A weather-resistant and wear-resistant waterborne polyurethane coating and its preparation method

Modified polycarbonate polyols were prepared by grafting modified nano-silica sol with isocyanate-terminated polycarbonate prepolymers, which solved the problems of weather resistance and abrasion resistance of waterborne polyurethane coatings in outdoor use and improved the weather resistance and abrasion resistance of the coating film.

CN123107518APending Publication Date: 2026-11-17JIANGXI HENGYI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611582347.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing waterborne polyurethane coatings suffer from insufficient film hardness, reduced abrasion resistance, sticky surface, loss of gloss, or yellowing during long-term outdoor use. Furthermore, nanoparticles tend to agglomerate in waterborne resins, affecting emulsion stability and application performance.

Method used

Organic solvent-dispersible modified nano-silica sol was prepared by modifying nano-silica sol with aminosilane and then dehydrating it by solvent displacement. Modified polycarbonate polyol was prepared by grafting it with isocyanate-terminated polycarbonate prepolymer. This modified polycarbonate polyol was then used in the preparation of waterborne polyurethane emulsions to improve the controllability of nano-component introduction and the weather resistance and wear resistance of the coating film.

Benefits of technology

It improves the weather resistance, abrasion resistance, and abrasion resistance retention of the coating film, while maintaining the workability and flexibility of the water-based system and reducing the risk of nanoparticle aggregation and emulsion stability decline.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention belongs to the field of waterborne coating technology and discloses a weather-resistant and wear-resistant waterborne polyurethane coating and its preparation method. The preparation method includes: reacting nano-silica sol with an aminosilane coupling agent, followed by solvent replacement and dehydration to obtain a low-moisture organic solvent-dispersible modified nano-silica sol; reacting polycarbonate diol with an alicyclic diisocyanate to obtain an isocyanate-terminated polycarbonate prepolymer; then adding the modified nano-silica sol dropwise to the prepolymer for a grafting reaction, and adding polycarbonate diol to continue the reaction to obtain a modified polycarbonate polyol with controlled hydroxyl value and residual isocyanate group content; subsequently, it is involved in the waterborne polyurethane prepolymerization, neutralization, emulsification, post-chain extension, and paint conditioning processes to obtain a weather-resistant and wear-resistant waterborne polyurethane coating. This invention introduces nano-silica through a modified polycarbonate polyol intermediate, which is beneficial to improving the controllability of nano-component introduction and the weather resistance and wear resistance of the coating film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of waterborne coatings technology, specifically relating to a weather-resistant and wear-resistant waterborne polyurethane coating and its preparation method. Background Technology

[0002] With increasingly stringent environmental regulations and growing demand for low-VOC coatings, waterborne polyurethane coatings have become widely used for protective coatings on surfaces such as metals, wood, plastics, and architectural decorative components due to their advantages including good film-forming properties, strong adhesion, good flexibility, and high application safety. For applications such as outdoor facilities, industrial equipment housings, and wear-resistant decorative surfaces, the coating not only needs good adhesion and application performance but also needs to maintain good weather resistance and abrasion resistance under ultraviolet light, rain, temperature and humidity changes, and friction. However, ordinary waterborne polyurethane coatings still experience problems such as insufficient film hardness, decreased abrasion resistance retention, surface stickiness, loss of gloss, or yellowing during long-term outdoor use.

[0003] To improve the aforementioned properties, existing research typically employs polycarbonate diols, alicyclic isocyanates, crosslinking chain extenders, or inorganic nanofillers to modify waterborne polyurethane systems. Polycarbonate diols help improve the hydrolysis resistance and weather resistance of the polyurethane soft segments, alicyclic isocyanates can reduce the risk of yellowing, and inorganic particles such as nano-silica and nano-alumina are often used to improve coating hardness and abrasion resistance. However, these modification methods still have shortcomings in practical preparation and application. For example, inorganic nanoparticles have high surface energy and are prone to agglomeration in waterborne resins, making long-term stable dispersion difficult when added directly; while pretreatment with coupling agents can improve compatibility, the bonding and distribution between nanoparticles and polyurethane resin are still significantly affected by the dispersion process; furthermore, excessive addition of nano-components can lead to decreased emulsion stability, reduced coating flexibility, or poor application performance. Summary of the Invention

[0004] To address the shortcomings mentioned in the background art, the present invention aims to provide a weather-resistant and wear-resistant waterborne polyurethane coating and its preparation method. This method involves modifying nano-silica sol with aminosilane and then performing solvent displacement dehydration, followed by grafting with isocyanate-terminated polycarbonate prepolymer to obtain a modified polycarbonate polyol with controlled hydroxyl value and residual isocyanate group content. This modified polyol is then used in the preparation of waterborne polyurethane emulsions and the paint mixing process, thereby improving the controllability of nano-component introduction and the weather-resistant and wear-resistant properties of the coating film.

[0005] The objective of this invention can be achieved through the following technical solutions: A method for preparing a weather-resistant and wear-resistant waterborne polyurethane coating includes the following steps: S1. The nano-silica sol is mixed and reacted with an aminosilane coupling agent. After the reaction, solvent replacement and water removal are performed to obtain an organic solvent-dispersible modified nano-silica sol. The water content of the organic solvent-dispersible modified nano-silica sol is not higher than 0.5% by mass. The amount of the aminosilane coupling agent is 3% to 15% of the mass of nano-silica solids in the nano-silica sol. S2. Reaction of polycarbonate diol with alicyclic diisocyanate yields isocyanate-terminated polycarbonate prepolymer; S3. The organic solvent-dispersible modified nano-silica sol is added dropwise to the isocyanate-terminated polycarbonate prepolymer for grafting reaction. The molar ratio of the amino groups in the organic solvent-dispersible modified nano-silica sol (calculated based on the amount of aminosilane coupling agent added) to the isocyanate-terminated polycarbonate prepolymer is 0.05-0.20:1. After the grafting reaction, polycarbonate diol is added and the reaction continues until the residual isocyanate group content is not higher than 0.05% based on the mass of the modified polycarbonate polyol, to obtain a modified polycarbonate polyol with a hydroxyl value of 20-50 mg KOH / g. S4. The modified polycarbonate polyol is reacted with polycarbonate diol, alicyclic diisocyanate, hydrophilic chain extender and catalyst to obtain a carboxyl-containing isocyanate-terminated polyurethane prepolymer. S5. The carboxyl-containing isocyanate-terminated polyurethane prepolymer is neutralized, emulsified, and then subjected to post-chain extension treatment to obtain a modified waterborne polyurethane emulsion. S6. The modified waterborne polyurethane emulsion is mixed with waterborne additives and deionized water to obtain the weather-resistant and wear-resistant waterborne polyurethane coating.

[0006] More preferably, in S1, the nano-silica sol is an alcohol-dispersed nano-silica sol, wherein the average particle size of the nano-silica in the alcohol-dispersed nano-silica sol is 10-50 nm, and the solid content is 20%-40% by mass; the aminosilane coupling agent is γ-aminopropyltriethoxysilane, and the amount of γ-aminopropyltriethoxysilane used is 5%-13% of the solid mass of the nano-silica.

[0007] More preferably, in S1, the nano-silica sol reacts with the aminosilane coupling agent at 50-70°C for 1-3 hours, and after the reaction, solvent replacement is carried out by vacuum distillation and the addition of a replacement solvent, wherein the replacement solvent is one or more of acetone, butanone, and dimethyl carbonate.

[0008] More preferably, in S2, the dehydrated polycarbonate diol is reacted with an alicyclic diisocyanate, wherein the NCO / OH equivalent ratio of the isocyanate group in the alicyclic diisocyanate to the hydroxyl group in the polycarbonate diol is 1.6 to 2.3, the reaction temperature is 70 to 85°C, and the reaction time is 2 to 4 hours.

[0009] More preferably, in step S3, the organic solvent-dispersed modified nano-silica sol is added dropwise to the isocyanate-terminated polycarbonate prepolymer at 50–65°C for 0.5–2 hours. After the addition is complete, the reaction continues for 0.5–1.5 hours. Then, polycarbonate diol is added to react. The amount of polycarbonate diol added is 40%–60% of the non-volatile matter in the system obtained from the grafting reaction. The reaction temperature after adding polycarbonate diol is 55–70°C, and the reaction time is 1–3 hours.

[0010] More preferably, in S3, the mass content of nano-silica in the non-volatile components of the modified polycarbonate polyol is 2% to 8%.

[0011] More preferably, in S4, based on the non-volatile matter mass of each raw material, the modified polycarbonate polyol is 15-35 parts, the polycarbonate diol is 35-60 parts, the hydrophilic chain extender is 3-6 parts, the catalyst is 0.02-0.08 parts, and the amount of alicyclic diisocyanate added is determined according to the NCO / OH equivalent ratio of the total amount of hydroxyl groups in the isocyanate group to the total amount of hydroxyl groups in the modified polycarbonate polyol, polycarbonate diol and hydrophilic chain extender in S4 is 1.3-1.9, wherein the hydroxyl groups in the modified polycarbonate polyol are converted according to their hydroxyl values.

[0012] More preferably, the polycarbonate diol in S2, S3 and S4 is a 1,6-hexanediol type polycarbonate diol with a number average molecular weight of 1000-3000; the alicyclic diisocyanate is one of isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate; the hydrophilic chain extender is one of 2,2-dimethylolpropionic acid and 2,2-dimethylolbutyric acid; and the catalyst is one of bismuth neodecanoate, bismuth isooctanoate and dibutyltin dilaurate.

[0013] More preferably, in S5, the neutralization is carried out using triethylamine, and the amount of triethylamine is 90% to 105% of the molar amount of carboxyl groups in the hydrophilic chain extender. The subsequent chain extension is carried out using either ethylenediamine or isophorone diamine.

[0014] A weather-resistant and wear-resistant waterborne polyurethane coating, by weight, comprises the following raw materials: 70-90 parts of modified waterborne polyurethane emulsion, 1-5 parts of film-forming aid, 0.1-0.5 parts of wetting agent, 0.1-0.5 parts of defoamer, 0.1-0.5 parts of leveling agent, 0.2-1.0 parts of thickener, and 5-20 parts of deionized water; wherein the modified waterborne polyurethane emulsion comprises a polyurethane resin formed by the reaction of modified polycarbonate polyol; wherein the modified polycarbonate polyol is prepared from organic solvent-dispersed modified nano-silica sol, isocyanate-terminated polycarbonate prepolymer, and polycarbonate diol; and wherein the hydroxyl value of the modified polycarbonate polyol is 20-50 mg. The KOH / g content, based on the mass of modified polycarbonate polyol, has a residual isocyanate group content of no more than 0.05%, the solid content of the modified waterborne polyurethane emulsion is 30% to 45%, and the content of nano-silica in the weather-resistant and wear-resistant waterborne polyurethane coating is 0.2% to 2.8% based on the resin solids mass.

[0015] The beneficial effects of this invention are: This invention utilizes an aminosilane coupling agent to modify the surface of nano-silica sol, and obtains a low-moisture organic solvent-dispersible modified nano-silica sol through solvent displacement and dehydration treatment. This reduces the risk of side reactions between moisture and isocyanate groups, providing a more stable reaction environment for subsequent grafting reactions. Based on this, the modified nano-silica sol is added dropwise to isocyanate-terminated polycarbonate prepolymers at a defined amino / NCO molar ratio. The nano-components participate in the prepolymer grafting process through the reaction of amino groups with isocyanate groups. Polycarbonate diol is then added to continue the reaction, resulting in an intermediate with a detectable hydroxyl value and keeping residual isocyanate groups at a low level. This forms a modified polycarbonate polyol that can be used as a polyol raw material in subsequent aqueous polyurethane prepolymerization reactions. This design moves the introduction of nano-silica to the polyurethane film-forming resin construction stage, which improves the controllability of nano-component introduction and reduces the risk of nanoparticle agglomeration and decreased emulsion stability due to post-addition. Meanwhile, the polycarbonate diol soft segment has good hydrolysis resistance and weather resistance, the alicyclic diisocyanate helps reduce the risk of yellowing of the coating, and the nano silica helps improve the surface hardness and wear resistance of the coating. The three are combined through the aforementioned intermediate route, so that the resulting waterborne polyurethane coating has good weather resistance, wear resistance and wear resistance retention after aging while maintaining the workability and coating flexibility of the waterborne system. Detailed Implementation

[0016] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0017] The present invention will be further described below with reference to the embodiments. Unless otherwise stated, the raw materials used in the following embodiments are all commercially available industrial products or reagents.

[0018] In this invention, the moisture content was determined using the Karl Fischer method, the isocyanate group content was determined using the di-n-butylamine back titration method, the hydroxyl value was determined according to the polyol hydroxyl value determination method, and the non-volatile matter content was calculated after drying to a constant mass. The "NCO / OH equivalent ratio" refers to the ratio of the isocyanate group equivalents to the hydroxyl group equivalents; the "content of nano-silica as resin solids" refers to the percentage of nano-silica mass in the coating relative to the polyurethane resin solids mass.

[0019] Example 1: This example describes the preparation of a weather-resistant and wear-resistant waterborne polyurethane coating. The specific steps are as follows: S1. Take 27.6 parts of alcohol-dispersed nano-silica sol, wherein the average particle size of the nano-silica is 20 nm and the solid content is 25%, i.e., the nano-silica solid content is 6.9 parts. Add 0.83 parts of γ-aminopropyltriethoxysilane to it and stir at 60℃ for 2 h. After the reaction is completed, the system is subjected to vacuum distillation at 45-50℃ and 20-30 kPa absolute pressure, and acetone is added in batches for solvent replacement, with a total of about 45 parts of acetone added, while removing water from the system. After solvent replacement, the non-volatile matter content of the obtained dispersion is adjusted to 30% with acetone, yielding about 25.8 parts of organic solvent-dispersed modified nano-silica sol. The water content of the obtained organic solvent-dispersed modified nano-silica sol is 0.34% by Karl Fischer method.

[0020] S2. Take 100 parts of 1,6-hexanediol-type polycarbonate diol with a number average molecular weight of 2000, dehydrate it under vacuum at 110°C for 1.5 h, cool it down to 75°C, and add 19.5 parts of isophorone diisocyanate so that the NCO / OH equivalent ratio of the isocyanate group in isophorone diisocyanate to the hydroxyl group in polycarbonate diol is 1.75. React at 80°C for 3 h to obtain isocyanate-terminated polycarbonate prepolymer.

[0021] S3. Take 25.8 parts of the organic solvent-dispersed modified nano-silica sol obtained in S1 and add it dropwise to the isocyanate-terminated polycarbonate prepolymer obtained in S2 at 55°C for 1.5 hours. The molar ratio of the organic solvent-dispersed modified nano-silica sol (calculated based on the amount of γ-aminopropyltriethoxysilane added) to the isocyanate-terminated polycarbonate prepolymer is 0.05:1. After the addition is complete, continue the reaction for 1 hour. Then add 76 parts of 1,6-hexanediol-type polycarbonate diol with a number-average molecular weight of 1000 and 0.10 parts of bismuth neodecanoate. Raise the temperature to 70°C and continue the reaction for 3 hours. The reaction endpoint is set at a residual isocyanate group content of no more than 0.05%, yielding the modified polycarbonate polyol. The test results showed that the non-volatile matter in the modified polycarbonate polyol contained 3.4% nano-silica, had a hydroxyl value of 24 mgKOH / g, and contained 0.03% residual isocyanate groups based on the mass of the modified polycarbonate polyol.

[0022] S4. Based on the non-volatile matter mass of each raw material, take 20 parts of the modified polycarbonate polyol obtained in S3, 55 parts of 1,6-hexanediol-type polycarbonate diol with a number average molecular weight of 2000, 4 parts of 2,2-dimethylolpropionic acid, and 0.06 parts of bismuth neodecanoate. After stirring and dispersing evenly, heat to 80℃, and add 19.2 parts of isophorone diisocyanate, so that the NCO / OH equivalent ratio of the total amount of hydroxyl groups in the isocyanate group to the modified polycarbonate polyol, polycarbonate diol, and 2,2-dimethylolpropionic acid is 1.4, wherein the hydroxyl groups in the modified polycarbonate polyol are converted according to their hydroxyl values. After the addition is complete, react at 80℃ for 3 hours to obtain a carboxyl-containing isocyanate-terminated polyurethane prepolymer.

[0023] S5. The carboxyl-containing isocyanate-terminated polyurethane prepolymer obtained in S4 was cooled to 40°C, and 2.9 parts of triethylamine were added for neutralization for 10 min. Then, 178 parts of deionized water were added under a shear rate of 2000 r / min for emulsification for 20 min. After emulsification, 7.0 parts of a 10% (w / w) ethylenediamine aqueous solution were added, and the chain extension reaction was carried out at 35–40°C for 30 min. After chain extension, acetone was removed under reduced pressure at 50°C and a vacuum of -0.09 MPa until almost no distillate remained. The solid content was then adjusted with deionized water to obtain a modified waterborne polyurethane emulsion with a solid content of 35%.

[0024] S6. Take 80 parts of the modified waterborne polyurethane emulsion obtained in S5, 3 parts of dipropylene glycol butyl ether, 0.3 parts of acetylenic diol wetting agent, 0.3 parts of mineral oil defoamer, 0.3 parts of acrylic leveling agent, 0.5 parts of polyurethane associative thickener and 15.6 parts of deionized water, stir and mix evenly, filter, and obtain weather-resistant and wear-resistant waterborne polyurethane coating.

[0025] In the coating obtained in this embodiment, the content of nano-silica, based on the resin solids mass, is 0.7%.

[0026] Example 2: This example describes the preparation of a weather-resistant and wear-resistant waterborne polyurethane coating. The specific steps are as follows: S1. Take 42 parts of alcohol-dispersed nano-silica sol, wherein the average particle size of the nano-silica is 40 nm and the solid content is 35%. Add 1.76 parts of γ-aminopropyltriethoxysilane to it and stir at 65°C for 2 hours. After the reaction is completed, distill under reduced pressure at 45-50°C and 20-30 kPa, and add methyl ethyl ketone (MEK) in batches for solvent replacement. After solvent replacement, adjust the non-volatile matter content of the obtained dispersion to 35% with MEK, obtaining approximately 47.0 parts of organic solvent-dispersed modified nano-silica sol. The moisture content of the obtained organic solvent-dispersed modified nano-silica sol is 0.30%.

[0027] S2. Take 100 parts of 1,6-hexanediol-type polycarbonate diol with a number average molecular weight of 1500, dehydrate it under vacuum at 110℃ for 1.5h, cool it down to 75℃, add 23.7 parts of isophorone diisocyanate to make the NCO / OH equivalent ratio 1.60, and react at 80℃ for 3h to obtain isocyanate-terminated polycarbonate prepolymer.

[0028] S3. Take 47.0 parts of the organic solvent-dispersed modified nano-silica sol obtained in S1 and add it dropwise to the isocyanate-terminated polycarbonate prepolymer obtained in S2 at 60°C for 2 hours. The molar ratio of the organic solvent-dispersed modified nano-silica sol (calculated based on the amount of γ-aminopropyltriethoxysilane added) to the isocyanate-terminated polycarbonate prepolymer is 0.10:1. After the addition is complete, continue the reaction for 1 hour. Then add 80 parts of 1,6-hexanediol-type polycarbonate diol with a number-average molecular weight of 1000 and 0.12 parts of bismuth neodecanoate. Raise the temperature to 70°C and continue the reaction for 3 hours. The reaction endpoint is set at a residual isocyanate group content of no more than 0.05%, yielding the modified polycarbonate polyol. The test results showed that the non-volatile matter in the modified polycarbonate polyol contained 6.7% nano-silica, had a hydroxyl value of 23 mgKOH / g, and contained 0.03% residual isocyanate groups based on the mass of the modified polycarbonate polyol.

[0029] S4. Based on the non-volatile matter content of each raw material, take 32 parts of the modified polycarbonate polyol obtained in S3, 38 parts of 1,6-hexanediol-type polycarbonate diol with a number average molecular weight of 1500, 5.5 parts of 2,2-dimethylolpropionic acid and 0.08 parts of bismuth neodecanoate, stir and disperse evenly, then heat to 82℃, add 28.2 parts of isophorone diisocyanate to make the NCO / OH equivalent ratio 1.75, and react at 82℃ for 3 hours to obtain a carboxyl-containing isocyanate-terminated polyurethane prepolymer.

[0030] S5. The carboxyl-containing isocyanate-terminated polyurethane prepolymer obtained in S4 was cooled to 40°C, and 4.1 parts of triethylamine were added for neutralization for 10 min. Subsequently, 160 parts of deionized water were added under a shear rate of 2500 r / min for emulsification for 20 min, followed by the addition of 14.8 parts of a 10% (w / w) ethylenediamine aqueous solution. The chain extension reaction was carried out at 35–40°C for 30 min. After the chain extension was completed, butanone was removed under reduced pressure at 50°C and a vacuum of -0.09 MPa until almost no distillate was obtained. The solid content was then adjusted with deionized water to obtain a modified waterborne polyurethane emulsion with a solid content of 38%.

[0031] S6. Take 82 parts of the modified waterborne polyurethane emulsion obtained in S5, 3 parts of dipropylene glycol butyl ether, 0.3 parts of acetylenic diol wetting agent, 0.3 parts of mineral oil defoamer, 0.3 parts of acrylic leveling agent, 0.6 parts of polyurethane associative thickener and 13.5 parts of deionized water, stir and mix evenly, filter, and obtain weather-resistant and wear-resistant waterborne polyurethane coating.

[0032] In the coating obtained in this embodiment, the content of nano-silica, based on the resin solids mass, is 2.1%.

[0033] Example 3: This example describes the preparation of a weather-resistant and wear-resistant waterborne polyurethane coating. The specific steps are as follows: S1. Take 33.3 parts of alcohol-dispersed nano-silica sol, wherein the average particle size of the nano-silica is 30 nm, the solid content is 30%, and the nano-silica solid content is 10.0 parts. Add 0.80 parts of γ-aminopropyltriethoxysilane to it and stir at 60℃ for 2 h. After the reaction is completed, distill under reduced pressure at 45-50℃ and 20-30 kPa, and add acetone in batches for solvent replacement. After solvent replacement, adjust the non-volatile matter content of the obtained dispersion to 30% with acetone to obtain approximately 36.0 parts of organic solvent-dispersed modified nano-silica sol. The moisture content of the obtained organic solvent-dispersed modified nano-silica sol is 0.32%.

[0034] S2. Take 100 parts of 1,6-hexanediol-type polycarbonate diol with a number average molecular weight of 3000, dehydrate it under vacuum at 110℃ for 1.5h, cool it down to 75℃, add 11.9 parts of isophorone diisocyanate to make the NCO / OH equivalent ratio 1.60, and react at 80℃ for 3h to obtain isocyanate-terminated polycarbonate prepolymer.

[0035] S3. Take 36.0 parts of the organic solvent-dispersed modified nano-silica sol obtained in S1, and add it dropwise to the isocyanate-terminated polycarbonate prepolymer obtained in S2 at 58℃ for 1.5 hours. The molar ratio of the organic solvent-dispersed modified nano-silica sol (calculated based on the amount of γ-aminopropyltriethoxysilane added) to the isocyanate-terminated polycarbonate prepolymer is 0.09:1. After the addition is complete, continue the reaction for 1 hour. Then add 70 parts of 1,6-hexanediol-type polycarbonate diol with a number-average molecular weight of 1000 and 0.10 parts of bismuth neodecanoate. Raise the temperature to 70℃ and continue the reaction for 3 hours. The reaction endpoint is set at a residual isocyanate group content of no more than 0.05%, yielding the modified polycarbonate polyol. The test results showed that the non-volatile matter in the modified polycarbonate polyol contained 5.2% nano-silica, had a hydroxyl value of 30 mg KOH / g, and contained 0.03% residual isocyanate groups based on the mass of the modified polycarbonate polyol.

[0036] S4. Based on the non-volatile matter content of each raw material, take 28 parts of the modified polycarbonate polyol obtained in S3, 47 parts of 1,6-hexanediol-type polycarbonate diol with a number average molecular weight of 2000, 4.5 parts of 2,2-dimethylolpropionic acid and 0.06 parts of bismuth neodecanoate, stir and disperse evenly, heat to 80℃, add 23.0 parts of isophorone diisocyanate to make the NCO / OH equivalent ratio 1.60, react at 80℃ for 3h to obtain a carboxyl-containing isocyanate-terminated polyurethane prepolymer.

[0037] S5. The carboxyl-containing isocyanate-terminated polyurethane prepolymer obtained in S4 was cooled to 40°C, and 3.3 parts of triethylamine were added for neutralization for 10 min. Subsequently, 170 parts of deionized water were added under shear conditions of 2200 r / min for emulsification for 20 min, followed by the addition of 10.7 parts of 10% ethylenediamine aqueous solution. The chain extension reaction was carried out at 35–40°C for 30 min. After the chain extension was completed, acetone was removed under reduced pressure at 50°C and a vacuum degree of -0.09 MPa until there was essentially no distillate. The solid content was then adjusted with deionized water to obtain a modified waterborne polyurethane emulsion with a solid content of 36%.

[0038] S6. Take 81 parts of the modified waterborne polyurethane emulsion obtained in S5, 3 parts of dipropylene glycol butyl ether, 0.3 parts of acetylenic diol wetting agent, 0.3 parts of mineral oil defoamer, 0.3 parts of acrylic leveling agent, 0.5 parts of polyurethane associative thickener and 14.6 parts of deionized water, stir and mix evenly, filter, and obtain weather-resistant and wear-resistant waterborne polyurethane coating.

[0039] In the coating obtained in this embodiment, the content of nano-silica, based on the resin solids mass, is 1.4%.

[0040] Comparative Example 1: This comparative example does not prepare organic solvent-dispersed modified nano-silica sol, nor does it prepare modified polycarbonate polyol through grafting reaction. Instead, it uses ordinary polycarbonate diol to prepare waterborne polyurethane emulsion, and directly adds unmodified nano-silica sol during the paint mixing stage, so that the content of nano-silica in the resulting coating, based on the resin solids mass, is basically the same as in Example 3. All parts below are parts by mass.

[0041] S1. Based on the non-volatile matter content of each raw material, take 75 parts of 1,6-hexanediol-type polycarbonate diol with a number average molecular weight of 2000, dehydrate it under vacuum at 110℃ for 1.5h, cool it to 75℃, add 4.5 parts of 2,2-dimethylolpropionic acid, 0.06 parts of bismuth neodecanoate and an appropriate amount of acetone, stir and disperse evenly, then heat it to 80℃, add 25.3 parts of isophorone diisocyanate to make the NCO / OH equivalent ratio 1.60, react at 80℃ for 3h to obtain a carboxyl-containing isocyanate-terminated polyurethane prepolymer.

[0042] S2. The carboxyl-containing isocyanate-terminated polyurethane prepolymer obtained in S1 was cooled to 40°C, and 3.3 parts of triethylamine were added for neutralization for 10 min. Subsequently, 170 parts of deionized water were added under a shear rate of 2200 r / min for emulsification for 20 min, followed by the addition of 11.5 parts of a 10% (w / w) ethylenediamine aqueous solution. The chain extension reaction was carried out at 35–40°C for 30 min. After the chain extension was completed, acetone was removed under reduced pressure at 50°C and a vacuum of -0.09 MPa until almost no distillate was obtained. The solid content was then adjusted with deionized water to obtain an aqueous polyurethane emulsion with a solid content of 36%.

[0043] S3. Take 81 parts of the waterborne polyurethane emulsion obtained in S2, 3 parts of dipropylene glycol butyl ether, 1.36 parts of unmodified alcohol-dispersed nano-silica sol, 0.3 parts of acetylenic diol wetting agent, 0.3 parts of mineral oil defoamer, 0.3 parts of acrylic leveling agent, 0.5 parts of polyurethane associative thickener, and 13.2 parts of deionized water. Stir and mix evenly, filter, and obtain waterborne polyurethane coating. The unmodified alcohol-dispersed nano-silica sol has an average nano-silica particle size of 30 nm and a solid content of 30%.

[0044] In the coating obtained in this comparative example, the content of nano-silica, based on the resin solids mass, is 1.4%.

[0045] Comparative Example 2: In this comparative example, the organic solvent-dispersible modified nano-silica sol was not added dropwise to the isocyanate-terminated polycarbonate prepolymer for grafting reaction, nor was a modified polycarbonate polyol prepared. Instead, the organic solvent-dispersible modified nano-silica sol was directly added during the ordinary waterborne polyurethane emulsion mixing stage, so that the content of nano-silica in the resulting coating, based on the resin solids mass, was essentially the same as in Example 3. All figures below are parts by mass.

[0046] S1. Prepare organic solvent-dispersible modified nano-silica sol according to S1 of Example 3.

[0047] S2. Based on the non-volatile matter content of each raw material, take 75 parts of 1,6-hexanediol-type polycarbonate diol with a number average molecular weight of 2000, dehydrate it under vacuum at 110℃ for 1.5h, cool it to 75℃, add 4.5 parts of 2,2-dimethylolpropionic acid, 0.06 parts of bismuth neodecanoate and 20 parts of acetone, stir and disperse evenly, then heat it to 80℃, add 25.3 parts of isophorone diisocyanate to make the NCO / OH equivalent ratio 1.60, react at 80℃ for 3h to obtain a carboxyl-containing isocyanate-terminated polyurethane prepolymer.

[0048] S3. The carboxyl-containing isocyanate-terminated polyurethane prepolymer obtained in S2 was cooled to 40°C, and 3.3 parts of triethylamine were added for neutralization for 10 min. Then, 170 parts of deionized water were added under shear conditions of 2200 r / min for emulsification for 20 min, followed by the addition of 11.5 parts of 10% ethylenediamine aqueous solution. The chain extension reaction was carried out at 35-40°C for 30 min. After the chain extension was completed, acetone was removed under reduced pressure at 50°C and a vacuum degree of -0.09 MPa until there was basically no distillate. The solid content was then adjusted with deionized water to obtain an aqueous polyurethane emulsion with a solid content of 36%.

[0049] S4. Take 81 parts of the waterborne polyurethane emulsion obtained in S3, 3 parts of dipropylene glycol butyl ether, 1.47 parts of the organic solvent-dispersed modified nano-silica sol obtained in S1, 0.3 parts of acetylenic diol wetting agent, 0.3 parts of mineral oil defoamer, 0.3 parts of acrylic leveling agent, 0.5 parts of polyurethane associative thickener, and 13.1 parts of deionized water, stir and mix evenly, filter, and obtain waterborne polyurethane coating.

[0050] In the coating obtained in this comparative example, the content of nano-silica, based on the resin solids mass, is 1.4%.

[0051] Comparative Example 3: In the preparation of organic solvent-dispersed modified nano-silica sol in Comparative Example S1, the moisture in the system was not fully removed, resulting in a moisture content of more than 0.5% in the obtained organic solvent-dispersed modified nano-silica sol; the specifications, amounts and process conditions of the other raw materials are the same as in Example 3.

[0052] S1. Take 33.3 parts of alcohol-dispersed nano-silica sol, wherein the average particle size of the nano-silica is 30 nm, the solid content is 30%, and the nano-silica solid content is 10.0 parts. Add 0.80 parts of γ-aminopropyltriethoxysilane to it and stir at 60℃ for 2 h. After the reaction is completed, distill under reduced pressure at 45-50℃ and 45-55 kPa, and add acetone in batches for solvent replacement. After solvent replacement, adjust the non-volatile matter content of the obtained dispersion to 30% with acetone to obtain approximately 36.0 parts of organic solvent-dispersed modified nano-silica sol. The moisture content of the obtained organic solvent-dispersed modified nano-silica sol is 0.82%.

[0053] S2. Prepare isocyanate-terminated polycarbonate prepolymer according to S2 of Example 3.

[0054] S3. Take 36.0 parts of the organic solvent-dispersed modified nano-silica sol obtained in S1, and carry out the grafting reaction and subsequent polycarbonate diol reaction according to the S3 conditions of Example 3 to obtain a comparative silicon-containing polycarbonate intermediate. During the reaction, the system showed an increase in bubbles, and the viscosity of the obtained intermediate was higher than that of Example 3.

[0055] S4. Prepare a carboxyl-containing isocyanate-terminated polyurethane prepolymer according to S4 of Example 3, wherein the modified polycarbonate polyol in Example 3 is replaced with a comparative silicon-containing polycarbonate intermediate obtained in S3 in equal amounts of non-volatile substances.

[0056] S5. Neutralize, emulsify, extend chains and desolventize according to S5 of Example 3 to obtain a comparative aqueous polyurethane emulsion with a solid content of 36%.

[0057] S6. Take 81 parts of the comparative water-based polyurethane emulsion obtained in S5, 3 parts of dipropylene glycol butyl ether, 0.3 parts of acetylenol wetting agent, 0.3 parts of mineral oil defoamer, 0.3 parts of acrylic leveling agent, 0.5 parts of polyurethane associative thickener and 14.6 parts of deionized water, stir and mix evenly, filter, and obtain water-based polyurethane coating.

[0058] In the coating obtained in this comparative example, the content of nano-silica, based on the resin solids mass, is 1.4%.

[0059] Comparative Example 4: This comparative example does not involve grafting the organic solvent-dispersed modified nano-silica sol with isocyanate-terminated polycarbonate prepolymer and further reacting it to prepare modified polycarbonate polyol. Instead, the organic solvent-dispersed modified nano-silica sol is directly added to the aqueous polyurethane prepolymerization reaction system, so that the content of nano-silica in the resulting coating, based on the resin solids mass, is basically the same as in Example 3. Except for the above differences, the raw material specifications and process conditions not specifically mentioned are the same as in Example 3.

[0060] S1. Prepare organic solvent-dispersible modified nano-silica sol according to S1 of Example 3.

[0061] S2. Based on the non-volatile matter content of each raw material, 75 parts of 1,6-hexanediol-type polycarbonate diol with a number-average molecular weight of 2000 were taken and vacuum dehydrated at 110℃ for 1.5 h. After cooling to 75℃, 4.5 parts of 2,2-dimethylolpropionic acid and 0.06 parts of bismuth neodecanoate were added, and the mixture was stirred and dispersed evenly before being heated to 80℃. Subsequently, 5.3 parts of the organic solvent-dispersed modified nano-silica sol obtained in S1 were added and stirred and dispersed for 30 min. Then, 25.4 parts of isophorone diisocyanate were added to make the NCO / OH equivalent ratio of the isocyanate group to the total hydroxyl groups contained in polycarbonate diol and 2,2-dimethylolpropionic acid 1.60. The mixture was reacted at 80℃ for 3 h to obtain the comparative silicon isocyanate-terminated polyurethane prepolymer.

[0062] S3. The comparative aqueous polyurethane prepolymer with silicone isocyanate end-capping obtained in S2 was cooled to 40°C, and 3.3 parts of triethylamine were added for neutralization for 10 min. Subsequently, 170 parts of deionized water were added under shear conditions of 2200 r / min for emulsification for 20 min, followed by the addition of 11.4 parts of 10% ethylenediamine aqueous solution. The chain extension reaction was carried out at 35–40°C for 30 min. After the chain extension was completed, acetone was removed under reduced pressure at 50°C and a vacuum degree of -0.09 MPa until there was essentially no distillate. The solid content was then adjusted with deionized water to obtain a comparative aqueous polyurethane emulsion with a solid content of 36%.

[0063] S4. Take 81 parts of the comparative water-based polyurethane emulsion obtained in S3, 3 parts of dipropylene glycol butyl ether, 0.3 parts of acetylenol wetting agent, 0.3 parts of mineral oil defoamer, 0.3 parts of acrylic leveling agent, 0.5 parts of polyurethane associative thickener and 14.6 parts of deionized water, stir and mix evenly, filter, and obtain water-based polyurethane coating.

[0064] In the coating obtained in this comparative example, the content of nano-silica, based on the resin solids mass, is 1.4%.

[0065] Performance testing: To verify the beneficial effects of the present invention, performance tests were conducted on the waterborne polyurethane emulsions and waterborne polyurethane coatings obtained in Examples 1-3 and Comparative Examples 1-4. Coating samples were prepared according to GB / T 1727-2021 "General Method for Preparing Paint Films," and test panels were treated according to GB / T 9271-2008 "Standard Test Panels for Paints and Varnishes." The coatings were applied using a scraping method, with the dry film thickness controlled at 45±5 μm. Testing was conducted after curing for 7 days at a temperature of 23±2℃ and a relative humidity of 50±5%.

[0066] 1. Emulsion storage stability test The storage stability of the emulsions was tested according to GB / T 6753.3-1986 "Test Method for Storage Stability of Coatings". The waterborne polyurethane emulsions obtained in Examples 1-3 and Comparative Examples 1-4 were respectively placed in sealed polyethylene bottles and allowed to stand at 25±2℃ for 30 days. Before and after storage, the emulsions were observed for stratification, sedimentation, coarse particles, gelation, or obvious flocculation. The apparent viscosity before and after storage was measured according to GB / T 9269-2009 "Determination of Viscosity of Coatings - Stormer Viscometer Method". The viscosity change rate was calculated using the following formula: Viscosity change rate / % = (viscosity after storage - viscosity before storage) / viscosity before storage × 100%.

[0067] 2. Wear resistance test before and after aging Abrasion resistance was determined according to GB / T 1768-2006, "Determination of Abrasion Resistance of Paints and Varnishes - Rotary Rubber Abrasive Wheel Method". The cured coating samples were placed on a rotary abrasion tester, and an abrasion test was performed using a rubber abrasive wheel. The mass loss of the coating after a specified number of revolutions was recorded. A smaller mass loss indicates better abrasion resistance. Each group of samples was tested in triplicate, and the average value was taken as the test result.

[0068] To evaluate abrasion resistance retention after aging, coated test panels from the same batch underwent accelerated aging treatment and were then subjected to abrasion resistance tests under the same conditions. The abrasion resistance retention rate was calculated using the following formula: Wear resistance retention rate / % = initial wear mass loss / wear mass loss after aging × 100%.

[0069] 3. Artificial accelerated aging performance test Artificial accelerated aging was conducted according to GB / T 23987.3-2025 "Laboratory Light Source Exposure Methods for Paints and Varnishes Part 3: Fluorescent Ultraviolet Lamps". The coating test panels were placed in a fluorescent ultraviolet aging chamber for cyclic exposure for 500 hours. After aging, the coating was observed for cracking, blistering, peeling, significant chalking, and significant discoloration, and its appearance was evaluated according to GB / T 1766-2008 "Rating Methods for Aging of Paint and Varnish Coatings". The 60° gloss of the coating was determined according to GB / T9754-2025 "Determination of 20°, 60° and 85° Gloss of Paints and Varnishes", and the gloss retention rate was calculated using the following formula: Gloss retention rate / % = 60° gloss after aging / 60° gloss before aging × 100%.

[0070] The test results are shown in Table 1.

[0071] Table 1. Performance test results of coatings obtained from the examples and comparative examples.

[0072] Table 1 shows that the aqueous polyurethane emulsions obtained in Examples 1-3 did not exhibit significant stratification, sedimentation, or gelation after 30 days of storage, with viscosity changes ranging from only 4.2% to 5.5%, significantly lower than those in Comparative Examples 1-4. This indicates that the present invention, through the introduction of nano-silica via low-moisture organic solvent-dispersed modified nano-silica sol and modified polycarbonate polyol intermediates, can reduce sedimentation, flocculation, and coarsening problems caused by the subsequent addition of nanoparticles. The initial wear mass loss of Examples 1-3 was 21.4-28.6 mg, both lower than that of the comparative examples, indicating that nano-silica, after being introduced into the polyurethane film-forming system via grafting intermediates, can more effectively exert its inorganic wear-resistant reinforcing effect. Among them, Example 2, due to its higher nano-silica content, exhibited the best initial wear resistance; Example 3 showed better performance in terms of gloss retention and wear resistance retention, indicating that a moderate silica content and good interfacial bonding are beneficial for balancing wear resistance and weather resistance. Comparative Examples 1 and 2 were added post-processed, Comparative Example 3 had a higher moisture content, and Comparative Example 4 was introduced directly through prepolymerization. None of them formed modified polycarbonate polyols with controlled hydroxyl value and residual NCO. Therefore, after aging, the wear increased and the gloss retention decreased.

[0073] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0074] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claimed invention.

Claims

1. A method for preparing a weather-resistant and wear-resistant waterborne polyurethane coating, characterized in that, Includes the following steps: S1. The nano-silica sol is mixed and reacted with an aminosilane coupling agent. After the reaction, solvent replacement and water removal are performed to obtain an organic solvent-dispersible modified nano-silica sol. The water content of the organic solvent-dispersible modified nano-silica sol is not higher than 0.5% by mass. The amount of the aminosilane coupling agent is 3% to 15% of the mass of nano-silica solids in the nano-silica sol. S2. Reaction of polycarbonate diol with alicyclic diisocyanate yields isocyanate-terminated polycarbonate prepolymer; S3. The organic solvent-dispersible modified nano-silica sol is added dropwise to the isocyanate-terminated polycarbonate prepolymer for grafting reaction. The molar ratio of the amino groups in the organic solvent-dispersible modified nano-silica sol (calculated based on the amount of amino silane coupling agent) to the isocyanate groups in the isocyanate-terminated polycarbonate prepolymer is 0.05-0.20:

1. After the grafting reaction, polycarbonate diol is added and the reaction continues until the residual isocyanate group content is not higher than 0.05% based on the mass of the modified polycarbonate polyol, to obtain a modified polycarbonate polyol with a hydroxyl value of 20-50 mgKOH / g. S4. The modified polycarbonate polyol is reacted with polycarbonate diol, alicyclic diisocyanate, hydrophilic chain extender and catalyst to obtain a carboxyl-containing isocyanate-terminated polyurethane prepolymer. S5. The carboxyl-containing isocyanate-terminated polyurethane prepolymer is neutralized, emulsified, and then subjected to post-chain extension treatment to obtain a modified waterborne polyurethane emulsion. S6. The modified waterborne polyurethane emulsion is mixed with waterborne additives and deionized water to obtain the weather-resistant and wear-resistant waterborne polyurethane coating.

2. The method for preparing a weather-resistant and wear-resistant waterborne polyurethane coating according to claim 1, characterized in that, In S1, the nano-silica sol is an alcohol-dispersed nano-silica sol, wherein the average particle size of the nano-silica in the alcohol-dispersed nano-silica sol is 10-50 nm, and the solid content is 20%-40% by mass. The aminosilane coupling agent is γ-aminopropyltriethoxysilane, and the amount of γ-aminopropyltriethoxysilane used is 5%-13% of the solid mass of the nano-silica.

3. The method for preparing a weather-resistant and wear-resistant waterborne polyurethane coating according to claim 1, characterized in that, In S1, the nano-silica sol reacts with the aminosilane coupling agent at 50-70°C for 1-3 hours. After the reaction, solvent replacement is carried out by vacuum distillation and the addition of a replacement solvent, wherein the replacement solvent is one or more of acetone, butanone, and dimethyl carbonate.

4. The method for preparing a weather-resistant and wear-resistant waterborne polyurethane coating according to claim 1, characterized in that, In S2, dehydrated polycarbonate diol is reacted with an alicyclic diisocyanate, wherein the NCO / OH equivalent ratio of the isocyanate group in the alicyclic diisocyanate to the hydroxyl group in the polycarbonate diol is 1.6 to 2.3, the reaction temperature is 70 to 85°C, and the reaction time is 2 to 4 hours.

5. The method for preparing a weather-resistant and wear-resistant waterborne polyurethane coating according to claim 1, characterized in that, In step S3, the organic solvent-dispersed modified nano-silica sol is added dropwise to the isocyanate-terminated polycarbonate prepolymer at 50–65°C for 0.5–2 hours. After the addition is complete, the reaction continues for 0.5–1.5 hours. Then, polycarbonate diol is added to react. The amount of polycarbonate diol added is 40%–60% of the non-volatile matter in the system obtained from the grafting reaction. The reaction temperature after adding polycarbonate diol is 55–70°C, and the reaction time is 1–3 hours.

6. The method for preparing a weather-resistant and wear-resistant waterborne polyurethane coating according to claim 1, characterized in that, In S3, the mass content of nano-silica in the non-volatile components of the modified polycarbonate polyol is 2% to 8%.

7. The method for preparing a weather-resistant and wear-resistant waterborne polyurethane coating according to claim 1, characterized in that, In S4, based on the non-volatile matter mass of each raw material, the modified polycarbonate polyol is 15-35 parts, the polycarbonate diol is 35-60 parts, the hydrophilic chain extender is 3-6 parts, the catalyst is 0.02-0.08 parts, and the amount of alicyclic diisocyanate added is determined according to the NCO / OH equivalent ratio of the total amount of hydroxyl groups in the isocyanate group to the total amount of hydroxyl groups in the modified polycarbonate polyol, polycarbonate diol and hydrophilic chain extender in S4 is 1.3-1.9, wherein the hydroxyl groups in the modified polycarbonate polyol are converted according to their hydroxyl values.

8. A method for preparing a weather-resistant and wear-resistant waterborne polyurethane coating according to any one of claims 1 to 7, characterized in that, The polycarbonate diols in S2, S3, and S4 are 1,6-hexanediol-type polycarbonate diols with a number average molecular weight of 1000-3000; the alicyclic diisocyanate is one of isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate; the hydrophilic chain extender is one of 2,2-dimethylolpropionic acid and 2,2-dimethylolbutyric acid; and the catalyst is one of bismuth neodecanoate, bismuth isooctanoate, and dibutyltin dilaurate.

9. The method for preparing a weather-resistant and wear-resistant waterborne polyurethane coating according to claim 1, characterized in that, In S5, the neutralization is carried out using triethylamine, and the amount of triethylamine used is 90% to 105% of the molar amount of carboxyl groups in the hydrophilic chain extender. The subsequent chain extension is carried out using either ethylenediamine or isophorone diamine.

10. A weather-resistant and wear-resistant waterborne polyurethane coating, characterized in that, The product comprises, by weight, the following raw materials: 70-90 parts of modified waterborne polyurethane emulsion, 1-5 parts of film-forming aid, 0.1-0.5 parts of wetting agent, 0.1-0.5 parts of defoamer, 0.1-0.5 parts of leveling agent, 0.2-1.0 parts of thickener, and 5-20 parts of deionized water; wherein the modified waterborne polyurethane emulsion comprises a polyurethane resin formed by the reaction of modified polycarbonate polyol; wherein the modified polycarbonate polyol is a modified sodium hydroxide dispersed in an organic solvent. The modified polycarbonate polyol is prepared from silica sol, isocyanate-terminated polycarbonate prepolymer, and polycarbonate diol. The hydroxyl value of the modified polycarbonate polyol is 20-50 mg KOH / g, and the residual isocyanate group content is not higher than 0.05% based on the mass of the modified polycarbonate polyol. The solid content of the modified waterborne polyurethane emulsion is 30%-45%, and the content of nano-silica in the weather-resistant and wear-resistant waterborne polyurethane coating is 0.2%-2.8% based on the solid mass of the resin.