that, unless otherwise specified, the embodiments and features described in the embodiments of the present invention can be combined with each other.
[0023] This invention addresses the problem that traditional epoxy intumescent fire-retardant coatings struggle to balance high expansion ratios with thermal conductivity and poor durability by providing a double-layer epoxy fire-retardant coating.
[0024] The double-layer epoxy fire-retardant coating of this invention includes a separately stored base coat and a top coat; by weight, the base coat includes: 40-50 parts (e.g., 40, 42, 44, 46, 48, or 50 parts) of polyboronsiloxane modified epoxy resin, 15-25 parts (e.g., 15, 18, 21, 24, or 25 parts) of hexagonal boron nitride, and 1-3 parts (e.g., 1 part) of nano-silica. The coating comprises, by weight, 30-40 parts epoxy resin (e.g., 1 part, 2 parts, or 3 parts), 1-2 parts epoxy silane coupling agent (e.g., 1 part, 1.3 parts, 1.6 parts, 1.8 parts, or 2 parts), 5-10 parts diluent (e.g., 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, or 10 parts), and 10-15 parts first curing agent (e.g., 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, or 15 parts); the surface ... For example, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts or 40 parts); ammonium polyphosphate 18-24 parts (for example, 18 parts, 20 parts, 22 parts or 24 parts); dipentaerythritol 8-12 parts (for example, 8 parts, 9 parts, 10 parts, 11 parts or 12 parts); melamine 6-10 parts (for example, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts); expandable graphite 10-15 parts (for example, 10 parts, 11 parts, ... The components include: 12, 13, 14, or 15 parts of epoxy resin, 5-10 parts of low-melting-point glass powder (e.g., 5, 6, 7, 8, 9, or 10 parts), 1-3 parts of boric acid (e.g., 1, 2, or 3 parts), 5-10 parts of thinner (e.g., 5, 6, 7, 8, 9, or 10 parts), and 10-15 parts of a second curing agent (e.g., 10, 11, 12, 13, 14, or 15 parts). Both the primer and topcoat are two-component formulations, prepared and used immediately (each epoxy resin component and corresponding curing agent are stored separately and mixed according to the specified proportions before application). Polyborosiloxane-modified epoxy resin in the undercoat helps improve the high-temperature stability of the resin matrix and enhances the interfacial compatibility between the resin and inorganic components such as hexagonal boron nitride and nano-silica, thereby helping to maintain the structural integrity and filler dispersion stability of the undercoat. If ordinary epoxy resin is used instead of polyborosiloxane-modified epoxy resin, the structural stability of ordinary epoxy resin under high-temperature conditions is relatively limited. Furthermore, its interfacial bonding and compatibility with inorganic fillers may be weakened, potentially leading to decreased uniformity of inorganic filler dispersion, increased interfacial defects, and adverse effects on the thermal conductivity stability, interfacial bonding performance, and high-temperature structural integrity of the undercoat. Epoxy silane coupling agents help improve the interfacial compatibility and dispersibility between inorganic components such as hexagonal boron nitride and nano-silica and epoxy resin.
[0025] Preferably, the coating formed by the surface coating can form an expanded carbon layer after being heated, which helps to suppress the transfer of heat to the steel substrate along the coating thickness direction.
[0026] Preferably, the expansion behavior of the coating formed by the surface coating is jointly influenced by the ammonium polyphosphate / dipentaerythritol / melamine intumescent flame retardant system, expandable graphite, and resin matrix. The expansion ratio of the coating formed by the surface coating after heating is ≥40 times.
[0027] In a preferred embodiment of the double-layer epoxy fire-retardant coating of the present invention, the polyborosiloxane-modified epoxy resin is prepared by compounding and modifying bisphenol A type epoxy resin with a polyborosiloxane modifier. Preferably, the mass of the polyborosiloxane modifier is 5%-15% of the mass of the bisphenol A type epoxy resin (for example, 5%, 8%, 11%, 13%, or 15%). The addition of the polyborosiloxane modifier is beneficial for introducing boron- and silicon-containing structures into the epoxy resin system, thereby improving the thermal stability of the resin matrix and the interfacial compatibility between the resin and the inorganic filler. When the amount of polyborosiloxane modifier added is too low, the degree of modification of the epoxy resin is limited, and it is difficult to fully exert its role in improving high-temperature stability and interfacial compatibility; when the amount of polyborosiloxane modifier added is too high, it may have a significant impact on the original curing and crosslinking process of the epoxy resin and the viscosity of the system, thereby affecting the coating's application performance, curing performance, and mechanical properties. Therefore, taking into account both the resin modification effect and the film-forming and application properties of the coating, the preferred amount of polyborosiloxane modifier is 5%-15% of the mass of bisphenol A epoxy resin.
[0028] Preferably, the polyborosiloxane modifier is prepared by a method comprising the following steps: A1, mixing hydroxyl silicone oil with boric acid to obtain a mixture; A2, heating the mixture to 160–190°C (e.g., 160°C, 170°C, 180°C, or 190°C) and continuing the reaction for 1–4 hours (e.g., 1 hour, 2 hours, 3 hours, or 4 hours), continuously stirring during the reaction, and removing the water generated by the condensation reaction from the reaction system, so that the terminal hydroxyl groups in the hydroxyl silicone oil undergo a dehydration condensation reaction with the boric acid, and cooling to room temperature to obtain the polyborosiloxane modifier (containing a Si-OB structure). In step A1, the hydroxyl silicone oil is a hydroxyl-terminated polydimethylsiloxane, and the mass ratio of hydroxyl silicone oil to boric acid is 10:1–40:1 (e.g., 10:1, 20:1, 30:1, or 40:1), preferably 20:1; in step A2, the reaction is preferably carried out at 180°C for 2 hours.
[0029] The "polyborosiloxane modifier" in this invention does not refer to all types of polyborosiloxane materials, but rather to boron-containing organosilicon polymers formed by dehydration condensation of the above-mentioned hydroxyl-terminated polydimethylsiloxane and boric acid as the main raw materials.
[0030] The polyborosiloxane-modified epoxy resin was prepared by the following method: Bisphenol A type epoxy resin was heated to 80°C, and a polyborosiloxane modifier was slowly added under stirring. The amount of polyborosiloxane modifier added was 5%–15% of the mass of the bisphenol A type epoxy resin. After addition, stirring was continued for 60 minutes at 80°C and 500 r / min to ensure uniform dispersion of the polyborosiloxane modifier in the bisphenol A type epoxy resin. The resin was then cooled to room temperature to obtain the polyborosiloxane-modified epoxy resin. The heating and stirring were used to promote mixing and uniform dispersion of the components; no curing agent was added in this step.
[0031] The B and Si structures contained in polyborosiloxanes are beneficial for improving the thermal stability and high-temperature residual structural stability of epoxy resin systems. They also help improve the interfacial compatibility between the epoxy resin matrix and inorganic fillers such as hexagonal boron nitride and nano-silica, thus helping to maintain the structural integrity of the underlying coating during heating. Epoxysilane coupling agents can also improve the interfacial bonding between inorganic fillers and the epoxy resin matrix to some extent. Therefore, through the synergistic effect of polyborosiloxane-modified epoxy resin, hexagonal boron nitride, nano-silica, and epoxysilane coupling agents, structural damage to the underlying coating during heating can be reduced.
[0032] In a preferred embodiment of the double-layer epoxy fire-retardant coating of the present invention, the softening point temperature of the low-melting-point glass powder is 400℃~600℃ (for example, 400℃, 450℃, 500℃, 550℃, or 600℃). If the softening point temperature of the low-melting-point glass powder is too low, it may soften and form a liquid phase before the surface expansion flame-retardant system has fully foamed and charred, thus adversely affecting the formation and volume development of the expanded char layer, limiting the thickness and porous structure formation of the expanded char layer. If the softening point temperature of the low-melting-point glass powder is too high, it is difficult to soften and form a liquid phase in time during the formation and high-temperature evolution of the surface expanded char layer, thus hindering the full effect of wetting, connecting, and structurally reinforcing the high-temperature residual components in the expanded char layer, which is detrimental to maintaining the structural integrity of the expanded char layer. Therefore, limiting the softening point temperature of the low-melting-point glass powder to the range of 400℃~600℃ is beneficial for balancing the expansion and charring process of the surface coating with the subsequent formation of the inorganic protective phase under high-temperature conditions.
[0033] In a preferred embodiment of the double-layer epoxy fire-retardant coating of the present invention, the median particle size of the low-melting-point glass powder is 5–15 μm; the particle size of hexagonal boron nitride is 1–10 μm; the nano-silica is fumed silica with an average particle size of 10–30 nm; and the initial expansion temperature of the expandable graphite is 180°C–220°C (e.g., 180°C, 190°C, 200°C, 210°C, or 220°C), with an expansion ratio of 200–400 times (e.g., 200 times, 250 times, 300 times, 350 times, or 400 times). Under high temperature, the low-melting-point glass powder softens to form an inorganic liquid phase, which interacts with boric acid and the high-temperature residual components in the surface expanded carbon layer. This facilitates the formation of a continuous glassy or ceramic-like inorganic protective phase inside and on the surface of the surface expanded carbon layer, thereby helping to improve the structural stability and integrity of the surface expanded carbon layer.
[0034] The present invention also proposes a double-layer epoxy fireproof coating, wherein the double-layer epoxy fireproof coating of the present invention is prepared by using the double-layer epoxy fireproof coating as described above.
[0035] The present invention also proposes a method for preparing a double-layer epoxy fireproof coating. The method for preparing the double-layer epoxy fireproof coating in the embodiments of the present invention includes the following steps: S1, applying a base coat to the surface of a steel substrate to obtain a base coat; S2, after the base coat is surface dry to the point where it is no longer sticky to the touch, applying a top coat to the surface of the base coat; S3, curing at room temperature to obtain a double-layer epoxy fireproof coating.
[0036] In a preferred embodiment of the preparation method of the double-layer epoxy fireproof coating of the present invention, the bottom coating is prepared by a method including the following steps: polyboron siloxane modified epoxy resin, epoxy silane coupling agent and diluent are mixed evenly, hexagonal boron nitride and nano silica are added for shear dispersion, and then a first curing agent is added and mixed evenly to obtain the bottom coating.
[0037] In a preferred embodiment of the preparation method of the double-layer epoxy fire-retardant coating of the present invention, the dry film thickness of the bottom layer coating formed after the bottom layer coating has been fully cured is 0.5-1.0 mm (e.g., 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, or 1.0 mm); the dry film thickness of the top layer coating formed after the top layer coating has been fully cured is 1.5-2.5 mm (e.g., 1.5 mm, 1.8 mm, 2.0 mm, 2.3 mm, or 2.5 mm). Herein, "dry film thickness" refers to the final coating thickness measured after the corresponding coating has been applied and fully cured. The bottom layer coating has good thermal conductivity, which helps dissipate heat; the top layer coating helps achieve longitudinal insulation, reducing heat conduction towards the steel substrate.
[0038] In a preferred embodiment of the preparation method of the double-layer epoxy fireproof coating of the present invention, the surface coating is prepared by a method including the following steps: epoxy resin and diluent are mixed evenly, and ammonium polyphosphate, dipentaerythritol, melamine, low melting point glass powder and boric acid are added slowly in sequence for shear dispersion (the shear dispersion speed can be 2500 r / min). Then, the shear speed is reduced and expandable graphite is added and dispersed evenly. Finally, a second curing agent is added and mixed evenly to obtain the surface coating.
[0039] In a preferred embodiment of the preparation method of the double-layer epoxy fire-retardant coating of the present invention, the expandable graphite is added after the shearing speed is reduced to 500-800 r / min (e.g., 500 r / min, 600 r / min, 700 r / min or 800 r / min).
[0040] The following detailed description of the double-layer epoxy fire-retardant coating, coating material, and preparation method of the present invention is provided through specific embodiments.
[0041] Unless otherwise specified, all raw materials used in the following embodiments are commercially available. To further illustrate the types and performance parameters of the raw materials used in this invention, the raw materials may, for example, be the following commercially available products.
[0042] Bisphenol A type epoxy resin can be E-51 type epoxy resin, such as CYD-128 type epoxy resin produced by Sinopec Baling Petrochemical (CYD-128 is a commercially available brand name of E-51 type epoxy resin).
[0043] Boric acid used to prepare polyborosiloxane modifiers can be the product of Shanghai Aladdin Biochemical Technology Co., Ltd., item number B111604, with a purity ≥99.5%; hydroxyl silicone oil can be hydroxyl-terminated polydimethylsiloxane, such as hydroxyl-terminated polydimethylsiloxane products from Sigma-Aldrich.
[0044] Hexagonal boron nitride (h-BN) can be made from 3M's Boron Nitride Cooling Filler Platelets, such as the CFP 007HS type plate hexagonal boron nitride, with a D50 particle size of about 5-8 μm and a BN content of more than 98.5%, and can be used as a thermally conductive filler in epoxy resin systems.
[0045] Nano-silica can be produced by Evonik Operations GmbH. 200 hydrophilic fumed silica has an average primary particle size of approximately 12 nm and a specific surface area of approximately 200 m². 2 / g, suitable for coatings and resin systems.
[0046] Epoxysilane coupling agents can be γ-glycidyl etheroxypropyltrimethoxysilane coupling agents, such as those produced by Momentive Performance Materials. A-187 is an epoxy-functionalized silane that can be used to improve the interfacial bonding between epoxy systems and inorganic fillers.
[0047] Low-melting-point glass powder can be Bi-B-Zn series lead-free low-melting-point glass powder produced by Guizhou Baibo New Material Technology Co., Ltd. This company has Bi2O3-B2O3-ZnO type low-melting-point glass powder products, and the particle size can be adjusted according to requirements. Specifically, the glass powder used should have a softening temperature within the range of 400-600℃ defined in this invention, and a median particle size D50 within the range of 5-15μm. Specific indicators are subject to the technical specifications or factory inspection report of the corresponding product batch.
[0048] Ammonium polyphosphate (APP) can be produced by Clariant. AP 422 type ammonium polyphosphate. This product is a fine-particle type II ammonium polyphosphate with low water solubility, suitable for intumescent fire-retardant coating systems.
[0049] Dipentaerythritol (DPER, CAS 126-58-9) can be commercially available products with a purity of not less than 98%, such as the 98% purity dipentaerythritol supplied by Shaanxi Dideu New Materials Co., Ltd.; in actual use, the purity recorded in the COA provided by the supplier shall prevail.
[0050] Melamine (MEL) can be Sigma-Aldrich M2659 melamine with a purity of 99%, or commercially available melamine products with comparable purity and particle size.
[0051] Expandable graphite (EG) uses low-temperature expandable graphite of approximately 100 mesh, with an optimal initial expansion temperature of 180-220℃. Expandable graphite can be sourced from domestic graphite material manufacturers such as Heilongjiang Guangshengda New Material Technology Co., Ltd., China Building Materials Heilongjiang Graphite New Material Co., Ltd., and Jixi Zhonghui Graphite Products Co., Ltd. Specific particle size, initial expansion temperature, and expansion ratio of the products are subject to the product technical specifications or the corresponding batch COA.
[0052] Example 1 The double-layer epoxy fire-retardant coating of this embodiment includes a separately stored base coat and a top coat. By weight, the base coat comprises: 45 parts of polyboron-siloxane modified epoxy resin, 20 parts of hexagonal boron nitride, 2 parts of nano-silica, 1.5 parts of epoxy silane coupling agent (KH560), 8 parts of diluent, and 14 parts of a first curing agent. The diluent is composed of xylene and n-butanol in a weight ratio of 3:1, and the first curing agent is… D-230 polyetheramine curing agent.
[0053] The polyborosiloxane-modified epoxy resin was prepared using a method comprising the following steps: (1) Preparation of polyborosiloxane modifier: Weigh 100 parts by mass of hydroxyl-terminated polydimethylsiloxane and 5 parts by mass of boric acid (so that the mass ratio of hydroxyl-terminated polydimethylsiloxane to boric acid is 20:1), mix the two and stir thoroughly until they are evenly dispersed; then heat to 180℃ and keep warm for 2 hours, stirring continuously during the heating process to allow the hydroxyl siloxane structure to undergo a condensation reaction with boric acid and promote the release of water generated during the reaction; after the reaction is completed, cool naturally to room temperature to obtain a polyborosiloxane modifier containing Si-OB structure.
[0054] (2) Preparation of polyborosiloxane-modified epoxy resin: Weigh 100 parts by weight of bisphenol A type E-51 epoxy resin, heat to 80°C and stir. Under continuous stirring, slowly add 10 parts of the polyborosiloxane modifier obtained in step (1), and continue stirring at a speed of 500 r / min for 60 min to uniformly disperse the polyborosiloxane modifier in the epoxy resin system. After mixing, cool to room temperature to obtain polyborosiloxane-modified epoxy resin. In this embodiment, the amount of polyborosiloxane modifier added is 10% of the mass of bisphenol A type epoxy resin.
[0055] By weight, the surface coating comprises: 35 parts epoxy resin, 20 parts ammonium polyphosphate (APP), 9 parts dipentaerythritol (DPER), 6 parts melamine (MEL), 12 parts expandable graphite, 8 parts low-melting-point glass powder, 2 parts boric acid, 8 parts diluent, and 11 parts second curing agent; wherein the diluent is composed of xylene and n-butanol in a weight ratio of 3:1, and the second curing agent is... D-230 polyetheramine curing agent.
[0056] The application amounts of the base coat and top coat are controlled based on the dry film thickness after the respective coatings have fully cured. In this embodiment, the dry film thickness of the base coat after full curing is 0.7 mm, and the dry film thickness of the top coat after full curing is 1.8 mm, thereby forming a double-layer epoxy fireproof coating with a total dry film thickness of 2.5 mm.
[0057] The preparation method of the double-layer epoxy fire-retardant coating in this embodiment includes the following steps: S1. Preparation of the primer: Polyborosiloxane-modified epoxy resin, diluent, and epoxy silane coupling agent KH560 were added to a dispersion container and stirred at 500 r / min. Hexagonal boron nitride and nano-silica were then slowly added, and the stirring speed was increased to 3500 r / min and dispersion continued for 60 min. The fineness of the slurry was controlled to be no greater than 40 μm using a scraper fineness meter to obtain the primer base agent. Before application, D-230 polyetheramine curing agent was added according to the formula in this embodiment and mixed evenly under low-speed stirring to obtain the primer.
[0058] Preparation of the surface coating: Epoxy resin was mixed evenly with a mixed diluent consisting of xylene and n-butanol in a mass ratio of 3:1. Ammonium polyphosphate (APP), dipentaerythritol (DPER), melamine (MEL), low-melting-point glass powder, and boric acid were added sequentially under stirring. The mixture was dispersed under high shear at 2500 rpm for 40 min. Then, the speed of the disperser was reduced to 600 rpm, and expandable graphite was slowly added and dispersed evenly. Finally, the second curing agent was added and mixed evenly under low-speed stirring to obtain the surface coating.
[0059] S2. Sandblast the surface of the steel substrate to Sa2.5 level, and apply the base coat to the surface of the steel substrate using an airless spraying method; cure at 25℃ for 3 hours to allow the base coat to reach a surface-dry state where it is not sticky to the touch, thus obtaining the base coating. S3. Spray the topcoat onto the surface of the base coating. S4. The sample with the completed surface coating is cured at 20-30℃ for 7 days to allow the base coat and the surface coat to fully cure, resulting in a double-layer epoxy fireproof coating with a total dry film thickness of 2.5mm (the dry film thickness of the base coat after full curing is 0.7mm, and the dry film thickness of the surface coat after full curing is 1.8mm).
[0060] Example 2 The double-layer epoxy fire-retardant coating of this embodiment includes a separately stored base coat and a top coat.
[0061] By weight, the base coat comprises: 45 parts of polyboron siloxane modified epoxy resin (same as in Example 1), 25 parts of hexagonal boron nitride, 2 parts of nano silica, 1.5 parts of epoxy silane coupling agent (KH560), 8 parts of diluent (same as in Example 1), and 14 parts of first curing agent (same as in Example 1). By weight, the surface coating comprises: 35 parts epoxy resin (same as in Example 1), 20 parts ammonium polyphosphate (APP), 9 parts dipentaerythritol (DPER), 6 parts melamine (MEL), 10 parts expandable graphite, 6 parts low melting point glass powder, 1 part boric acid, 8 parts diluent (same as in Example 1), and 11 parts second curing agent (same as in Example 1).
[0062] The double-layer epoxy fire-retardant coating in this embodiment is prepared using the aforementioned double-layer epoxy fire-retardant paint, and its preparation method is the same as in Example 1. The application amounts of the base coat and the top coat are controlled based on the dry film thickness after the respective coatings have fully cured. In this embodiment, the dry film thickness of the base coat after full curing is 0.7 mm, the dry film thickness of the top coat after full curing is 1.8 mm, and the total dry film thickness of the double-layer epoxy fire-retardant coating is 2.5 mm.
[0063] Example 3 The double-layer epoxy fire-retardant coating of this embodiment includes a separately stored base coat and a top coat.
[0064] By weight, the base coat comprises: 45 parts of polyboron siloxane modified epoxy resin (same as in Example 1), 15 parts of hexagonal boron nitride, 2 parts of nano silica, 1.5 parts of epoxy silane coupling agent (KH560), 8 parts of diluent (same as in Example 1), and 14 parts of first curing agent (same as in Example 1); wherein the composition of the diluent and the type of curing agent are the same as in Example 1.
[0065] By weight, the surface coating comprises: 35 parts epoxy resin (same as in Example 1), 18 parts ammonium polyphosphate (APP), 10 parts dipentaerythritol (DPER), 7 parts melamine (MEL), 14 parts expandable graphite, 10 parts low melting point glass powder, 3 parts boric acid, 8 parts diluent (same as in Example 1), and 11 parts second curing agent (same as in Example 1); wherein the composition of the diluent and the type of curing agent are the same as in Example 1.
[0066] The double-layer epoxy fire-retardant coating in this embodiment is prepared using the aforementioned double-layer epoxy fire-retardant paint, and its preparation method is the same as in Example 1. The application amounts of the primer and topcoat are controlled based on the dry film thickness after the respective coatings have fully cured. In this embodiment, the dry film thickness of the primer after full curing is 0.7 mm, the dry film thickness of the topcoat after full curing is 1.8 mm, and the total dry film thickness of the double-layer epoxy fire-retardant coating is 2.5 mm.
[0067] Example 4 The double-layer epoxy fire-retardant coating of this embodiment includes a separately stored base coat and a top coat.
[0068] By weight, the base coat comprises: 40 parts of polyboron siloxane modified epoxy resin (same as in Example 1), 15 parts of hexagonal boron nitride, 1 part of nano silica, 1 part of epoxy silane coupling agent (KH560), 5 parts of diluent (same as in Example 1), and 12 parts of first curing agent (same as in Example 1). By weight, the surface coating comprises: 30 parts epoxy resin (same as in Example 1), 18 parts ammonium polyphosphate (APP), 8 parts dipentaerythritol (DPER), 9 parts melamine (MEL), 10 parts expandable graphite, 5 parts low melting point glass powder, 1 part boric acid, 5 parts diluent (same as in Example 1), and 10 parts second curing agent (same as in Example 1).
[0069] The preparation methods for the base coat, top coat, and double-layer epoxy fire-retardant coating in this embodiment are the same as in Example 1, and each raw material is weighed according to the mass proportions listed in this embodiment. In this embodiment, the dry film thickness of the base coat after full curing is 0.7 mm, the dry film thickness of the top coat after full curing is 1.8 mm, and the total dry film thickness of the double-layer epoxy fire-retardant coating is 2.5 mm.
[0070] Example 5 The double-layer epoxy fire-retardant coating of this embodiment includes a separately stored base coat and a top coat.
[0071] By weight, the base coat comprises: 50 parts of polyboron siloxane modified epoxy resin (same as in Example 1), 25 parts of hexagonal boron nitride, 3 parts of nano silica, 2 parts of epoxy silane coupling agent (KH560), 10 parts of diluent (same as in Example 1), and 15 parts of first curing agent (same as in Example 1).
[0072] By weight, the surface coating comprises: 40 parts epoxy resin (same as in Example 1), 20 parts ammonium polyphosphate (APP), 8 parts dipentaerythritol (DPER), 7 parts melamine (MEL), 15 parts expandable graphite, 10 parts low melting point glass powder, 3 parts boric acid, 10 parts diluent (same as in Example 1), and 13 parts second curing agent (same as in Example 1).
[0073] The preparation method of the double-layer epoxy fireproof coating in this embodiment is the same as that in Example 1; the dry film thickness of the bottom coating after full curing is 0.7 mm, the dry film thickness of the top coating after full curing is 1.8 mm, and the total dry film thickness of the double-layer epoxy fireproof coating is 2.5 mm.
[0074] Comparative Example 1 This comparative example uses a single-layer hybrid fire-retardant coating, which combines the resin and functional components from the primer and topcoat of Example 1, and forms a single-layer coating on the surface of a steel substrate for performance comparison with the double-layer coating of Example 1. Specifically: By weight, the single-layer mixed fire-retardant coating of this comparative example comprises: 45 parts of polyboron siloxane modified epoxy resin (same as in Example 1), 35 parts of epoxy resin (same as in Example 1), 20 parts of hexagonal boron nitride, 2 parts of nano silica, 1.5 parts of epoxy silane coupling agent KH560, 20 parts of ammonium polyphosphate, 9 parts of dipentaerythritol, 6 parts of melamine, 12 parts of expandable graphite, 8 parts of low melting point glass powder, 2 parts of boric acid, 16 parts of diluent (same as in Example 1), and 25 parts of curing agent (same as in Example 1).
[0075] The single-layer hybrid fire-retardant coating of this comparative example was applied to the surface of a steel substrate that had been sandblasted to Sa2.5 grade, forming a coating without distinguishing between the base layer and the top layer formulation. The total dry film thickness after full curing was 2.5 mm, so that its total dry film thickness was consistent with that of the double-layer epoxy fire-retardant coating of Example 1.
[0076] Comparative Example 2 The only difference between this comparative example and Example 1 is that low-melting-point glass powder and boric acid are not added to the surface coating; all other aspects are the same as in Example 1.
[0077] Comparative Example 3 The difference between this comparative example and Example 1 is that hexagonal boron nitride is not added to the undercoat; all other aspects are the same as in Example 1.
[0078] Comparative Example 4 The only difference between this comparative example and Example 1 is that expandable graphite was added and dispersed at 2500 r / min when preparing the surface coating; all other aspects are the same as in Example 1.
[0079] Comparative Example 5 The only difference between this comparative example and Example 1 is that in the base coat, 45 parts of bisphenol A type E-51 epoxy resin are used instead of 45 parts of polyborosiloxane modified epoxy resin; all other aspects are the same as in Example 1.
[0080] Comparative Example 6 The only difference between this comparative example and Example 1 is that the amount of polyborosiloxane modifier added during the preparation of the polyborosiloxane modified epoxy resin is 3% of that of the bisphenol A type epoxy resin; all other aspects are consistent with Example 1.
[0081] Comparative Example 7 The only difference between this comparative example and Example 1 is that, in the preparation of the polyborosiloxane modified epoxy resin, the amount of polyborosiloxane modifier added is adjusted to 17% of the mass of bisphenol A type E-51 epoxy resin; the rest remains the same as in Example 1.
[0082] Comparative Example 8 The only difference between this comparative example and Example 1 is that this comparative example uses a single-layer fire-retardant coating, and the single-layer fire-retardant coating in this comparative example is the same as the surface coating in Example 1 (the dry film thickness of the single-layer fire-retardant coating is 2.5 mm); all other aspects are consistent with Example 1.
[0083] Comparative Example 9 The only difference between this comparative example and Example 1 is that the dry film thickness of the bottom coating in this comparative example after it has been fully dried and cured is 0.3 mm (the dry film thickness of the top coating after it has been fully dried and cured is 2.2 mm); all other aspects are the same as in Example 1.
[0084] Comparative Example 10 The only difference between this comparative example and Example 1 is that the dry film thickness of the bottom coating in this comparative example after it has been fully dried and cured is 1.2 mm (the dry film thickness of the top coating after it has been fully dried and cured is 1.3 mm); all other aspects are the same as in Example 1.
[0085] Experimental Example The performance of the double-layer epoxy fire-retardant coating of the present invention was tested: Temperature rise test of the back-fired side of the steel plate: A 150mm×150mm×3mm Q235 steel plate was used as the substrate, and the total dry film thickness of the coating was controlled at 2.5±0.1mm. The coated side of the sample was placed facing the heat source, and the temperature inside the test furnace was controlled according to the ISO 834 standard temperature rise curve. The temperature change over time at each measuring point on the back-fired side of the steel plate was recorded. All groups of samples used the same clamping method, effective exposed area, edge treatment method, and temperature measuring point arrangement. The time when the arithmetic mean temperature at the specified measuring points on the back-fired side first reached 500℃ was used as the comparison index, denoted as t. 500 .
[0086] Carbon layer compressive strength test: A miniature universal testing machine was used. The carbon layer, after being treated with a specified heating procedure and cooled, was prepared into a specimen with a compression surface size of 30mm × 30mm. The specimen height was measured and recorded. Compression tests were performed using the testing machine at a loading rate of 2mm / min. The load-displacement curve was recorded, and the maximum load Fmax was determined according to the specified carbon layer collapse criterion. The carbon layer compressive strength was calculated as σ = Fmax / Calculation, where This represents the initial compressive area of the sample. Fmax is expressed in N. In mm 2 The unit of σ is MPa. The char layer compressive strength is used to evaluate the structural stability of the expanded char layer formed after the intumescent fire-retardant coating is heated. It mainly reflects the ability of the expanded char layer to resist compressive deformation, collapse, and damage. A higher char layer compressive strength indicates that the expanded char layer has better structural integrity, which is beneficial for maintaining the continuity of the heat insulation protective layer during fire exposure.
[0087] Thermal conductivity testing: Cured samples were prepared using the base coats of each group, and the thermal conductivity was determined using the hot wire method specified in GB / T 10297-2015. Comparative Example 1 used its single-layer mixed fire-retardant coating to prepare cured samples. All groups used the same sample preparation method, curing conditions, test temperature, and instrument settings, and the thermal conductivity of the corresponding cured materials under the test conditions was recorded.
[0088] Expansion ratio test: Measure the total dry film thickness of the coating on the sample before heating. Each group of samples was treated with the same heating program and heating time. After cooling, the height from the surface of the steel substrate to the outer surface of the residual coating was measured at specified measuring points, and the arithmetic mean was taken. Overall expansion ratio according to calculate.
[0089] Airflow erosion resistance test: The sample, after being burned under specified conditions to form a complete expanded carbon layer, is fixed. A stable airflow is used to vertically scour the surface of the carbon layer at a certain distance from the carbon layer surface for 60 seconds. After scouring, the carbon layer is observed and recorded for phenomena such as cracking, pitting, local detachment, or large-area peeling to evaluate the airflow erosion resistance of the expanded carbon layer.
[0090] The test results are shown in Table 1 below: Table 1. Comparison of performance test results between the examples and comparative examples.
[0091] The samples used for evaluating the compressive strength, overall expansion ratio, and resistance to airflow erosion of the carbon layer were treated with the same heating program, heating time, and cooling method.
[0092] As shown in Table 1, under the experimental conditions, the t values of Examples 1-5 were... 500 The time was 84–92 min, compared to 66 min for Comparative Example 1. These results indicate that, under the same total dry film thickness, the double-layer epoxy fire-retardant coating of this invention has a better performance in delaying the temperature rise of the unexposed surface of the steel plate compared to the single-layer hybrid fire-retardant coating of Comparative Example 1.
[0093] Compared to Example 1, Comparative Example 2, which did not include low-melting-point glass powder and boric acid, showed a decrease in the compressive strength of its carbon layer from 0.26 MPa to 0.08 MPa, and a decline in the integrity of the carbon layer after airflow erosion. These results indicate that the combined addition of low-melting-point glass powder and boric acid helps improve the mechanical properties and airflow erosion resistance of the carbon layer.
[0094] Compared to Example 1, Comparative Example 3 did not contain hexagonal boron nitride, and the thermal conductivity of its underlayer cured material increased from 1.12 W / ( Reduced to 0.21W / ( ), t500 The time was reduced from 92 min to 69 min. These results indicate that the addition of hexagonal boron nitride improved the thermal conductivity of the bottom layer material, and the corresponding bilayer sample exhibited a longer t... 500 .
[0095] Compared to Example 1, in Comparative Example 4, expandable graphite was added and dispersed at 2500 r / min, resulting in an overall expansion ratio that decreased from 47 to 28. 500 The time was reduced from 92 min to 76 min. The above results indicate that, with other conditions remaining constant, the dispersion speed during the expansion graphite addition stage affects the expansion and thermal insulation performance of the coating. The 600 r / min condition used in this experiment has better overall performance.
[0096] Compared to Example 1, Comparative Example 5 used an equal mass of ordinary bisphenol A type E-51 epoxy resin instead of polyborosiloxane modified epoxy resin, and its t 500 As the time decreased from 92 min to 71 min, the compressive strength of the char layer decreased from 0.26 MPa to 0.20 MPa. These results indicate that replacing the underlying resin system affects the fire-retardant properties of the double-layer coating.
[0097] In Comparative Examples 6 and 7, the amounts of polyborosiloxane modifier added were 3% and 17% of the mass of bisphenol A type E-51 epoxy resin, respectively, corresponding to t 500 The measured times were 85 min and 78 min, respectively, both lower than the 92 min achieved with a 10% addition in Example 1. These results indicate that among the three addition amounts compared, the 10% addition amount resulted in the best performance in delaying the temperature rise of the unexposed side. When the amount of polyborosiloxane modifier added is too high during the preparation of polyborosiloxane-modified epoxy resin, the excessive polyborosiloxane structure may affect the original curing and crosslinking process of the epoxy resin system, potentially leading to significant changes in the system's viscosity and rheological properties. This can adversely affect the coating's application performance, curing film-forming properties, and the structural stability of the cured coating.
[0098] Figure 1 Comparison of cross-sectional morphology and expansion height of the expanded carbon layer formed after high-temperature burning of the double-layer epoxy fireproof coatings in Examples 1-5 of the present invention; Depend on Figure 1It can be seen that under the same heating conditions, Examples 1 to 5 all formed continuous expanded char layers, indicating that the surface expansion flame retardant system described in this invention can effectively promote the thermal expansion of the coating into char. Among them, the expanded char layer formed in Example 3 has a relatively large thickness, which is consistent with the test results in Table 1 showing that Example 3 has a high overall expansion ratio (51 times) and a high char layer compressive strength (0.32 MPa). The expanded char layers formed in Examples 1 and 5 also maintain good continuity and integrity, corresponding to their high overall expansion ratio and good char layer state after airflow scouring. The expanded char layer formed in Example 4 has a slightly lower thickness, but still maintains a basically intact structure, which is consistent with the results in Table 1 showing that its overall expansion ratio is relatively low and that there is slight cracking after airflow scouring.
[0099] The above results indicate that the present invention, through the synergistic effect of the surface expansion flame retardant system, low melting point glass powder, and boric acid reinforcing components, can form an expanded char layer with a certain thickness and structural stability, thereby helping to maintain the heat insulation and protection effect during the fire process.
[0100] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A double-layer epoxy fire-retardant coating, characterized in that, The double-layer epoxy fireproof coating includes a separately stored base coat and a top coat; By weight, the underlying coating comprises: 40-50 parts of polyboron siloxane modified epoxy resin, 15-25 parts of hexagonal boron nitride, 1-3 parts of nano silica, 1-2 parts of epoxy silane coupling agent, 5-10 parts of diluent, and 10-15 parts of first curing agent. By weight, the surface coating comprises: 30-40 parts epoxy resin, 18-24 parts ammonium polyphosphate, 8-12 parts dipentaerythritol, 6-10 parts melamine, 10-15 parts expandable graphite, 5-10 parts low melting point glass powder, 1-3 parts boric acid, 5-10 parts diluent, and 10-15 parts second curing agent.
2. The double-layer epoxy fire-retardant coating as described in claim 1, characterized in that, The polyborosiloxane-modified epoxy resin is prepared by compounding and modifying bisphenol A type epoxy resin with a polyborosiloxane modifier. The mass of the polyborosiloxane modifier is 5%-15% of the mass of the bisphenol A type epoxy resin.
3. The double-layer epoxy fire-retardant coating as described in claim 1, characterized in that, The softening point temperature of the low melting point glass powder is 400℃-600℃, and the median particle size is 5-15μm; The hexagonal boron nitride has a particle size of 1-10 μm, and the nano-silica is fumed silica with an average particle size of 10-30 nm. The expandable graphite has an initial expansion temperature of 180℃-220℃ and an expansion ratio of 200-400 times.
4. A double-layer epoxy fire-retardant coating, characterized in that, The double-layer epoxy fireproof coating is prepared using the double-layer epoxy fireproof coating described in any one of claims 1 to 3; The double-layer epoxy fireproof coating includes a base coating formed by curing the base coating and a surface coating formed by curing the surface coating. The undercoat is in contact with the surface of the steel substrate, and the topcoat is located on the side of the undercoat away from the steel substrate.
5. The method for preparing the double-layer epoxy fire-retardant coating as described in claim 4, characterized in that, Includes the following steps: S1. Adhere the underlying coating to the surface of the steel substrate to obtain the underlying coating layer; S2. After the bottom coating is dry to the point where it is no longer sticky to the touch, the top coating is applied to the surface of the bottom coating. S3. Curing at room temperature yields the double-layer epoxy fireproof coating.
6. The method for preparing the double-layer epoxy fire-retardant coating as described in claim 5, characterized in that, The underlying coating is prepared by a method including the following steps: polyborosiloxane modified epoxy resin, epoxy silane coupling agent and diluent are mixed evenly, hexagonal boron nitride and nano silica are added for shear dispersion, and then the first curing agent is added and mixed evenly to obtain the underlying coating.
7. The method for preparing the double-layer epoxy fire-retardant coating as described in claim 5, characterized in that, The dry film thickness of the underlying coating formed after the underlying coating has fully cured is 0.5~1.0 mm; The dry film thickness of the surface coating formed after the surface coating has fully cured is 1.5~2.5mm.
8. The method for preparing the double-layer epoxy fire-retardant coating as described in claim 5, characterized in that, The surface coating is prepared by a method including the following steps: epoxy resin and diluent are mixed evenly, ammonium polyphosphate, dipentaerythritol, melamine, low melting point glass powder and boric acid are added sequentially for shear dispersion, then expandable graphite is added and dispersed evenly by reducing the shear speed, and finally the second curing agent is added and mixed evenly to obtain the surface coating.
9. The method for preparing the double-layer epoxy fire-retardant coating as described in claim 8, characterized in that, The expandable graphite was added after the shearing speed was reduced to 500-800 r / min.