A composite protective coating, its preparation method, and its application in the preparation of wood and bamboo products.
Through the chemical reaction of reactive phosphorus-containing waterborne polyurethane emulsion, dynamic hydrogel network and tannic acid modified expandable graphite in composite protective coating, a continuous carbon layer and electrostatic anti-mold mechanism are formed, which solves the problems of flame retardancy and mildew prevention on the surface of wood and bamboo, and achieves efficient heat insulation and mildew prevention effects.
Patent Information
- Application Number
- CN202611297550.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
Existing protective coatings for wood and bamboo surfaces, while achieving both flame retardancy and mildew resistance, suffer from problems such as poor film formation, low stability, and migration of flame retardant components, and lack thermal insulation effects.
The composite material, consisting of reactive phosphorus-containing waterborne polyurethane emulsion, dynamic hydrogel network, and tannic acid-modified expandable graphite, forms a continuous carbon layer through chemical reaction. Combined with the electrostatic effect of hydroxypropyltrimethylammonium chloride chitosan, it achieves flame retardant, heat insulation, and mildew prevention effects.
It provides a composite protective coating with good stability, good film-forming properties, good flexibility, good flame retardancy, good heat insulation and good mildew prevention, which significantly improves the overall protective performance of wood and bamboo.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to a composite protective coating, its preparation method, and its application in the preparation of wood and bamboo products. Background Technology
[0002] Wood and bamboo contain cellulose, hemicellulose, and lignin, and are characterized by their renewability, ease of processing, and natural texture. However, they also contain a high number of hydrophilic groups and combustible organic components, making them prone to moisture absorption and mold growth under humid and hot conditions, and susceptible to pyrolysis and the release of flammable volatiles in the event of a fire. Therefore, protective coatings for wood and bamboo surfaces need to simultaneously provide both daily mold prevention and fire resistance and heat insulation.
[0003] Traditional physical additive flame retardant coatings typically involve directly dispersing phosphorus-based flame retardants, expandable graphite, or inorganic fillers in resin. However, this approach has several drawbacks: when the content of flame retardant components is too low, it is difficult to form a continuous char layer; when the content is too high, it may cause agglomeration, increased viscosity, decreased film-forming properties, and reduced adhesion. Furthermore, phosphorus-containing small molecules may migrate during long-term service, making it difficult to achieve both flame retardant effect and coating stability.
[0004] For example, existing heat-insulating, flame-retardant, and anti-corrosion coatings, as a type of physically additive heat-insulating and flame-retardant coating, include water-based polyurethane emulsions, fillers, flame retardants, and additives. The fillers include graphene aerogel and phosphorylated nanocellulose, and the flame retardants include zinc borate and melamine polyphosphate. Furthermore, it involves glass micropowder / silica / polyaniline modified graphene aerogel. It mainly achieves heat insulation, flame retardancy, and anti-corrosion effects by physically compounding porous aerogels and inorganic / nitrogen- and phosphorus-containing flame retardants. On the one hand, the preparation method of physical mixing is not conducive to reducing the risk of filler agglomeration and film discontinuity, resulting in high viscosity and poor film-forming properties of the coating. On the other hand, it does not have anti-mildew function.
[0005] In addition, no reports have been seen to date regarding "chemically reactive heat-insulating, flame-retardant, and mildew-proof coatings".
[0006] For the reasons stated above, this invention is proposed. Summary of the Invention
[0007] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a composite protective coating with good stability, good film-forming properties, good flexibility, good flame retardancy, good heat insulation and mildew prevention, as well as its preparation method and its application in the preparation of wood and bamboo products.
[0008] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: A composite protective coating, wherein the raw materials for preparing the composite protective coating include a reactive phosphorus-containing waterborne polyurethane emulsion, a dynamic hydrogel network, and tannic acid-modified expandable graphite; the mass ratio of the reactive phosphorus-containing waterborne polyurethane emulsion, the dynamic hydrogel network, and the tannic acid-modified expandable graphite is 10:0.30-0.40:0.10-0.20. The reactive phosphorus-containing waterborne polyurethane emulsion is prepared by prepolymerization, phosphorus-containing chain extension, hydrophilic chain extension, neutralization and water dispersion of polypropylene glycol, isophorone diisocyanate, DOPO-containing diol, 2,2-dimethylolpropionic acid, 1,4-butanediol, triethylamine and dibutyltin dilaurate as raw materials. The dynamic hydrogel network is prepared from polyvinyl alcohol, tannic acid, phytic acid, cellulose nanofibers and hydroxypropyltrimethylammonium chloride chitosan as raw materials; before being mixed with the reactive phosphorus-containing waterborne polyurethane emulsion, the following treatment is also included: adjusting the pH value of the dynamic hydrogel network to 6.8-7.2 with triethylamine; The tannic acid-modified expandable graphite is prepared by modifying expandable graphite with tannic acid.
[0009] In a further improvement of the aforementioned composite protective coating, the molar ratio of the DOPO-structured diol to polypropylene glycol is 1:0.81–1.50; and the molar ratio of the NCO groups in the isophorone diisocyanate to the OH groups in all the hydroxyl-containing raw materials is 1.8–2.1:1. More preferably, the molar ratio of the NCO groups in the isophorone diisocyanate to the OH groups in all the hydroxyl-containing raw materials is 2.0:1.
[0010] In a further improvement of the aforementioned composite protective coating, the number average molecular weight of the polypropylene glycol is 2000 g / mol, i.e., the polypropylene glycol is PPG-2000.
[0011] In a further improvement of the aforementioned composite protective coating, the molar ratio of tannic acid, phytic acid, and the quaternary ammonium groups contained in the hydroxypropyltrimethylammonium chloride chitosan is 1:1:1.00 to 1.20.
[0012] In a further improvement of the aforementioned composite protective coating, the mass ratio of expandable graphite to tannic acid is 10:1.0 to 1.8.
[0013] In a further improvement to the aforementioned composite protective coating, the raw materials for preparing the composite protective coating also include a defoamer; the amount of the defoamer is 0.5% of the total mass of the composite protective coating.
[0014] In a further improvement of the aforementioned composite protective coating, the defoamer is a polyether-modified silicone solution.
[0015] As a general technical concept, the present invention also provides a method for preparing the above-mentioned composite protective coating, comprising the following steps: adding a dynamic hydrogel network to a reactive phosphorus-containing waterborne polyurethane emulsion under stirring conditions of 800 r / min to 1200 r / min, stirring for 5 min to 20 min, adding tannic acid-modified expandable graphite and defoamer, stirring for 10 min to 30 min, and obtaining the composite protective coating.
[0016] As a general technical concept, the present invention also provides the application of the above-described composite protective coating or the composite protective coating prepared by the above-described preparation method in the preparation of wood products and bamboo products.
[0017] The above-mentioned application, further improved, includes the following steps: applying a composite protective coating to the surface of wood or bamboo, curing it to form a composite protective coating on the surface of wood or bamboo; the curing time is 24 hours; the thickness of the composite protective coating is 100±10μm.
[0018] In the actual preparation process, relevant preparation standards and product performance requirements must be met.
[0019] Compared with the prior art, the advantages of the present invention are as follows: (1) In the composite protective coating of the present invention, a reactive phosphorus-containing waterborne polyurethane emulsion is used as the continuous film-forming phase, a dynamic hydrogel network containing polyvinyl alcohol, tannic acid, phytic acid, cellulose nanofibers and hydroxypropyltrimethylammonium chloride chitosan is used as the water storage, char formation, reinforcement and mildew prevention functional unit, and tannic acid-modified expandable graphite is used as the thermal expansion structural unit. During the fire response process, the water contained in the hydrogel evaporates and absorbs heat first, the phosphorus-containing structures in the tannic acid, phytic acid and polyurethane chains participate in char formation, the expandable graphite expands under heat to form a porous heat-insulating structure, and the cellulose nanofibers participate in the construction of the reinforced carbon skeleton. Therefore, under their combined action, the stability, film-forming properties and flexibility, flame retardancy and heat insulation can be significantly improved. At the same time, during the mildew prevention process, the quaternary ammonium groups contained in hydroxypropyltrimethylammonium chloride chitosan can interact electrostatically with the negatively charged structures on the surface of mold cells, interfering with cell membrane permeability. The polyphenolic structure of tannic acid can also participate in inhibiting mold adhesion and growth. Therefore, in its The combined effect of these components can significantly improve the anti-mildew effect. In addition, the present invention introduces a DOPO-containing diol into the molecular chain of waterborne polyurethane through a chemical reaction, which can effectively reduce the risk of migration of physically added phosphorus-containing flame retardants. By introducing tannic acid, phytic acid, cellulose nanofibers and hydroxypropyltrimethylammonium chloride chitosan into the polyvinyl alcohol network and adjusting the pH value to near neutral before compounding with waterborne polyurethane, the risk of emulsion demulsification caused by acidic hydrogel can be reduced. By controlling the proportion of each component and the pH of the dynamic hydrogel network, the risks of emulsion demulsification, filler agglomeration and coating discontinuity can be significantly reduced. Thus, a composite protective coating with good stability, good film-forming properties and flexibility, good flame retardancy, good heat insulation and anti-mildew effect can be obtained. As a comprehensive heat-insulating, flame-retardant and mildew-proof coating with excellent performance, it can effectively protect the surface of wood and bamboo materials while taking into account daily mildew prevention and fire-retardant heat insulation. It has high use value and good application prospects.
[0020] (2) In this invention, by optimizing the mass ratio of reactive phosphorus-containing waterborne polyurethane emulsion, dynamic hydrogel network, and tannic acid-modified expandable graphite to 10:0.30-0.40:0.10-0.20, the reactive phosphorus-containing waterborne polyurethane can maintain a continuous film-forming phase, and the dynamic hydrogel network and tannic acid-modified expandable graphite can be dispersed more uniformly in the coating film, thereby taking into account the storage stability, application viscosity, and film continuity of the coating, and playing the roles of heat absorption, carbonization promotion, and expansion insulation. However, when the amount of dynamic hydrogel network is too low, the system's water storage heat absorption, acid source, and carbon source contribution are insufficient, and the heat-induced carbonization and mildew-inhibiting effects may be weakened. When the amount is too high, the system's hydrophilicity and viscosity increase, and flocculation, slow drying, and decreased water resistance and continuity of the coating film are likely to occur. Furthermore, when the amount of tannic acid-modified expandable graphite is too low, it is difficult to form a continuous and dense expandable heat insulation layer after ignition. Conversely, when the amount is too high, the solid particles are prone to agglomeration or sedimentation, which may lead to a rough coating surface, reduced flexibility, and decreased adhesion. Therefore, the above mass ratio is beneficial for achieving a balance between continuous film formation, system stability, and flame-retardant and heat-insulating functions.
[0021] (3) In this invention, by optimizing the molar ratio of DOPO-containing diol to polypropylene glycol to 1:0.81-1.50, the proportion of phosphorus-containing structure can be adjusted, making the coating more flame-retardant, while also improving the emulsion stability and film flexibility. At the same time, by optimizing the molar ratio of NCO groups in isophorone diisocyanate to OH groups in all hydroxyl-containing raw materials to 1.8-2.1:1, a certain number of NCO end groups are retained in the prepolymer, which facilitates the formation of urea bond structures during subsequent water dispersion and chain extension, thereby improving the cohesive effect of hard segments, film strength, and heat resistance. However, if the ratio is too low, there will be insufficient NCO groups available for subsequent chain extension, and the molecular weight and hard segment content of the resulting polymer may be low, which will reduce the mechanical strength, water resistance, and heat resistance of the film. If the ratio is too high, there will be too many residual NCO groups, which will release more carbon dioxide when reacting with water, easily causing foaming, local gelation, a sudden increase in viscosity, and a decrease in emulsion stability. Therefore, this ratio should be controlled in combination with the actual NCO content and dispersion stability after the prepolymerization reaction, so as to balance the prepolymerization reaction, subsequent chain extension and film formation performance.
[0022] (4) In this invention, the dynamic hydrogel network is prepared from polyvinyl alcohol, tannic acid, phytic acid, cellulose nanofibers and hydroxypropyltrimethylammonium chloride chitosan. Since both tannic acid and phytic acid are acidic, they may reduce the pH of the emulsion and cause demulsification when compounded with waterborne polyurethane. At the same time, if the ratio of polymer, acidic component and fiber component is not right, it may also lead to excessive gel strength or difficulty in dispersion. In this invention, the molar ratio of quaternary ammonium groups in tannic acid, phytic acid and hydroxypropyltrimethylammonium chloride chitosan is optimized to 1:1:1.00-1.20, so that the acidic and polyphenolic sites provided by phytic acid and tannic acid are in relative balance with the quaternary ammonium group cationic sites. A dynamic network with reversible cross-linking characteristics is formed through hydrogen bonding and electrostatic interaction. At the same time, the adverse effects of free acid on the stability of waterborne polyurethane emulsion are reduced, and the phosphorus-containing carbonization, nitrogen-containing synergistic effect and quaternary ammonium group antifungal effect are taken into account. However, when the proportion of quaternary ammonium groups is too low, the acidic component is relatively excessive, the system pH decreases, and emulsion flocculation or demulsification is easily induced. Furthermore, insufficient cationic sites weaken the dynamic network and antifungal effect. Conversely, when the proportion of quaternary ammonium groups is too high, the excessive cationic polymer may cause charge neutralization and bridging flocculation, resulting in excessively high system viscosity or gel strength, making dispersion, application, and continuous film formation difficult. Therefore, controlling the molar ratio of the three components within the above-mentioned range is beneficial for balancing dynamic network stability, emulsion compatibility, application performance, and flame retardant and antifungal functions.
[0023] (5) Although conventional expandable graphite can form a porous thermal insulation structure after heating, its surface polarity is low, and its compatibility with waterborne polyurethane and hydrogel networks is limited. In this invention, tannic acid is used to modify the surface of expandable graphite, which can improve its interfacial effect by utilizing polyphenol groups. By optimizing the mass ratio of expandable graphite to tannic acid to 10:1.0-1.8, the expandable graphite can take into account both surface compatibility and thermal expansion structure function. In addition, if the amount of tannic acid is too small, the modification may be insufficient, while if the amount is too large, excessive free polyphenols may be introduced and affect the stability of the system.
[0024] (6) The raw materials for preparing the composite protective coating of the present invention also include a defoamer, wherein the amount of defoamer is 0.5% of the total mass of the composite protective coating. It can suppress the foam introduced and stabilized by waterborne polyurethane, dynamic hydrogel network and solid particles during high-speed dispersion and stirring, reduce bubbles, pinholes and craters in the coating film, and make the coating and the carbon layer formed after firing more continuous and dense. However, when the amount of defoamer is too low, the microbubbles in the system are difficult to remove completely, which can easily cause coating defects and weaken adhesion, water resistance and barrier properties; while when the amount is too high, the excess defoamer may migrate or precipitate due to insufficient compatibility, causing craters, fish eyes, surface slippage, decreased interlayer adhesion and poor storage stability. Therefore, controlling the amount of defoamer to 0.5% of the total mass of the composite protective coating is beneficial to achieving a balance between effective defoaming and coating surface quality, adhesion performance and system stability.
[0025] (7) In this invention, except for triethylamine, other organic amines or alkaline substances cannot be used to adjust the pH value of the dynamic hydrogel network. This is because these substances have different effects on volatility, ionic strength, degree of phytic acid / tannic acid dissociation, and stability of the dynamic network and waterborne polyurethane emulsion, which will have an adverse effect on the stability and film-forming properties of the dynamic hydrogel network. Detailed Implementation
[0026] The present invention will be further described below with reference to specific preferred embodiments, but this does not limit the scope of protection of the present invention.
[0027] The following examples all use the same bamboo material, the same spraying method, the same dry film thickness, and the same curing conditions; the only difference lies in the formulation ratio. Each example begins with the preparation of a reactive phosphorus-containing waterborne polyurethane emulsion, a dynamic hydrogel network, and tannic acid-modified expandable graphite, and proceeds sequentially to the formulation, coating, and curing of the composite coating, independently constituting a complete technical solution. The IPDI dosage is calculated based on a relative molecular mass of 222.32 and an NCO / OH ratio of 2.0:1; the dosage of the DOPO-containing diol is calculated based on a relative molecular mass of 324.27.
[0028] In this invention, PPG-2000 is polypropylene glycol with a number-average molecular weight of approximately 2000 g / mol; IPDI is isophorone diisocyanate with the molecular formula C12H18N2O2 and a relative molecular mass of 222.32; the DOPO-containing diol is 10-(2,5-dihydroxyphenyl)-10-hydro-9-oxa-10-phosphaphenanthrene-10-oxide with the molecular formula C18H13PO4, a relative molecular mass of 324.27, and CAS number 99208-50-1; DMPA is 2,2-dimethylolpropionic acid; BDO is 1,4-butanediol; TEA is triethylamine; and DBTDL is dibutyltin dilaurate. The above definitions and calculation standards apply to all examples and comparative examples.
[0029] Example 1 A composite protective coating is prepared using raw materials including a reactive phosphorus-containing waterborne polyurethane emulsion, a dynamic hydrogel network, and tannic acid-modified expandable graphite, wherein the mass ratio of the reactive phosphorus-containing waterborne polyurethane emulsion, the dynamic hydrogel network, and the tannic acid-modified expandable graphite is 10:0.30:0.10. This allows for the preparation of the composite protective coating under the lower limit of the mixing ratio.
[0030] In this embodiment, the reactive phosphorus-containing waterborne polyurethane emulsion used is prepared from polypropylene glycol (PPG-2000), isophorone diisocyanate (IPDI), DOPO-containing diol, 2,2-dimethylolpropionic acid (DMPA), 1,4-butanediol (BDO), triethylamine (TEA), and dibutyltin dilaurate (DBTDL) through prepolymerization, phosphorus-containing chain extension, hydrophilic chain extension, neutralization, and water dispersion. The specific preparation process is as follows: Weigh 30.00g of PPG-2000 and dehydrate it under vacuum for 2 hours at 105℃ and 1000r / min with stirring. After cooling to 75℃, add 38.03g of IPDI and 0.05g of DBTDL, and react for 2 hours. Then add 6.01g (18.52mmol) of a DOPO-containing diol to make the molar ratio of the DOPO-containing diol to PPG-2000 1:0.81, and continue reacting for 2 hours. Finally, add 4.00g of DMPA and 2.00g of... BDO was used for chain extension. The amount of IPDI used was calculated based on a ratio of 2.0:1 between the total number of NCO groups in IPDI and the total number of OH groups in PPG-2000, DOPO-structured diol, DMPA, and BDO. After the reaction was completed, the temperature was lowered to 40-50°C, and 3.02g of TEA was added for neutralization. Deionized water was slowly added while stirring at 1000r / min. The reactive phosphorus-containing waterborne polyurethane emulsion was obtained by phase inversion.
[0031] In this embodiment, the dynamic hydrogel network used was prepared from polyvinyl alcohol (PVA, CAS: 9002-89-5, degree of polymerization 500, molecular weight: 22025), tannic acid, phytic acid, cellulose nanofibers, and hydroxypropyltrimethylammonium chloride chitosan. The specific preparation process is as follows: 10.00 g of PVA was weighed and added to 90.00 g of deionized water. The solution was dissolved under stirring at 90 °C and 1000 rpm. After cooling to room temperature, the cellulose nanofiber dispersion was added, and the solution was dispersed at 1000 rpm for 30 min. Using 1.00 mmol each of tannic acid and phytic acid as a basis, 1.00 mmol of tannic acid, 1.00 mmol of phytic acid, and 1.00 mmol of hydroxypropyltrimethylammonium chloride chitosan (calculated based on the amount of quaternary ammonium compounds) were added to achieve a molar ratio of tannic acid, phytic acid, and hydroxypropyltrimethylammonium chloride chitosan of 1:1:1.00. The cellulose nanofibers were added in excess, and the dry basis amount was calculated based on the solid content of the dispersion. After the system was thoroughly mixed, a dynamic hydrogel network was obtained.
[0032] In this embodiment, the dynamic hydrogel network used is further treated as follows before being mixed with the reactive phosphorus-containing waterborne polyurethane emulsion: triethylamine (TEA) is added dropwise to the dynamic hydrogel network, and the pH value of the dynamic hydrogel network is adjusted to 6.8-7.2 using triethylamine (TEA).
[0033] In this embodiment, the tannic acid-modified expandable graphite used is prepared by modifying expandable graphite with tannic acid. The specific preparation process is as follows: Weigh 10.00g of expandable graphite and 1.00g of tannic acid to make the mass ratio of expandable graphite to tannic acid 10:1.00; dissolve tannic acid in 100mL of deionized water and add expandable graphite, sonicate for 30min, then stir at 1000r / min for 2h, filter and dry to obtain tannic acid modified expandable graphite.
[0034] In this embodiment, the raw materials for preparing the composite protective coating also include a defoamer, wherein the amount of defoamer is 0.5% of the total mass of the composite protective coating, and the defoamer is a polyether-modified organosilicon solution (ZH-7011).
[0035] A method for preparing the composite protective coating in this embodiment includes the following steps: Using 10.00 parts by weight of reactive phosphorus-containing waterborne polyurethane emulsion, 0.30 parts by weight of the aforementioned dynamic hydrogel network and 0.10 parts by weight of the aforementioned tannic acid-modified expandable graphite were added, making the mass ratio of the three components 10:0.30:0.10. First, the dynamic hydrogel network was slowly added to the waterborne polyurethane emulsion at 1000 r / min and mixed for 10 min. Then, the tannic acid-modified expandable graphite and 0.5% by weight of ZH-7011 polyether-modified silicone defoamer (based on the total mass of the composite protective coating) were added, and the mixture was dispersed at 1000 r / min for 20 min, followed by degassing to obtain the composite protective coating.
[0036] The application of the composite protective coating prepared in this embodiment in the preparation of bamboo products includes the following steps: (1) Select bamboo samples from the same batch, sand the surface and clean with ethanol; (2) The composite protective coating is sprayed onto the surface of bamboo and the thickness of the dry film is controlled to be 100±10μm. It is cured at room temperature for 24h to form a composite protective coating on the surface of bamboo, and a sample of anti-mildew and flame-retardant water-based polyurethane bamboo protective coating is obtained.
[0037] All the following examples and comparative examples used the same spraying process to apply the composite protective coating in multiple coats. The sample size, sandpaper grit, coating amount per coat, drying time between coats, and curing environment were kept consistent.
[0038] In this embodiment, the prepared composite protective coating can also be used to prepare wood products.
[0039] Example 2 A composite protective coating is prepared using raw materials including a reactive phosphorus-containing waterborne polyurethane emulsion, a dynamic hydrogel network, and tannic acid-modified expandable graphite, wherein the mass ratio of the reactive phosphorus-containing waterborne polyurethane emulsion, the dynamic hydrogel network, and the tannic acid-modified expandable graphite is 10:0.33:0.13. This allows for the preparation of the composite protective coating under medium to low mixing ratio conditions.
[0040] In this embodiment, the reactive phosphorus-containing waterborne polyurethane emulsion used is prepared from polypropylene glycol (PPG-2000), isophorone diisocyanate (IPDI), DOPO-containing diol, 2,2-dimethylolpropionic acid (DMPA), 1,4-butanediol (BDO), triethylamine (TEA), and dibutyltin dilaurate (DBTDL) through prepolymerization, phosphorus-containing chain extension, hydrophilic chain extension, neutralization, and water dispersion. The specific preparation process is as follows: Weigh 30.00 g of PPG-2000 and dehydrate it under vacuum for 2 h at 105 °C and 1000 r / min with stirring. After cooling to 75 °C, add 36.47 g of IPDI and 0.05 g of DBTDL, and react for 2 h. Add 4.86 g (15.00 mmol) of a DOPO-containing diol to make the molar ratio of the DOPO-containing diol to PPG-2000 1:1.00, and continue reacting for 2 h. Then add 4.00 g of DMPA and 2.00 g of BDO for chain extension. The amount of IPDI used is calculated based on a ratio of 2.0:1 between the total number of NCO groups in IPDI and the total number of OH groups in PPG-2000, the DOPO-containing diol, DMPA, and BDO. After the reaction was completed, the temperature was lowered to 40-50℃, 3.02g of TEA was added for neutralization, and deionized water was slowly added while stirring at 1000r / min. The reactive phosphorus-containing waterborne polyurethane emulsion was obtained by phase inversion.
[0041] In this embodiment, the dynamic hydrogel network used is prepared from polyvinyl alcohol (PVA), tannic acid, phytic acid, cellulose nanofibers, and hydroxypropyltrimethylammonium chloride chitosan. The specific preparation process is as follows: 10.00 g of PVA was weighed and added to 90.00 g of deionized water, and dissolved under stirring at 90 °C and 1000 r / min. After cooling to room temperature, cellulose nanofiber dispersion was added, and dispersed at 1000 r / min for 30 min. Using 1.00 mmol each of tannic acid and phytic acid as a basis, 1.00 mmol of tannic acid, 1.00 mmol of phytic acid, and 1.05 mmol of hydroxypropyltrimethylammonium chloride chitosan (calculated based on the amount of quaternary ammonium compounds) were added to achieve a molar ratio of tannic acid, phytic acid, and hydroxypropyltrimethylammonium chloride chitosan of 1:1:1.05. Cellulose nanofibers were added in excess, with the dry basis amount calculated based on the solid content of the dispersion. After the system was thoroughly mixed, a dynamic hydrogel network was obtained.
[0042] In this embodiment, the dynamic hydrogel network used is further treated as follows before being mixed with the reactive phosphorus-containing waterborne polyurethane emulsion: triethylamine (TEA) is added dropwise to the dynamic hydrogel network, and the pH value of the dynamic hydrogel network is adjusted to 6.8-7.2 using triethylamine (TEA).
[0043] In this embodiment, the tannic acid-modified expandable graphite used is prepared by modifying expandable graphite with tannic acid. The specific preparation process is as follows: Weigh 10.00g of expandable graphite and 1.20g of tannic acid to make the mass ratio of expandable graphite to tannic acid 10:1.20; dissolve tannic acid in 100mL of deionized water and add expandable graphite, sonicate for 30min, then stir at 1000r / min for 2h, filter and dry to obtain tannic acid modified expandable graphite.
[0044] In this embodiment, the raw materials for preparing the composite protective coating also include a defoamer, wherein the amount of defoamer is 0.5% of the total mass of the composite protective coating, and the defoamer is a polyether-modified organosilicon solution (ZH-7011).
[0045] A method for preparing the composite protective coating in this embodiment includes the following steps: Using 10.00 parts by weight of reactive phosphorus-containing waterborne polyurethane emulsion, 0.33 parts by weight of the aforementioned dynamic hydrogel network and 0.13 parts by weight of the aforementioned tannic acid-modified expandable graphite were added, making the mass ratio of the three components 10:0.33:0.13. First, the dynamic hydrogel network was slowly added to the waterborne polyurethane emulsion at 1000 r / min and mixed for 10 min. Then, the tannic acid-modified expandable graphite and 0.5% by weight of ZH-7011 polyether-modified silicone defoamer (based on the total mass of the composite protective coating) were added, dispersed at 1000 r / min for 20 min, and then defoamed to obtain the composite protective coating.
[0046] The application of the composite protective coating prepared in this embodiment in the preparation of bamboo products includes the following steps: (1) Select bamboo samples from the same batch, sand the surface and clean with ethanol; (2) The composite protective coating is sprayed onto the surface of bamboo and the thickness of the dry film is controlled to be 100±10μm. It is cured at room temperature for 24h to form a composite protective coating on the surface of bamboo, and a sample of anti-mildew and flame-retardant water-based polyurethane bamboo protective coating is obtained.
[0047] In this embodiment, the prepared composite protective coating can also be used to prepare wood products.
[0048] Example 3 A composite protective coating is prepared using raw materials including a reactive phosphorus-containing waterborne polyurethane emulsion, a dynamic hydrogel network, and tannic acid-modified expandable graphite, wherein the mass ratio of the reactive phosphorus-containing waterborne polyurethane emulsion, the dynamic hydrogel network, and the tannic acid-modified expandable graphite is 10:0.36:0.16. This allows for the preparation of the composite protective coating under medium to high mixing ratio conditions.
[0049] In this embodiment, the reactive phosphorus-containing waterborne polyurethane emulsion used is prepared from polypropylene glycol (PPG-2000), isophorone diisocyanate (IPDI), DOPO-containing diol, 2,2-dimethylolpropionic acid (DMPA), 1,4-butanediol (BDO), triethylamine (TEA), and dibutyltin dilaurate (DBTDL) through prepolymerization, phosphorus-containing chain extension, hydrophilic chain extension, neutralization, and water dispersion. The specific preparation process is as follows: Weigh 30.00 g of PPG-2000 and dehydrate it under vacuum for 2 h at 105 °C and 1000 r / min with stirring. After cooling to 75 °C, add 35.36 g of IPDI and 0.05 g of DBTDL, and react for 2 h. Add 4.05 g (12.50 mmol) of a DOPO-containing diol to make the molar ratio of the DOPO-containing diol to PPG-2000 1:1.20, and continue reacting for 2 h. Then add 4.00 g of DMPA and 2.00 g of BDO for chain extension. The amount of IPDI used is calculated based on a ratio of 2.0:1 between the total number of NCO groups in IPDI and the total number of OH groups in PPG-2000, the DOPO-containing diol, DMPA, and BDO. After the reaction was completed, the temperature was lowered to 40-50℃, 3.02g of TEA was added for neutralization, and deionized water was slowly added while stirring at 1000r / min. The reactive phosphorus-containing waterborne polyurethane emulsion was obtained by phase inversion.
[0050] In this embodiment, the dynamic hydrogel network used is prepared from polyvinyl alcohol (PVA), tannic acid, phytic acid, cellulose nanofibers, and hydroxypropyltrimethylammonium chloride chitosan. The specific preparation process is as follows: 10.00 g of PVA was weighed and added to 90.00 g of deionized water, and dissolved under stirring at 90 °C and 1000 r / min. After cooling to room temperature, cellulose nanofiber dispersion was added, and dispersed at 1000 r / min for 30 min. Using 1.00 mmol each of tannic acid and phytic acid as a basis, 1.00 mmol of tannic acid, 1.00 mmol of phytic acid, and 1.10 mmol of hydroxypropyltrimethylammonium chloride chitosan (calculated based on the amount of quaternary ammonium compounds) were added to achieve a molar ratio of tannic acid, phytic acid, and hydroxypropyltrimethylammonium chloride chitosan of 1:1:1.10. Cellulose nanofibers were added in excess, with the dry basis amount calculated based on the solid content of the dispersion. After the system was thoroughly mixed, a dynamic hydrogel network was obtained.
[0051] In this embodiment, the dynamic hydrogel network used is further treated as follows before being mixed with the reactive phosphorus-containing waterborne polyurethane emulsion: triethylamine (TEA) is added dropwise to the dynamic hydrogel network, and the pH value of the dynamic hydrogel network is adjusted to 6.8-7.2 using triethylamine (TEA).
[0052] In this embodiment, the tannic acid-modified expandable graphite used is prepared by modifying expandable graphite with tannic acid. The specific preparation process is as follows: Weigh 10.00g of expandable graphite and 1.50g of tannic acid to make the mass ratio of expandable graphite to tannic acid 10:1.50; dissolve tannic acid in 100mL of deionized water and add expandable graphite, sonicate for 30min, then stir at 1000r / min for 2h, filter and dry to obtain tannic acid modified expandable graphite.
[0053] In this embodiment, the raw materials for preparing the composite protective coating also include a defoamer, wherein the amount of defoamer is 0.5% of the total mass of the composite protective coating, and the defoamer is a polyether-modified organosilicon solution (ZH-7011).
[0054] A method for preparing the composite protective coating in this embodiment includes the following steps: 10.00 parts by weight of reactive phosphorus-containing waterborne polyurethane emulsion were mixed with 0.36 parts by weight of the aforementioned dynamic hydrogel network and 0.16 parts by weight of the aforementioned tannic acid-modified expandable graphite, making the mass ratio of the three components 10:0.36:0.16. The dynamic hydrogel network was first slowly added to the waterborne polyurethane emulsion at 1000 r / min and mixed for 10 min. Then, the tannic acid-modified expandable graphite and 0.5% by weight of ZH-7011 polyether-modified silicone defoamer (based on the total mass of the composite protective coating) were added, dispersed at 1000 r / min for 20 min, and then defoamed to obtain the composite protective coating.
[0055] The application of the composite protective coating prepared in this embodiment in the preparation of bamboo products includes the following steps: (1) Select bamboo samples from the same batch, sand the surface and clean with ethanol; (2) The composite protective coating is sprayed onto the surface of bamboo and the thickness of the dry film is controlled to be 100±10μm. It is cured at room temperature for 24h to form a composite protective coating on the surface of bamboo, and a sample of anti-mildew and flame-retardant water-based polyurethane bamboo protective coating is obtained.
[0056] In this embodiment, the prepared composite protective coating can also be used to prepare wood products.
[0057] Example 4 A composite protective coating is prepared using raw materials including a reactive phosphorus-containing waterborne polyurethane emulsion, a dynamic hydrogel network, and tannic acid-modified expandable graphite, wherein the mass ratio of the reactive phosphorus-containing waterborne polyurethane emulsion, the dynamic hydrogel network, and the tannic acid-modified expandable graphite is 10:0.40:0.20. This allows for the preparation of the composite protective coating under the upper limit of the mixing ratio.
[0058] In this embodiment, the reactive phosphorus-containing waterborne polyurethane emulsion used is prepared from polypropylene glycol (PPG-2000), isophorone diisocyanate (IPDI), DOPO-containing diol, 2,2-dimethylolpropionic acid (DMPA), 1,4-butanediol (BDO), triethylamine (TEA), and dibutyltin dilaurate (DBTDL) through prepolymerization, phosphorus-containing chain extension, hydrophilic chain extension, neutralization, and water dispersion. The specific preparation process is as follows: Weigh 30.00 g of PPG-2000 and dehydrate it under vacuum for 2 h at 105 °C and 1000 r / min with stirring. After cooling to 75 °C, add 34.24 g of IPDI and 0.05 g of DBTDL, and react for 2 h. Add 3.24 g (10.00 mmol) of a DOPO-containing diol to make the molar ratio of the DOPO-containing diol to PPG-2000 1:1.50, and continue reacting for 2 h. Then add 4.00 g of DMPA and 2.00 g of BDO for chain extension. The amount of IPDI used is calculated based on a ratio of 2.0:1 between the total number of NCO groups in IPDI and the total number of OH groups in PPG-2000, the DOPO-containing diol, DMPA, and BDO. After the reaction was completed, the temperature was lowered to 40-50℃, 3.02g of TEA was added for neutralization, and deionized water was slowly added while stirring at 1000r / min. The reactive phosphorus-containing waterborne polyurethane emulsion was obtained by phase inversion.
[0059] In this embodiment, the dynamic hydrogel network used is prepared from polyvinyl alcohol (PVA), tannic acid, phytic acid, cellulose nanofibers, and hydroxypropyltrimethylammonium chloride chitosan. The specific preparation process is as follows: 10.00 g of PVA was weighed and added to 90.00 g of deionized water, and dissolved under stirring at 90 °C and 1000 r / min. After cooling to room temperature, cellulose nanofiber dispersion was added, and dispersed at 1000 r / min for 30 min. Using 1.00 mmol each of tannic acid and phytic acid as a basis, 1.00 mmol of tannic acid, 1.00 mmol of phytic acid, and 1.20 mmol of hydroxypropyltrimethylammonium chloride chitosan (calculated based on the amount of quaternary ammonium compounds) were added to achieve a molar ratio of tannic acid, phytic acid, and hydroxypropyltrimethylammonium chloride chitosan of 1:1:1.20. Cellulose nanofibers were added in excess, with the dry basis amount calculated based on the solid content of the dispersion. After the system was thoroughly mixed, a dynamic hydrogel network was obtained.
[0060] In this embodiment, the dynamic hydrogel network used is further treated as follows before being mixed with the reactive phosphorus-containing waterborne polyurethane emulsion: triethylamine (TEA) is added dropwise to the dynamic hydrogel network, and the pH value of the dynamic hydrogel network is adjusted to 6.8-7.2 using triethylamine (TEA).
[0061] In this embodiment, the tannic acid-modified expandable graphite used is prepared by modifying expandable graphite with tannic acid. The specific preparation process is as follows: Weigh 10.00g of expandable graphite and 1.80g of tannic acid to make the mass ratio of expandable graphite to tannic acid 10:1.80; dissolve tannic acid in 100mL of deionized water and add expandable graphite, sonicate for 30min, then stir at 1000r / min for 2h, filter and dry to obtain tannic acid modified expandable graphite.
[0062] In this embodiment, the raw materials for preparing the composite protective coating also include a defoamer, wherein the amount of defoamer is 0.5% of the total mass of the composite protective coating, and the defoamer is a polyether-modified organosilicon solution (ZH-7011).
[0063] A method for preparing the composite protective coating in this embodiment includes the following steps: Using 10.00 parts by weight of reactive phosphorus-containing waterborne polyurethane emulsion, 0.40 parts by weight of the aforementioned dynamic hydrogel network and 0.20 parts by weight of the aforementioned tannic acid-modified expandable graphite were added, making the mass ratio of the three components 10:0.40:0.20. First, the dynamic hydrogel network was slowly added to the waterborne polyurethane emulsion at 1000 r / min and mixed for 10 min. Then, the tannic acid-modified expandable graphite and 0.5% by weight of ZH-7011 polyether-modified silicone defoamer (based on the total mass of the composite protective coating) were added, dispersed at 1000 r / min for 20 min, and then defoamed to obtain the composite protective coating.
[0064] The application of the composite protective coating prepared in this embodiment in the preparation of bamboo products includes the following steps: (1) Select bamboo samples from the same batch, sand the surface and clean with ethanol; (2) The composite protective coating is sprayed onto the surface of bamboo and the thickness of the dry film is controlled to be 100±10μm. It is cured at room temperature for 24h to form a composite protective coating on the surface of bamboo, and a sample of anti-mildew and flame-retardant water-based polyurethane bamboo protective coating is obtained.
[0065] In this embodiment, the prepared composite protective coating can also be used to prepare wood products.
[0066] All comparative examples below are based on Example 2, with only one key factor changed to verify the potential adverse effects of exceeding the intended scale range or omitting a key processing step. Whether a comparative example is considered an "unsuccessful attempt" should be confirmed by a combination of emulsion appearance, particle size, storage stability, viscosity, film-forming state, and subsequent performance data. Existing records have confirmed that Comparative Examples 1, 2, and 4 experienced precipitation or dispersion difficulties during the preparation or compounding stage; other unproven performance characteristics are not presumed upon.
[0067] Comparative Example 1 A composite protective coating is prepared using raw materials including a reactive phosphorus-containing waterborne polyurethane emulsion, a dynamic hydrogel network, and tannic acid-modified expandable graphite, wherein the mass ratio of the reactive phosphorus-containing waterborne polyurethane emulsion, the dynamic hydrogel network, and the tannic acid-modified expandable graphite is 10:0.33:0.13. This allows for the preparation of the composite protective coating under medium to low mixing ratio conditions.
[0068] In this comparative example, the reactive phosphorus-containing waterborne polyurethane emulsion used was prepared from polypropylene glycol (PPG-2000), isophorone diisocyanate (IPDI), DOPO-containing diol, 2,2-dimethylolpropionic acid (DMPA), 1,4-butanediol (BDO), triethylamine (TEA), and dibutyltin dilaurate (DBTDL) as raw materials through prepolymerization, phosphorus-containing chain extension, hydrophilic chain extension, neutralization, and water dispersion. The specific preparation process is as follows: Weigh 30.00 g of PPG-2000 and dehydrate it under vacuum for 2 h at 105 °C and 1000 r / min with stirring. After cooling to 75 °C, add 40.91 g of IPDI and 0.05 g of DBTDL, and react for 2 h. Add 8.11 g (25.00 mmol) of a DOPO-containing diol to make the molar ratio of the DOPO-containing diol to PPG-2000 1:0.60, and continue reacting for 2 h. Then add 4.00 g of DMPA and 2.00 g of BDO for chain extension. The amount of IPDI used is calculated based on a ratio of 2.0:1 between the total number of NCO groups in IPDI and the total number of OH groups in PPG-2000, the DOPO-containing diol, DMPA, and BDO. After the reaction was complete, the temperature was lowered to 40–50°C, and 3.02 g of TEA was added for neutralization. Deionized water was then slowly added while stirring at 1000 r / min. The reaction was reverse-phased to obtain a reactive phosphorus-containing aqueous polyurethane emulsion. Compared to Example 2, Comparative Example 1 contained an excessively high proportion of DOPO-structured diols.
[0069] In this comparative example, the dynamic hydrogel network used was prepared from polyvinyl alcohol (PVA), tannic acid, phytic acid, cellulose nanofibers, and hydroxypropyltrimethylammonium chloride chitosan. The specific preparation process is as follows: 10.00 g of PVA was weighed and added to 90.00 g of deionized water, and dissolved under stirring at 90 °C and 1000 r / min. After cooling to room temperature, cellulose nanofiber dispersion was added, and dispersed at 1000 r / min for 30 min. Using 1.00 mmol each of tannic acid and phytic acid as a basis, 1.00 mmol of tannic acid, 1.00 mmol of phytic acid, and 1.05 mmol of hydroxypropyltrimethylammonium chloride chitosan (calculated based on the amount of quaternary ammonium compounds) were added to achieve a molar ratio of tannic acid, phytic acid, and hydroxypropyltrimethylammonium chloride chitosan of 1:1:1.05. Cellulose nanofibers were added in excess, with the dry basis amount calculated based on the solid content of the dispersion. After the system was thoroughly mixed, a dynamic hydrogel network was obtained.
[0070] In this comparative example, the dynamic hydrogel network used further includes the following treatment before being mixed with the reactive phosphorus-containing aqueous polyurethane emulsion: adding triethylamine (TEA) dropwise to the dynamic hydrogel network and adjusting the pH value of the dynamic hydrogel network to 6.8-7.2 using triethylamine (TEA).
[0071] In this comparative example, the tannic acid-modified expandable graphite used was prepared by modifying expandable graphite with tannic acid. The specific preparation process is as follows: Weigh 10.00g of expandable graphite and 1.20g of tannic acid to make the mass ratio of expandable graphite to tannic acid 10:1.20; dissolve tannic acid in 100mL of deionized water and add expandable graphite, sonicate for 30min, then stir at 1000r / min for 2h, filter and dry to obtain tannic acid modified expandable graphite.
[0072] In this comparative example, the raw materials for preparing the composite protective coating also include a defoamer, wherein the amount of defoamer is 0.5% of the total mass of the composite protective coating, and the defoamer is a polyether-modified organosilicon solution (ZH-7011).
[0073] A method for preparing the composite protective coating in the above comparative example includes the following steps: Using 10.00 parts by weight of reactive phosphorus-containing waterborne polyurethane emulsion, 0.33 parts by weight of the aforementioned dynamic hydrogel network and 0.13 parts by weight of the aforementioned tannic acid-modified expandable graphite were added, making the mass ratio of the three components 10:0.33:0.13. First, the dynamic hydrogel network was slowly added to the waterborne polyurethane emulsion at 1000 r / min and mixed for 10 min. Then, the tannic acid-modified expandable graphite and 0.5% by weight of ZH-7011 polyether-modified silicone defoamer (based on the total mass of the composite protective coating) were added, dispersed at 1000 r / min for 20 min, and then defoamed to obtain the composite protective coating.
[0074] The application of the composite protective coating prepared in the above comparative example in the preparation of bamboo products includes the following steps: (1) Select bamboo samples from the same batch, sand the surface and clean with ethanol; (2) The composite protective coating is sprayed onto the surface of bamboo and the thickness of the dry film is controlled to be 100±10μm. It is cured at room temperature for 24h to form a composite protective coating on the surface of bamboo, and a sample of anti-mildew and flame-retardant water-based polyurethane bamboo protective coating is obtained.
[0075] In this comparative example, the prepared composite protective coating can also be used to prepare wood products.
[0076] Comparative Example 2 A composite protective coating is prepared using raw materials including a reactive phosphorus-containing waterborne polyurethane emulsion, a dynamic hydrogel network, and tannic acid-modified expandable graphite, wherein the mass ratio of the reactive phosphorus-containing waterborne polyurethane emulsion, the dynamic hydrogel network, and the tannic acid-modified expandable graphite is 10:0.33:0.13. This allows for the preparation of the composite protective coating under medium to low mixing ratio conditions.
[0077] In this comparative example, the reactive phosphorus-containing waterborne polyurethane emulsion used was prepared from polypropylene glycol (PPG-2000), isophorone diisocyanate (IPDI), DOPO-containing diol, 2,2-dimethylolpropionic acid (DMPA), 1,4-butanediol (BDO), triethylamine (TEA), and dibutyltin dilaurate (DBTDL) as raw materials through prepolymerization, phosphorus-containing chain extension, hydrophilic chain extension, neutralization, and water dispersion. The specific preparation process is as follows: Weigh 30.00 g of PPG-2000 and dehydrate it under vacuum for 2 h at 105 °C and 1000 r / min with stirring. After cooling to 75 °C, add 36.47 g of IPDI and 0.05 g of DBTDL, and react for 2 h. Add 4.86 g (15.00 mmol) of a DOPO-containing diol to make the molar ratio of the DOPO-containing diol to PPG-2000 1:1.00, and continue reacting for 2 h. Then add 4.00 g of DMPA and 2.00 g of BDO for chain extension. The amount of IPDI used is calculated based on a ratio of 2.0:1 between the total number of NCO groups in IPDI and the total number of OH groups in PPG-2000, the DOPO-containing diol, DMPA, and BDO. After the reaction was completed, the temperature was lowered to 40-50℃, 3.02g of TEA was added for neutralization, and deionized water was slowly added while stirring at 1000r / min. The reactive phosphorus-containing waterborne polyurethane emulsion was obtained by phase inversion.
[0078] In this comparative example, the dynamic hydrogel network used was prepared from polyvinyl alcohol (PVA), tannic acid, phytic acid, cellulose nanofibers, and hydroxypropyltrimethylammonium chloride chitosan. The specific preparation process is as follows: 10.00 g of PVA was weighed and added to 90.00 g of deionized water, and dissolved under stirring at 90 °C and 1000 r / min. After cooling to room temperature, cellulose nanofiber dispersion was added, and dispersed at 1000 r / min for 30 min. Using 1.00 mmol each of tannic acid and phytic acid as a basis, 1.00 mmol of tannic acid, 1.00 mmol of phytic acid, and 1.05 mmol of hydroxypropyltrimethylammonium chloride chitosan (calculated based on the amount of quaternary ammonium compounds) were added to achieve a molar ratio of tannic acid, phytic acid, and hydroxypropyltrimethylammonium chloride chitosan of 1:1:1.05. Cellulose nanofibers were added in excess, with the dry basis amount calculated based on the solid content of the dispersion. After the system was thoroughly mixed, a dynamic hydrogel network was obtained.
[0079] In contrast to Example 2, the dynamic hydrogel network in Comparative Example 2 was not neutralized, maintaining the acidic state of the obtained dynamic hydrogel network, and was directly used for subsequent compounding.
[0080] In this comparative example, the tannic acid-modified expandable graphite used was prepared by modifying expandable graphite with tannic acid. The specific preparation process is as follows: Weigh 10.00g of expandable graphite and 1.20g of tannic acid to make the mass ratio of expandable graphite to tannic acid 10:1.20; dissolve tannic acid in 100mL of deionized water and add expandable graphite, sonicate for 30min, then stir at 1000r / min for 2h, filter and dry to obtain tannic acid modified expandable graphite.
[0081] In this comparative example, the raw materials for preparing the composite protective coating also include a defoamer, wherein the amount of defoamer is 0.5% of the total mass of the composite protective coating, and the defoamer is a polyether-modified organosilicon solution (ZH-7011).
[0082] A method for preparing the composite protective coating in the above comparative example includes the following steps: Using 10.00 parts by weight of reactive phosphorus-containing waterborne polyurethane emulsion, 0.33 parts by weight of the aforementioned dynamic hydrogel network and 0.13 parts by weight of the aforementioned tannic acid-modified expandable graphite were added, making the mass ratio of the three components 10:0.33:0.13. First, the dynamic hydrogel network was slowly added to the waterborne polyurethane emulsion at 1000 r / min and mixed for 10 min. Then, the tannic acid-modified expandable graphite and 0.5% by weight of ZH-7011 polyether-modified silicone defoamer (based on the total mass of the composite protective coating) were added, dispersed at 1000 r / min for 20 min, and then defoamed to obtain the composite protective coating.
[0083] The application of the composite protective coating prepared in the above comparative example in the preparation of bamboo products includes the following steps: (1) Select bamboo samples from the same batch, sand the surface and clean with ethanol; (2) The composite protective coating is sprayed onto the surface of bamboo and the thickness of the dry film is controlled to be 100±10μm. It is cured at room temperature for 24h to form a composite protective coating on the surface of bamboo, and a sample of anti-mildew and flame-retardant water-based polyurethane bamboo protective coating is obtained.
[0084] In this comparative example, the prepared composite protective coating can also be used to prepare wood products.
[0085] Comparative Example 3 A composite protective coating is prepared using raw materials including a reactive phosphorus-containing waterborne polyurethane emulsion, a dynamic hydrogel network, and expandable graphite, wherein the mass ratio of the reactive phosphorus-containing waterborne polyurethane emulsion, the dynamic hydrogel network, and the expandable graphite is 10:0.33:0.13. This allows for the preparation of the composite protective coating under medium to low mixing ratio conditions.
[0086] In this comparative example, the reactive phosphorus-containing waterborne polyurethane emulsion used was prepared from polypropylene glycol (PPG-2000), isophorone diisocyanate (IPDI), DOPO-containing diol, 2,2-dimethylolpropionic acid (DMPA), 1,4-butanediol (BDO), triethylamine (TEA), and dibutyltin dilaurate (DBTDL) as raw materials through prepolymerization, phosphorus-containing chain extension, hydrophilic chain extension, neutralization, and water dispersion. The specific preparation process is as follows: Weigh 30.00 g of PPG-2000 and dehydrate it under vacuum for 2 h at 105 °C and 1000 r / min with stirring. After cooling to 75 °C, add 36.47 g of IPDI and 0.05 g of DBTDL, and react for 2 h. Add 4.86 g (15.00 mmol) of a DOPO-containing diol to make the molar ratio of the DOPO-containing diol to PPG-2000 1:1.00, and continue reacting for 2 h. Then add 4.00 g of DMPA and 2.00 g of BDO for chain extension. The amount of IPDI used is calculated based on a ratio of 2.0:1 between the total number of NCO groups in IPDI and the total number of OH groups in PPG-2000, the DOPO-containing diol, DMPA, and BDO. After the reaction was completed, the temperature was lowered to 40-50℃, 3.02g of TEA was added for neutralization, and deionized water was slowly added while stirring at 1000r / min. The reactive phosphorus-containing waterborne polyurethane emulsion was obtained by phase inversion.
[0087] In this comparative example, the dynamic hydrogel network used was prepared from polyvinyl alcohol (PVA), tannic acid, phytic acid, cellulose nanofibers, and hydroxypropyltrimethylammonium chloride chitosan. The specific preparation process is as follows: 10.00 g of PVA was weighed and added to 90.00 g of deionized water, and dissolved under stirring at 90 °C and 1000 r / min. After cooling to room temperature, cellulose nanofiber dispersion was added, and dispersed at 1000 r / min for 30 min. Using 1.00 mmol each of tannic acid and phytic acid as a basis, 1.00 mmol of tannic acid, 1.00 mmol of phytic acid, and 1.05 mmol of hydroxypropyltrimethylammonium chloride chitosan (calculated based on the amount of quaternary ammonium compounds) were added to achieve a molar ratio of tannic acid, phytic acid, and hydroxypropyltrimethylammonium chloride chitosan of 1:1:1.05. Cellulose nanofibers were added in excess, with the dry basis amount calculated based on the solid content of the dispersion. After the system was thoroughly mixed, a dynamic hydrogel network was obtained.
[0088] In this comparative example, the dynamic hydrogel network used was further treated before being mixed with the reactive phosphorus-containing waterborne polyurethane emulsion: triethylamine (TEA) was added dropwise to the dynamic hydrogel network, and the pH value of the dynamic hydrogel network was adjusted to 6.8-7.2 using triethylamine (TEA).
[0089] In this comparative example, expandable graphite was used instead of the tannic acid-modified expandable graphite prepared in Example 2.
[0090] In this comparative example, the raw materials for preparing the composite protective coating also include a defoamer, wherein the amount of defoamer is 0.5% of the total mass of the composite protective coating, and the defoamer is a polyether-modified organosilicon solution (ZH-7011).
[0091] A method for preparing the composite protective coating in the above comparative example includes the following steps: Using 10.00 parts by weight of reactive phosphorus-containing waterborne polyurethane emulsion, 0.33 parts by weight of the aforementioned dynamic hydrogel network and 0.13 parts by weight of the aforementioned expandable graphite were added, making the mass ratio of the three components 10:0.33:0.13. First, the dynamic hydrogel network was slowly added to the waterborne polyurethane emulsion at 1000 r / min and mixed for 10 min. Then, expandable graphite and 0.5% by weight of ZH-7011 polyether-modified silicone defoamer (based on the total mass of the composite protective coating) were added, and the mixture was dispersed at 1000 r / min for 20 min, followed by degassing to obtain the composite protective coating.
[0092] The application of the composite protective coating prepared in the above comparative example in the preparation of bamboo products includes the following steps: (1) Select bamboo samples from the same batch, sand the surface and clean with ethanol; (2) The composite protective coating is sprayed onto the surface of bamboo and the thickness of the dry film is controlled to be 100±10μm. It is cured at room temperature for 24h to form a composite protective coating on the surface of bamboo, and a sample of anti-mildew and flame-retardant water-based polyurethane bamboo protective coating is obtained.
[0093] In this comparative example, the prepared composite protective coating can also be used to prepare wood products.
[0094] Comparative Example 4 A composite protective coating is prepared using raw materials including a reactive phosphorus-containing waterborne polyurethane emulsion, a dynamic hydrogel network, and tannic acid-modified expandable graphite, wherein the mass ratio of the reactive phosphorus-containing waterborne polyurethane emulsion, the dynamic hydrogel network, and the tannic acid-modified expandable graphite is 10:0.60:0.30. This indicates that the amounts of hydrogel and tannic acid-modified expandable graphite added are excessive.
[0095] In this comparative example, the reactive phosphorus-containing waterborne polyurethane emulsion used was prepared from polypropylene glycol (PPG-2000), isophorone diisocyanate (IPDI), DOPO-containing diol, 2,2-dimethylolpropionic acid (DMPA), 1,4-butanediol (BDO), triethylamine (TEA), and dibutyltin dilaurate (DBTDL) as raw materials through prepolymerization, phosphorus-containing chain extension, hydrophilic chain extension, neutralization, and water dispersion. The specific preparation process is as follows: Weigh 30.00 g of PPG-2000 and dehydrate it under vacuum for 2 h at 105 °C and 1000 r / min with stirring. After cooling to 75 °C, add 36.47 g of IPDI and 0.05 g of DBTDL, and react for 2 h. Add 4.86 g (15.00 mmol) of a DOPO-containing diol to make the molar ratio of the DOPO-containing diol to PPG-2000 1:1.00, and continue reacting for 2 h. Then add 4.00 g of DMPA and 2.00 g of BDO for chain extension. The amount of IPDI used is calculated based on a ratio of 2.0:1 between the total number of NCO groups in IPDI and the total number of OH groups in PPG-2000, the DOPO-containing diol, DMPA, and BDO. After the reaction was completed, the temperature was lowered to 40-50℃, 3.02g of TEA was added for neutralization, and deionized water was slowly added while stirring at 1000r / min. The reactive phosphorus-containing waterborne polyurethane emulsion was obtained by phase inversion.
[0096] In this comparative example, the dynamic hydrogel network used was prepared from polyvinyl alcohol (PVA), tannic acid, phytic acid, cellulose nanofibers, and hydroxypropyltrimethylammonium chloride chitosan. The specific preparation process is as follows: 10.00 g of PVA was weighed and added to 90.00 g of deionized water, and dissolved under stirring at 90 °C and 1000 r / min. After cooling to room temperature, cellulose nanofiber dispersion was added, and dispersed at 1000 r / min for 30 min. Using 1.00 mmol each of tannic acid and phytic acid as a basis, 1.00 mmol of tannic acid, 1.00 mmol of phytic acid, and 1.05 mmol of hydroxypropyltrimethylammonium chloride chitosan (calculated based on the amount of quaternary ammonium compounds) were added to achieve a molar ratio of tannic acid, phytic acid, and hydroxypropyltrimethylammonium chloride chitosan of 1:1:1.05. Cellulose nanofibers were added in excess, with the dry basis amount calculated based on the solid content of the dispersion. After the system was thoroughly mixed, a dynamic hydrogel network was obtained.
[0097] In this comparative example, the dynamic hydrogel network used was further treated before being mixed with the reactive phosphorus-containing waterborne polyurethane emulsion: triethylamine (TEA) was added dropwise to the dynamic hydrogel network, and the pH value of the dynamic hydrogel network was adjusted to 6.8-7.2 using triethylamine (TEA).
[0098] In this comparative example, the tannic acid-modified expandable graphite used was prepared by modifying expandable graphite with tannic acid. The specific preparation process is as follows: Weigh 10.00g of expandable graphite and 1.20g of tannic acid to make the mass ratio of expandable graphite to tannic acid 10:1.20; dissolve tannic acid in 100mL of deionized water and add expandable graphite, sonicate for 30min, then stir at 1000r / min for 2h, filter and dry to obtain tannic acid modified expandable graphite.
[0099] In this comparative example, the raw materials for preparing the composite protective coating also include a defoamer, wherein the amount of defoamer is 0.5% of the total mass of the composite protective coating, and the defoamer is a polyether-modified organosilicon solution (ZH-7011).
[0100] A method for preparing the composite protective coating in the above comparative example includes the following steps: Using 10.00 parts by weight of reactive phosphorus-containing waterborne polyurethane emulsion, 0.60 parts by weight of the aforementioned dynamic hydrogel network and 0.30 parts by weight of the aforementioned tannic acid-modified expandable graphite were added, making the mass ratio of the three components 10:0.60:0.30. First, the dynamic hydrogel network was slowly added to the waterborne polyurethane emulsion at 1000 r / min and mixed for 10 min. Then, the tannic acid-modified expandable graphite and 0.5% by weight of ZH-7011 polyether-modified silicone defoamer (based on the total mass of the composite protective coating) were added, and the mixture was dispersed at 1000 r / min for 20 min, followed by degassing to obtain the composite protective coating.
[0101] The application of the composite protective coating prepared in the above comparative example in the preparation of bamboo products includes the following steps: (1) Select bamboo samples from the same batch, sand the surface and clean with ethanol; (2) The composite protective coating is sprayed onto the surface of bamboo and the thickness of the dry film is controlled to be 100±10μm. It is cured at room temperature for 24h to form a composite protective coating on the surface of bamboo, and a sample of anti-mildew and flame-retardant water-based polyurethane bamboo protective coating is obtained.
[0102] In this comparative example, the prepared composite protective coating can also be used to prepare wood products.
[0103] Comparative Example 5 A composite protective coating is prepared from raw materials including a reactive phosphorus-containing waterborne polyurethane emulsion, a dynamic hydrogel network, and tannic acid-modified expandable graphite, wherein the mass ratio of the reactive phosphorus-containing waterborne polyurethane emulsion, the dynamic hydrogel network, and the tannic acid-modified expandable graphite is 10:0.33:0.13.
[0104] In this comparative example, the reactive phosphorus-containing waterborne polyurethane emulsion used was prepared from polypropylene glycol (PPG-2000), isophorone diisocyanate (IPDI), DOPO-containing diol, 2,2-dimethylolpropionic acid (DMPA), 1,4-butanediol (BDO), triethylamine (TEA), and dibutyltin dilaurate (DBTDL) as raw materials through prepolymerization, phosphorus-containing chain extension, hydrophilic chain extension, neutralization, and water dispersion. The specific preparation process is as follows: Weigh 30.00 g of PPG-2000 and dehydrate it under vacuum for 2 h at 105 °C and 1000 r / min with stirring. After cooling to 75 °C, add 36.47 g of IPDI and 0.05 g of DBTDL, and react for 2 h. Add 4.86 g (15.00 mmol) of a DOPO-containing diol to make the molar ratio of the DOPO-containing diol to PPG-2000 1:1.00, and continue reacting for 2 h. Then add 4.00 g of DMPA and 2.00 g of BDO for chain extension. The amount of IPDI used is calculated based on a ratio of 2.0:1 between the total number of NCO groups in IPDI and the total number of OH groups in PPG-2000, the DOPO-containing diol, DMPA, and BDO. After the reaction was completed, the temperature was lowered to 40-50℃, 3.02g of TEA was added for neutralization, and deionized water was slowly added while stirring at 1000r / min. The reactive phosphorus-containing waterborne polyurethane emulsion was obtained by phase inversion.
[0105] In this comparative example, the dynamic hydrogel network used was prepared from polyvinyl alcohol (PVA), tannic acid, phytic acid, and cellulose nanofibers. The specific preparation process is as follows: 10.00 g of PVA was weighed and added to 90.00 g of deionized water, and dissolved under stirring at 90 °C and 1000 rpm. After cooling to room temperature, cellulose nanofiber dispersion was added, and dispersed at 1000 rpm for 30 min. Using 1.00 mmol each of tannic acid and phytic acid as a basis, 1.00 mmol of tannic acid and 1.00 mmol of phytic acid were added, but hydroxypropyltrimethylammonium chloride chitosan was not added. Cellulose nanofibers were added in excess, and their dry basis dosage was calculated based on the solid content of the dispersion. After the system was thoroughly mixed, a dynamic hydrogel network was obtained.
[0106] In this comparative example, the dynamic hydrogel network used was further treated before being mixed with the reactive phosphorus-containing waterborne polyurethane emulsion: triethylamine (TEA) was added dropwise to the dynamic hydrogel network, and the pH value of the dynamic hydrogel network was adjusted to 6.8-7.2 using triethylamine (TEA).
[0107] In this comparative example, the tannic acid-modified expandable graphite used was prepared by modifying expandable graphite with tannic acid. The specific preparation process is as follows: Weigh 10.00g of expandable graphite and 1.20g of tannic acid to make the mass ratio of expandable graphite to tannic acid 10:1.20; dissolve tannic acid in 100mL of deionized water and add expandable graphite, sonicate for 30min, then stir at 1000r / min for 2h, filter and dry to obtain tannic acid modified expandable graphite.
[0108] In this comparative example, the raw materials for preparing the composite protective coating also include a defoamer, wherein the amount of defoamer is 0.5% of the total mass of the composite protective coating, and the defoamer is a polyether-modified organosilicon solution (ZH-7011).
[0109] A method for preparing the composite protective coating in the above comparative example includes the following steps: Using 10.00 parts by weight of reactive phosphorus-containing waterborne polyurethane emulsion, 0.33 parts by weight of the aforementioned dynamic hydrogel network and 0.13 parts by weight of the aforementioned tannic acid-modified expandable graphite were added, making the mass ratio of the three components 10:0.33:0.13. First, the dynamic hydrogel network was slowly added to the waterborne polyurethane emulsion at 1000 r / min and mixed for 10 min. Then, the tannic acid-modified expandable graphite and 0.5% by weight of ZH-7011 polyether-modified silicone defoamer (based on the total mass of the composite protective coating) were added, dispersed at 1000 r / min for 20 min, and then defoamed to obtain the composite protective coating.
[0110] The application of the composite protective coating prepared in the above comparative example in the preparation of bamboo products includes the following steps: (1) Select bamboo samples from the same batch, sand the surface and clean with ethanol; (2) The composite protective coating is sprayed onto the surface of bamboo and the thickness of the dry film is controlled to be 100±10μm. It is cured at room temperature for 24h to form a composite protective coating on the surface of bamboo, and a sample of anti-mildew and flame-retardant water-based polyurethane bamboo protective coating is obtained.
[0111] In this comparative example, the prepared composite protective coating can also be used to prepare wood products.
[0112] Experimental data and verification requirements 1. Feasibility of preparation and stability of phosphorus-containing waterborne polyurethane emulsion Table 1 lists the basic properties of the phosphorus-containing aqueous polyurethane emulsions prepared in the various embodiments and comparative examples of the present invention: emulsion stratification, particle size, mechanical stability, and storage stability. The particle sizes of Examples 1-4 ranged from 38.84 to 107.38 nm, and no stratification or precipitation was observed after the mechanical stability test. Existing storage records show that all emulsions were stored for more than 12 months. Comparative Example 1 exhibited stratification and precipitation due to an excessively high proportion of DOPO-structured diols. Comparative Examples 2-4 differed only in the compounding steps after emulsion preparation; the phosphorus-containing aqueous polyurethane emulsions used themselves showed no abnormalities.
[0113] Table 1. Basic properties of phosphorus-containing aqueous polyurethane emulsions prepared in various embodiments and comparative examples of the present invention.
[0114] As shown in Table 1, as the amount of DOPO-containing diol gradually decreased from Example 1 to Example 4, the emulsion particle size decreased from 107.38 nm to 38.84 nm, indicating that a higher proportion of aromatic phosphorus-containing chain-extended structures enhances inter-segment interactions and increases the dispersed particle size. Examples 1-4 all maintained mechanical stability and were stored for more than 12 months; Comparative Example 1 showed stratification and precipitation after further increasing the proportion of DOPO-containing diol, indicating that this proportion exceeded the emulsion's stable range. The phosphorus-containing waterborne polyurethane formulations of Comparative Examples 2-5 were the same as those of Example 2, with particle sizes concentrated in the range of 63.18-68.45 nm, indicating that the subsequent differences in these comparative examples mainly came from hydrogel neutralization, graphite modification, compounding ratios, or quaternary ammonium salt components, rather than the phosphorus-containing waterborne polyurethane emulsion itself.
[0115] 2. Stability and film-forming properties of composite protective coatings The zeta potential of the composite protective coating was determined at 25°C with the same dilution factor, the apparent viscosity was determined at 25°C with the same rotor and rotation speed, and the flexibility was determined according to GB / T 1731-2020. Three parallel samples were used for each test, and the results are expressed as mean ± standard deviation.
[0116] Table 2. Basic properties of the composite protective coatings prepared in the various embodiments and comparative examples of the present invention.
[0117] Note: n=3, expressed as "mean ± standard deviation"; items marked "-" are not applicable because uniform coating or continuous film was not obtained.
[0118] As shown in Table 2, the Zeta potential of Examples 1-4 changed from -31.8 mV to -40.6 mV, and the apparent viscosity increased from 420 mPa·s to 688 mPa·s. This is because the increased amount of dynamic hydrogel network and tannic acid-modified expandable graphite led to an increase in ionizable groups and solid network in the system, enhanced electrostatic repulsion between particles, and increased flow resistance of the continuous phase. Examples 2 and 3 formed a continuous and smooth coating with a flexibility of 1 mm, exhibiting good overall performance. Although Example 4 remained stable, the higher filler ratio resulted in a slightly rougher surface. Comparative Example 3, using unmodified expandable graphite, showed a decrease in the absolute value of the Zeta potential to 24.7 mV and the appearance of local agglomeration, indicating that tannic acid surface modification contributes to interfacial stability. In Comparative Example 5, the removal of the positively charged hydroxypropyltrimethylammonium chloride chitosan resulted in a more negative Zeta potential and a decrease in viscosity, reflecting the synchronous changes in charge composition and hydrogel network strength.
[0119] 3. Flame retardant and heat insulation properties Limiting oxygen index (LOI) was determined according to GB / T 2406.2-2009. Ignition time (TTI), peak heat release rate (pHRR), and total heat release (THR) were determined according to GB / T 16172-2007 under cone calorimetry conditions with the same external heat flux. Three parallel samples were set for each test, and the results are expressed as mean ± standard deviation.
[0120] Table 3. Fire resistance properties of the composite protective coatings obtained in various embodiments and comparative examples of the present invention.
[0121] Note: n=3, expressed as "mean ± standard deviation"; Comparative Examples 1, 2 and 4 are marked "-" because no qualified coating samples were obtained.
[0122] As shown in Table 3, from Example 1 to Example 4, the LOI increased from 28.6% to 34.1%, the TTI increased from 40.8s to 57.8s, and the pHRR increased from 182kW / m 2 Reduced to 112kW / m 2 THR is 35.8 MJ / m 2 Reduced to 24.1 MJ / m 2The reason for this is that the hydrogel absorbs heat upon evaporation, phytic acid and DOPO-containing structures participate in char formation, and expandable graphite forms a heat-insulating layer. As the proportion of hydrogel and modified expandable graphite increases, the multiple effects become more pronounced. Compared to Example 2, Comparative Example 3 showed a decrease in LOI and an increase in pHRR and THR, indicating that interfacial aggregation of unmodified expandable graphite weakens the continuity of the char layer. The fire resistance of Comparative Example 5 was slightly lower than that of Example 2, indicating that the nitrogen-containing structure in hydroxypropyltrimethylammonium chloride chitosan contributes to synergistic char formation, but the flame-retardant components are still phosphorus-containing polyurethane, hydrogel, and modified expandable graphite.
[0123] 4. Anti-mildew properties Anti-mildew performance was evaluated according to GB / T 1741-2020. Each group used the same combination of microbial strains, inoculation concentration, culture temperature, relative humidity, culture time, and grading method, with three parallel samples. Comparative Examples 1-5 are listed in Table 4; however, Comparative Examples 1, 2, and 4 were not assessed for anti-mildew resistance because no qualified coating samples were obtained.
[0124] Table 4. Antifungal properties of coatings with different hydroxypropyltrimethylammonium chloride-chitosan ratios
[0125] Table 4 shows that the mold resistance level of Examples 1 and 2 is Grade 1, while Examples 3 and 4 reach Grade 0 after increasing the proportion of hydroxypropyltrimethylammonium chloride chitosan, indicating that increasing the quaternary ammonium content can enhance the interference with mold cell membranes and adhesion growth. Although Comparative Example 3 uses unmodified expandable graphite, the anti-mold functional component is the same as that of Example 2, and it is still Grade 1, indicating that the surface modification of expandable graphite mainly affects dispersion and carbon layer structure, and is not the main controlling factor of anti-mold performance. Comparative Example 5, after removing hydroxypropyltrimethylammonium chloride chitosan, drops to Grade 4, further indicating that quaternary ammonium salt chitosan is the key component for achieving anti-mold effect in this system. Comparative Examples 1, 2, and 4 are marked with "-" because a qualified coating could not be obtained.
[0126] 5. Macrostructure, microstructure, and elemental distribution of the coating before and after combustion The macroscopic expansion structure was recorded by cross-sectional thickness measurement and residual char morphology. The pore size and pore wall continuity of the char layer were observed by scanning electron microscopy. The content and distribution of P and N elements before and after combustion were compared by XPS or SEM-EDS. The dry film thickness of each group before combustion was 100±10μm. Comparative Examples 1, 2, and 4 were not subjected to post-combustion structural testing because qualified coating samples were not obtained.
[0127] Table 5. Structural and elemental distribution of each embodiment and comparative example of the present invention before and after combustion.
[0128] Table 5 shows that the residual char thickness of Examples 1-4 increased from 2.6 mm to 4.8 mm, the expansion ratio increased from 26 times to 48 times, the average pore size decreased from 185 μm to 110 μm, and the pore walls gradually changed from local cracking to dense continuity. The phosphorus content increased synchronously after combustion, indicating that a higher proportion of hydrogel and modified expandable graphite is beneficial for constructing a thicker and more uniform phosphorus-containing expanded char layer. Comparative Example 3 had a residual char thickness of only 2.2 mm, an average pore size increased to 230 μm, and more cracks, indicating that insufficient interfacial compatibility of unmodified graphite would disrupt the continuity of the char layer. Comparative Example 5 had a slightly lower residual char thickness and expansion ratio than Example 2, and the lowest nitrogen content after combustion, indicating that hydroxypropyltrimethylammonium chloride chitosan, in addition to its anti-mildew properties, also participated in the construction of the nitrogen-containing char layer. Comparative Examples 1, 2, and 4 were not tested because no qualified coating samples were obtained.
[0129] As can be seen from the above results, compared with conventional physical additive heat-insulating and flame-retardant coatings, the composite protective coating of the present invention has good stability, good film-forming properties and flexibility, good flame retardancy, good heat insulation and mildew prevention. As a chemically reactive heat-insulating, flame-retardant and mildew-proof coating with excellent comprehensive performance, it can effectively protect the surface of wood and bamboo materials while taking into account daily mildew prevention and fire-retardant heat insulation. It has high use value and good application prospects.
[0130] The above embodiments are merely preferred embodiments of the present invention, and the scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, improvements and modifications made without departing from the principles of the present invention should also be considered within the scope of protection of the present invention.
Claims
1. A composite protective coating, characterized in that, The raw materials for preparing the composite protective coating include a reactive phosphorus-containing waterborne polyurethane emulsion, a dynamic hydrogel network, and tannic acid-modified expandable graphite; the mass ratio of the reactive phosphorus-containing waterborne polyurethane emulsion, the dynamic hydrogel network, and the tannic acid-modified expandable graphite is 10:0.30-0.40:0.10-0.
20. The reactive phosphorus-containing waterborne polyurethane emulsion is prepared by prepolymerization, phosphorus-containing chain extension, hydrophilic chain extension, neutralization and water dispersion of polypropylene glycol, isophorone diisocyanate, DOPO-containing diol, 2,2-dimethylolpropionic acid, 1,4-butanediol, triethylamine and dibutyltin dilaurate as raw materials. The dynamic hydrogel network is prepared from polyvinyl alcohol, tannic acid, phytic acid, cellulose nanofibers and hydroxypropyltrimethylammonium chloride chitosan as raw materials; before being mixed with the reactive phosphorus-containing waterborne polyurethane emulsion, the following treatment is also included: adjusting the pH value of the dynamic hydrogel network to 6.8-7.2 with triethylamine; The tannic acid-modified expandable graphite is prepared by modifying expandable graphite with tannic acid.
2. The composite protective coating according to claim 1, characterized in that, The molar ratio of the DOPO-structured diol to polypropylene glycol is 1:0.81 to 1.50; the molar ratio of the NCO groups in the isophorone diisocyanate to the OH groups in all hydroxyl-containing raw materials is 1.8 to 2.1:
1.
3. The composite protective coating according to claim 2, characterized in that, The number-average molecular weight of the polypropylene glycol is 2000 g / mol.
4. The composite protective coating according to claim 1, characterized in that, The molar ratio of tannic acid, phytic acid and the quaternary ammonium group contained in the hydroxypropyltrimethylammonium chloride chitosan is 1:1:1.00 to 1.
20.
5. The composite protective coating according to claim 1, characterized in that, The mass ratio of expandable graphite to tannic acid is 10:1.0 to 1.
8.
6. The composite protective coating according to any one of claims 1 to 5, characterized in that, The raw materials for preparing the composite protective coating also include a defoamer; the amount of the defoamer is 0.5% of the total mass of the composite protective coating.
7. The composite protective coating according to claim 6, characterized in that, The defoamer is a polyether-modified organosilicon solution.
8. A method for preparing a composite protective coating as described in claim 7, characterized in that, Includes the following steps: Under stirring conditions of 800 r / min to 1200 r / min, a dynamic hydrogel network was added to a reactive phosphorus-containing waterborne polyurethane emulsion and stirred for 5 min to 20 min. Tannic acid-modified expandable graphite and defoamer were then added and stirred for 10 min to 30 min to obtain a composite protective coating.
9. The application of a composite protective coating as described in any one of claims 1 to 7 or a composite protective coating prepared by the preparation method described in claim 8 in the preparation of wood products and bamboo products.
10. The application according to claim 9, characterized in that, The process includes the following steps: applying a composite protective coating to the surface of wood or bamboo, curing it to form a composite protective coating on the surface of the wood or bamboo; the curing time is 24 hours; and the thickness of the composite protective coating is 100±10μm.