A polyurethane-based superhydrophobic anti-icing coating, its preparation method and application

By using a polyurethane-based superhydrophobic anti-icing coating, nano-SiO2 modified with a silane coupling agent is combined with polyurethane resin to form a multi-scale micro-nano structure coating, which solves the problem of anti-icing of radar radomes in harsh environments and maintains the high-efficiency operation of radar systems.

CN123107519APending Publication Date: 2026-11-17HARBIN TOPFRP COMPOSITE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611604089.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing superhydrophobic anti-icing coatings for radar radomes cannot effectively resist the impact of harsh environments, affecting the working efficiency and accuracy of radar systems.

Method used

A polyurethane-based superhydrophobic anti-icing coating is used. By modifying nano-SiO2 with a silane coupling agent and combining it with polyurethane resin, a multi-scale micro-nano structure coating is formed. Combined with spraying or brushing processes, a wear-resistant and self-cleaning coating is prepared.

Benefits of technology

The coating achieves superhydrophobic and anti-icing properties on the surface of the radar radome. The static hydrophobic angle of the coating is greater than 150°, the roll-off angle is less than 5°, the dielectric constant is low, the loss tangent is small, and the wear resistance is excellent, thus maintaining the high efficiency of the radar system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107519A_ABST
    Figure CN123107519A_ABST
Patent Text Reader

Abstract

This invention belongs to the technical field of superhydrophobic anti-icing coatings, and discloses a polyurethane-based superhydrophobic anti-icing coating, its preparation method, and its application. The coating comprises component A and component B. Component A includes silane coupling agent-modified nano-SiO2, polyurethane resin A, and an organic solvent. Component B includes an isocyanate curing agent. This invention uses polyurethane resin as the base material; the combination of soft and hard segments in polyurethane results in stronger flexibility and superior cold resistance. The nano-SiO2 is modified with a silane coupling agent for oleophilic modification. The polyurethane-based superhydrophobic anti-icing coating of this invention forms a coating on the radome surface with a static hydrophobic angle greater than 150°, a roll-off angle less than 5°, a dielectric constant less than 3.6, and a loss tangent less than or equal to 0.006. The coating exhibits excellent wear resistance and self-cleaning properties, achieving superhydrophobic and anti-icing characteristics on the radome surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of superhydrophobic anti-icing coating technology, and in particular to a polyurethane-based superhydrophobic anti-icing coating, its preparation method, and its application. Background Technology

[0002] As the most important protective layer in a radar system, the radome must protect the radar system from damage caused by strong winds, rain, snow, sandstorms, and hail, and must also withstand various challenges such as ultraviolet radiation, salt spray, acid and alkaline environments, and alternating hot and cold temperatures. Most radar radomes are made of fiberglass, which features good wave transmission, excellent mechanical properties, and a low dielectric constant, serving as the "electromagnetic window" of the radar system. However, this still cannot completely solve the problem of maintaining excellent electrical performance under outdoor icing and freezing rain conditions; the thicker the covering material (rainwater, sand, snow, etc.) on the radar radome, the greater the decrease in operating efficiency. The superhydrophobic anti-icing coating, as part of the radar system, also needs to meet the performance specifications of the radar radome, possessing characteristics such as low dielectric constant, high wave transmission, wide operating temperature range, and simple molding process.

[0003] Therefore, how to provide a superhydrophobic anti-icing coating that can protect the radar radome from various harsh environments without affecting the radar system's efficiency and accuracy is an urgent problem to be solved. Summary of the Invention

[0004] The purpose of this invention is to provide a polyurethane-based superhydrophobic anti-icing coating, its preparation method, and its application, thereby solving the problems existing in the surface superhydrophobic anti-icing coatings of existing radar radomes.

[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a polyurethane-based superhydrophobic anti-icing coating, comprising component A and component B; The A component comprises the following raw materials: silane coupling agent modified nano-SiO2, polyurethane resin A material, and organic solvent; Component B includes the following raw materials: isocyanate curing agent; The mass ratio of polyurethane resin A to component B in component A is 1~4:1.

[0006] Preferably, the mass of the silane coupling agent-modified nano-SiO2 is 10-35% of the mass of polyurethane resin A; the mass ratio of polyurethane resin A to organic solvent is 1-8:5-10.

[0007] Preferably, the polyurethane resin A is the main component in the two-component polyurethane adhesive; and the isocyanate curing agent is the curing agent in the two-component polyurethane adhesive.

[0008] Preferably, the organic solvent is ethyl acetate.

[0009] Preferably, the method for preparing the silane coupling agent modified nano-SiO2 includes the following steps: Nano-SiO2 and ethanol solution were ultrasonically dispersed to obtain SiO2 dispersion; Oxalic acid solution, anhydrous ethanol, and silane coupling agent are mixed to obtain the modified solution; SiO2 dispersion and modified liquid were mixed and reacted to obtain silane coupling agent modified nano-SiO2.

[0010] Preferably, the particle size of the nano-SiO2 is 7~15nm; the silane coupling agent is γ-methacryloyloxypropyltrimethoxysilane; and the mass of the silane coupling agent is 15~20% of the mass of the nano-SiO2.

[0011] Preferably, the reaction temperature is 70~80℃ and the reaction time is 3~8h.

[0012] This invention also provides a method for preparing a polyurethane-based superhydrophobic anti-icing coating, comprising the following steps: Silane coupling agent modified nano-SiO2, organic solvent, and polyurethane resin A are mixed to obtain component A; component A and component B are packaged separately to obtain polyurethane-based superhydrophobic anti-icing coating.

[0013] This invention also provides the application of a polyurethane-based superhydrophobic anti-icing coating in the preparation of a surface coating for an radome, wherein the preparation method of the radome surface coating includes the following steps: After mixing components A and B, the mixture is applied to the surface of the radome. After curing at room temperature, the temperature is raised and maintained to obtain the radome surface coating. The coating thickness is 200~400μm; the curing time at room temperature is 2~5h; the heating and holding temperature is 50~60℃; and the heating and holding time is 1~2h.

[0014] As can be seen from the above technical solution, compared with the prior art, the present invention has the following beneficial effects: (1) The polyurethane-based superhydrophobic anti-icing coating of the present invention forms a coating on the surface of the radome with a static hydrophobic angle greater than 150°, a roll-off angle less than 5°, a dielectric constant less than 3.6, and a loss tangent less than or equal to 0.006. The coating has excellent wear resistance and is self-cleaning, thus achieving superhydrophobic and anti-icing properties on the surface of the radome.

[0015] (2) This invention uses polyurethane resin as the base material. The structure of polyurethane with soft and hard segments has stronger flexibility and better cold resistance. The superhydrophobic anti-icing coating made based on general-purpose polyurethane has extremely high adhesion performance, and also has multiple advantages such as water resistance, high wear resistance, resistance to dilute acids, resistance to oils and esters, and antifreeze.

[0016] (3) Nano-SiO2 itself contains a large number of hydroxyl bonds and has extremely strong hydrophilicity. It has very poor dispersibility in organic solvents. In order to reduce its surface energy and improve the dispersibility of fillers in the coating, this invention uses silane coupling agents to modify it for hydrophilicity. After adding modified nano-SiO2 material, the hydrophobic nanoparticles in the formed coating are grafted onto the micron-scale structure of the coating to construct a multi-scale micro-nano bilayer structure surface, achieving a hydrophobic angle greater than 150°; and the freezing delay time can be extended. After the frosting-defrosting cycle, the hydrophobicity of the coating does not change significantly, and the stability of the coating is guaranteed.

[0017] (4) The present invention uses spraying or brushing process to prepare the surface coating of radar radome, which has the characteristics of simple construction, low process requirements and suitability for mass production. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below.

[0019] Figure 1 The water contact angle of the radome surface coating in Example 1; Figure 2 The water contact angle of the radome unit plate without polyurethane-based superhydrophobic anti-icing coating; Figure 3 Macroscopic photograph of water droplets rolling on the surface coating of the radome in Example 1. Detailed Implementation

[0020] This invention provides a polyurethane-based superhydrophobic anti-icing coating, comprising component A and component B; The A component comprises the following raw materials: silane coupling agent modified nano-SiO2, polyurethane resin A material, and organic solvent; Component B includes the following raw material: isocyanate curing agent.

[0021] In this invention, the mass ratio of polyurethane resin A to component B in component A is preferably 1 to 4:1, and more preferably 4:1.

[0022] In this invention, the mass of the silane coupling agent modified nano-SiO2 is preferably 10-35% of the mass of polyurethane resin A, and more preferably 12.5%.

[0023] In this invention, the mass ratio of polyurethane resin A to organic solvent is preferably 1~8:5~10, and more preferably 8:10.

[0024] In this invention, the polyurethane resin A is preferably the main component in a two-component polyurethane adhesive. The two-component polyurethane adhesive used in this invention is derived from the RS101 two-component polyurethane adhesive component A from Changzhou Jintan Rongsheng Chemical Co., Ltd.

[0025] In this invention, the isocyanate curing agent is preferably a curing agent in a two-component polyurethane adhesive. The two-component polyurethane adhesive used in this invention is derived from the RS201 two-component polyurethane adhesive, component B, of Changzhou Jintan Rongsheng Chemical Co., Ltd.

[0026] In this invention, the organic solvent is preferably ethyl acetate.

[0027] In this invention, the preparation method of the silane coupling agent modified nano-SiO2 includes the following steps: Nano-SiO2 and ethanol solution were ultrasonically dispersed to obtain SiO2 dispersion; Oxalic acid solution, anhydrous ethanol, and silane coupling agent are mixed to obtain the modified solution; SiO2 dispersion and modified liquid were mixed and reacted to obtain silane coupling agent modified nano-SiO2.

[0028] In this invention, the particle size of the nano-SiO2 is preferably 7-15 nm; the silane coupling agent is preferably γ-methacryloyloxypropyltrimethoxysilane; the mass of the silane coupling agent is preferably 15-20% of the mass of the nano-SiO2, more preferably 20%; the ethanol solution is preferably a mixture of anhydrous ethanol and water in a volume ratio of 3:1; the volume ratio of the oxalic acid solution to anhydrous ethanol is preferably 1:1; the pH of the oxalic acid solution is preferably 3-4, more preferably 3; the reaction temperature is preferably 70-80℃, more preferably 75℃; the reaction time is preferably 3-8 h, more preferably 8 h; after the reaction, the reaction product is further subjected to centrifugation, ultrasonic cleaning, and vacuum drying; the vacuum drying temperature is preferably 80℃; the vacuum drying time is preferably 6 h.

[0029] This invention also provides a method for preparing a polyurethane-based superhydrophobic anti-icing coating, comprising the following steps: Silane coupling agent modified nano-SiO2, organic solvent, and polyurethane resin A are mixed to obtain component A; component A and component B are packaged separately to obtain polyurethane-based superhydrophobic anti-icing coating.

[0030] In this invention, the method for mixing the silane coupling agent modified nano-SiO2, organic solvent, and polyurethane resin A is as follows: first, the silane coupling agent modified nano-SiO2 is ultrasonically dispersed in the organic solvent, then polyurethane resin A is added, and mechanical stirring is performed; the speed of the mechanical stirring is preferably 2000 rpm; the time of the mechanical stirring is preferably 30~50 min, and more preferably 30 min.

[0031] This invention also provides the application of a polyurethane-based superhydrophobic anti-icing coating in the preparation of a surface coating for an radome, wherein the preparation method of the radome surface coating includes the following steps: After mixing components A and B, the mixture is applied to the surface of the radome. After curing at room temperature, the mixture is heated and kept at a constant temperature to obtain the radome surface coating.

[0032] In this invention, the coating method is preferably spraying or brushing, and more preferably spraying.

[0033] In this invention, the coating thickness is preferably 200~400μm, and more preferably 300μm.

[0034] In this invention, the curing time at room temperature is preferably 2 to 5 hours, and more preferably 4 hours.

[0035] In this invention, the temperature for heating and heat preservation is preferably 50~60℃, more preferably 50℃; the time for heating and heat preservation is preferably 1~2h, more preferably 2h.

[0036] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0037] Example 1

[0038] a. Dry nano-SiO2 (particle size 7~15nm) at 80℃ for 6h to remove moisture; add 100g of dried nano-SiO2 to 400mL of ethanol solution (a mixture of anhydrous ethanol and deionized water in a volume ratio of 3:1), and disperse by ultrasonication to obtain SiO2 dispersion. b. Mix oxalic acid solution with pH=3 and anhydrous ethanol at a volume ratio of 1:1 until homogeneous. Add 20g of γ-methacryloyloxypropyltrimethoxysilane (KH-570) to 400mL of the mixture and stir magnetically at 1000rpm for 1h. Then add the mixture to the SiO2 dispersion to obtain a modified SiO2 mixture; wherein the mass of KH-570 is 20% of the mass of nano-SiO2. c. The modified SiO2 mixture obtained in step b is reacted in a constant temperature water bath at 75℃ at a speed of 1000 rpm for 8 hours to obtain a modified SiO2 reaction emulsion. d. The modified SiO2 reactive emulsion was centrifuged and ultrasonically cleaned three times with ethanol solution to obtain the cleaned emulsion. e. The cleaned emulsion was heated at 80°C for 6 hours in a vacuum drying oven and then ground to obtain modified nano-SiO2 powder. f. Weigh the modified nano-SiO2 powder, polyurethane resin A, and ethyl acetate according to the mass ratio of 1:8:10. Disperse the modified nano-SiO2 powder in ethyl acetate using ultrasonication, then add polyurethane resin A and stir at 2000 rpm for 30 min to obtain component A. g. Weigh the isocyanate curing agent as component B according to the mass ratio of polyurethane resin A to isocyanate curing agent of 8:2. Stir component A and component B at 1000 rpm for 30 min, let stand to defoam, and obtain the mixed slurry. h. Use 200-grit sandpaper to sand the surface of the radome unit plate and dry it at room temperature for 4 hours; then spray a mixed slurry on the surface with a thickness of 300μm, cure it at room temperature for 4 hours, and then heat it to 50℃ and keep it at that temperature for 2 hours to obtain the radome surface coating.

[0039] The water contact angle of the radome surface coating obtained in this embodiment is as follows: Figure 1 As shown, the water contact angle is 151.49°. This is the water contact angle of the radome unit panel (excluding the surface coating) without the polyurethane-based superhydrophobic anti-icing coating of this invention. Figure 2 As shown, it is 68.87°.

[0040] The macroscopic photograph of water droplet rolling on the radome surface coating obtained in this embodiment is shown below. Figure 3 As shown.

[0041] The dielectric constant of the radome surface coating obtained in this embodiment is 3.5, and the loss tangent is 0.006.

[0042] Example 2

[0043] For details, please refer to Example 1, except that: in step b, the mass of KH-570 is 15% of the mass of nano-SiO2; in step f, the mass ratio of modified nano-SiO2 powder, polyurethane resin A, and ethyl acetate is 1.6:8:9; and in step g, the mass ratio of polyurethane resin A and isocyanate curing agent is 1:1.

[0044] The water contact angle of the radome surface coating obtained in this embodiment is 150.64°, the dielectric constant is 3.4, and the loss tangent is 0.005.

[0045] Example 3

[0046] For details, please refer to Example 1, except that: in step b, the mass of KH-570 is 17% of the mass of nano-SiO2; in step f, the mass ratio of modified nano-SiO2 powder, polyurethane resin A, and ethyl acetate is 2.4:8:7; and in step g, the mass ratio of polyurethane resin A and isocyanate curing agent is 2:1.

[0047] The water contact angle of the radome surface coating obtained in this embodiment is 151.12°, the dielectric constant is 3.5, and the loss tangent is 0.005.

[0048] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A polyurethane-based superhydrophobic anti-icing coating, characterized in that, Includes component A and component B; The A component comprises the following raw materials: silane coupling agent modified nano-SiO2, polyurethane resin A material, and organic solvent; Component B includes the following raw materials: isocyanate curing agent; The mass ratio of polyurethane resin A to component B in component A is 1~4:

1.

2. The polyurethane-based superhydrophobic anti-icing coating according to claim 1, characterized in that, The mass of the silane coupling agent modified nano-SiO2 is 10-35% of the mass of polyurethane resin A; the mass ratio of polyurethane resin A to organic solvent is 1-8:5-10.

3. The polyurethane-based superhydrophobic anti-icing coating according to claim 1, characterized in that, The polyurethane resin A is the main component in the two-component polyurethane adhesive; the isocyanate curing agent is the curing agent in the two-component polyurethane adhesive.

4. The polyurethane-based superhydrophobic anti-icing coating according to claim 1, characterized in that, The organic solvent is ethyl acetate.

5. The polyurethane-based superhydrophobic anti-icing coating according to claim 1, characterized in that, The preparation method of the silane coupling agent modified nano-SiO2 includes the following steps: Nano-SiO2 and ethanol solution were ultrasonically dispersed to obtain SiO2 dispersion; Oxalic acid solution, anhydrous ethanol, and silane coupling agent are mixed to obtain the modified solution; SiO2 dispersion and modified liquid were mixed and reacted to obtain silane coupling agent modified nano-SiO2.

6. The polyurethane-based superhydrophobic anti-icing coating according to claim 5, characterized in that, The particle size of the nano-SiO2 is 7~15nm; the silane coupling agent is γ-methacryloyloxypropyltrimethoxysilane; the mass of the silane coupling agent is 15~20% of the mass of the nano-SiO2.

7. The polyurethane-based superhydrophobic anti-icing coating according to claim 5, characterized in that, The reaction temperature is 70~80℃; the reaction time is 3~8h.

8. A method for preparing a polyurethane-based superhydrophobic anti-icing coating according to any one of claims 1 to 7, characterized in that, Includes the following steps: Silane coupling agent modified nano-SiO2, organic solvent, and polyurethane resin A are mixed to obtain component A; component A and component B are packaged separately to obtain polyurethane-based superhydrophobic anti-icing coating.

9. The application of the polyurethane-based superhydrophobic anti-icing coating according to any one of claims 1 to 7 in the preparation of a radome surface coating, characterized in that, The method for preparing the coating on the radome surface includes the following steps: After mixing components A and B, the mixture is applied to the surface of the radome. After curing at room temperature, the temperature is raised and maintained to obtain the radome surface coating. The coating thickness is 200~400μm; the curing time at room temperature is 2~5h; the heating and holding temperature is 50~60℃; and the heating and holding time is 1~2h.