A UV coating, its preparation method and application
By combining quaternary resins and using specific fillers, the problem of UV coatings being unable to simultaneously achieve good performance in terms of hardness, flexibility, fingerprint resistance, and damp heat resistance has been solved, resulting in a simultaneous improvement in multiple dimensions of performance.
Patent Information
- Application Number
- CN202611015345.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-09
- Publication Date
- 2026-11-17
Abstract
Description
Technical Field
[0001] This invention relates to the field of coating production technology, specifically to a UV coating, its preparation method, and its application. Background Technology
[0002] Ultraviolet (UV) curing coatings are environmentally friendly coatings that transform from a liquid to a solid coating within seconds through a photoinitiator-induced polymerization and cross-linking reaction of active monomers or oligomers under ultraviolet light. Compared to traditional thermosetting coatings, UV coatings offer significant advantages such as faster curing speed, energy efficiency, environmental friendliness, and superior film performance, making them widely used in wood coating, plastic decoration, metal protection, electronics, and optical devices.
[0003] In recent years, with the rapid iteration and upgrading of consumer electronics products, UV coatings have been increasingly widely used in the surface coating of 3C products such as smartphones, tablets, wearable devices, and laptop casings. In particular, the rise of foldable screen phones and the widespread adoption of 5G communication technology have placed extremely stringent and multi-dimensional demands on the performance of electronic device casing coatings. High-end electronic product coatings have evolved from a single protective function to a multi-functional composite carrier, requiring simultaneous capabilities of: 1. Fingerprint resistance (water contact angle >100°), enhancing the user's touch experience; 2. Excellent abrasion resistance (RCA test >500 cycles), resisting wear and tear from daily use; 3. Stability to damp heat (no change at 65℃ / 95%RH for 72 hours), meeting the reliability requirements for use under different climate conditions worldwide; 4. Excellent adhesion (5B cross-cut adhesion test) ensures a strong bond between the coating and the substrate (PC, ABS, aluminum-magnesium alloy, etc.).
[0004] However, there are significant mutual constraints among the above functions: for example, the fluorosilicone components introduced to reduce surface energy to achieve fingerprint resistance often have poor compatibility with the host resin, resulting in a decrease in the mechanical properties of the coating; the multifunctional monomers added to improve hardness will exacerbate curing shrinkage stress and reduce adhesion and bending performance.
[0005] Chinese patent CN116285653B discloses a UV coating for automotive interior parts and its preparation method. It uses a combination of hexafunctional aliphatic polyurethane acrylic resin and difunctional polyurethane acrylic resin to achieve a balance between high hardness and good flexibility. However, the solution does not involve anti-fingerprint function and nanofiller synergistic toughening technology, and its resistance to damp heat is also not disclosed. Summary of the Invention
[0006] The first technical problem to be solved by the present invention is to provide a UV coating that combines hardness and flexibility, anti-fingerprint function and good resistance to damp heat, in order to address the shortcomings of the existing technology.
[0007] To solve the first technical problem mentioned above, the technical solution of the present invention is: A UV coating, by weight, comprises the following components: 25-35 parts of fluorocarbon-modified polyurethane acrylate oligomer. 10-15 parts of hexafunctional aliphatic polyurethane acrylate 20-30 parts of tetrafunctional hydroxyl polyurethane acrylate 25-35 parts of tetrahydrofuran acrylate 3-5 parts of trimethylolpropane triacrylate 5-8 parts of core-shell structured elastic nanoparticles 5-8 parts of silane coupling agent-modified hydrophobic nano-attapulgites 3-5 parts of free radical photoinitiator 1.5-2.5 parts of polymeric dispersant. Fluorine-modified acrylate leveling agent, 0.2-0.5 parts. Polymer-type defoamer 0.2-0.4 parts.
[0008] Preferably, the core-shell structured elastic nanoparticles are polybutadiene core / polymethyl methacrylate shell structures with a particle size of 80-120 nm and a core glass transition temperature below -40°C.
[0009] Preferably, the silane coupling agent-modified hydrophobic nano-attapulgites are prepared by the following method: (1) Vacuum dry the attapulgite at 100-130℃ for 3-5 hours; (2) Dissolve KH-570 silane coupling agent in a mixed solvent of ethanol / water volume ratio of 95:5, adjust the pH to 4-5 with acetic acid, and hydrolyze for 20-40 min; (3) Disperse the dried attapulgite in the hydrolysate obtained in step (2) with a solid-liquid ratio of 1:8-1:12 and reflux at 70-90℃ for 4-6 hours; (4) Separate, wash, dry and grind to obtain hydrophobic nano-attapulgs, wherein the water contact angle of the hydrophobic nano-attapulgs is greater than 120°.
[0010] Preferably, the free radical photoinitiator is a compound system of acylphosphine oxide initiator and α-hydroxy ketone initiator, wherein the mass ratio of acylphosphine oxide initiator to α-hydroxy ketone initiator is 1:0.8-1:1.2; the acylphosphine oxide initiator is selected from at least one of TPO, TEPO or BAPO, and the α-hydroxy ketone initiator is 184.
[0011] Preferably, the polymeric dispersant is an anchoring polyurethane dispersant, preferably BYK-163; The fluorinated modified acrylate leveling agent is selected from at least one of Rieter LD-91084 or BYK-349; The polymeric defoamer is selected from at least one of BYK-1795 or BYK-A530.
[0012] The second technical problem to be solved by the present invention is to provide a method for preparing a UV coating that addresses the shortcomings of the existing technology. The UV coating obtained has both hardness and flexibility, as well as good anti-fingerprint function and resistance to damp heat.
[0013] To solve the second technical problem mentioned above, the technical solution of the present invention is: A method for preparing a UV coating includes the following steps: S1: Preparation of filler predispersion liquid A polymeric dispersant was dissolved in tetrahydrofuran acrylate, which accounted for 40-50% of the total weight of tetrahydrofuran acrylate. Core-shell structured elastic nanoparticles and hydrophobic nano-attapulgites modified with silane coupling agent were added. After high-speed pre-dispersion, the mixture was ground to a fineness of ≤5μm by a sand mill to obtain a filler pre-dispersion liquid. S2: Resin premix Fluorocarbon modified polyurethane acrylate oligomer, hexafunctional aliphatic polyurethane acrylate, tetrafunctional hydroxyl polyurethane acrylate and the remaining tetrahydrofuran acrylate are mixed and stirred at 50-60℃ until completely transparent and homogeneous to obtain a resin mixture. S3: Packing material inlet Add the pre-dispersed filler solution obtained in step S1 to the resin mixture obtained in step S2, and stir to mix evenly; S4: Add crosslinking monomers and initiators Cool the system to below 40°C, add trimethylolpropane triacrylate and free radical photoinitiator under light-protected conditions, and stir at low speed until completely dissolved; S5: Adding additives Add fluorinated modified acrylate leveling agent and polymeric defoamer, and continue stirring to mix evenly; S6: Filtration and Packaging The mixture obtained in step S5 is filtered through a 1μm filter and sealed in a light-proof package to obtain the UV coating.
[0014] Preferably, in step S1, the grinding process using the sand mill employs zirconia beads with a particle size of 0.3-0.5 mm.
[0015] Preferably, the stirring time in step S3 is 15-30 min; the stirring time in step S4 is 10-20 min; and the stirring time in step S5 is 5-15 min.
[0016] Preferably, the application and curing process of the UV coating is as follows: The UV coating is applied to the surface of the substrate, and after leveling, it is UV cured under inert gas protection.
[0017] Specifically, the UV coating is applied to the surface of the substrate, the wet film thickness is controlled to be 18-22μm, and after leveling at 50-60℃ for 3-5 minutes, UV curing is performed using a high-pressure mercury lamp under nitrogen protection (oxygen content <500ppm), with a lamp power of 80-120W / cm and a cumulative exposure energy of 800-1200mJ / cm².
[0018] The third technical problem to be solved by the present invention is to provide an application of UV coating in the surface coating of electronic device housings, foldable screen mobile phones or 5G devices, in view of the shortcomings of the existing technology.
[0019] Due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. This invention innovatively employs a quaternary gradient resin compound system constructed from fluorocarbon-modified polyurethane acrylate oligomers, hexafunctional aliphatic polyurethane acrylates, tetrafunctional hydroxyl polyurethane acrylates, and tetrahydrofuran acrylate flexible monomers, breaking the limitations of traditional single or binary resin systems with limited functionality. The hexafunctional resin provides high crosslinking density, ensuring a base hardness ≥6H and excellent wear resistance of the coating. The tetrafunctional hydroxyl polyurethane acrylates and tetrahydrofuran acrylate flexible monomers synergistically release curing internal stress through the compliant movement of molecular chains, significantly reducing the coating's curing shrinkage rate and effectively alleviating common industry problems such as large curing shrinkage and poor adhesion in high-functionality resin systems. Simultaneously, the fluorocarbon-modified resin endows the coating with low surface energy characteristics at the molecular level, laying the foundation for anti-fingerprint functionality. The three components synergistically achieve initial compatibility of high hardness, high flexibility, and hydrophobicity.
[0020] 2. This invention synergistically applies core-shell structured elastic nanoparticles with hydrophobically modified attapulgites using silane coupling agents to a UV coating system. The core-shell elastic particles utilize their polybutadiene soft core (Tg < -40℃) / polymethyl methacrylate hard shell core-shell structure to absorb impact energy through a physical toughening mechanism of "stress concentration-cavitation-shear yielding," enabling the coating to withstand over 300,000 folds at a bending radius R = 2mm. The hydrophobically modified attapulgites (water contact angle > 120°) form a labyrinthine physical barrier layer in the coating with their nanorod-like structure, extending the water molecule penetration path. This ensures the coating remains free of whitening and blistering, and maintains a 5B adhesion rating for 72 hours in a humid environment of 65℃ / 95%RH. Furthermore, they construct a micro-rough hydrophobic structure on the coating surface, synergistically enhancing anti-fingerprint performance with fluorocarbon resin. The two fillers are complementary in function and synergistic in performance. When used in combination, their toughening and moisture-heat resistance enhancement effects are superior to those of adding a single filler alone. In this system, through hydrogen bonding-assisted compatibility and core-shell particle toughening, the amount of fluorocarbon resin added can be increased to 25-35 parts while maintaining an adhesion of 5B, exhibiting a better mechanical retention rate compared to conventional fluorosilicone additive systems. The core-shell elastic particles, relying on the polybutadiene soft core / PMMA hard shell structure, absorb external impact through stress concentration, cavitation, and shear yielding mechanisms, improving the coating's resistance to bending fatigue. The hydrophobic modified attapulgite, relying on its one-dimensional rod-like structure, forms a physical barrier channel for water vapor within the coating, extending the water penetration path and simultaneously constructing a micro-rough hydrophobic structure on the paint film surface, further enhancing the anti-fingerprint effect. The two types of fillers optimize coating performance from the two dimensions of mechanical toughening and moisture-heat resistance hydrophobicity, respectively, and their combined use creates a synergistic effect of complementary performance.
[0021] 3. This invention employs a compound system of acylphosphine oxide initiators and α-hydroxy ketone initiators, combined with a nitrogen-based low-oxygen curing process (oxygen content <500ppm), to achieve simultaneous and thorough curing of the coating surface and deep layers, avoiding over-curing of the surface layer and under-curing of the deep layer. Acylphosphine oxide initiators possess excellent long-wave absorption characteristics, ensuring sufficient cross-linking of the deep layers of the coating; α-hydroxy ketone initiators possess excellent short-wave absorption characteristics, ensuring sufficient curing of the coating surface. The synergistic effect of both initiators avoids the dual defects of over-curing (brittleness, high shrinkage stress) on the surface and under-curing (insufficient hardness, poor adhesion) on the deep layer caused by a single initiator. Combined with nitrogen protection, it effectively inhibits oxygen inhibition on the surface, ensuring a stable surface hardness of 6H, making it more suitable for the curing and processing requirements of this multi-resin, high-filler compound system, and ensuring stable performance of all properties.
[0022] 4. This invention employs a segmented preparation process of "filler pre-dispersion - resin pre-mixing - low-temperature addition of functional components," which can significantly alleviate common industry problems such as poor compatibility between inorganic nanofillers and organic resins, and easy agglomeration during processing. First, core-shell elastic nanoparticles and hydrophobically modified attapulgite are milled to a fineness ≤5μm in tetrahydrofuran acrylate monomer with a polymeric dispersant, allowing the filler to be stably dispersed in a primary particle state, reducing agglomeration. In the subsequent resin mixing and functional component addition stages, the temperature is controlled, with photoinitiators added below 40℃ in the dark to avoid premature decomposition of the initiator, thermal degradation of fluorocarbon segments, and failure of various functional additives caused by high temperatures. This maximizes the preservation of the original properties of each component and fully leverages the synergistic effect of the multi-component combination. Although stepwise pre-dispersion is a conventional processing method for nano-coatings, when adapted to the filler and resin system of this formulation, it can significantly improve key indicators such as film transmittance and storage stability.
[0023] 5. This invention addresses the industry challenge of simultaneously achieving high hardness and flexibility, hydrophobicity and fingerprint resistance, and resistance to damp heat in existing UV coatings. Through synergistic design of the formulation system, it significantly improves three common technical pain points in the industry: Firstly, addressing the common problems of high crosslinking density, large curing shrinkage, and brittle coatings associated with high-functionality resins, this invention combines tetrahydrofuran acrylate flexible monomers with tetrafunctional hydroxyl polyurethane acrylates to synergistically release curing internal stress. With an addition of 10-15 parts of hexafunctional aliphatic polyurethane acrylate, the measured shrinkage rate of this system can be as low as 3.8% to 4.5%, far lower than conventional high-functionality systems. At the same time, the coating's flexural strength is improved to over 300,000 cycles (with the appearance of visible cracks as the termination condition). Although existing technologies can improve brittleness through flexible monomers, it is difficult to achieve both low shrinkage and ultra-high flexural strength simultaneously with a high amount of hexafunctional resin. The quaternary resin compound system of this invention can further amplify this balancing effect.
[0024] Secondly, addressing the issues of poor compatibility between unmodified nano-inorganic fillers and organic resins, and the tendency for high addition amounts to agglomerate and degrade film performance, this invention employs KH-570 silane coupling agent to hydrophobically modify attapulgite, coupled with a three-stage filler pre-dispersion and milling process. This allows for the stable addition of modified attapulgite to 5-8 parts. The modified filler and dispersion process together reduce the risk of filler agglomeration, improving the coating's barrier and moisture resistance while simultaneously maintaining a hardness of 6H or higher and excellent flexural strength. Although silane-modified inorganic fillers and pre-dispersion milling are common methods for improving filler compatibility, when adapted to this quaternary fluorocarbon polyurethane resin system, both effectively increase the upper limit of filler addition and simultaneously improve overall film performance.
[0025] Thirdly, addressing the issues of low surface energy in fluorocarbon modified resins, which easily lead to phase separation and limited addition amounts with polyurethane acrylate systems, this invention constructs a gradient compatibility structure of fluorocarbon segments, polyurethane segments, and hydroxyl polar groups. The tetrafunctional hydroxyl groups of the polyurethane acrylate molecular chain can form intermolecular hydrogen bonds with the urethane groups of the fluorocarbon modified polyurethane acrylate, creating a molecularly compatible auxiliary bridge to alleviate the macroscopic phase separation phenomenon between the fluorocarbon component and the resin matrix. This allows for a stable increase in the addition amount of fluorocarbon modified polyurethane acrylate to 25-35 parts. Although existing technologies have utilized hydrogen bonds to improve the compatibility of fluorocarbon resins, few solutions can simultaneously achieve high hydrophobicity and anti-fingerprint effects while maintaining complete mechanical properties within this addition range.
[0026] 6. The core technical advantage of this invention lies in its approach: instead of simply stacking various functional components, it matches the effective ranges and compatibility relationships of each raw material to build a multi-level synergistic system covering the molecular, microscopic, and macroscopic levels. At the molecular level, fluorocarbon segments tend to accumulate on the coating surface during curing, forming a low-surface-energy hydrophobic surface layer. At the microscopic level, core-shell elastic particles absorb impact energy, and modified attapulgite blocks water vapor erosion, respectively enhancing the coating's toughness and resistance to damp heat. At the macroscopic level, the quaternary gradient compound resin forms a low-shrinkage, highly cross-linked, and uniformly cross-linked network. The three-level structure works together to achieve simultaneous improvement in multiple dimensions of performance with just a single coating layer. Traditional single-layer UV coatings often struggle to balance high hardness, high flexural strength, long-lasting anti-fingerprint properties, and excellent resistance to damp heat, typically requiring multi-layer coatings to achieve each function. This formulation system simplifies the coating process while significantly increasing the overall performance limit of a single-layer paint film. Detailed Implementation
[0027] The present invention will be further illustrated below with reference to the embodiments. Example
[0028] A UV coating, by weight, comprises the following components: 25 parts of fluorocarbon-modified polyurethane acrylate oligomer (Guangzhou Songda New Material Technology Co., Ltd. SD1338B), 10 parts of hexafunctional aliphatic polyurethane acrylate (Guangdong Boxin New Material B-615), 20 parts of tetrafunctional hydroxyl polyurethane acrylate (Guangdong Boxin New Material B-6263), 25 parts of tetrahydrofuran acrylate (Guangzhou Yashide New Material THFA), 3 parts of trimethylolpropane triacrylate (AgiSyn™ 2811), and 5 parts of core-shell structured elastic nanoparticles (ArkemaDurastrength®). (400 series), the core-shell structured elastic nanoparticles are polybutadiene core / polymethyl methacrylate shell structures with a particle size of 80-120 nm and a core glass transition temperature below -40℃. The composition includes 5 parts of silane coupling agent-modified hydrophobic nano-attapulgites, 3 parts of free radical photoinitiator (the free radical photoinitiator is a compound system of acylphosphine oxide initiator and α-hydroxy ketone initiator, wherein the mass ratio of acylphosphine oxide initiator to α-hydroxy ketone initiator is 1:0.8; the acylphosphine oxide initiator is TPO, and the α-hydroxy ketone initiator is 184), 1.5 parts of polymeric dispersant (the polymeric dispersant is an anchoring polyurethane dispersant, specifically BYK-163), 0.2 parts of fluorinated acrylate leveling agent (fluorinated acrylate leveling agent is Lida LD-91084), and 0.2 parts of polymeric defoamer (polymeric defoamer is BYK-1795).
[0029] The silane coupling agent-modified hydrophobic nano-attapulgites were prepared by the following method: (1) Dry the attapulgite under vacuum at 100℃ for 3 hours; (2) Dissolve KH-570 silane coupling agent in a mixed solvent of ethanol / water volume ratio of 95:5, adjust the pH to 4 with acetic acid, and hydrolyze for 20 min; (3) Disperse the dried attapulgite in the hydrolysate obtained in step (2) with a solid-liquid ratio of 1:8, and reflux at 70°C for 4 hours; (4) Separate, wash, dry and grind to obtain hydrophobic nano-attapulgites with a water contact angle greater than 120°. Example
[0030] A UV coating, by weight, comprises the following components: 30 parts of fluorocarbon-modified polyurethane acrylate oligomer (Guangzhou Songda New Material Technology Co., Ltd. SD1338B), 12 parts of hexafunctional aliphatic polyurethane acrylate (Guangdong Boxin New Material B-615), 25 parts of tetrafunctional hydroxyl polyurethane acrylate (Guangdong Boxin New Material B-6263), 30 parts of tetrahydrofuran acrylate (Guangzhou Yashide New Material THFA), 4 parts of trimethylolpropane triacrylate (AgiSyn™ 2811), and 6 parts of core-shell structured elastic nanoparticles (Kaneka, Japan). (MX series), the core-shell structured elastic nanoparticles are polybutadiene core / polymethyl methacrylate shell structures with a particle size of 80-120 nm and a core glass transition temperature below -40℃. The composition includes 7 parts of silane coupling agent-modified hydrophobic nano-attapulgites, 4 parts of free radical photoinitiator (the free radical photoinitiator is a compound system of acylphosphine oxide initiator and α-hydroxy ketone initiator, wherein the mass ratio of acylphosphine oxide initiator to α-hydroxy ketone initiator is 1:1; the acylphosphine oxide initiator is TEPO, and the α-hydroxy ketone initiator is 184), 2 parts of polymeric dispersant (the polymeric dispersant is an anchoring polyurethane dispersant, specifically BYK-163), 0.35 parts of fluorinated acrylate leveling agent (fluorinated acrylate leveling agent is BYK-349), and 0.3 parts of polymeric defoamer (polymeric defoamer is BYK-A530).
[0031] The silane coupling agent-modified hydrophobic nano-attapulgites were prepared by the following method: (1) Dry the attapulgite under vacuum at 120°C for 4 hours; (2) Dissolve KH-570 silane coupling agent in a mixed solvent of ethanol / water volume ratio of 95:5, adjust the pH to 5 with acetic acid, and hydrolyze for 30 min; (3) Disperse the dried attapulgite in the hydrolysate obtained in step (2) with a solid-liquid ratio of 1:10 and reflux at 80°C for 5 hours; (4) Separate, wash, dry and grind to obtain hydrophobic nano-attapulgites with a water contact angle greater than 120°. Example
[0032] A UV coating, by weight, comprises the following components: 35 parts of fluorocarbon-modified polyurethane acrylate oligomer (Guangzhou Songda New Material Technology Co., Ltd. SD1338B), 15 parts of hexafunctional aliphatic polyurethane acrylate (Guangdong Boxin New Material B-615), 30 parts of tetrafunctional hydroxyl polyurethane acrylate (Guangdong Boxin New Material B-6263), 35 parts of tetrahydrofuran acrylate (Guangzhou Yashide New Material THFA), 5 parts of trimethylolpropane triacrylate (AgiSyn™ 2811), and 8 parts of core-shell structured elastic nanoparticles (ArkemaDurastrength®). (400 series), the core-shell structured elastic nanoparticles are polybutadiene core / polymethyl methacrylate shell structures with a particle size of 80-120 nm and a core glass transition temperature below -40℃. It also includes 8 parts of silane coupling agent-modified hydrophobic nano-attapulgites and 5 parts of free radical photoinitiator (the free radical photoinitiator is a compound system of acylphosphine oxide initiator and α-hydroxy ketone initiator, wherein the mass ratio of acylphosphine oxide initiator to α-hydroxy ketone initiator is 1:1.2; the acylphosphine oxide initiator is TPO and BAPO mixed according to...). The mixture is prepared by mixing the following components in a 1:1 mass ratio: α-hydroxy ketone initiator (184), 2.5 parts of polymeric dispersant (the polymeric dispersant is an anchoring polyurethane dispersant, specifically BYK-163), 0.5 parts of fluorinated acrylate leveling agent (fluorinated acrylate leveling agent is obtained by mixing Rieter LD-91084 and BYK-349 in a 2:1 mass ratio), and 0.4 parts of polymeric defoamer (polymeric defoamer is obtained by mixing BYK-1795 or BYK-A530 in a 1:1 mass ratio).
[0033] The silane coupling agent-modified hydrophobic nano-attapulgites were prepared by the following method: (1) Dry the attapulgite under vacuum at 130℃ for 5 hours; (2) Dissolve KH-570 silane coupling agent in a mixed solvent of ethanol / water volume ratio of 95:5, adjust the pH to 5 with acetic acid, and hydrolyze for 40 min; (3) Disperse the dried attapulgite in the hydrolysate obtained in step (2) with a solid-liquid ratio of 1:12 and reflux at 90°C for 6 hours; (4) Separate, wash, dry and grind to obtain hydrophobic nano-attapulgites with a water contact angle greater than 120°. Example
[0034] The preparation method of the UV coatings in Examples 1-3 includes the following steps: S1: Preparation of filler predispersion liquid A polymeric dispersant was dissolved in tetrahydrofuran acrylate at 45% of the total weight of tetrahydrofuran acrylate. Core-shell structured elastic nanoparticles and hydrophobic nano-attapulgites modified with silane coupling agent were added. After high-speed pre-dispersion, the mixture was ground to a fineness of ≤5μm by a sand mill to obtain a filler pre-dispersion liquid. S2: Resin premix Fluorocarbon modified polyurethane acrylate oligomer, hexafunctional aliphatic polyurethane acrylate, tetrafunctional hydroxyl polyurethane acrylate and the remaining tetrahydrofuran acrylate were mixed and stirred at 55°C until completely transparent and homogeneous to obtain a resin mixture. S3: Packing material inlet Add the pre-dispersed filler solution obtained in step S1 to the resin mixture obtained in step S2, and stir to mix evenly; S4: Add crosslinking monomers and initiators Cool the system to below 40°C, add trimethylolpropane triacrylate and free radical photoinitiator under light-protected conditions, and stir at low speed until completely dissolved; S5: Adding additives Add fluorinated modified acrylate leveling agent and polymeric defoamer, and continue stirring to mix evenly; S6: Filtration and Packaging The mixture obtained in step S5 is filtered through a 1μm filter and sealed in a light-proof package to obtain the UV coating.
[0035] Preferably, in step S1, the grinding process using the sand mill uses zirconia beads with a particle size of 0.4 mm.
[0036] Preferably, the stirring time in step S3 is 20 min; the stirring time in step S4 is 15 min; and the stirring time in step S5 is 10 min.
[0037] Preferably, the application and curing process of the UV coating is as follows: The UV coating is applied to the surface of the substrate, and after leveling, it is UV cured under inert gas protection.
[0038] Specifically, the UV coating is applied to the surface of the substrate, the wet film thickness is controlled to be 20 μm, and after leveling at 55°C for 4 min, UV curing is performed using a high-pressure mercury lamp under nitrogen protection (oxygen content <500 ppm), with a lamp power of 100 W / cm and a cumulative exposure energy of 1000 mJ / cm².
[0039] The tetrafunctional hydroxyl polyurethane acrylate (B-6263) and THFA were omitted, the hexafunctional aliphatic polyurethane acrylate was increased to 30 parts, the trimethylolpropane triacrylate was increased to 20 parts, and the remaining parameters were exactly the same as in Example 2.
[0040] The core-shell structured elastic nanoparticles and silane coupling agent-modified hydrophobic nano-attapulgites were omitted, and 10 parts of unmodified nano-SiO2 (untreated hydrophilic fumed silica) were added. All other parameters were exactly the same as in Example 2.
[0041] The fluorinated acrylate leveling agent was replaced with an equal amount of BYK-333 (silicone leveling agent), and all other parameters were exactly the same as in Example 2.
[0042] The fluorocarbon modified polyurethane acrylate oligomer was omitted, and the hexafunctional aliphatic polyurethane acrylate was adjusted to 42 parts to keep the total resin content unchanged. The remaining parameters were exactly the same as in Example 2.
[0043] The hydrophobic nano-attapulgites modified with silane coupling agent were omitted, and the number of core-shell structured elastic nanoparticles was increased to 16, while the remaining parameters were exactly the same as in Example 2.
[0044] The core-shell structured elastic nanoparticles were omitted, and the amount of silane coupling agent-modified hydrophobic nano-attapulgites was increased to 16 parts, while the remaining parameters were exactly the same as in Example 2.
[0045] TPO was removed, and 184 was increased to 4 copies. All other parameters were exactly the same as in Example 2.
[0046] All components were added in one step and stirred at high speed for 30 minutes, but not in a sand mill. All other parameters were exactly the same as in Example 2.
[0047] The UV coatings in Examples 1-3 and Comparative Examples 1-8 were subjected to performance tests. The test methods are shown in Table 1, and the test results are shown in Table 2. Table 1 Test Project Test standards / methods Test conditions and equipment Pencil hardness ASTM D3363 Pencil hardness tester, 750g load, 45° scratch, Mitsubishi UNI hardness pencils (6B-9H). Adhesion ASTM D3359-17 Grid marking tool (1mm x 1mm, 100 grids), 3M 610 tape vertical peeling. Bending resistance ASTM D522 / D4145 MIT folding tester, R=2mm, 180°, 60 cycles / min abrasion resistance ASTM F2357 RCA paper tape abrasion tester, load 175g Water contact angle Seat drip method Contact angle measuring instrument, 2μL deionized water, stand at 25℃ for 30s Moist heat resistance Constant temperature and humidity chamber method Incubate at 65℃ / 95%RH for 72 hours, then remove and place at 25℃ for 2 hours. Curing shrinkage Density method <![CDATA[The pycnometer method is used to measure the liquid density ρ₁, and the water displacement method is used to measure the paint film density ρ₂]]> VOC content GB / T 23986 Gas chromatography Storage stability Accelerated aging method After being placed in a sealed oven at 50℃ for 7 days, the fineness and viscosity were measured. Chemical resistance Soaking method Soak at 25℃ for 24 hours with artificial sweat (pH=4.7), 50% ethanol, and hand cream. Optical properties (transmittance) UV-Vis spectrophotometry 15μm dry film (PC substrate), 400-800nm wavelength Optical performance (haze) Haze meter method 15μm dry film (PC substrate), standard haze meter Optical properties (gloss) ASTM D523 60° Gloss Meter Anti-fingerprint durability (dry wiping) Friction testing machine method Cotton cloth, 500g load, 500 water contact angle recordings up to 5000 times. Anti-fingerprint durability (alcohol rub-off) Friction testing machine method Anhydrous ethanol cotton swabs, 500g load, water contact angle recorded 100 times up to 500 times. QUV accelerates aging. GB / T 31895-2015 UVA-340, 60℃ / 8h illumination (0.89W / m²·nm) + 50℃ / 4h condensation, 500h Recoating / screen printing adhesion Hundred-grid method UV paint is sprayed onto the cured coating, and a cross-cut test is performed after curing. Table 2 Test Project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Pencil hardness 6H 6H 7H 7H 5H 5H 6H 5H 6H 5H 5H Adhesion (100-grid test) 5B 5B 5B 3B 4B 3B 3B 4B 5B 3B 3B Bending resistance (10,000 cycles, R=2mm) >30 >32 >28 8 15 10 15 12 20 14 10 RCA abrasion resistant (175g, per cycle) >500 >550 >600 >400 >300 >350 >450 >400 >500 >350 >320 Water contact angle (°) 107 110 112 75 98 102 90 108 112 110 98 Moist heat resistance ① pass pass pass Severe whitening white Slightly white white pass foaming Slightly white Slightly white Adhesion after humid heat 5B 5B 5B 2B 3B 3B 3B 5B 3B 3B 3B Curing shrinkage rate (%) 4.2 3.8 4.5 16.5 11.2 11.8 13.5 9.5 10.2 12.5 13.0 Storage stability ② qualified qualified qualified qualified coarse qualified qualified qualified qualified qualified coarse Light transmittance (%) 93.5 93.8 92.1 90.5 88.5 91.0 90.0 91.0 90.5 91.5 89.0 Haze (%) 0.8 0.7 1.0 1.5 3.2 1.8 2.0 1.5 1.2 1.8 3.5 60° gloss 98 99 97 92 82 93 90 93 95 92 85 Water contact angle (°) after 5000 dry rubbing cycles 104 106 108 — 85 92 — 104 108 106 104 Water contact angle (°) after 500 alcohol rubs 101 103 105 — 80 86 — 101 104 103 100 Recoating / screen printing adhesion 5B 5B 5B 5B 4B 3B 4B 5B 5B 4B 4B QUV light retention rate (500h, %) 92.5 93.1 91.8 80.5 83.5 87.0 85.0 90.0 92.5 87.5 84.0 QUV color difference ΔE (500h) 0.8 0.7 0.9 3.2 2.2 1.8 2.5 1.2 0.8 2.0 2.5 Among them: ① "Resistance to damp heat" evaluation criteria: After 72 hours at 65℃ / 95%RH, no whitening, no blistering, and adhesion ≥4B is "passed"; adhesion <4B or visible whitening / blistering is "failed", and the specific phenomena should be noted.
[0048] ② "Storage stability" evaluation criteria: After accelerated aging at 50℃ / 7d, a fineness change of ≤1μm and a viscosity change rate of <10% is considered "qualified"; a fineness change of >5μm or a viscosity change rate of >20% is considered "coarsening".
[0049] ③ Comparative Example 1 (without dual resin + THFA) and Comparative Example 4 (omitting fluorocarbon resin) have low water contact angles due to the lack of fluorocarbon resin (75° for Comparative Example 1 and 90° for Comparative Example 4), and do not have effective anti-fingerprint function. Therefore, anti-fingerprint durability test was not conducted.
[0050] By comparing the systems of Example 2 with those of Comparative Examples 1-8, the following conclusions can be drawn: 1. Each component in a quaternary gradient resin system is indispensable. Comparative Example 1 (a tetrafunctional hydroxyl-containing polyurethane acrylate lacking tetrafunctionality + tetrahydrofuran acrylate) resulted in high shrinkage and brittle fracture; Comparative Example 4 (omitting the fluorocarbon-modified polyurethane acrylate oligomer) caused the water contact angle to plummet from 110° to 90°, folding endurance to drop from >320,000 cycles to 150,000 cycles, and adhesion to decrease from 5B to 3B. The fluorocarbon-modified polyurethane acrylate oligomer not only contributes to anti-fingerprint properties, but its synergistic network structure of rigid fluorocarbon segments and flexible polyurethane segments also participates in the regulation of mechanical properties—the introduction of fluorocarbon segments changes the microscopic phase separation morphology of the crosslinking network, making the stress distribution more uniform. The "rigid-flexible" synergistic effect produced by the quaternary gradient resin compound cannot be achieved by single or ternary systems. After omitting the fluorocarbon-modified polyurethane acrylate oligomer, the proportion of rigid segments in the crosslinking network is too high and the proportion of flexible segments is insufficient, leading to stress concentration, increased shrinkage, and decreased flexibility. The hydroxyl groups on the tetrafunctional hydroxyl polyurethane acrylate molecule can form intermolecular hydrogen bonds with the urethane groups on the fluorocarbon modified polyurethane acrylate molecule. These hydrogen bonds act as auxiliary compatibility bridges, mitigating the phase separation tendency between the fluorocarbon segments and the polyurethane matrix. This is one of the key factors enabling this system to increase the fluorocarbon resin addition to 25-35 parts without significantly deteriorating mechanical properties. The fluorocarbon modified polyurethane acrylate itself carries polyurethane segments, which share chemical structural similarities with the tetrafunctional hydroxyl polyurethane acrylate, providing basic compatibility for this system. The hydrogen bonding further strengthens the interfacial bonding between the two phases, and together they ensure the homogeneous stability of the resin system.
[0051] 2. The combined use of core-shell structured elastic nanoparticles and hydrophobically modified attapulgite exhibits superior overall performance compared to adding either filler alone, demonstrating a synergistic effect. Comparative Example 5, with only core-shell particles, shows insufficient coating hardness, while Comparative Example 6, with only attapulgite, shows deteriorated adhesion after hydrothermal treatment (omitting the core-shell particles significantly alters the total solids content and resin / filler ratio, potentially affecting the exposure of the attapulgite on the coating surface. The lack of a significant increase in water contact angle indicates that excessive attapulgite is embedded in the resin and not effectively exposed on the surface). The combined system demonstrates that the overall performance of either filler alone is inferior to that of the combined system.
[0052] 3. The "fluorine-fluorine homologous" surface design is key to fingerprint resistance and compatibility with recoating processes. Comparative Example 3 (organosilicon leveling agent) showed a reduced water contact angle and severely deteriorated recoating adhesion.
[0053] 4. A compound initiation system of acylphosphine oxide initiators and α-hydroxy ketone initiators is essential for the uniform curing of thick coatings containing fillers. Comparative Example 7 (using a single α-hydroxy ketone initiator) suffered from a comprehensive performance degradation due to insufficient deep curing.
[0054] 5. The three-stage process of "pre-dispersion-milling-inoculation" is a prerequisite for the proper functioning of nanofillers. Comparative Example 8 (one-step method) suffers from severe degradation of optical properties and storage stability due to filler agglomeration.
[0055] 6. This formulation system, combined with the above five key design elements, enables a single-layer coating to simultaneously achieve comprehensive performance characteristics such as hardness ≥6H, flexural resistance >300,000 cycles, water contact angle >105°, and no abnormalities after 72 hours of humid heat at 65℃ / 95%RH. The system contains no solvent-based active diluents, meeting low-VOC environmentally friendly coating standards. The comparative results of each group show that the absence of any one of the key components significantly reduces at least one core performance characteristic of the paint film, demonstrating the holistic and unique advantages of the formulation's component combination.
[0056] It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.
Claims
1. A UV coating, characterized in that, By weight, it includes the following components: 25-35 parts of fluorocarbon-modified polyurethane acrylate oligomer. 10-15 parts of hexafunctional aliphatic polyurethane acrylate 20-30 parts of tetrafunctional hydroxyl polyurethane acrylate 25-35 parts of tetrahydrofuran acrylate 3-5 parts of trimethylolpropane triacrylate 5-8 parts of core-shell structured elastic nanoparticles 5-8 parts of silane coupling agent-modified hydrophobic nano-attapulgites 3-5 parts of free radical photoinitiator 1.5-2.5 parts of polymeric dispersant. Fluorine-modified acrylate leveling agent, 0.2-0.5 parts. Polymer-type defoamer 0.2-0.4 parts.
2. The UV coating as described in claim 1, characterized in that: The core-shell structured elastic nanoparticles are polybutadiene core / polymethyl methacrylate shell structures with a particle size of 80-120 nm and a core glass transition temperature below -40°C.
3. The UV coating as described in claim 1, characterized in that, The silane coupling agent-modified hydrophobic nano-attapulgites were prepared by the following method: (1) Vacuum dry the attapulgite at 100-130℃ for 3-5 hours; (2) Dissolve KH-570 silane coupling agent in a mixed solvent of ethanol / water volume ratio of 95:5, adjust the pH to 4-5 with acetic acid, and hydrolyze for 20-40 min; (3) Disperse the dried attapulgite in the hydrolysate obtained in step (2) with a solid-liquid ratio of 1:8-1:12 and reflux at 70-90℃ for 4-6 hours; (4) Separate, wash, dry and grind to obtain hydrophobic nano-attapulgites.
4. The UV coating as described in claim 1, characterized in that: The free radical photoinitiator is a compound system of acylphosphine oxide initiator and α-hydroxy ketone initiator, wherein the mass ratio of acylphosphine oxide initiator to α-hydroxy ketone initiator is 1:0.8-1:1.2; the acylphosphine oxide initiator is selected from at least one of TPO, TEPO or BAPO, and the α-hydroxy ketone initiator is 184.
5. A UV coating as described in claim 1, characterized in that: The polymeric dispersant is an anchoring polyurethane dispersant; The fluorinated modified acrylate leveling agent is selected from at least one of Rieter LD-91084 or BYK-349; The polymeric defoamer is selected from at least one of BYK-1795 or BYK-A530.
6. A method for preparing a UV coating as described in any one of claims 1-5, characterized in that, Includes the following steps: S1: Preparation of filler predispersion liquid A polymeric dispersant was dissolved in tetrahydrofuran acrylate, which accounted for 40-50% of the total weight of tetrahydrofuran acrylate. Core-shell structured elastic nanoparticles and hydrophobic nano-attapulgites modified with silane coupling agent were added. After high-speed pre-dispersion, the mixture was ground to a fineness of ≤5μm by a sand mill to obtain a filler pre-dispersion liquid. S2: Resin premix Fluorocarbon modified polyurethane acrylate oligomer, hexafunctional aliphatic polyurethane acrylate, tetrafunctional hydroxyl polyurethane acrylate and the remaining tetrahydrofuran acrylate are mixed and stirred at 50-60℃ until completely transparent and homogeneous to obtain a resin mixture. S3: Packing material inlet Add the pre-dispersed filler solution obtained in step S1 to the resin mixture obtained in step S2, and stir to mix evenly; S4: Add crosslinking monomers and initiators Cool the system to below 40°C, add trimethylolpropane triacrylate and free radical photoinitiator under light-protected conditions, and stir at low speed until completely dissolved; S5: Adding additives Add fluorinated modified acrylate leveling agent and polymeric defoamer, and continue stirring to mix evenly; S6: Filtration and Packaging The mixture obtained in step S5 is filtered through a 1μm filter and sealed in a light-proof package to obtain the UV coating.
7. The method for preparing a UV coating as described in claim 6, characterized in that: In step S1, the grinding process in the sand mill uses zirconia beads with a particle size of 0.3-0.5 mm.
8. The method for preparing a UV coating as described in claim 6, characterized in that: The stirring time for step S3 is 15-30 min; the stirring time for step S4 is 10-20 min; and the stirring time for step S5 is 5-15 min.
9. The method for preparing a UV coating as described in claim 6, characterized in that, The application and curing process of the UV coating is as follows: The UV coating is applied to the surface of the substrate, and after leveling, it is UV cured under inert gas protection.
10. The application of a UV coating as described in any one of claims 1-5 in the surface coating of electronic device housings, foldable screen mobile phones or 5G devices.
Citation Information
Patent Citations
A kind of UV double-curing high-gloss paint and preparation method thereof
CN116285653B